Abstract
Laser powder bed fusion (LPBF) Ti–6Al–4V shows orientation-dependent fatigue behavior that tensile properties and bulk density do not fully explain. Vertical (VT) and horizontal (HZ) specimens were annealed at 850 °C for 2 h (furnace cooling) and characterized by optical and scanning electron microscopy, X-ray diffraction (XRD) with Rietveld refinement, micro-computed tomography (micro-CT), Vickers hardness, tensile tests, and high-cycle fatigue tests (R = 0.1). The annealed material consisted of α + β (approximately 88–92 vol.% α and 8–12 vol.% β). Tensile properties of the two orientations were similar, with HZ specimens slightly stronger and of similar elongation. Despite a bulk density above 99.9%, micro-CT revealed isolated pores of roughly 60–270 μm. At 600 MPa, VT specimens failed after 6.79 × 104 and 7.36 × 104 cycles, whereas HZ specimens failed after 8.82 × 105 and 1.37 × 106 cycles. Fatigue data at other stress levels are limited, so the orientation effect is demonstrated only at 600 MPa, where two specimens per orientation were tested. The results indicate that defect size, morphology, and orientation relative to the load, rather than tensile properties or density, are the likely cause of the anisotropy. An orientation-sensitive descriptor, F = dmax cos2θ, is proposed as a hypothesis; specimen-resolved defect data exist for only three VT specimens, so it remains to be validated. No as-built control was tested, and conclusions apply to the annealed condition.
1. Introduction
Ti–6Al–4V is one of the most widely used engineering alloys for biomedical, aerospace, and high-performance structural applications because of its specific strength, corrosion resistance, biocompatibility, and fatigue resistance [1,2,3,4]. Demand for patient-specific implants and geometrically complex components has accelerated the adoption of laser powder bed fusion (LPBF), also known as selective laser melting (SLM), for Ti–6Al–4V [5,6,7,8,9,10,11]. In this paper, the term LPBF is used throughout.
LPBF offers near-net-shape manufacturing with great design freedom [2,3,12]. However, the rapid melting and solidification cycles generate acicular α′ martensite, elongated prior-β grains, residual stresses, and process-induced defects such as gas pores, keyhole pores, and lack-of-fusion (LOF) defects [2,3,13,14,15]. Defect formation is governed by the combination of laser power, scan speed, hatch spacing, layer thickness, powder characteristics, and the stability of the melt pool, so that the process window for fully dense material is narrow and stochastic events (spatter, recoating irregularities) can still produce isolated large defects [15,16,17]. Such defects are difficult to detect in-process and, in fatigue-critical applications, they determine component reliability [17,18].
Tensile properties of LPBF Ti–6Al–4V have been studied extensively, but fatigue performance remains a concern because it is controlled by local defects rather than bulk properties [10,13,18,19,20,21]. Pores, LOF defects, and unmelted particles act as stress concentrators, so specimens with similar tensile strength can show very different fatigue lives depending on defect size, morphology, and orientation [18,20,21,22,23,24,25]. Build orientation affects fatigue through grain morphology, layer interfaces, and the alignment of defects relative to the loading direction [26,27,28,29,30,31,32]. Vertically built specimens, whose loading axis is parallel to the build direction, often have shorter lives because planar LOF defects lie in the layer planes, perpendicular to the load [26,28,32].
Post-build heat treatment is routinely used to relieve residual stress. Sub-β-transus annealing decomposes the metastable α′ martensite into α + β and improves ductility, but it cannot close internal defects, which requires processes such as hot isostatic pressing [33]; see also [34,35,36,37,38,39,40,41,42]. After annealing, the fatigue response is therefore expected to depend mainly on the defect population.
Traditional defect-based approaches such as Murakami’s √area parameter and Kitagawa–Takahashi analysis describe defect size well but do not explicitly account for defect orientation relative to the load [24,43]. Here, “defect-related” anisotropy means that the orientation dependence of fatigue life persists although the tensile properties and bulk density of the two orientations are nearly equal, and that it coincides with differences in the defects seen by micro-CT and fractography. This differs from conventional orientation-related anisotropy, which is usually attributed to texture, grain morphology, or tensile property differences. The present work therefore combines micro-CT, fractography, Weibull analysis, and √area estimates to examine how defects relate to the fatigue lives of annealed VT and HZ specimens, and it proposes an orientation-sensitive descriptor as a hypothesis for further validation.
2. Materials and Methods
2.1. Material and LPBF Fabrication
Ti–6Al–4V blocks (72 mm × 13 mm × 13 mm) were fabricated on an EOSINT M280 system (EOS GmbH, Krailling, Germany) in vertical (VT) and horizontal (HZ) orientations using identical, optimized processing parameters for all specimens (Table 1). For VT specimens, the long axis of the block, and later the loading axis, was parallel to the build direction; for HZ specimens, it was perpendicular to the build direction. The complete experimental sequence is summarized in Figure 1a.
Table 1.
LPBF processing parameters and post-processing conditions.
Figure 1.
(a) Experimental workflow with the main LPBF parameters. (b) Geometry of the machined tensile/fatigue specimens (ASTM E8/E8M [44]); gauge diameter 4.4 mm, gauge length 25 mm.
The volumetric energy density, VED = P/(vht), is approximately 78 J/mm3 and lies in the range reported to give near-full density in LPBF Ti–6Al–4V [2,13,18,20,21,34,35]. The rotating scan strategy was used to reduce texture and residual stress accumulation.
2.2. Heat Treatment
All specimens were vacuum annealed at 850 °C for 2 h and furnace cooled. The temperature lies below the β-transus of Ti–6Al–4V (approximately 940 °C for the present material), so the α + β phase field is retained and coarse prior-β grains and thick lamellar α, which impair ductility and fatigue resistance, are avoided. Annealing in this range is widely used for LPBF Ti–6Al–4V to decompose α′ martensite and relieve residual stress [34,35,36,40,41]. Because the original aim was to study the heat-treated condition relevant to implants, no as-built specimens were tested.
2.3. Density, Porosity, and Micro-CT
Density was determined by the Archimedes method and porosity was analyzed by micro-CT. Scans were acquired at the Central Analytical Facilities, Stellenbosch University (Stellenbosch, South Africa), at a voxel size of approximately 8–12 μm. Pore size distributions are given as pore diameter, and pore sphericity is also reported. For selected defects, the maximum dimension dmax and the principal-axis orientation were extracted from the reconstructed three-dimensional data with image analysis software. The measurement uncertainty was estimated as ±2 voxels, i.e., approximately ±20 µm for the larger defects. Defects smaller than about 2–3 voxels cannot be resolved reliably.
The orientation of a defect is described by the angle αp between its principal (longest) axis and the loading axis. For flat LOF defects, the angle θ between the defect-plane normal and the loading axis is θ = 90° − αp; θ = 0° means that the defect plane is perpendicular to the load and fully opens under tension.
2.4. Microstructure and Hardness
Sections were cut parallel and perpendicular to the build direction, mounted in conductive resin, ground (320–1200 grit SiC), polished with 1 µm diamond suspension, and etched with Kroll’s reagent (2% HF, 6% HNO3, 92% water) for 10–15 s. Optical microscopy (BX51M, Olympus Corporation, Hachioji, Japan) and SEM (JSM-IT500, JEOL Ltd., Akishima, Japan) were used to examine the α/β morphology. The α-lath thickness was measured by the linear intercept method. Vickers microhardness was measured according to ASTM E384 [45] (Falcon 500, INNOVATEST Europe BV, Maastricht, The Netherlands; HV0.5, 500 gf, 15 s dwell) with at least five indentations per specimen along the line shown in Section 3.2, and reported as mean ± standard deviation.
2.5. X-Ray Diffraction and Rietveld Refinement
XRD patterns of the annealed material were recorded on a Shimadzu diffractometer (Shimadzu Corporation, Kyoto, Japan) with Cu Kα radiation (λ = 1.5406 Å) over 2θ = 30–90° with a step of 0.02°. Phases were identified by comparison with the International Centre for Diffraction Data (ICDD) PDF cards for α-Ti (hcp, PDF 44-1294) and β-Ti (bcc, PDF 44-1288). Phase fractions and lattice parameters were obtained by Rietveld refinement using α-Ti and β-Ti structure models, refining background, scale factors, lattice parameters, and peak-shape parameters, with a preferred-orientation correction where necessary. Crystallite size was estimated from peak broadening using a Williamson–Hall approach after instrumental correction with a standard reference material. Only the annealed condition was measured.
2.6. Mechanical Testing and Fractography
Cylindrical specimens (gauge diameter 4.4 mm, gauge length 25 mm; Figure 1b) were machined according to ASTM E8/E8M [44] and tested on an Instron servo-hydraulic machine (Instron, Norwood, MA, USA). Tensile tests followed ISO 6892-1:2019 [46] and ASTM E8/E8M [44] at a crosshead rate of 0.5 mm/min; three specimens per orientation were tested. High-cycle fatigue tests followed ASTM E466-15 [47] and ISO 1099:2017 [48] under load control with a sinusoidal waveform at 10 Hz and R = 0.1, up to 2 × 106 cycles or failure. Six VT and five HZ specimens were tested. The maximum stress levels were not identical for the two orientations (Section 3.5), so a direct comparison is possible only at 600 MPa, where two specimens per orientation were tested. Fracture surfaces were examined by SEM.
2.7. Statistical and Defect Analyses
Fatigue-life scatter was described with a two-parameter Weibull distribution fitted by maximum likelihood. The Murakami parameter was computed as √area = √A, with A the projected defect area; where only dmax was available, a circular equivalent A = πd2/4 was assumed, giving √area = 0.8862 dmax.
3. Results and Discussion
3.1. Microstructure of the Annealed Material
Figure 2 shows the annealed microstructure: elongated α laths and retained β, together with some equiaxed α, on planes parallel and perpendicular to the build direction. The transverse planes (VTx and HZx) show a fairly uniform mixture of elongated and equiaxed α, with longer α laths in VTx. The axial plane of HZ (HZy) shows thinner laths than its transverse plane. The α-lath thickness from the linear intercept method was approximately 1.2–1.5 µm for HZ and 1.6–1.9 µm for VT, i.e., only a small orientation difference. No excessive grain coarsening was observed, consistent with annealing below the β-transus. The prior-β grains are expected to remain columnar along the build direction, particularly in VT specimens [2,3,13,26,27,32].
Figure 2.
Optical and SEM micrographs of annealed LPBF Ti–6Al–4V: (a) VT axial plane (VTz), (b) VT transverse plane (VTx), (c) HZ axial plane (HZy), (d) HZ transverse plane (HZx). Elongated α laths, retained β, and equiaxed α are indicated. Scale bars: 50 µm.
Because no as-built specimens were examined in this study, the decomposition of the as-built α′ martensite is inferred from the literature on LPBF Ti–6Al–4V annealed in this temperature range [34,35,36,40,41] and from the α + β microstructure and phase composition reported here (Section 3.8), not from a direct before-and-after comparison.
3.2. Microhardness
The mean hardness of the annealed specimens was approximately 350 HV0.5 for VT and 340 HV0.5 for HZ, with standard deviations of about 3–4 HV (five indentations each, positions in Figure 3). The difference is small and comparable with the scatter, so no orientation effect on hardness is claimed. For reference, as-built LPBF Ti–6Al–4V typically exhibits higher hardness (about 380–420 HV) because of the α′ martensite [34,35,36]; this value is taken from the literature and was not measured here.
Figure 3.
Layout of the Vickers (HV0.5) indentations on the polished and etched sections of VT and HZ specimens: five indents along a line with equal spacing of at least 2.5 diagonal lengths. Black arrows indicate the build direction; the red line marks the line of indentation.
3.3. Porosity and Internal Defects
Archimedes and micro-CT measurements gave a relative density above 99.9% for both orientations. The micro-CT analysis in Figure 4 gives a relative density of 99.9993% for VT and 99.9992% for HZ, consistent with the reported >99.9%. The pores in Figure 4 are therefore sparse in volume terms; the figure reports their diameter and sphericity, not their volume fraction.
Figure 4.
Micro-CT analysis of annealed LPBF Ti–6Al–4V: (a) VT and (b) HZ specimens. Pore size is col-or-coded; cross-sectional slices, enlarged views of irregular LOF pores (>100 µm) and small spherical pores (<100 µm), and pore size distributions are shown.
Pores persist in both orientations: their diameters are about 90–200 µm in VT and 60–270 µm in HZ, and their sphericity (about 0.5–0.7) decreases with increasing pore size, i.e., smaller pores are more spherical. Notably, the HZ specimens contain more pores and a wider range of pore sizes than the VT specimens, yet they have the longer fatigue lives (Section 3.5). Pore size and volume fraction alone therefore cannot explain the fatigue anisotropy, which points to defect shape and orientation relative to the load as additional factors [18,20,21]. The occurrence of isolated large pores in otherwise dense material is consistent with the narrow LPBF process window: the VED of about 78 J/mm3 lies within the range reported for Ti–6Al–4V, but local variations in melt pool stability, powder packing, and spatter can still produce isolated LOF pores even under optimized parameters [16,17,49]. Porosity-related stress concentration also reduces tensile properties and fatigue resistance [19,34,50].
3.4. Tensile Properties
The tensile properties of the annealed VT and HZ specimens were similar (Figure 5, Table 2). HZ specimens showed slightly higher strength and similar elongation: the representative curves give a yield strength of about 880 MPa (VT) and 920 MPa (HZ), an ultimate tensile strength of about 995 MPa (VT) and 1065 MPa (HZ), and an elongation of about 14.2% (VT) and 16.3% (HZ). The mean values and standard deviations of the three specimens per orientation are listed in Table 2. The difference in UTS between orientations is about 1.5%, so the combination of optimized parameters and annealing yields limited tensile anisotropy. The slightly higher HZ values may be related to the orientation of layer interfaces and defects relative to the load [26,32].
Figure 5.
Engineering stress–strain curves of annealed LPBF Ti–6Al–4V for (a) VT and (b) HZ specimens (representative curves; three specimens per orientation were tested, see Table 2).
Table 2.
Tensile properties of annealed LPBF Ti–6Al–4V (mean ± standard deviation, n = 3 per orientation).
Despite these small tensile differences, a pronounced fatigue anisotropy remained after annealing (Section 3.5), so tensile properties alone do not explain the fatigue behavior.
3.5. Fatigue Behavior
Maximum stresses, lives, and specimen labels are given in Table 3 and Table 4 and plotted in Figure 6. All specimens failed before the 2 × 106-cycle limit, so there are no run-outs. The orientation effect is clear at 600 MPa, the only level with replicate tests in both orientations: the two VT specimens failed after 7.36 × 104 and 6.79 × 104 cycles, whereas the two HZ specimens failed after 1.37 × 106 and 8.82 × 105 cycles, i.e., roughly 12–20 times longer. At other stress levels, the comparison is less direct because the levels differ between orientations. HZ specimens tested at 550 MPa lasted 4.20 × 105 and 7.61 × 105 cycles, whereas a VT specimen at the higher stress of 570 MPa lasted 2.03 × 105 cycles. At 540 MPa, however, the single HZ specimen failed earlier (1.45 × 105 cycles) than the single VT specimen (1.42 × 106 cycles), and one VT specimen at 640 MPa outlasted both VT specimens at 600 MPa. These results illustrate the large scatter typical of defect-controlled fatigue and show that more tests at common stress levels are needed before an S–N curve or an endurance limit can be defined. No clear endurance limit was observed in the tested range.
Table 3.
Fatigue test data for VT specimens (R = 0.1, 10 Hz).
Table 4.
Fatigue test data for HZ specimens (R = 0.1, 10 Hz).
Figure 6.
Fatigue data (maximum stress versus cycles to failure, R = 0.1) of annealed VT and HZ specimens. All specimens failed; the dotted line marks the 2 × 106-cycle test limit.
Fatigue-life scatter was assessed with a two-parameter Weibull analysis of the lives in Table 3 and Table 4. The maximum-likelihood Weibull moduli are approximately 0.87 (VT) and 1.73 (HZ), indicating greater scatter in the VT group, and the characteristic life is higher for HZ (about 8.0 × 105 versus 3.2 × 105 cycles). Because the lives pooled in each group were obtained at different stress levels and the groups are small (six and five specimens), the moduli also contain the effect of stress and should be regarded as descriptive only.
3.6. Fractography
SEM fractographs of VT and HZ specimens (Figure 7 and Figure 8) show the features typical of fatigue failure of Ti–6Al–4V: fatigue striations (fine parallel ridges perpendicular to the local crack-growth direction), secondary cracks, ductile dimples and voids (cup-like cavities) in the final-fracture region, and defect-like cavities. These features were identified from their morphology according to the literature [18,20,21,26,32] and are marked in the images; the regions of interest (ROI) are small areas of the fracture surfaces. The images show that cavities and cracks occur on the fracture surfaces of both orientations; they do not by themselves establish the initiation site of each specimen. The link between crack initiation and large defects is therefore supported by the micro-CT defect sizes and by published observations on LPBF Ti–6Al–4V [18,20,21], and is treated here as consistent with, but not proven by, the present fractographs.
Figure 7.
SEM fractographs of fatigue-tested VT specimens: (a) ROI 3, dimples and a void; (b) ROI 1, cracks; (c) ROI 2, dimples and a defect; (d) fatigue striations and crack growth with cracks. Scale bars: (a) 20 µm, (b) 50 µm, (c) 20 µm, (d) 10 µm.
Figure 8.
SEM fractographs of fatigue-tested HZ specimens: (a) ROI 3, dimples and a void; (b) ROI 1, crack path (white line); (c) cracks and dimples; (d) striations, a crack, and a defect. Scale bars: (a) 20 µm, (b) 50 µm.
Both orientations show ductile final fracture with dimples and voids and fatigue striations in the propagation region. In the HZ specimens, the crack path appears to follow the layer arrangement, which may contribute to slower crack growth.
3.7. Relation Between Defects and Fatigue Life
The defects expected to be most harmful are large LOF defects lying in the layer planes. In VT specimens, these planes are perpendicular to the loading axis, so the defects are fully opened by the applied stress, whereas in HZ specimens the layer planes are parallel to the loading axis and the same defects are loaded much less severely [18,20,26,28,32]. This is consistent with the shorter VT lives at 600 MPa despite smaller porosity and fewer large pores in VT (Section 3.3).
Specimen-resolved defect measurements are available only for specimens VT1–VT3 (Table 5); no corresponding HZ data are available yet. The √area values follow from dmax as described in Section 2.7. Because the specimens were tested at different stresses (570, 590, and 600 MPa), the comparison of defect size and life in Table 5 is confounded by stress: the largest defect (VT3, 190 µm) is associated with the shortest life, but this was also the highest stress. This three-point dataset is therefore insufficient for a regression or for a statistically robust defect–life relationship, and no regression coefficients are reported.
Table 5.
Specimen-resolved critical-defect data from micro-CT for VT1–VT3 and the derived quantities (±: estimated uncertainty).
An orientation-sensitive descriptor is considered in the form F = dmax g(θ), where g(θ) is an orientation weighting function and θ is defined in Section 2.3. For a flat defect whose normal makes an angle θ with the loading axis, the normal stress resolved on the defect plane is proportional to cos2θ. The simplest choice, g(θ) = cos2θ, gives F = dmax cos2θ. The descriptor is phenomenological, motivated by the orientation dependence of the crack-opening stress, and is not a derivation from linear elastic fracture mechanics. It can be compared with the Murakami parameter √area, whose small-defect approximation gives ΔK ≈ 0.65 Δσ √(π√area) for surface defects. The appropriate coefficient depends on whether the defect is internal, subsurface, or surface-connected, and on its morphology; the defect location relative to the surface was not determined here, so no ΔK or ΔKth comparison is made.
For VT1–VT3 the defects are nearly perpendicular to the load (θ ≤ 8°), so cos2θ ≈ 0.98–1.00 and F is practically equal to dmax. The data therefore do not yet allow F to be distinguished from dmax or √area. The value of the orientation term can be tested only when defects in HZ specimens, where θ is expected to be larger, and in the remaining VT specimens are included. The descriptor is therefore proposed as a hypothesis. It was derived for the annealed condition only; because no as-built fatigue specimens were tested, its applicability to as-built material is not known.
3.8. Phase Analysis by XRD
Figure 9 shows the XRD pattern of the annealed material together with the reference positions of the α-Ti (PDF 44-1294) and β-Ti (PDF 44-1288) cards. The strong reflections at 2θ ≈ 35.1°, 38.4°, 40.1°, 53.0°, and 70.4° are indexed as α-(10-10), (0002), (10-11), (10-12), and (10-13). The weaker reflection at 55.5° is tentatively assigned to β-(200), and the shoulder on the low-angle side of the α-(10-13) peak (about 69.6°) is assigned to β-(211); the β-(110) reflection (≈39.5°) overlaps the α-(0002) and α-(10-11) peaks. The pattern is therefore consistent with α and β reflections, but the β assignments are tentative because the β peaks are weak and overlap α reflections. The α-(11-20) reflection (≈63°) is not resolved and the relative intensities differ from the powder card, which suggests a preferred orientation (texture) of the α phase.
Figure 9.
XRD pattern of annealed LPBF Ti–6Al–4V with indexed reflections. The reference positions of α-Ti (ICDD PDF 44-1294, hcp) and β-Ti (ICDD PDF 44-1288, bcc) are shown below the pattern; the β-Ti positions were calculated from the cubic cell.
Rietveld refinement gave approximately 88–92 vol.% α and 8–12 vol.% β (Table 6), which should be regarded as a semi-quantitative estimate. The ranges reflect the limited precision of the quantification of the small, weakly diffracting β fraction in a textured sample. The agreement indices were Rp = 7.2%, Rwp = 9.1%, Rexp = 6.4%, χ2 = 2.02, and GOF = 1.42, which indicates an acceptable fit of the α + β model. The refined lattice parameters of α-Ti were a ≈ 2.93 Å and c ≈ 4.68 Å (c/a ≈ 1.60). The crystallite size of the α phase estimated from peak broadening was approximately 200–350 nm.
Table 6.
Results of the Rietveld refinement of the XRD pattern of annealed LPBF Ti–6Al–4V.
A single XRD pattern of the annealed condition cannot show phase evolution, peak narrowing, or a change in microstrain, because no as-built pattern was measured; no such statements are made. Moreover, α′ and α are both hexagonal with very similar lattice parameters, so laboratory XRD alone cannot confirm the α′ → α + β transformation. What the pattern suggests is the presence of a small fraction of retained β (about 8–12 vol.%, semi-quantitative) and of a dominant α phase, which together with the lamellar α + β microstructure (Figure 2) is consistent with the expected result of sub-β-transus annealing [34,35,36,40,41]. The absence of β-derived coarse lamellae and of peak splitting is consistent with an annealing temperature below the β-transus.
3.9. Limitations
- i.
- No as-built control was tested, so the effect of the annealing treatment itself on hardness, tensile, and fatigue properties was not measured and the 850 °C/2 h condition was not compared with other heat treatments.
- ii.
- Replicates in both orientations exist only at 600 MPa.
- iii.
- Specimen-resolved defect data exist for three VT specimens only.
- iv.
- The Weibull moduli combine different stress levels. These limitations restrict the conclusions to the annealed condition and the trends described above.
4. Conclusions
Annealed (850 °C, 2 h) LPBF Ti–6Al–4V specimens built vertically and horizontally were compared by microstructural, defect, tensile, and fatigue testing. The main findings are:
- The annealed material consisted of α laths and retained β; XRD with Rietveld refinement gave approximately 88–92 vol.% α and 8–12 vol.% β. The α-lath thickness was 1.2–1.5 µm (HZ) and 1.6–1.9 µm (VT), and the hardness was about 340–350 HV0.5 for both orientations.
- Tensile properties of the two orientations differed only by a few percent (mean UTS of 959 MPa for VT and 973 MPa for HZ), whereas the fatigue lives at 600 MPa differed by roughly an order of magnitude (6.79 × 104–7.36 × 104 cycles for VT versus 8.82 × 105–1.37 × 106 cycles for HZ).
- Micro-CT gave a relative density of 99.9993% (VT) and 99.9992% (HZ), but isolated pores of about 90–200 µm (VT) and 60–270 µm (HZ) persisted. The HZ specimens contained more pores and a wider size range yet lasted longer, which indicates that defect shape and orientation relative to the load, rather than porosity or tensile strength, is the likely origin of the anisotropy.
- The orientation effect was observed only at 600 MPa (two specimens per orientation); at 540 MPa the single HZ specimen failed earlier than the single VT specimen. Weibull moduli (0.87 for VT and 1.73 for HZ) are descriptive because stress levels were pooled.
- The descriptor F = dmax cos2θ is proposed as a hypothesis. For the three VT defects measured (dmax = 140–190 µm, θ ≤ 8°), F ≈ dmax, so validation requires specimen-level defect data, including HZ specimens, and fatigue tests at common stress levels, together with as-built control specimens.
Author Contributions
Conceptualization, F.O.O.; methodology, F.O.O.; software, F.O.O.; validation, F.O.O.; formal analysis, F.O.O.; investigation, F.O.O.; data curation, F.O.O.; writing—original draft preparation, F.O.O.; writing—review and editing, F.O.O. and M.W.; visualization, F.O.O.; supervision, M.W.; project administration, F.O.O.; funding acquisition, M.W. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Acknowledgments
The authors gratefully acknowledge the support of Durban University of Technology (DUT), South Africa, for providing the institutional environment and support.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Gibson, I.; Rosen, D.W.; Stucker, B. Additive Manufacturing Technologies: 3D Printing, Rapid Prototyping, and Direct Digital Manufacturing, 3rd ed.; Springer: New York, NY, USA, 2021. [Google Scholar]
- DebRoy, T.; Wei, H.L.; Zuback, J.S.; Mukherjee, T.; Elmer, J.W.; Milewski, J.O.; Beese, A.M.; Wilson-Heid, A.; De, A.; Zhang, W. Additive manufacturing of metallic components—Process, structure and properties. Prog. Mater. Sci. 2018, 92, 112–224. [Google Scholar] [CrossRef] [Scilit]
- Herzog, D.; Seyda, V.; Wycisk, E.; Emmelmann, C. Additive manufacturing of metals. Acta Mater. 2016, 117, 371–392. [Google Scholar] [CrossRef] [Scilit]
- Frazier, W.E. Metal additive manufacturing: A review. J. Mater. Eng. Perform. 2014, 23, 1917–1928. [Google Scholar] [CrossRef] [Scilit]
- Abd-Elaziem, W.; Darwish, M.A.; Hamada, A.; Daoush, W.M. Titanium-based alloys and composites for orthopedic implants. Mater. Des. 2024, 241, 112850. [Google Scholar] [CrossRef] [Scilit]
- Wu, Y.; Liu, J.; Kang, L.; Tian, J.; Zhang, X.; Hu, J.; Huang, Y.; Liu, F.; Wang, H.; Wu, Z. 3D-printed metal implants in orthopedics: Present and future. Heliyon 2023, 9, e17718. [Google Scholar] [CrossRef] [Scilit]
- Bocchetta, P.; Chen, L.-Y.; Tardelli, J.D.C.; Reis, A.C.d.; Almeraya-Calderón, F.; Leo, P. Passive Layers and Corrosion Resistance of Biomedical Ti-6Al-4V and β-Ti Alloys. Coatings 2021, 11, 487. [Google Scholar] [CrossRef] [Scilit]
- Al-Shalawi, F.D.; Mohamed Ariff, A.H.; Jung, D.-W.; Mohd Ariffin, M.K.A.; Kim, C.L.S.; Brabazon, D.; Al-Osaimi, M.O. Biomaterials as implants in the orthopedic field for regenerative medicine: Metal versus synthetic polymers. Polymers 2023, 15, 2601. [Google Scholar] [CrossRef] [Scilit]
- Kim, T.; See, C.W.; Li, X.; Zhu, D. Orthopedic implants and devices for bone fractures and defects: Past, present and perspective. Eng. Regen. 2020, 1, 6–18. [Google Scholar] [CrossRef] [Scilit]
- Rouf, S.; Malik, A.; Singh, N.; Raina, A.; Naveed, N.; Siddiqui, M.I.H.; Haq, M.I.U. Additive manufacturing technologies for industrial and medical applications. Sustain. Oper. Comput. 2022, 3, 258–274. [Google Scholar] [CrossRef] [Scilit]
- Tang, Z.; Zhou, Y.; Ma, L.; Li, J. Flow performance of porous implants with different geometry: Line, surface, and volume structures. Int. J. Bioprint. 2023, 9, 700. [Google Scholar] [CrossRef] [Scilit]
- Gu, D. Laser Additive Manufacturing of High-Performance Materials; Springer: Berlin/Heidelberg, Germany, 2015. [Google Scholar]
- Becker, T.H.; Beck, M.; Scheffer, C. Microstructure and mechanical properties of direct metal laser sintered Ti–6Al–4V. S. Afr. J. Ind. Eng. 2015, 26, 1–10. [Google Scholar] [CrossRef] [Scilit]
- Narasimharaju, S.R.; Zeng, W.; See, T.L.; Zhu, Z.; Scott, P.; Jiang, X.; Lou, S. A comprehensive review on laser powder bed fusion of steels: Processing, microstructure, defects and control methods, mechanical properties, current challenges and future trends. J. Manuf. Process. 2022, 75, 375–414. [Google Scholar] [CrossRef] [Scilit]
- Su, J.; Jiang, F.; Teng, J.; Chen, L.; Requena, G.; Yan, M.; Zhang, L.C.; Wang, Y.M.; Okulov, I.V.; Zhu, H.M.; et al. Laser additive manufacturing of titanium alloys: Process, materials and post-processing. Rare Met. 2024, 43, 6288–6328. [Google Scholar] [CrossRef] [Scilit]
- Wang, J.; Zhu, R.; Liu, Y.; Zhang, L. Understanding melt pool characteristics in laser powder bed fusion: An overview of single- and multi-track melt pools for process optimization. Adv. Powder Mater. 2023, 2, 100137. [Google Scholar] [CrossRef] [Scilit]
- Edwards, A.; Huynh, D.Q.; Gillham, B.; Wang, J.; Sercombe, T.B. Application of machine learning for in-situ defect detection in metal powder bed fusion: A critical review. J. Intell. Manuf. 2026, 1–48. [Google Scholar] [CrossRef] [Scilit]
- Sanaei, N.; Fatemi, A. Defects in additive manufactured metals and their effect on fatigue performance: A state-of-the-art review. Prog. Mater. Sci. 2021, 117, 100724. [Google Scholar] [CrossRef] [Scilit]
- Song, Z.; Xiao, K.; Xiao, S.; Du, K.; Mao, Z.; Li, T.; Wang, B. Effect of porosity on tensile strength and micromechanisms of composites. Mater. Des. 2024, 247, 113429. [Google Scholar] [CrossRef] [Scilit]
- Tammas-Williams, S.; Withers, P.J.; Todd, I.; Prangnell, P.B. The influence of porosity on fatigue crack initiation in additively manufactured titanium components. Sci. Rep. 2017, 7, 7308. [Google Scholar] [CrossRef] [Scilit]
- Masuo, H.; Tanaka, Y.; Morokoshi, S.; Yagura, H.; Uchida, T.; Yamamoto, Y.; Murakami, Y. Influence of defects, surface roughness and HIP on the fatigue strength of Ti-6Al-4V manufactured by additive manufacturing. Int. J. Fatigue 2018, 117, 163–179. [Google Scholar] [CrossRef] [Scilit]
- Pegues, J.W.; Shao, S.; Shamsaei, N.; Sanaei, N.; Fatemi, A.; Warner, D.H.; Li, P.; Phan, N. Fatigue of additive manufactured Ti-6Al-4V, Part I: The effects of powder feedstock, manufacturing, and post-process conditions on the resulting microstructure and defects. Int. J. Fatigue 2020, 132, 105358. [Google Scholar] [CrossRef] [Scilit]
- Molaei, R.; Fatemi, A.; Sanaei, N.; Pegues, J.; Shamsaei, N.; Shao, S.; Li, P.; Warner, D.H.; Phan, N. Fatigue of additive manufactured Ti-6Al-4V, Part II: The relationship between microstructure, material cyclic properties, and component performance. Int. J. Fatigue 2020, 132, 105363. [Google Scholar] [CrossRef] [Scilit]
- Romano, S.; Beretta, S.; Brandão, A.; Gumpinger, J.; Ghidini, T. Defect sensitivity and fatigue performance of laser powder bed fused Ti–6Al–4V and AlSi10Mg alloys. Eng. Fract. Mech. 2018, 187, 165–189. [Google Scholar]
- Leuders, S.; Thöne, M.; Riemer, A.; Niendorf, T.; Tröster, T.; Richard, H.A.; Maier, H.J. On the mechanical behaviour of titanium alloy TiAl6V4 manufactured by selective laser melting: Fatigue resistance and crack growth performance. Int. J. Fatigue 2013, 48, 300–307. [Google Scholar] [CrossRef] [Scilit]
- Sun, W.; Ma, Y.E.; Huang, W.; Zhang, W.; Qian, X. Effects of build direction on tensile and fatigue performance of selective laser melting Ti6Al4V titanium alloy. Int. J. Fatigue 2020, 130, 105260. [Google Scholar] [CrossRef] [Scilit]
- Rans, C.; Michielssen, J.; Walker, M.; Wang, W.; Hoen-Velterop, L. Beyond the orthogonal: On the influence of build orientation on fatigue crack growth in SLM Ti-6Al-4V. Int. J. Fatigue 2018, 116, 344–354. [Google Scholar] [CrossRef] [Scilit]
- Qian, G.; Li, Y.; Paolino, D.S.; Tridello, A.; Berto, F.; Hong, Y. Very-high-cycle fatigue behavior of Ti-6Al-4V manufactured by selective laser melting: Effect of build orientation. Int. J. Fatigue 2020, 136, 105628. [Google Scholar] [CrossRef] [Scilit]
- Kasperovich, G.; Hausmann, J. Improvement of fatigue resistance and ductility of Ti6Al4V processed by selective laser melting. J. Mater. Process. Technol. 2015, 220, 202–214. [Google Scholar] [CrossRef] [Scilit]
- Qian, G.; Jian, Z.; Pan, X.; Berto, F. In-situ investigation on fatigue behaviors of Ti-6Al-4V manufactured by selective laser melting. Int. J. Fatigue 2020, 133, 105424. [Google Scholar] [CrossRef] [Scilit]
- Greitemeier, D.; Palm, F.; Syassen, F.; Melz, T. Fatigue performance of additive manufactured TiAl6V4 using electron and laser beam melting. Int. J. Fatigue 2017, 94, 211–217. [Google Scholar] [CrossRef] [Scilit]
- Fatemi, A.; Molaei, R.; Simsiriwong, J.; Sanaei, N.; Pegues, J.; Torries, B.; Phan, N.; Shamsaei, N. Fatigue behaviour of additive manufactured materials: An overview of some recent experimental studies on Ti-6Al-4V considering various processing and loading direction effects. Fatigue Fract. Eng. Mater. Struct. 2019, 42, 991–1009. [Google Scholar] [CrossRef] [Scilit]
- Moran, T.P.; Carrion, P.E.; Lee, S.; Shamsaei, N.; Phan, N.; Warner, D.H. Hot isostatic pressing for fatigue critical additively manufactured Ti-6Al-4V. Materials 2022, 15, 2051. [Google Scholar] [CrossRef] [Scilit]
- Jaber, H.; Kónya, J.; Kulcsár, K.; Kovács, T. Effects of Annealing and Solution Treatments on the Microstructure and Mechanical Properties of Ti6Al4V Manufactured by Selective Laser Melting. Materials 2022, 15, 1978. [Google Scholar]
- Ter Haar, G.M.; Becker, T.H.; Blaine, D.C. Influence of heat treatments on the microstructure and tensile behaviour of selective laser melting-produced Ti–6Al–4V parts. S. Afr. J. Ind. Eng. 2016, 27, 1663. [Google Scholar] [CrossRef] [Scilit]
- Li, C.-L.; Hong, J.-K.; Narayana, P.L.; Choi, S.-W.; Lee, S.W.; Park, C.H.; Yeom, J.-T.; Mei, Q. Realizing superior ductility of selective laser melted Ti-6Al-4V through a multi-step heat treatment. Mater. Sci. Eng. A 2021, 799, 140367. [Google Scholar] [CrossRef] [Scilit]
- Chao, Q.; Thomas, S.; Birbilis, N.; Cizek, P.; Hodgson, P.D.; Fabijanic, D. Post-processing effects in additively manufactured alloys. Mater. Sci. Eng. A 2021, 821, 141611. [Google Scholar]
- Dinița, A.; Neacșa, A.; Portoacă, A.I.; Tănase, M.; Ilinca, C.N.; Ramadan, I.N. Additive manufacturing post-processing treatments: A review. Materials 2023, 16, 4610. [Google Scholar] [CrossRef] [Scilit]
- Haase, F.; Siemers, C.; Rösler, J. Novel titanium alloys for medical applications: Thermomechanical treatment and fracture analysis. Mater. Sci. Eng. A 2022, 837, 142589. [Google Scholar]
- Semiatin, S.L. Thermomechanical processing of α/β titanium alloys. Metall. Mater. Trans. A 2020, 51, 2593–2612. [Google Scholar] [CrossRef] [Scilit]
- Jamhari, F.I.; Foudzi, F.M.; Buhairi, M.A.; Sulong, A.B.; Radzuan, N.A.M.; Muhamad, N.; Mohamed, I.F.; Jamadon, N.H.; Tan, K.S. Heat treatment effects in LPBF titanium alloys: A review. J. Mater. Res. Technol. 2023, 24, 4091–4110. [Google Scholar] [CrossRef] [Scilit]
- Pede, D.; Li, M.; Virovac, L.; Poleske, T.; Müller, C.; Mozaffari-Jovein, H. LPBF processing of novel β-Ti–Nb–Ta alloys. Mater. Des. 2025, 242, 113526. [Google Scholar]
- Murakami, Y. Metal Fatigue: Effects of Small Defects and Nonmetallic Inclusions; Elsevier: Oxford, UK, 2002. [Google Scholar]
- ASTM E8/E8M-22; Standard Test Methods for Tension Testing of Metallic Materials. ASTM International: West Conshohocken, PA, USA, 2022.
- ASTM E384-22; Standard Test Method for Microindentation Hardness of Materials. ASTM International: West Conshohocken, PA, USA, 2022.
- ISO 6892-1:2019; Metallic Materials—Tensile Testing Part 1: Method of Test at Room Temperature. International Organization for Standardization: Geneva, Switzerland, 2019.
- Owolabi, G.M.; Thom, M.; Ajide, O.; Kumar, N.; Azimi, A.; Warner, H.W.G. Fatigue Responses of Three AA 2000 Series Aluminum Alloys. J. Mater. Sci. Chem. Eng. 2019, 7, 32–48. [Google Scholar] [CrossRef]
- ISO 1099:2017; Metallic Materials—Fatigue Testing—Axial Force-Controlled Method. International Organization for Standardization: Geneva, Switzerland, 2017.
- Shuai, Y.; Liu, J.; Zhu, J.; Huang, Z.; Zha, W.; Yang, Y.; Zhang, R.; Zhang, K. Microstructural Evolution and Mechanical Properties of LPBF Ti-6Al-4V with Different Process Parameters. Materials 2026, 19, 1049. [Google Scholar] [CrossRef] [Scilit]
- Aliyu, A.A.A.; Puncreobutr, C.; Kuimalee, S.; Phetrattanarangsi, T.; Boonchuduang, T.; Taweekitikul, P.; Panwisawas, C.; Shinjo, J.; Lohwongwatana, B. Laser-inherent porosity in AM Ti–6Al–4V implants. J. Mater. Res. Technol. 2024, 30, 5121–5132. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.