A pH/NIR-Responsive Nanocomposite Hydrogel Incorporating Ferulic Acid and Betamethasone for Radiation-Induced Skin Injury

,
,
,
,
,
,
and
1
School of Pharmaceutical Sciences, Zhengzhou University, Zhengzhou 450001, China
2
State Key Laboratory of Antiviral Drugs, Pingyuan Laboratory, Xinxiang 453007, China
3
School of Pharmacy, Henan Normal University, Xinxiang 453500, China
4
Henan Food and Drug Administration, Zhengzhou 450012, China
Pharmaceutics2026, 18(12), 1522;https://doi.org/10.3390/pharmaceutics18121522 
(registering DOI)
This article belongs to the Special Issue Biomaterials for Drug Delivery and Advanced In Vitro Models in Pharmaceutical Research

Abstract

Background/Objectives: Radiation-induced skin injury (RISI) is a form of tissue damage resulting from exposure to ionizing radiation, characterized by excessive reactive oxygen species (ROS) accumulation, persistent inflammation, and bacterial colonization, posing significant challenges to conventional wound management. Herein, we report a dual-crosslinked photothermal nanocomposite hydrogel (BT-MPDA@FA-Gel) that integrates pH/NIR-responsive drug release with photothermal antibacterial activity for RISI treatment. Methods: The hydrogel matrix, composed of methacrylated chitosan (CSMA) and oxidized konjac glucomannan (OKGM), integrates a dynamic Schiff base network with a photo-crosslinked framework, conferring dynamic adaptability and robust structural integrity. Betamethasone (BT) was adsorbed onto PEGylated mesoporous polydopamine nanoparticles (PEG-MPDA) to obtain BT-MPDA. The resulting BT-MPDA nanoparticles, together with ferulic acid (FA), were incorporated into the hydrogel matrix to form BT-MPDA@FA-Gel. The physicochemical and mechanical properties of BT-MPDA@FA-Gel were characterized, and its ROS-scavenging activity, photothermal performance, antibacterial efficacy, and drug-release behavior under different pH conditions and NIR irradiation were evaluated. Cytocompatibility and hemostatic performance were assessed in vitro, and the therapeutic efficacy of the hydrogel was investigated in a murine RISI model. Results: Drug release studies demonstrated pH-responsive release of both BT and FA, with NIR irradiation further enhancing BT release. BT-MPDA@FA-Gel exhibited ROS-scavenging activity and photothermal performance, accompanied by reductions in viable counts of both S. aureus and E. coli. The hydrogel also demonstrated favorable cytocompatibility and hemostatic performance in vitro. In the murine RISI model, BT-MPDA@FA-Gel significantly accelerated wound closure, attenuated inflammatory responses and promoted collagen deposition. Conclusions: This study presents a dual-crosslinked nanocomposite hydrogel that combines pH-responsive release of both FA and BT, NIR-enhanced BT release and photothermal antibacterial activity. This multifunctional platform offers a promising approach to the treatment of radiation-induced skin injury.

1. Introduction

Radiation-induced skin injury (RISI), occurring in more than 90% of radiotherapy patients [1], is a common adverse effect of exposure to therapeutic ionizing radiation during cancer treatment. Ionizing radiation induces direct DNA damage and indirectly generates reactive oxygen species (ROS) through water radiolysis, resulting in oxidative stress and activation of NF-κB/MAPK/NLRP3 inflammatory cascades, with subsequent upregulation of proinflammatory cytokines such as TNF-α and IL-1β. Concurrent radiation-induced microvascular damage further compromises tissue perfusion, leading to hypoxia and nutrient deficiency and ultimately contributing to tissue necrosis and impaired repair. These radiation-initiated molecular and vascular injuries drive the progression from acute inflammation to chronic non-healing wounds, in which disruption of the skin barrier promotes bacterial colonization and sustains inflammatory cycles [2,3,4]. Thus, RISI is not a single-stage injury process but a dynamically evolving disease driven by oxidative stress, inflammation, infection risk, and impaired tissue regeneration, highlighting multifunctional therapeutic strategies that address these complex pathological features.
In recent years, the application of biomaterials in the treatment of RISI has attracted increasing attention, with research focusing on the development of functional nanomaterials and bioactive hydrogels. Carbon-based nanomaterials [5], transition-metal carbide and nitride nanomaterials [6], and metal-based nanomaterials and compounds [7,8] have been explored to modulate radiation-induced oxidative stress and infection-related microenvironments through various functions, including ROS scavenging, nanozyme-like catalytic activity, photothermal conversion, and antibacterial effects. In this context, bioactive hydrogels have evolved from conventional wound dressings into therapeutic platforms for the incorporation and localized delivery of functional components. By incorporating antioxidants, anti-inflammatory agents, and functional nanomaterials, together with diverse polymer compositions and network architectures, hydrogels can provide multiple therapeutic functions, including ROS scavenging, inflammation modulation, and antibacterial activity. However, the integration of multiple therapeutic functions and the regulation of drug release remain important challenges. In particular, the development of hydrogel systems that combine microenvironment-responsive drug release with external stimulus-responsive functions, while maintaining network structural stability and dynamic adaptability, warrants further investigation.
Mesoporous polydopamine nanoparticles (MPDA) are photothermal nanomaterials with near-infrared (NIR) responsiveness [9]. Upon NIR irradiation, the localized heat generated by MPDA can disrupt bacterial membrane integrity and interfere with essential cellular functions, thereby exerting a photothermal antibacterial effect. In addition, the mesoporous structure of MPDA provides space for therapeutic drug loading, making it a promising nanocarrier that integrates photothermal functionality with drug delivery. However, the dispersibility and colloidal stability of MPDA nanoparticles in aqueous environments may affect their biomedical applications. PEG modification can enhance nanoparticle hydrophilicity and improve their dispersibility and colloidal stability in aqueous media [10]. Therefore, MPDA was first modified with PEG, followed by loading with the anti-inflammatory drug betamethasone (BT) to obtain BT-MPDA. This design not only utilizes the photothermal effect of MPDA for NIR-mediated antibacterial activity but also takes advantage of photothermal heating to enhance BT release, thereby combining photothermal functionality with drug delivery. Meanwhile, considering the need to alleviate oxidative stress in RISI treatment, ferulic acid (FA), a natural phenolic compound with antioxidant and anti-inflammatory properties, was further introduced into the hydrogel system as an additional bioactive component [11]. Unlike BT, which was loaded into MPDA, FA was directly incorporated into the hydrogel in its free form, and its release was mainly associated with changes in the hydrogel network structure and molecular diffusion.
Natural polysaccharides, owing to their abundance, favorable biocompatibility, and intrinsic bioactivity, are attractive candidates for wound-healing materials [12]. Chitosan (CS) can promote fibroblast proliferation, collagen deposition, and angiogenesis, while its cationic nature may help reduce the risk of bacterial infection [13]. Konjac glucomannan (KGM) exhibits excellent hydrophilicity, which supports moisture retention at the wound site and may alleviate chronic inflammation through modulation of macrophage function [14,15]. CS and oxidized konjac glucomannan (OKGM) have been employed to construct dynamically crosslinked hydrogels for wound repair, with reversible Schiff base bonds contributing to gel formation, self-healing, and environmental responsiveness [16]. However, the reversible nature of Schiff base bonds may limit the structural stability of hydrogels based solely on dynamic crosslinking, potentially resulting in relatively rapid degradation during prolonged use. Previous studies have attempted to improve the stability of such hydrogels by introducing additional components, such as tannic acid, to enhance interactions within the network [17]. Another strategy involves introducing a second, more stable crosslinking mechanism. For example, photocrosslinkable groups can be incorporated into chitosan derivatives and subsequently polymerized under light irradiation to form a stable covalent network, complementing the dynamic Schiff base network [18].
Inspired by these strategies, CS and KGM were selected as the hydrogel matrix components and chemically modified to construct a dual-crosslinked network. Specifically, CS was methacrylated to obtain photocrosslinkable chitosan methacrylate (CSMA), while KGM was oxidized to introduce aldehyde groups, yielding OKGM. The remaining amino groups of CSMA reacted with the aldehyde groups of OKGM to form a dynamic Schiff base network. To establish a stable covalent network, lithium phenyl-2,4,6 trimethylbenzoylphosphinate (LAP) was selected as the photoinitiator. Compared with the commonly used photoinitiator Irgacure 2959 (I2959), LAP offers favorable water solubility and efficient photoinitiation under near-UV irradiation, making it suitable for photocrosslinking in aqueous hydrogel precursor systems [19]. Upon 365 nm irradiation, LAP generates free radicals that initiate the polymerization of methacrylate groups attached to the CSMA chains, thereby crosslinking the CSMA chains to form a stable covalent network. This dual-crosslinked architecture combines the adaptability of dynamic Schiff base bonds with the structural stability of covalent crosslinking, providing a suitable platform for the local loading and delivery of functional nanocomponents.
In this study, BT-MPDA nanoparticles and FA were incorporated into a CSMA/OKGM hydrogel matrix to construct a dual-crosslinked nanocomposite hydrogel (BT-MPDA@FA-Gel) through dynamic Schiff base bonding and UV-induced photocrosslinking. The system was designed to integrate pH-responsive release of BT and FA with NIR-enhanced BT release and photothermal antibacterial activity. This study provides a potential materials-based approach for the treatment of radiation-induced skin injury by combining responsive drug delivery with photothermal antibacterial functionality.

2. Materials and Methods

2.1. Materials

Chitosan (CS, Mw = 430 kDa, degree of deacetylation 89%) was purchased from Hunan Xinlvfang Pharmaceutical Co., Ltd. (Changsha, China). Pluronic F-127 was obtained from BASF (Ludwigshafen, Germany). Methacrylic anhydride (MA, purity ≥ 94%), sodium periodate, dopamine hydrochloride, amino-terminated methoxy polyethylene glycol (NH2-mPEG2000, MW = 2000 Da), ferulic acid (FA, purity ≥ 99%), and betamethasone (BT, purity ≥ 99%) were purchased from Aladdin Biochemical Technology Co., Ltd. (Shanghai, China). Lithium phenyl-2,4,6-trimethylbenzoylphosphinate (LAP, purity ≥ 98%) was purchased from Beijing InnoCare Technology Co., Ltd. (Beijing, China). Fetal bovine serum (FBS, Gibco) was obtained from Gibco Life Technologies (Grand Island, NY, USA). Streptomycin–penicillin solution (100×) and 0.25% trypsin–EDTA were purchased from Solarbio (Beijing, China). CCK-8 assay kits were purchased from SAB (Suzhou, China). ELISA kits for TNF-α, IL-1β, and IL-4 were obtained from Shanghai Enzyme-linked Biotechnology Co., Ltd. (Shanghai, China).

2.2. Cell Culture and Animals

HaCaT human immortalized keratinocytes were obtained from the Cell Bank of the Chinese Academy of Sciences (Shanghai, China). Male BALB/c mice (6–8 weeks old, 18–22 g) were purchased from Beijing Sibeifu Co., Ltd. (Beijing, China). All animal procedures were approved by the Animal Care and Use Committee of Zhengzhou University (ethical approval No. 26-YXY-010) and were conducted in accordance with the Guide for the Care and Use of Laboratory Animals issued by the National Research Council.

2.3. Preparation and Characterization of CSMA and OKGM

CSMA was synthesized with minor modifications according to previously reported methods [20]. Briefly, 1.0 g of chitosan was dissolved in 100 mL of 1% (v/v) acetic acid solution under stirring at room temperature until complete dissolution. Then, 1.0 mL of methacrylic anhydride (MA) was added dropwise under continuous stirring, and the reaction proceeded at room temperature for 24 h. The reaction mixture was transferred into a dialysis bag (MWCO = 14 kDa) and dialyzed against deionized water for 3 days to remove unreacted monomers and small-molecule impurities. The dialyzed solution was lyophilized to obtain CSMA, which was stored at 4 °C for further use.
OKGM was prepared via sodium periodate oxidation [21]. Briefly, 2.0 g of konjac glucomannan (KGM) was dispersed in 200 mL of deionized water under stirring at room temperature until homogeneous. Then, 2.0 g of sodium periodate was added, and the reaction proceeded in the dark for 24 h. Ethylene glycol (4 mL) was added to terminate the oxidation reaction, and the mixture was stirred in the dark for an additional 2 h. The solution was transferred to a 14 kDa MWCO dialysis bag and dialyzed against deionized water for 3 days. After dialysis, the solution was centrifuged at 4000 rpm for 10 min to remove insoluble impurities, and the supernatant was lyophilized to obtain OKGM powder, which was stored at 4 °C.
Fourier-transform infrared (FT-IR) spectroscopy (Nicolet iS10, Thermo Fisher Scientific, Madison, WI, USA) was further used to analyze functional group changes in CSMA and OKGM, with spectra recorded over a range of 4000–400 cm−1 to confirm the characteristic absorption peaks of methacryloyl groups in CSMA and aldehyde groups in OKGM.
The chemical structures of CSMA and OKGM were characterized by 1H NMR spectroscopy (400 MHz, Bruker AVANCE III, Karlsruhe, Germany) using D2O as the solvent. The degree of methacrylation (DM) of CSMA was calculated based on the integral ratio of the vinyl proton signals of methacryloyl groups (δ5.5–5.7 ppm) to the protons of the glucopyranose backbone (δ2.5–4.1 ppm) in the 1H NMR spectrum. The calculation was performed according to the following equation:
DM % = I 5.5 – 5.7   /   2 I 2.5 – 4.1   /   5 × DD
where I5.5–5.7 represents the integral area of the vinyl proton signals of methacryloyl groups, I2.5–4.1 represents the integral area of the glucopyranose backbone protons, and DD represents the degree of deacetylation of chitosan (89%).
The oxidation degree of OKGM was determined by hydroxylamine hydrochloride titration according to a previously reported method [22]. Briefly, OKGM was dissolved in 50 mL of 0.25 mol/L hydroxylamine hydrochloride solution (pH 4.5), and the pH was adjusted to 4.5 using 3% HCl or 5% NaOH. The mixture was stirred at room temperature for 24 h. The released HCl was then titrated with 0.1 mol/L NaOH until the pH reached 4.5. The NaOH consumption was recorded, and the oxidation degree was calculated using the following equation:
OD % = ( V 1 − V 0 ) × C NaOH × 162 2 W × 1000 × 100 %
where V1 and V0 represent the NaOH consumption volumes for OKGM and unoxidized KGM samples, respectively, CNaOH is the concentration of NaOH solution, W is the weight of the OKGM sample, and 162 represents the molecular weight of an anhydroglucose unit.

2.4. Preparation and Characterization of BT-MPDA Nanoparticles

2.4.1. Preparation of Mesoporous Polydopamine (MPDA) Nanoparticles

MPDA nanoparticles were synthesized using a one-pot method as previously reported with slight modifications [23]. Briefly, 0.15 g of dopamine hydrochloride and 0.10 g of Pluronic F127 were dissolved in a mixed solvent consisting of 5 mL deionized water and 5 mL absolute ethanol under magnetic stirring until complete dissolution. Subsequently, 145 μL of trimethylbenzene (TMB) was slowly added to the solution, followed by ultrasonication to obtain a milky emulsion. Then, 375 μL of ammonia solution was added under a fume hood, and the reaction was allowed to proceed under stirring at room temperature for 2 h. The product was collected by centrifugation (5000 rpm, 10 min), washed sequentially with ether and deionized water, and finally lyophilized to obtain dry MPDA nanoparticles.

2.4.2. Preparation of NH2-mPEG2000-Modified MPDA Nanoparticles (PEG-MPDA)

MPDA nanoparticles were dispersed in ultrapure water (1 mg mL−1). NH2-mPEG2000 was added at a mass ratio of 10:1 (MPDA:NH2-mPEG2000), and the mixture was stirred to ensure uniform dispersion. The pH was adjusted to 7.0 using 0.1 mol L−1 NaOH, followed by continuous stirring at room temperature for 24 h [24]. After the reaction, the suspension was centrifuged at 8000 rpm for 10 min, and the precipitate was washed three times with deionized water. The resulting PEGylated MPDA nanoparticles, designated as PEG-MPDA, were collected by lyophilization and stored at 4 °C.

2.4.3. Preparation of BT-Adsorbed PEGylated Mesoporous Polydopamine (BT-MPDA) Nanoparticles and Optimization of Drug Loading

BT-MPDA nanoparticles were prepared using a solution-based adsorption method, adapted with modifications from a previously reported procedure for drug loading onto PEG-modified mesoporous polydopamine nanoparticles [25]. Briefly, PEG-MPDA nanoparticles were dispersed in ultrapure water at a concentration of 1 mg·mL−1. Subsequently, 100 μL of BT ethanol solution (10 mg·mL−1) was added dropwise to the PEG-MPDA suspension, and the mixture was stirred in the dark at room temperature for 24 h. The suspension was then centrifuged at 8000 rpm for 10 min, and the precipitate was washed three times with deionized water to obtain BT-MPDA nanoparticles. To optimize drug loading, different mass ratios of PEG-MPDA to betamethasone (0.25:1, 0.5:1, 1:1, 2:1, and 4:1) were investigated. Following centrifugation, the concentration of unadsorbed BT in the supernatant was quantified at 238 nm using a UV-Vis spectrophotometer. The amount of adsorbed BT was calculated by subtracting the mass of unadsorbed BT from the initial mass of BT added. The adsorption efficiency (AE) and drug loading capacity (DL) were calculated according to the following equations:
AE % = W total − W free W total × 100 %
DL % = W total − W free W PEG − MPDA × 100 %
where Wtotal is the total amount of betamethasone initially added, Wfree is the amount of free betamethasone detected in the supernatant, and WPEG−MPDA is the mass of PEG-MPDA used for drug loading (n = 3).

2.4.4. Characterization of BT-MPDA Nanoparticles

The hydrodynamic diameter and zeta potential of MPDA, PEG-MPDA, and BT-MPDA nanoparticles were measured using a dynamic light scattering analyzer (Nano-ZS90, Malvern Instruments Ltd., Malvern, Worcestershire, UK). Samples were diluted to 1 mg·mL−1 and ultrasonicated for 10 min before measurement. Each sample was analyzed in triplicate. Ultraviolet-visible (UV-Vis) absorption spectra of BT, PEG-MPDA, and BT-MPDA were recorded using a UV-Vis spectrophotometer (8453, Agilent Technologies, Santa Clara, CA, USA) over a wavelength range of 200–800 nm. Successful loading of betamethasone into BT-MPDA nanoparticles was confirmed by the characteristic absorption peak of BT at 238 nm. The morphology of BT-MPDA nanoparticles was examined using transmission electron microscopy (TEM, Talos F200X, FEI, Hillsboro, OR, USA). Briefly, BT-MPDA nanoparticles were dispersed in water and ultrasonicated for 30 min. An aliquot of the resulting suspension was deposited onto a copper TEM grid and air-dried at room temperature prior to observation. The elemental composition and distribution of C, N, O, and F within BT-MPDA nanoparticles were analyzed by energy-dispersive X-ray spectroscopy (EDS) mapping coupled with TEM.

2.5. Fabrication and Physicochemical Characterization of BT-MPDA@FA-Gel Hydrogel

2.5.1. Fabrication of BT-MPDA@FA-Gel Hydrogel

CSMA and OKGM were separately dissolved in deionized water to prepare 2 wt% solutions. FA was added to the CSMA solution to a final concentration of 0.08 wt% and stirred until completely dissolved to obtain the FA/CSMA precursor solution. Meanwhile, BT-MPDA nanoparticles were dispersed in the OKGM solution under ultrasonication to obtain a BT-MPDA/OKGM dispersion. For the Gel group, the FA/CSMA precursor solution was mixed with the blank OKGM solution at a 1:1 volume ratio. For the BT-MPDA@FA-Gel group, the FA/CSMA precursor solution was mixed with the BT-MPDA/OKGM dispersion at the same volume ratio to obtain a homogeneous precursor mixture. LAP (0.20 wt%) was then added as the photoinitiator. The precursor mixtures were subjected to UV irradiation (365 nm, 6 mW·cm−2) for 20 s to induce photocrosslinking, followed by equilibration at room temperature for 5 min to complete hydrogel formation.

2.5.2. Injectability, Self-Healing, and Adhesive Properties of BT-MPDA@FA-Gel Hydrogel

The injectability of BT-MPDA@FA-Gel was evaluated by loading the hydrogel into a 1 mL syringe and extruding it through a 24-gauge needle into water. To assess moldability and shape fidelity, the precursor solution was extruded onto filter paper through a syringe to form the patterns “Gel” and “2026”. For self-healing evaluation, the formed hydrogel was cut into two halves, and the freshly exposed surfaces were immediately brought into contact. After incubation at room temperature for 15 min without external intervention, the self-healing behavior was visually assessed. The rheological recovery of BT-MPDA@FA-Gel was further evaluated using an oscillatory strain sweep and a step-strain test. The strain sweep was performed at 37 °C and a frequency of 1 Hz over a strain range of 0.1–1000% to determine the linear viscoelastic region (LVR). Subsequently, alternating low-strain (1%, 60 s) and high-strain (300%, 60 s) intervals were applied at 37 °C and 1 Hz, followed by a return to low strain (1%, 60 s). The low- and high-strain sequence was repeated for at least two cycles, while the storage modulus (G′) and loss modulus (G″) were continuously recorded to assess the recovery of viscoelastic properties after high-strain perturbation. Tissue adhesiveness was evaluated by attaching freshly prepared hydrogels to finger joints and observing their adhesion during bending at different angles. To evaluate tissue adhesiveness, freshly prepared hydrogels were attached to the surface of finger joints and observed under different bending angles to assess interfacial adhesion stability.

2.5.3. Compression Testing of BT-MPDA@FA-Gel Hydrogel

FA-Gel and BT-MPDA@FA-Gel hydrogels were fabricated into cylindrical specimens with a diameter of 10 mm and a height of 10 mm. Compression tests were performed using a universal testing machine (CMT6103, MTS Co. Ltd., Shenzhen, China) equipped with a 500 N load cell. Samples were compressed at a rate of 1 mm·min−1 until a strain of 60% was reached. Stress–strain curves were recorded, and the compressive modulus was calculated. All measurements were conducted in triplicate.

2.5.4. Rheological Properties of BT-MPDA@FA-Gel Hydrogel

FA-Gel and BT-MPDA@FA-Gel hydrogels were prepared as circular samples with a diameter of approximately 40 mm and a thickness of 1–3 mm. Rheological measurements were performed using a rheometer (Haake Mars 60, Karlsruhe, Germany) equipped with a 25 mm parallel-plate geometry and a 1.0 mm gap at 37 °C. Frequency sweep tests were conducted over an angular frequency range of 1–100 rad s−1 at a constant strain of 1%, and the G′ and G″ were recorded. Strain sweep measurements were subsequently performed to determine the LVR.

2.5.5. Swelling Behavior of BT-MPDA@FA-Gel Hydrogel

FA-Gel and BT-MPDA@FA-Gel hydrogels were fabricated into cylindrical specimens (diameter 10 mm, height 5 mm, n = 3) and lyophilized. The initial dry weight of each sample was recorded as Wa. Samples were then immersed in 10 mL phosphate-buffered saline (PBS, pH 7.4) in centrifuge tubes and incubated at 37 °C. At predetermined time points (2, 4, 6, 8, 10, 12, 18, 24, 48 h), the hydrogels were removed, their surface water gently blotted with filter paper, and weighed (Wb). Swelling was monitored until consecutive weight measurements varied by less than 1%, indicating equilibrium swelling. The swelling ratio (SR) was calculated as:
SR ( % ) = W b − W a W a × 100 %

2.5.6. In Vitro Degradation of BT-MPDA@FA-Gel Hydrogel

Cylindrical FA-Gel and BT-MPDA@FA-Gel samples (diameter 10 mm, height 5 mm) were accurately weighed and recorded as W1 (n = 3). Samples were immersed in PBS (pH 7.4) containing 0.25 mg·mL−1 lysozyme and incubated at 37 °C with shaking at 50 rpm. At scheduled time points (2, 4, 6, 8, 10, 12, 24 h), hydrogels were removed, blotted to remove excess surface liquid, and weighed (W2). After each measurement, the medium was replaced with fresh lysozyme solution to maintain enzymatic activity. Degradation was calculated as:
Degradation % = W 1 − W 2 W 1 × 100 %

2.6. Photothermal Performance Evaluation

2.6.1. Photothermal Effect

The photothermal performance of BT-MPDA nanoparticles and BT-MPDA@FA-Gel hydrogels was assessed using NIR irradiation. Aliquots of 200 μL of BT-MPDA nanoparticle suspension, FA-Gel, and BT-MPDA@FA-Gel hydrogels were placed in 1.5 mL centrifuge tubes and irradiated with an 808 nm NIR laser (model 808-10W, Xi’an Leize Electronic Co., Ltd., Xi’an, China) at a fixed power density of 1.0 W·cm−2 for 5 min. Temperature changes were continuously recorded using an infrared thermal imaging camera (Ti400, Fluke Corporation, Everett, WA, USA). To investigate the concentration-dependent photothermal response, BT-MPDA@FA-Gel hydrogels containing different concentrations of BT-MPDA (0.5, 1.0, 1.5, and 2.0 mg·mL−1) were irradiated at a laser power density of 0.5 W·cm−2 for 5 min. Additionally, to investigate the effect of laser power density, BT-MPDA@FA-Gel hydrogels containing 1.0 mg·mL−1 BT-MPDA were irradiated at power densities of 0.5, 1.0, 1.5, and 2.0 W·cm−2 for 5 min. All experiments were performed in triplicate.

2.6.2. Photothermal Stability

BT-MPDA@FA-Gel hydrogels containing 2.0 mg·mL−1 BT-MPDA (200 μL) were subjected to three consecutive NIR irradiation on/off cycles using an 808 nm laser at a power density of 1.0 W·cm−2. Each cycle consisted of 10 min of irradiation followed by 10 min of natural cooling. Temperature was recorded every 30 s during both heating and cooling phases, and infrared thermal images were acquired simultaneously. Photothermal stability was evaluated by comparing the temperature profiles and peak temperatures across the three irradiation cycles.

2.7. In Vitro Drug Release from BT-MPDA@FA-Gel Hydrogel

The release profiles of FA and BT from BT-MPDA@FA-Gel hydrogels were quantified using HPLC (Agilent 1200, Agilent Technologies, Santa Clara, CA, USA). Standard calibration curves were prepared for each drug. Chromatographic conditions were as follows: ZORBAX SB-C18 column (250 mm × 4.6 mm, 5 μm), mobile phase methanol: 0.1% aqueous phosphoric acid (60:40, v/v), column temperature 30 °C, flow rate 1.0 mL·min−1, and injection volume 10 μL. Following HPLC separation, both FA and BT were detected at 238 nm.
BT-MPDA@FA-Gel hydrogels were prepared as cylindrical samples (diameter 10 mm, height 5 mm) and the total initial drug content (W) was recorded. Each sample was immersed in 10 mL of release medium (PBS, pH 7.4 or pH 5.5, containing 0.5% Tween-80) and incubated at 37 °C under shaking (100 rpm). At predetermined intervals (0, 12, 24, 36, 48, 72 h), 2 mL of the release medium was withdrawn and immediately replaced with an equal volume of fresh medium to maintain a constant volume. Drug concentrations were determined by HPLC at each time point. To evaluate NIR-triggered release, a separate set of BT-MPDA@FA-Gel samples was irradiated with an 808 nm laser at 1 W·cm−2 for 5 min at the indicated time points, with other conditions unchanged. All measurements were performed in triplicate. The cumulative release percentage (CR) of FA and BT was calculated as follows:
CR % = C n V + ∑ i = 1 n − 1 C i V i W × 100 %
where Cn is the drug concentration in the nth sample (μg·mL−1), V is the total volume of the release medium (10 mL), Ci is the drug concentration in the ith sample (μg·mL−1), Vi is the volume of the ith withdrawn sample (2 mL), and W is the initial total drug content in the hydrogel (μg).

2.8. Antioxidant Activity Evaluation

2.8.1. DPPH Radical Scavenging Assay

Lyophilized BT-MPDA, FA-Gel, and BT-MPDA@FA-Gel samples were accurately weighed (40 mg each) and dispersed in 10 mL deionized water to prepare stock solutions at 4 mg·mL−1. The stock solutions were further diluted to 0.5, 1.0, 2.0, and 4.0 mg·mL−1. A 0.2 mM DPPH solution in ethanol was prepared freshly. Briefly, 1 mL of each sample solution at different concentrations was mixed with 2 mL anhydrous ethanol and 1 mL DPPH solution, vortexed thoroughly, and incubated in the dark for 30 min. The absorbance at 517 nm was measured using a microplate reader and recorded as As. Deionized water instead of sample solution served as the blank control (Ac). Each experiment was performed in triplicate. The DPPH radical scavenging rate was calculated as:
Scavenging   rate % = A c − A s A c × 100 %

2.8.2. Superoxide Anion (O2·−) Scavenging Assay

The superoxide anion radical (O2·−) scavenging activity was evaluated using the pyrogallol autoxidation method [26]. Sample solutions were prepared at concentrations of 0.5, 1.0, 2.0, and 4.0 mg·mL−1. Fresh 15 mM pyrogallol solution and pH 8.2 Tris-HCl buffer were prepared. Briefly, 400 μL of sample solution was mixed with 1.5 mL of Tris-HCl buffer and 0.3 mL of pyrogallol solution and incubated at room temperature for 20 min. The absorbance at 420 nm was then measured (A1). PBS buffer without the sample was used as the control (A0). Experiments were conducted in triplicate. The O2·− scavenging rate was calculated as follows:
Scavenging   rate % = A 0 − A 1 A 0 × 100 %

2.9. Cytocompatibility Evaluation

2.9.1. CCK-8 Assay

HaCaT human immortalized keratinocytes were used to evaluate the cytocompatibility of BT-MPDA@FA-Gel hydrogels. Extracts of BT-MPDA nanoparticles, FA-Gel, and BT-MPDA@FA-Gel were prepared by incubating each sample at 0.1 g·mL−1 in DMEM containing 10% fetal bovine serum (FBS) at 37 °C for 72 h, followed by sterile filtration through a 0.22 μm polyethersulfone (PES) membrane filter. HaCaT cells were seeded in 96-well plates at 5 × 103 cells per well and cultured overnight at 37 °C under 5% CO2 to allow attachment. The culture medium was replaced with 100 μL of different sample extracts and incubated for 24 h and 48 h. Then, 10 μL of CCK-8 reagent was added per well and incubated for 1 h. Absorbance at 450 nm was measured using a microplate reader. Untreated cells served as the control, and wells without cells were used as blanks. Cell viability was calculated as:
Cell   viability % = A sample − A blank A control − A blank × 100 %
where Asample, Acontrol, and Ablank represent the absorbance values of the experimental, control, and blank groups, respectively.

2.9.2. Calcein-AM Staining

HaCaT cells were seeded in 12-well plates at a density of 1 × 105 cells per well and incubated overnight to allow cell attachment. The culture medium was replaced with fresh complete DMEM for the Control group and the corresponding sterile-filtered sample extracts for the treatment groups. The cells were then incubated for 24 and 48 h. After incubation, the cells were stained with 500 μL of DMEM containing 2 μM Calcein-AM and incubated at 37 °C in the dark for 30 min. Subsequently, the staining solution was removed, and the cells were gently washed three times with PBS to eliminate excess dye. Fluorescence images were acquired using an inverted fluorescence microscope (IX73, Olympus Corporation, Tokyo, Japan). Green fluorescence indicated viable cells.

2.10. In Vitro Antibacterial Assessment

2.10.1. Plate Colony Counting

E. coli (Gram-negative) and S. aureus (Gram-positive) were used to evaluate antibacterial activity. Experimental groups included FA-Gel, BT-MPDA and BT-MPDA@FA-Gel, with sterile PBS as a negative control. Each group was tested under NIR irradiation (808 nm, 1.0 W·cm−2, 5 min) or in the dark. A total of 200 μL of each sample was mixed with 100 μL bacterial suspension (≈1 × 106 CFU·mL−1) in a 24-well plate and incubated at 37 °C with shaking at 180 rpm. After incubation, 30 μL of the mixture was plated on agar and incubated at 37 °C overnight. Colony numbers were counted, and the percentage reduction in viable bacterial counts was calculated as follows:
Reduction   in   viable   bacterial   counts   ( % )   = N c − N x N c × 100 %
where Nc and Nx represent the viable bacterial counts (CFU) in the control and experimental groups, respectively. For each irradiation condition, the corresponding PBS control was used as the reference.

2.10.2. Bacterial Growth Curve

Sample extracts were mixed with bacterial suspensions as described above. Cultures were incubated at 37 °C with shaking (180 rpm) for 12 h. OD600 values were measured at 0, 1, 2, 4, 6, 8, 10, and 12 h. Growth curves were plotted as time versus OD600.

2.11. Hemocompatibility and Hemostatic Evaluation

2.11.1. Hemolysis Assay

Fresh BALB/c mouse blood was collected into sodium citrate-containing anticoagulant tubes. Deionized water and 0.9% (w/v) NaCl solution served as the positive and negative controls, respectively. For the sample groups, 200 μL of anticoagulated whole blood was mixed with 800 μL of 0.9% (w/v) NaCl solution and 200 μL of the corresponding formulation (FA-Gel, BT-MPDA suspension at 1 mg/mL, or BT-MPDA@FA-Gel). The control groups contained 200 μL of blood mixed with 1 mL of the respective control solution. All samples were incubated at 37 °C for 1 h and centrifuged at 2000 rpm for 5 min. The absorbance of the supernatants was measured at 540 nm. The hemolysis rate was calculated as follows (n = 3):
Hemolysis   % = A sample − A negative A positive − A negative × 100 %
where Asample, Anegative, and Apositive are the absorbance values measured at 540 nm for the experimental group, negative control, and positive control, respectively.

2.11.2. In Vitro Blood Clotting Index (BCI) Assay

The blood clotting index (BCI) was measured to evaluate the hemostatic performance of the different materials. Briefly, 200 μL of FA-Gel, 200 μL of BT-MPDA suspension (1 mg/mL), or 200 μL of BT-MPDA@FA-Gel formulation was added to individual wells of a 24-well plate. To maintain comparable liquid volumes, 200 μL of PBS was added to each preformed hydrogel sample. In the Gauze group, a standardized piece of sterile gauze measuring 5 mm × 5 mm was used as the reference material, and 200 μL of PBS was added. The control group received 200 μL of PBS without any material. Subsequently, 50 μL of sodium citrate-anticoagulated whole blood and 20 μL of 0.2 M CaCl2 solution were added to each group. The samples were incubated at 37 °C for 10 min. After incubation, 800 μL of ultrapure water was added to lyse the remaining unclotted red blood cells. The resulting mixtures were centrifuged at 2000 rpm for 5 min, and the absorbance of the supernatants was measured at 540 nm using a microplate reader. Each group was tested in triplicate. The BCI was calculated using the following equation:
BCI   % = 1 − A sample A control × 100 %
where Asample and Acontrol represent the absorbance values of the sample group and the material-free control group, respectively.

2.11.3. In Vivo Hemostatic Performance

Male Balb/c mice were used to establish liver bleeding and tail amputation models. After anesthesia and disinfection, a standardized liver injury was induced, and pre-weighed filter paper (initial weight Ha) was placed beneath the liver. The experimental groups received sterile gauze or BT-MPDA@FA-Gel hydrogel, whereas the control group received no treatment. The BT-MPDA@FA-Gel hydrogel contained BT-MPDA at a final concentration of 1 mg/mL. For the liver bleeding model, hemostasis time was measured using a stopwatch from the induction of liver injury until visible bleeding had ceased continuously for 30 s. After hemostasis, the filter paper was weighed again (Hb), and blood loss was calculated as follows:
BL = H b − H a
For the tail amputation model, mouse tails were disinfected, and the mid-tail was amputated using sterile scissors. The resulting wounds were left untreated or treated with sterile gauze or BT-MPDA@FA-Gel hydrogel, according to the experimental group. Hemostasis time was measured using a stopwatch from the moment of tail amputation until visible bleeding had ceased for 30 s. Blood loss was also recorded.

2.12. Establishment and Treatment of the RISI Model

Healthy male Balb/c mice (18–22 g) were used to establish the RISI model. Animals were acclimatized for 7 days prior to experimentation. All animal procedures were approved by the Ethics Committee of Zhengzhou University (Approval No. 26-yxy-010) and conducted in accordance with the ARRIVE guidelines.
Twenty-four hours before irradiation, the hair on the right hind limb of each mouse was carefully removed to fully expose the irradiation area. Prior to irradiation, mice were anesthetized via intraperitoneal injection of 1% sodium pentobarbital (50 mg·kg−1) and immobilized on the irradiation platform. An X-ray irradiator (X-RAD 320, Precision X-Ray Inc., North Branford, CT, USA) was used to establish the RISI model with a single dose of 40 Gy [27]. The distance between the X-ray source and the skin was set at 50 cm, with a dose rate of 1 Gy·min−1. Lead shielding was applied to protect non-irradiated body regions, exposing only the depilated right hind limb. Following irradiation, animals were allowed free access to food and water. The mice were divided into five groups (n = 7 per group). The healthy control group underwent depilation without irradiation. The remaining mice received irradiation to induce the RISI model and, after visible skin lesions developed, were randomly assigned to four groups: (i) the RISI model group, which received no treatment, (ii) the FA-Gel group, which received topical application of the hydrogel matrix with FA, (iii) the BT-MPDA group, which received topical application of BT-MPDA nanoparticle suspension at a concentration of 1.0 mg·mL−1 followed by NIR irradiation; and (iv) the BT-MPDA@FA-Gel group, which received topical application of the BT-MPDA@FA-Gel hydrogel containing BT-MPDA at a final concentration of 1.0 mg·mL−1 followed by NIR irradiation.
Treatment was initiated once visible skin lesions had developed in the irradiated area.
The corresponding formulations (1 mL per treatment) were applied topically and evenly to the irradiated skin area once daily for 21 consecutive days. Before each daily treatment, residual formulation from the previous application was gently removed from the treated skin area. For the BT-MPDA and BT-MPDA@FA-Gel groups, the treated area was irradiated immediately after sample application using an 808 nm NIR laser at a power density of 1 W·cm−2 for 1 min. Treatments were continued for 21 consecutive days. Wound healing progression and animal survival status were monitored throughout the experimental period.

2.13. Wound Healing Evaluation and Inflammatory Cytokine Analysis

2.13.1. Radiation-Induced Skin Injury Scoring

Skin lesions in the irradiated area were evaluated on days 0, 1, 3, 5, 7, 9, 12, 15, 18, and 21 after treatment initiation. Clinical manifestations, including erythema, alopecia, desquamation, ulceration, and tissue necrosis, were recorded and scored according to the Radiation Therapy Oncology Group (RTOG) acute radiation dermatitis grading criteria [28]. The grading system was defined as follows: Grade 0, normal skin; Grade 1, mild erythema or slight hair loss; Grade 2, moderate to severe erythema with patchy hair loss; Grade 3, moist desquamation; and Grade 4, ulceration or necrosis. Higher scores represented more severe radiation-induced skin damage.

2.13.2. Determination of Inflammatory Cytokine

On days 7 and 21 after treatment, skin tissues from the irradiated region were harvested from three randomly selected mice in each group. Tissues were rinsed with normal saline, minced, and homogenized to prepare 10% (w/v) tissue homogenates. The homogenates were centrifuged at 5000 rpm for 10 min at 4 °C, and the supernatants were collected for analysis. The expression levels of IL-1β, TNF-α, and IL-4 were quantified using commercial ELISA kits according to the manufacturer’s instructions. Absorbance was measured at 450 nm, and cytokine concentrations were calculated based on the corresponding standard curves.

2.14. Histological Analysis

On days 7 and 21 post-treatment, skin tissues from the irradiated area were collected from three mice per group and fixed in 4% paraformaldehyde. After fixation, tissues were dehydrated through a graded ethanol series, cleared in xylene, embedded in paraffin, and sectioned into 4 μm thick slices. The sections were stained with hematoxylin and eosin (H&E) and Masson’s trichrome staining following standard protocols. Histological morphology, inflammatory infiltration, epidermal regeneration, and collagen deposition were observed and imaged using an optical microscope.
Quantitative histological analysis was performed using ImageJ software (version 1.53). For epidermal thickness, measurements were taken perpendicular to the epidermal surface at multiple locations using a consistent measurement criterion across all groups. Inflammatory cell infiltration was quantified by counting inflammatory cells within predefined regions of interest (ROIs) in the dermis and expressing the results as cell density (cells/mm2). Collagen fiber alignment was evaluated from Masson’s trichrome-stained sections using a coherency-based directional analysis of collagen fibers within predefined dermal ROIs. The same image acquisition and analysis settings were applied across all groups. Multiple measurements or ROIs from each mouse were averaged to obtain one value per animal, and the mouse was considered the biological experimental unit (n = 3).

2.15. In Vivo Biosafety Assessment

To evaluate the in vivo biosafety of the developed nanoparticles and hydrogel system, hematological, serum biochemical, histopathological, and organ index analyses were performed in mice at the end of the treatment period. After 21 days of treatment, whole blood samples were collected from the mice via orbital venous sampling and transferred into anticoagulant-containing tubes, followed by gentle mixing to prevent coagulation. An appropriate volume of whole blood was subsequently analyzed using an automated hematology analyzer according to the manufacturer’s standard operating procedures. The hematological parameters, including white blood cell count (WBC), red blood cell count (RBC), hemoglobin (HGB), platelet count (PLT), hematocrit (HCT), and mean corpuscular volume (MCV), were determined. Meanwhile, whole blood samples were collected and centrifuged at 3500 rpm for 10 min at 4 °C. The resulting serum was collected for biochemical analysis. Serum alanine aminotransferase (ALT) and aspartate aminotransferase (AST) levels were determined using the corresponding assay kits to evaluate potential liver injury, while serum urea (UREA) and creatinine (CREA) levels were measured to evaluate renal function.
At the end of the treatment period, the mice were euthanized, and the major organs, including the heart, liver, spleen, lungs, and kidneys, were carefully excised. The organs were thoroughly rinsed with physiological saline, fixed, and subjected to tissue processing, paraffin embedding, sectioning, and H&E staining. The histological morphology and pathological changes of the major organs were examined using a light microscope. In addition, the body weight and weights of the major organs were recorded, and the organ indices of the heart, liver, spleen, lungs, and kidneys were calculated according to Equation (15) to further evaluate the potential effects of the treatments on major organs.
Organ   index   % = W Organ W Body × 100 %
where WOrgan and WBody represent the organ weight and final body weight, respectively.

2.16. Statistical Analysis

All quantitative data are presented as the mean ± standard deviation (SD). Statistical analyses were performed using GraphPad Prism 10.1.2 and Origin 2024. Comparisons between two groups were conducted using Student’s t-test. Comparisons among multiple groups were conducted using one-way analysis of variance (one-way ANOVA) followed by Tukey’s multiple-comparisons test. For experiments involving two independent variables, two-way ANOVA followed by appropriate multiple-comparisons tests was performed. For longitudinal measurements obtained from the same experimental units at multiple time points, two-way repeated-measures ANOVA was used. A 95% confidence level was adopted, with p < 0.05 considered statistically significant. Statistical significance is indicated as follows: * p < 0.05, ** p < 0.01, *** p < 0.001, and **** p < 0.0001.

3. Results and Discussion

3.1. Synthesis and Characterization of OKGM and CSMA

As illustrated in Figure 1a, CS was chemically modified through methacrylation to introduce methacryloyl groups into its polysaccharide backbone. The successful methacrylation of CS was characterized by FTIR and 1H NMR spectroscopy. As shown in Figure 1c, the comparison of the FTIR spectra of CS and CSMA revealed characteristic spectral changes following methacrylation. In particular, the CSMA spectrum exhibited characteristic absorption bands at 1656 and 1585 cm−1, corresponding to C=O and C=C stretching vibrations associated with the introduced methacryloyl groups, respectively. The additional absorption bands at 1331 and 1104 cm−1 were associated with C–N-related vibrations and C–O/C–O–C stretching vibrations in the polysaccharide structure, respectively [29]. These bands reflect the characteristic chemical structure of CSMA. Further evidence was provided by 1H NMR spectroscopy (Figure 1e), which showed characteristic signals at δ5.41–5.62 ppm and approximately δ1.9 ppm [30], corresponding to the vinyl and methyl protons of the methacryloyl groups, respectively. The degree of methacrylation was calculated to be 21.4%, further supporting the successful introduction of methacryloyl groups into the chitosan backbone.
Figure 1. Characterization of CSMA, OKGM and BT-MPDA nanoparticles. (a) Schematic illustration of CSMA synthesis by methacrylation of chitosan. (b) Schematic illustration of OKGM synthesis by periodate oxidation of KGM. (c) FT-IR spectra of CS and CSMA. The dashed line indicates the characteristic absorption band of the CS backbone at 1656 cm−1. (d) FT-IR spectra of KGM and OKGM. The dashed lines indicate the characteristic absorption bands of the KGM backbone, corresponding to O–H stretching (3400 cm−1) and C–H stretching (2882 cm−1), respectively. (e) 1H NMR spectra of CS and CSMA. (f) 1H NMR spectra of KGM and OKGM. (g) UV-Vis absorption spectra of BT, PEG-MPDA, and BT-MPDA. (h) EDS spectrum of BT-MPDA. (i) Merged elemental mapping image of C, N, O, and F. (j–m) Elemental mapping images of C, N, O, and F in BT-MPDA nanoparticles. (n) TEM image of BT-MPDA nanoparticles. (o) Hydrodynamic diameter, PDI and Zeta potentials (p) of MPDA, PEG-MPDA, and BT-MPDA. Statistical analysis was performed using one-way ANOVA followed by Tukey’s multiple-comparison test. In (n), * and # denote significant differences in particle size and PDI, respectively. * p < 0.05, ** p < 0.01, *** p < 0.001; ## p < 0.01, ### p < 0.001.
OKGM was prepared by sodium periodate oxidation of KGM, as illustrated in Figure 1b. The structural modifications were verified by FT-IR and 1H NMR analyses. As shown in Figure 1d, compared with pristine KGM, OKGM exhibited a more pronounced absorption peak at 1728 cm−1, corresponding to the stretching vibration of aldehyde groups. Additionally, a characteristic peak at 882 cm−1, attributed to hemiacetal structures, appeared, indicating the successful introduction of aldehyde functionalities through oxidation [31]. Further evidence was provided by 1H NMR spectroscopy (Figure 1f). A distinct resonance signal at δ9.2 ppm corresponded to aldehyde protons [32]. The oxidation degree of OKGM was determined to be 34.5%.

3.2. Fabrication and Characterization of BT-MPDA Nanoparticles

TEM images revealed that the BT-MPDA nanoparticles possessed a well-defined spherical morphology with uniform size distribution and negligible aggregation (Figure 1n). Dynamic light scattering (DLS) analysis showed that the average hydrodynamic diameter of MPDA, PEG-MPDA, and BT-MPDA was 190.0 ± 8.1, 181.3 ± 7.3, and 201.0 ± 1.3 nm, respectively. The slight decrease in particle size after PEGylation may be associated with improved colloidal dispersion, whereas the subsequent increase following BT loading is consistent with BT adsorption onto the nanoparticle surface. All three formulations had hydrodynamic diameters within the range of 180–210 nm and PDI values below 0.2 (Figure 1o), indicating relatively narrow particle size distributions. Zeta potential measurements further characterized the surface properties of the nanoparticles. MPDA nanoparticles exhibited a strongly negative surface charge of −30.4 ± 1.2 mV, which may be attributed to the ionization of phenolic hydroxyl and quinone-related groups on the polydopamine surface [33]. Following PEGylation, the zeta potential of PEG-MPDA nanoparticles increased to −25.2 ± 1.1 mV. After BT loading, a further increase to −22.7 ± 0.9 mV was observed (Figure 1p). These changes in surface charge are consistent with PEG modification and subsequent BT adsorption, suggesting alterations in the nanoparticle surface properties.
The FT-IR spectrum of PEG-MPDA retained the characteristic absorption features of MPDA, with bands at approximately 3419 and 1605 cm−1. In addition, absorption features were observed in the C-H stretching region (2800–3000 cm−1) and the 1000–1150 cm−1 region, with a band at approximately 1117 cm−1, consistent with PEG-related C-H and C-O-C vibrations (Figure S1). These spectral features provide supporting evidence for the incorporation of PEG into the MPDA-based system. MPDA nanoparticles displayed a strongly negative surface potential of −30.4 ± 1.2 mV, whereas the values for PEG-MPDA and BT-MPDA were −25.2 ± 1.1 and −22.7 ± 0.9 mV, respectively (Figure 1p).
Different mass ratios of PEG-MPDA to BT were investigated to optimize drug loading, and a mass ratio of 4:1 was selected based on the highest drug loading capacity. At this ratio, the AE and DL were 77.18 ± 0.92% and 16.17 ± 0.16%, respectively. The UV-Vis spectra are presented in Figure 1g. BT-MPDA nanoparticles exhibited a distinct absorption peak at 238 nm, corresponding to the characteristic absorption of BT, confirming successful drug loading. Elemental mapping analysis further verified the successful fabrication of BT-MPDA nanoparticles (Figure 1i–m). Carbon, nitrogen, oxygen, and fluorine were uniformly distributed throughout the nanoparticles, with atomic percentages of 80.7 ± 4.5%, 6.8 ± 1.4%, 12.1 ± 2.5%, and 0.4 ± 0.1%, respectively. The presence of fluorine, a characteristic element originating from the molecular structure of betamethasone, provides direct evidence of successful drug incorporation into the nanoparticle system, corroborating the successful construction of BT-MPDA nanoparticles.

3.3. Construction and Physicochemical Properties of BT-MPDA@FA-Gel Hydrogels

BT-MPDA@FA-Gel hydrogels were constructed via dual crosslinking through dynamic Schiff-base reactions and photopolymerization. Upon 365 nm UV irradiation, the precursor solution rapidly gelled within 20 s (Figure 2b), demonstrating excellent in situ gelation capability. Such rapid gelation not only reduces the operational time during application but also enhances material retention at wound sites. For wound dressings, injectability is a critical property to ensure conformity to irregular wound geometries [34]. When loaded into a syringe, BT-MPDA@FA-Gel could be continuously extruded to form patterns such as the word “Gel” or “2026” (Figure 2d), demonstrating its excellent injectability.
Figure 2. Characterization of BT-MPDA@FA-Gel. (a) Schematic illustration of the preparation mechanism of BT-MPDA@FA-Gel through photo crosslinking and Schiff base crosslinking. The blue and green wavy lines represent CSMA and OKGM, respectively. The pink, orange, and cyan symbols indicate methacrylate groups (C=C), amino groups (−NH2), and aldehyde groups (−CHO), respectively. The orange dots represent the LAP photoinitiator, the purple symbol represents UV irradiation, the yellow stars represent FA, and the dark spherical particles represent BT-MPDA nanoparticles. (b) Photographs illustrating the preparation of FA-Gel by mixing OKGM with FA/CSMA and BT-MPDA@FA-Gel by mixing BT-MPDA/OKGM with FA/CSMA. (c) SEM images of FA-Gel and BT-MPDA@FA-Gel at 50× and 200× magnification. (d) Injectability of BT-MPDA@FA-Gel. (e) Photographs showing BT-MPDA@FA-Gel at bending angles of 0° and 90°. (f) Self-healing behavior of BT-MPDA@FA-Gel after cutting and recontacting. (g) Swelling behavior of FA-Gel and BT-MPDA@FA-Gel. (h) Degradation profile. (i) Compressive stress–strain curves. (j) Compressive modulus. (k) Frequency-sweep rheological analysis. (l) Viscosity measurement. Data are presented as the mean ± SD (n = 3). Statistical significance of the equilibrium swelling ratio at 24 h was assessed using an unpaired Welch’s t-test. Compressive modulus was analyzed using one-way ANOVA (** p < 0.01).
In addition, BT-MPDA@FA-Gel exhibited macroscopic self-healing behavior (Figure 2f). To quantitatively evaluate this property, strain-amplitude sweep and step-strain rheological tests were performed. The strain-amplitude sweep showed that the G′ remained higher than the G″ at low strain amplitudes, indicating predominantly elastic behavior. As the strain increased, G′ decreased markedly and approached G″ at high strain amplitudes, suggesting progressive disruption of the hydrogel network under large deformation (Figure S2). In the step-strain test, G′ decreased substantially under high-strain conditions and recovered upon returning to low strain during repeated cycles (Figure S3). The G′ recovery efficiency reached 94.50 ± 0.87% across three independent hydrogel samples (n = 3), demonstrating substantial recovery of the hydrogel’s viscoelastic properties following repeated mechanical perturbation. Furthermore, when applied onto human joint surfaces at various angles, BT-MPDA@FA-Gel remained stably adhered to freely bending finger joints (Figure 2e), indicating strong tissue adhesion and wound adaptability. This behavior is mainly due to the abundance of dynamic Schiff-base linkages and polyphenolic moieties in the hydrogel, which can establish multiple non-covalent and covalent interactions with tissue interfaces, thereby enhancing interfacial adhesion [35].
SEM imaging revealed that BT-MPDA@FA-Gel hydrogels possess a uniform three-dimensional porous network (Figure 2c), which facilitates water uptake and nutrient transport. Swelling behavior analysis showed that both FA-Gel and BT-MPDA@FA-Gel hydrogels rapidly absorbed water during the initial stage, followed by a gradual approach to equilibrium. The swelling ratios became relatively stable after approximately 24 h (Figure 2g). At 24 h, the equilibrium swelling ratio of BT-MPDA@FA-Gel (46.1%) was significantly higher than that of FA-Gel (32.7%). Enhanced water retention is beneficial for absorbing wound exudates and maintaining a moist healing microenvironment, which is favorable for the repair of radiation-induced skin injuries [36].
The in vitro degradation profiles in PBS (pH 7.4, 37 °C) indicated that both hydrogels degraded relatively quickly within the first 12 h and were nearly fully degraded by 24 h (Figure 2h). BT-MPDA@FA-Gel displayed a slightly faster degradation rate than FA-Gel, potentially due to BT-MPDA nanoparticles increasing network hydrophilicity and promoting water penetration. This moderate degradability can reduce secondary damage during dressing removal, enhancing wound safety and tissue recovery [37].
Compression tests demonstrated that BT-MPDA@FA-Gel maintained structural integrity under 60% strain (Figure 2i,j), suggesting that the dual-crosslinked network formed by CSMA and OKGM can resist external mechanical forces. Rheological analysis further revealed that both FA-Gel and BT-MPDA@FA-Gel exhibited G′ values higher than G″ across the frequency range, confirming their elastic solid-like behavior. Moreover, the stability of G′ and G″ throughout the scanning range indicates a robust internal crosslinked network, providing mechanical integrity and resistance to deformation (Figure 2k,l).

3.4. Photothermal Performance of BT-MPDA@FA-Gel Hydrogels

The photothermal performance of BT-MPDA@FA-Gel was evaluated under NIR irradiation. As shown in Figure 3a, the temperature of FA-Gel remained relatively stable at 25.8 °C, whereas both BT-MPDA nanoparticles and BT-MPDA@FA-Gel containing 1 mg·mL−1 BT-MPDA exhibited rapid temperature increases, reaching approximately 45.6 and 44.9 °C, respectively, after 5 min of irradiation at a laser power density of 1 W·cm−2. The corresponding thermal images further illustrated the temperature changes in the three groups (Figure 3d). These results indicate that the photothermal heating capability of BT-MPDA was retained after incorporation into the hydrogel network, although no apparent enhancement in heating was observed compared with BT-MPDA nanoparticles alone. This photothermal response can be attributed to the conjugated structure of polydopamine, which facilitates NIR absorption and conversion into heat [9]. The effect of BT-MPDA concentration on photothermal heating was further investigated at a laser power density of 0.5 W·cm−2 (Figure 3b). The temperature increased with increasing BT-MPDA concentration from 0 to 2 mg·mL−1, demonstrating a concentration-dependent photothermal response. Furthermore, at a fixed BT-MPDA concentration of 1 mg·mL−1, increasing the laser power density from 0.5 to 2.0 W·cm−2 resulted in progressively greater temperature increases, with the temperature reaching 75.4 °C at 2.0 W·cm−2 (Figure 3c). The photothermal stability of BT-MPDA@FA-Gel was subsequently evaluated over three consecutive NIR on/off cycles (Figure 3e). The hydrogel repeatedly reached peak temperatures of approximately 45.7 °C during irradiation and cooled to approximately 32.1 °C during the off periods, without an obvious decline in peak temperature across the cycles. Collectively, these results demonstrate that BT-MPDA@FA-Gel retains the photothermal capability of BT-MPDA and exhibits concentration-dependent, power-dependent, and repeatable thermal responses under NIR irradiation.
Figure 3. Photothermal effect, drug release, and in vitro antioxidant performance. (a) Time-dependent temperature profiles of FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel containing 1 mg·mL−1 BT-MPDA under NIR irradiation for 5 min at a laser power density of 1 W·cm−2. (b) Time-dependent temperature profiles of BT-MPDA@FA-Gel containing different concentrations of BT-MPDA (0, 0.5, 1, 1.5, and 2 mg·mL−1) under NIR irradiation at a laser power density of 0.5 W·cm−2. (c) Time-dependent temperature profiles of BT-MPDA@FA-Gel at a fixed BT-MPDA concentration (1 mg·mL−1) under varying laser power densities (0.5, 1, 1.5, and 2 W·cm−2). (d) Thermal images of FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel containing 1 mg mL−1 BT-MPDA under NIR irradiation for 5 min at a laser power density of 1 W·cm−2. (e) Photothermal stability of BT-MPDA@FA-Gel over three consecutive NIR on/off cycles. (f) Cumulative release profiles of FA and BT under different pH conditions (pH 7.4 and pH 5.5). (g) Cumulative release profiles of BT under different pH conditions, with and without NIR irradiation. (h) DPPH radical scavenging activity. (i) Superoxide (O2·−) radical scavenging activity. Data are presented as mean ± SD (n = 3). Statistical analyses for (f,g) were performed using two-way repeated-measures ANOVA followed by Šídák’s multiple-comparisons test. The indicated pairwise comparisons in (f,g) refer to cumulative drug release at 72 h. Statistical analyses for (h,i) were performed using one-way ANOVA followed by Tukey’s multiple-comparisons test. Statistical significance is indicated as follows: ns, not significant difference; ** p < 0.01, *** p < 0.001, and **** p < 0.0001.

3.5. In Vitro Drug Release

To investigate pH-dependent drug release, in vitro release studies were conducted under physiological conditions (pH 7.4) and acidic conditions (pH 5.5), following previously reported protocols for hydrogels designed for RISI treatment [38]. Wound pH generally decreases as healing progresses, whereas chronic and non-healing wounds tend to exhibit elevated pH [39]. At 72 h, the cumulative release of FA and BT under acidic conditions reached 66.3% and 48.8%, respectively, compared with 57.5% and 32.2% under physiological conditions (Figure 3f). The higher release of both drugs at pH 5.5 may be attributed to the hydrolysis of dynamic Schiff base bonds, which may induce relaxation of the CSMA/OKGM hydrogel network and increase its permeability, thereby facilitating drug diffusion. Furthermore, NIR irradiation enhanced BT release under both conditions. At pH 7.4, the cumulative release of BT increased from 32.2% without NIR irradiation to 64.2% with NIR irradiation, whereas at pH 5.5, it increased from 48.8% to 85.0% (Figure 3g). This enhancement may be attributed to the photothermal effect of MPDA nanoparticles. The resulting temperature increase may accelerate molecular diffusion and weaken the non-covalent interactions between BT and the MPDA nanoparticle surface, facilitating BT desorption and subsequent release.
These findings demonstrate the complementary roles of pH-responsive and NIR-triggered release in regulating BT delivery. The pH-responsive hydrogel network enables drug release to adapt to changes in the surrounding wound environment, while the photothermal effect of MPDA nanoparticles provides an external means of further modulating drug release. This combination offers both environment-responsive and externally controllable drug delivery, providing greater flexibility in regulating local BT availability during wound healing.

3.6. Antioxidant Activity of BT-MPDA@FA-Gel Hydrogels

Excessive ROS induce persistent oxidative stress, aggravating cell damage, inflammatory infiltration, and tissue necrosis, thereby impairing RISI healing [40]. The antioxidant activity of the hydrogels was evaluated using DPPH and O2·− scavenging assays. With increasing sample concentration, the radical scavenging efficiency of all materials increased in a dose-dependent manner. Compared with FA-Gel, BT-MPDA exhibited significantly higher DPPH and O2·− scavenging activity (Figure 3h,i), consistent with the reported antioxidant properties of polydopamine. The phenolic and quinone-related functional groups of polydopamine may contribute to its radical-scavenging activity through redox-related interactions [9]. BT-MPDA@FA-Gel exhibited the highest scavenging efficiency in both radical models, indicating enhanced antioxidant activity under the tested conditions. The presence of FA, a natural phenolic acid with reported radical-scavenging properties [41], may contribute to the observed activity of BT-MPDA@FA-Gel.

3.7. Antibacterial Performance of BT-MPDA@FA-Gel Hydrogel

The antibacterial activity of BT-MPDA@FA-Gel hydrogels was evaluated using plate counting and bacterial growth curve methods. In the absence of NIR irradiation, FA-Gel exhibited appreciable antibacterial activity, with reductions in viable S. aureus and E. coli counts of 60.4% and 64.3%, respectively. This activity may be partly attributed to the chitosan structure retained in CSMA. Under suitable conditions, protonation of amino groups in chitosan enables electrostatic interactions with negatively charged components on bacterial surfaces, potentially disrupting membrane integrity and contributing to antibacterial activity [42]. Incorporation of BT-MPDA further enhanced the antibacterial activity, with BT-MPDA@FA-Gel achieving reductions in viable S. aureus and E. coli counts of 82.0% and 79.3%, respectively. Following NIR irradiation, the antibacterial activity of FA-Gel changed only slightly, with reductions in viable S. aureus and E. coli counts increasing to 67.7% and 65.6%, respectively. The BT-MPDA-containing groups exhibited enhanced antibacterial activity after irradiation.
The reductions in viable S. aureus counts reached 98.8% and 97.3% for BT-MPDA and BT-MPDA@FA-Gel, respectively, while the corresponding reductions in viable E. coli counts were 95.4% and 96.9% (Figure 4a–c). The polydopamine structure in BT-MPDA absorbs NIR light and converts it into heat. The resulting local temperature elevation may increase thermal stress on bacterial cells, damage cell membranes and associated protein structures, and thereby promote bacterial inactivation [43].
Figure 4. Antibacterial performance of different groups and in vitro biocompatibility. (a) Antibacterial photographs of each group with and without NIR irradiation. (b) Antibacterial efficiency against S. aureus for different groups. (c) Antibacterial efficiency against E. coli for different groups. (d) Growth curves of S. aureus under different treatments. (e) Growth curves of E. coli under different treatments. Data are presented as mean ± SD (n = 3). Statistical significance analysis in (b,c) was performed using two-way repeated-measures ANOVA followed by Tukey’s multiple-comparisons test. For comparisons between the No-NIR and NIR conditions within each group, ** p < 0.01 and *** p < 0.001. For comparisons between Gel and BT-MPDA@FA-Gel under the same irradiation condition, # p < 0.05, ## p < 0.01, and ### p < 0.001; ns, not significant.
The bacterial growth curves showed lower bacterial growth in the BT-MPDA-containing treatment groups, particularly under NIR irradiation (Figure 4d,e). BT-MPDA@FA-Gel exhibited substantial antibacterial activity even without irradiation and achieved high reductions in viable counts of both bacterial species under NIR irradiation. The antibacterial effects of BT-MPDA@FA-Gel were similar against Gram-positive S. aureus and Gram-negative E. coli, despite the generally greater intrinsic resistance of Gram-negative bacteria. These findings indicate that the hydrogel matrix contributes to baseline antibacterial activity, while the photothermal response of BT-MPDA provides an additional antibacterial benefit.

3.8. Cytocompatibility and Hemostatic Performances of BT-MPDA@FA-Gel Hydrogel

HaCaT cells were used to evaluate the cytocompatibility of the developed materials. Calcein-AM staining was first performed to visualize viable cells. Green fluorescence was observed in the Control and BT-MPDA@FA-Gel groups after 24 and 48 h of incubation, indicating the presence of viable cells (Figure 5a). CCK-8 assays showed that cell viability in the FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel groups remained above approximately 90% after 24 and 48 h of incubation (Figure 5b), indicating no apparent cytotoxic effects of the tested material extracts on HaCaT cells under the specified experimental conditions. Together, the CCK-8 assay and Calcein-AM staining results support the cytocompatibility of BT-MPDA@FA-Gel toward HaCaT keratinocytes under the tested conditions. Although BT-MPDA@FA-Gel exhibited favorable cytocompatibility toward HaCaT keratinocytes under the tested conditions, its effects on other wound-relevant cell types, such as dermal fibroblasts and endothelial cells, and its cytocompatibility under therapeutic NIR irradiation remain to be clarified. The effects of NIR-induced heating on cell viability and function also warrant further investigation.
Figure 5. Biocompatibility, hemocompatibility, and in vivo hemostatic performance of the BT-MPDA@FA-Gel hydrogel. (a) Calcein-AM staining images of HaCaT cells in the Control and BT-MPDA@FA-Gel groups after 24 and 48 h. Green fluorescence indicates viable cells, scale bar = 100 μm. (b) Cell viability of HaCaT cells after treatment with FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel, as determined by the CCK-8 assay. The BT-MPDA concentration in the relevant treatment groups was 1 mg mL−1. (c) Hemolysis assay of FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel. Deionized water and 0.9% (w/v) NaCl solution were used as the positive and negative controls, respectively. (d) Blood clotting index (BCI) and representative photographs of blood clotting in different groups. Control represents the material-free control group. A higher BCI value indicates a greater extent of blood clot formation. (e,f) Blood loss (BL) and hemostatic time, respectively, in the mouse tail bleeding model. (g,h) Blood loss and hemostatic time, respectively, in the mouse liver amputation model. For (e–h), Control represents the group without hemostatic treatment, whereas Gauze represents the group treated with sterile gauze as a reference material. Data are presented as mean ± SD (n = 3). Statistical significance was determined by one-way ANOVA followed by Tukey’s multiple-comparison test. ** p < 0.01 and **** p < 0.0001 versus the Control group; ns, not significant; ### p < 0.001 and #### p < 0.0001 versus the Gauze group.
Hemostatic performance was subsequently evaluated using hemolysis, coagulation, tail amputation, and liver bleeding assays. Hemolysis rates in the FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel groups were all below 2%, whereas water induced nearly complete hemolysis (Figure 5c), indicating a low hemolytic response under the tested conditions. The BCI results showed that BT-MPDA@FA-Gel exhibited the highest blood clotting performance among all groups (Figure 5d), indicating its enhanced ability to promote blood clot formation. In the tail bleeding model, BT-MPDA@FA-Gel reduced blood loss and shortened hemostasis time compared with the Control and gauze groups, reaching 30.53 ± 2.89 mg and 53.33 ± 6.24 s, respectively (Figure 5e,f). Similar effects were observed in the tail bleeding model (Figure 5g,h). The favorable hemostatic performance of BT-MPDA@FA-Gel may be associated with rapid gel formation, physical barrier effects, and the local retention of blood cells and coagulation components within the hydrogel network [44].

3.9. Therapeutic Efficacy of BT-MPDA@FA-Gel Hydrogel for RISI

Given its excellent antioxidant, antibacterial, and cytocompatible properties in vitro, the therapeutic efficacy of BT-MPDA@FA-Gel hydrogel was further evaluated in a murine model of RISI (Figure 6a). As shown in Figure 6b, untreated irradiated mice (X-ray group) gradually developed severe erythema, edema, ulceration, and tissue necrosis, indicating progressive skin damage following radiation exposure. The FA-Gel group exhibited partial improvement in wound appearance, whereas visible skin lesions persisted. The BT-MPDA group also showed partial improvement in skin lesions under NIR irradiation. Notably, the BT-MPDA@FA-Gel group exhibited more apparent improvement in wound appearance during the later observation period. By Day 21, the visible skin lesions had substantially improved, indicating recovery from radiation-induced skin damage.
Figure 6. Therapeutic evaluation of BT-MPDA@FA-Gel hydrogel in RISI model mice. (a) Schematic illustration of RISI induction and the subsequent treatment protocol. (b) Representative wound images of RISI model mice on days 0, 7, 14, and 21 after treatment. (c) Heatmap showing the time-dependent skin injury scores (0–4) assigned according to the adapted RTOG acute radiation dermatitis grading criteria. Higher scores indicate more severe skin injury.
RTOG scores revealed that the BT-MPDA@FA-Gel group maintained the lowest skin injury scores throughout the entire treatment period (Figure 6c). These findings indicate that the hydrogel effectively improves the pathological wound microenvironment through the combined antioxidant and anti-inflammatory properties, the intrinsic antibacterial activity observed in the FA-Gel group, and the additional antibacterial effect induced by NIR-triggered photothermal heating, thereby accelerating wound healing.
Histological evaluation using H&E and Masson’s trichrome staining provided further insight into tissue damage and repair following radiation-induced skin injury (Figure 7a,b). The X-ray group exhibited pronounced epidermal abnormalities, substantial inflammatory cell infiltration, and altered dermal architecture. The FA-Gel and BT-MPDA groups showed varying degrees of histological improvement, whereas the BT-MPDA@FA-Gel group exhibited less inflammatory infiltration and improved tissue organization, particularly at Day 21.
Figure 7. Histological and inflammatory evaluation of RISI following treatment. (a) Representative H&E-stained skin sections collected at Days 7 and 21. (b) Representative Masson’s trichrome-stained skin sections collected at Days 7 and 21. (c–e) ELISA measurements of TNF-α, IL-1β, and IL-4 levels in wound tissues, respectively. (f) Quantification of epidermal thickness. (g) Quantification of inflammatory cell density. (h) Quantification of collagen fiber coherency. Data are presented as mean ± SD (n = 3). Quantitative data were analyzed using two-way ANOVA, followed by Dunnett’s multiple-comparisons test for comparisons with the X-ray group and Tukey’s multiple-comparisons test for pairwise comparisons among treatment groups at each time point. # p < 0.05, ## p < 0.01, and #### p < 0.0001 versus the X-ray group; * p < 0.05, ** p < 0.01, *** p < 0.001, and **** p < 0.0001 for pairwise comparisons among treatment groups.
Quantitative analysis showed that epidermal thickness was greater in the FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel groups than in the X-ray group at both time points (Figure 7f). Inflammatory cell density was also lower in all three treatment groups than in the X-ray group, with the BT-MPDA@FA-Gel group exhibiting the lowest values among the treatment groups at both time points (Figure 7g). Collagen fiber coherency analysis revealed time-dependent differences in fiber alignment among the groups (Figure 7h). At Day 7, coherency in the X-ray group was higher than that in the Control, FA-Gel, and BT-MPDA groups, whereas no significant difference was observed between the X-ray and BT-MPDA@FA-Gel groups. By Day 21, coherency in the BT-MPDA and BT-MPDA@FA-Gel groups was higher than that in the X-ray group, and both groups exhibited higher values than the FA-Gel group. No significant difference was detected between the BT-MPDA and BT-MPDA@FA-Gel groups. These findings indicate that BT-MPDA@FA-Gel treatment was associated with improved epidermal recovery, reduced inflammatory cell infiltration, and time-dependent changes in collagen fiber organization.
To further evaluate the regulatory effect of BT-MPDA@FA-Gel on the local inflammatory status of RISI wounds, the levels of TNF-α, IL-1β, and IL-4 in wound tissues were determined by ELISA (Figure 7c–e). During wound healing, multiple cytokines are involved in the local inflammatory response and its regulation. TNF-α and IL-1β are well-established pro-inflammatory cytokines, whereas IL-4 is generally considered an anti-inflammatory and immunoregulatory cytokine involved in type 2 immune responses and tissue repair [45]. Previous studies of RISI have also evaluated TNF-α, IFN-γ, and IL-4 in wound tissues to characterize changes in local inflammation-associated cytokines following radiation injury [46]. Compared with the healthy control group, the X-ray group exhibited increased levels of TNF-α and IL-1β, together with a decreased level of IL-4, at days 7, 14, and 21, indicating abnormal changes in inflammation-associated cytokine levels in the wound tissues following radiation exposure. Compared with the X-ray group, BT-MPDA@FA-Gel treatment significantly decreased the levels of TNF-α and IL-1β while increasing the level of IL-4. These findings indicate that BT-MPDA@FA-Gel modulates the levels of pro-inflammatory and immunoregulatory cytokines in RISI wounds, thereby improving the abnormal local inflammatory cytokine profile following radiation injury.

3.10. In Vivo Biosafety Evaluation

H&E staining was performed to examine the heart, liver, spleen, lungs, and kidneys of mice from each group. As shown in Figure 8a, the major organs in the Control, X-ray, FA-Gel, BT-MPDA, and BT-MPDA@FA-Gel groups exhibited generally intact tissue architecture, with no obvious structural disruption, cellular abnormalities, or other prominent pathological changes. In addition, no significant differences were observed in the indices of the heart, liver, spleen, lungs, or kidneys among the groups (Figure 8b), further indicating that the treatments did not cause obvious changes in the major organs. These results demonstrated that, during the 21-day treatment period, the treatments did not cause obvious histopathological alterations in the major organs or significant changes in the corresponding organ indices, supporting the favorable histocompatibility of the developed nanoparticle and hydrogel system.
Figure 8. Histological evaluation of the in vivo safety of the BT-MPDA@FA-Gel system. (a) H&E staining images of the major organs (heart, liver, spleen, lungs, and kidneys) after 21 days of treatment; (b) organ indices of the major organs.
To further evaluate the in vivo biosafety of the developed nanoparticles and hydrogel system, hematological, serum biochemical, and histopathological analyses were performed after the treatment period. As shown in Figure 9a–f, significant differences were observed in WBC, RBC, and PLT levels among the groups, whereas no significant differences were detected in HGB, HCT, or MCV. Compared with the Control group, the X-ray group exhibited significantly higher WBC, RBC, and PLT levels. The PLT levels in the FA-Gel and BT-MPDA groups were also significantly higher than those in the Control group, whereas no significant difference was observed in the BT-MPDA@FA-Gel group. These results indicate that no statistically significant differences in the examined hematological parameters were detected between the BT-MPDA@FA-Gel and Control groups.
Figure 9. Hematological and serum biochemical evaluation of the BT-MPDA@FA-Gel system. (a–f) Hematological analysis, including WBC, RBC, HGB, PLT, HCT, and MCV; (g–j) serum biochemical analysis, including AST, ALT, CREA, and UREA. Data are presented as the mean ± SD (n = 5). Statistical significance was determined using one-way ANOVA followed by Tukey’s multiple comparisons test. Each group was compared with the control group. * p < 0.05, ** p < 0.01, **** p < 0.0001; ns, not significant.
Further analysis of serum biochemical parameters revealed no significant differences in AST levels among the groups (Figure 9g). In contrast, significant differences were observed in ALT, CREA, and UREA levels (Figure 9h–j). Compared with the Control group, the X-ray group exhibited significantly elevated levels of ALT, CREA, and UREA, whereas no significant differences were observed between the FA-Gel, BT-MPDA, or BT-MPDA@FA-Gel groups and the Control group. These findings suggest that no statistically significant alterations in the examined serum biochemical parameters were detected in the BT-MPDA@FA-Gel group compared with the Control group.

4. Conclusions

In this study, a dual-crosslinked nanocomposite hydrogel (BT-MPDA@FA-Gel) was developed by integrating FA and BT-MPDA nanoparticles into a CSMA/OKGM network to address the complex pathological features of RISI. The dual-crosslinked network combined dynamic adaptability with structural stability, providing a matrix for the local delivery of therapeutic components. Drug-release studies demonstrated pH-responsive release of both BT and FA, while NIR irradiation further enhanced BT release. The hydrogel also exhibited ROS-scavenging activity, antibacterial activity, and NIR-enhanced photothermal antibacterial activity, together with favorable cytocompatibility and hemostatic performance in vitro. In a murine RISI model, BT-MPDA@FA-Gel accelerated wound closure, attenuated inflammatory responses, promoted collagen deposition, and enhanced tissue regeneration. Collectively, these findings highlight the potential of integrating responsive drug delivery and photothermal antibacterial functionality within a dual-crosslinked hydrogel platform for the treatment of RISI.
NIR irradiation enhanced BT release from the MPDA carrier, potentially through photothermal heating. As temperature can influence drug diffusion and transport within hydrogel networks, further studies will investigate the mechanisms by which photothermal heating regulates BT release. In addition, different sterilization methods may affect the physicochemical properties and biological performance of hydrogel systems. Future work will explore an appropriate sterilization strategy that preserves the properties and functionality of BT-MPDA@FA-Gel to facilitate its further translational development. Furthermore, the effects of NIR-induced photothermal heating on cell viability and blood compatibility require further investigation to establish the biosafety of the hydrogel under therapeutic conditions.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/pharmaceutics18121522/s1: Figure S1: FT-IR spectra of MPDA, NH2-mPEG2000, and PEG-MPDA; Figure S2: Strain-amplitude sweep of the BT-MPDA@FA-Gel hydrogel, showing G′ and G″ as a function of strain; Figure S3: Step-strain rheological test of the BT-MPDA@FA-Gel hydrogel, showing the changes in G′ and loss modulus G″ during repeated high-strain perturbation and subsequent recovery under low-strain conditions.

Author Contributions

Conceptualization, M.G.; methodology, J.Z., R.W., R.Z. and Y.B.; software, M.W.; validation, L.C.; formal analysis, Y.W.; writing—original draft preparation, J.Z. and M.W.; writing—review and editing, R.W., R.Z., Y.B., Y.W., L.C. and M.G.; visualization, R.W. and M.W.; supervision, J.Z., L.C. and M.G.; project administration, L.C. and M.G. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

The animal study protocol was approved by the Ethics Committee of Zhengzhou University (protocol code 26-YXY-010; approval date: 10 February 2026).

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Dadkhahfar, S.; Farokh, P.; Demehri, S.; Nazarian, R.M. Radiation-Induced Skin Injury: Mechanisms, Clinical Manifestations, and Management. Int. J. Dermatol. 2026, 65, 963–973. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Cui, J.; Wang, T.-J.; Zhang, Y.-X.; She, L.-Z.; Zhao, Y.-C. Molecular biological mechanisms of radiotherapy-induced skin injury occurrence and treatment. Biomed. Pharmacother. 2024, 180, 117470. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  3. Singh, M.; Alavi, A.; Wong, R.; Akita, S. Radiodermatitis: A Review of Our Current Understanding. Am. J. Clin. Dermatol. 2016, 17, 277–292. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Kost, Y.; Deutsch, A.; Mieczkowska, K.; Nazarian, R.; Muskat, A.; Hosgood, H.D.; Lin, J.; Daily, J.P.; Ohri, N.; Kabarriti, R.; et al. Bacterial Decolonization for Prevention of Radiation Dermatitis: A Randomized Clinical Trial. JAMA Oncol. 2023, 9, 940–945. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Hao, J.; Sun, M.; Li, D.; Zhang, T.; Li, J.; Zhou, D. An IFI6-based hydrogel promotes the healing of radiation-induced skin injury through regulation of the HSF1 activity. J. Nanobiotechnol. 2022, 20, 288. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  6. Fu, Y.; Yuan, Y.; Zeng, C.; Lai, S.; Yuan, L.; Mu, Y. MXene-Integrated Dual Network Hydrogel Accelerates Radiation-Combined Wound Healing through Modulating Oxidative Stress and Immune Response. ACS Appl. Mater. Interfaces 2025, 17, 51671–51690. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  7. Zhou, D.; Du, M.; Luo, H.; Ran, F.; Zhao, X.; Dong, Y.; Zhang, T.; Hao, J.; Li, D.; Li, J. Multifunctional mesoporous silica-cerium oxide nanozymes facilitate miR129 delivery for high-quality healing of radiation-induced skin injury. J. Nanobiotechnol. 2022, 20, 409. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Dong, J.; Lang, Y.; He, J.; Cui, J.; Liu, X.; Yuan, H.; Li, L.; Zhou, M.; Wang, S. Phycocyanin-based multifunctional microspheres for treatment of infected radiation-induced skin injury. Biomaterials 2025, 317, 123061. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Liu, Y.; Ai, K.; Lu, L. Polydopamine and Its Derivative Materials: Synthesis and Promising Applications in Energy, Environmental, and Biomedical Fields. Chem. Rev. 2014, 114, 5057–5115. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Nath, J.; Philips, R.; Pilli, J.; Bhattacharjee, A. Polydopamine-based Surface Modifications for Tissue Engineering and Biosensing: From Understanding Chemistry to Diverse Applications. JOM 2025, 77, 4312–4327. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  11. Cerqueira, A.F.L.W.; de Mello Brandão, H.; Tavares, G.D.; Rodarte, M.P. Ferulic Acid: A Review of Mechanisms of Action, Absorption, Toxicology, Application on Wound Healing. Anti-Inflamm. Anti-Allergy Agents Med. Chem. 2024, 23, 205–214. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  12. Ma, C.; Du, L.; Guo, Y.; Yang, X. A review of polysaccharide hydrogels as materials for skin repair and wound dressing: Construction, functionalization and challenges. Int. J. Biol. Macromol. 2024, 280, 135838. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  13. Li, A.; Ma, B.; Hua, S.; Ping, R.; Ding, L.; Tian, B.; Zhang, X. Chitosan-based injectable hydrogel with multifunction for wound healing: A critical review. Carbohydr. Polym. 2024, 333, 121952. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Jain, A.; Sarsaiya, S.; Gong, Q.; Wu, Q.; Shi, J. Amorphophallus konjac: Traditional uses, bioactive potential, and emerging health applications. Front. Plant Sci. 2025, 16, 1530814. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Kulkarni, D.; Agnihotri, V.; Bhinge, S.; Ban, M.; Bari, D.; Pardeshi, C.V. Konjac glucomannan: A functional biopolymer for multifaceted drug delivery applications. Polym. Adv. Technol. 2024, 35, e6512. [Google Scholar] [CrossRef] [Scilit]
  16. Gu, H.; Li, H.; Wei, L.; Lu, J.; Wei, Q. Collagen-based injectable and self-healing hydrogel with multifunction for regenerative repairment of infected wounds. Regen. Biomater. 2023, 10, rbad018. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  17. Wu, Y.; Xu, W.; Li, J.; Zhong, Z.; Huang, L.; Li, S.; Tan, H. Influence of tannic acid post-treatment on the degradation and drug release behavior of Schiff base crosslinked konjac glucomannan/chitosan hydrogel. Eur. Polym. J. 2024, 202, 112592. [Google Scholar] [CrossRef] [Scilit]
  18. Yang, J.; Du, L.; Guo, J.; Zhang, L.; Wang, S.; Wang, X. Injectable carboxymethyl chitosan/konjac glucomannan/catechin hydrogel with free radical-scavenging, antimicrobial, and pro-healing abilities for infected wound repair. Int. J. Biol. Macromol. 2025, 308, 142572. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  19. Fairbanks, B.D.; Schwartz, M.P.; Bowman, C.N.; Anseth, K.S. Photoinitiated polymerization of PEG-diacrylate with lithium phenyl-2,4,6-trimethylbenzoylphosphinate: Polymerization rate and cytocompatibility. Biomaterials 2009, 30, 6702–6707. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. Cheng, C.; Peng, X.; Luo, Y.; Shi, S.; Wang, L.; Wang, Y.; Yu, X. A photocrosslinked methacrylated carboxymethyl chitosan/oxidized locust bean gum double network hydrogel for cartilage repair. J. Mater. Chem. B. 2023, 11, 10464–10481. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Fan, L.; Yi, J.; Tong, J.; Zhou, X.; Ge, H.; Zou, S.; Wen, H.; Nie, M. Preparation and characterization of oxidized konjac glucomannan/carboxymethyl chitosan/graphene oxide hydrogel. Int. J. Biol. Macromol. 2016, 91, 358–367. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  22. Zhu, L.; Chen, J.; Mao, X.; Tang, S. A γ-PGA/KGM-based injectable hydrogel as immunoactive and antibacterial wound dressing for skin wound repair. Mater. Sci. Eng. C 2021, 129, 112374. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  23. Qin, P.; Meng, Y.; Yang, Y.; Gou, X.; Liu, N.; Yin, S.; Hu, Y.; Sun, H.; Fu, Z.; Wang, Y.; et al. Mesoporous polydopamine nanoparticles carrying peptide RL-QN15 show potential for skin wound therapy. J. Nanobiotechnol. 2021, 19, 309. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  24. Hong, J.; Tang, Y.; Zhou, M.; Deng, J.; Hu, H.; Xu, D. Polyethylene glycol-modified mesoporous polydopamine nanoparticles co-loaded with dimethylcurcumin and indocyanine green for combination therapy of castration-resistant prostate cancer. J. Drug Deliv. Sci. Technol. 2022, 69, 103158. [Google Scholar] [CrossRef] [Scilit]
  25. Zhang, L.; Yang, P.; Guo, R.; Sun, J.; Xie, R.; Yang, W. Multifunctional Mesoporous Polydopamine with Hydrophobic Paclitaxel For Photoacoustic Imaging-Guided Chemo-Photothermal Synergistic Therapy. Int. J. Nanomed. 2019, 14, 8647–8663. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Marklund, S.; Marklund, G. Involvement of the Superoxide Anion Radical in the Autoxidation of Pyrogallol and a Convenient Assay for Superoxide Dismutase. Eur. J. Biochem. 1974, 47, 469–474. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Jang, W.H.; Shim, S.; Wang, T.; Yoon, Y.; Jang, W.S.; Myung, J.K.; Park, S.; Kim, K.H. In vivo characterization of early-stage radiation skin injury in a mouse model by two-photon microscopy. Sci. Rep. 2016, 6, 19216. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  28. Cox, J.D.; Stetz, J.; Pajak, T.F. Toxicity criteria of the Radiation Therapy Oncology Group (RTOG) and the European organization for research and treatment of cancer (EORTC). Int. J. Radiat. Oncol. Biol. Phys. 1995, 31, 1341–1346. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Bucciarelli, A.; Selicato, N.; Coricciati, C.; Rainer, A.; Capodilupo, A.L.; Gigli, G.; Moroni, L.; Polini, A.; Gervaso, F. Modelling methacrylated chitosan hydrogel properties through an experimental design approach: From composition to material properties. J. Mater. Chem. B 2024, 12, 10221–10240. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  30. Maiz-Fernández, S.; Pérez-Álvarez, L.; Silván, U.; Vilas-Vilela, J.L.; Lanceros-Mendez, S. Photocrosslinkable and self-healable hydrogels of chitosan and hyaluronic acid. Int. J. Biol. Macromol. 2022, 216, 291–302. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  31. Korkiatithaweechai, S.; Umsarika, P.; Praphairaksit, N.; Muangsin, N. Controlled release of diclofenac from matrix polymer of chitosan and oxidized konjac glucomannan. Mar. Drugs 2011, 9, 1649–1663. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  32. Sun, A.; Hu, D.; He, X.; Ji, X.; Li, T.; Wei, X.; Qian, Z. Mussel-inspired hydrogel with injectable self-healing and antibacterial properties promotes wound healing in burn wound infection. NPG Asia Mater. 2022, 14, 86. [Google Scholar] [CrossRef] [Scilit]
  33. Dai, G.; Chu, J.C.H.; Chan, C.K.W.; Choi, C.H.J.; Ng, D.K.P. Reactive oxygen species-responsive polydopamine nanoparticles for targeted and synergistic chemo and photodynamic anticancer therapy. Nanoscale 2021, 13, 15899–15915. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  34. Zhao, X.; Wu, H.; Guo, B.; Dong, R.; Qiu, Y.; Ma, P.X. Antibacterial anti-oxidant electroactive injectable hydrogel as self-healing wound dressing with hemostasis and adhesiveness for cutaneous wound healing. Biomater. 2017, 122, 34–47. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. Zhang, X.; Li, F.; Li, Z.; Bai, Y. Mussel-inspired strong and tough hydrogel with self-adhesive properties based on dynamic interactions for flexible wearable electronics. J. Mater. Chem. A 2025, 13, 5304–5314. [Google Scholar] [CrossRef] [Scilit]
  36. Nasra, S.; Patel, M.; Shukla, H.; Bhatt, M.; Kumar, A. Functional hydrogel-based wound dressings: A review on biocompatibility and therapeutic efficacy. Life Sci. 2023, 334, 122232. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  37. Zhong, Y.; Wei, E.-T.; Wu, L.; Wang, Y.; Lin, Q.; Wu, N.; Chen, H.; Tang, N. Novel Biomaterials for Wound Healing and Tissue Regeneration. ACS Omega 2024, 9, 32268–32286. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  38. Yu, X.; Yang, T.; Bei, Z.; Liu, J.; Song, Y.; Wang, Q.; Li, J.; Liang, S.; Qian, Z. Microenvironment-responsive injectable dynamic hydrogel for sequential antioxidant and tissue regeneration therapy of radiation-induced skin injury. Bioact. Mater. 2026, 63, 778–794. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  39. Rembe, J.-D.; Witte, M.; Ertas, N.; Dissemond, J.; Garabet, W.; Hovhannisyan, M.; Beckamp, K.; Schelzig, H.; Wagenhäuser, M.U.; Stuermer, E.K. PH profiling reveals progressive wound acidification during healing and higher pH in chronic non-healing wounds: A prospective, multicenter cohort study. Sci. Rep. 2026, 16, 10522. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  40. Liu, J.; Han, X.; Zhang, T.; Tian, K.; Li, Z.; Luo, F. Reactive oxygen species (ROS) scavenging biomaterials for anti-inflammatory diseases: From mechanism to therapy. J. Hematol. Oncol. 2023, 16, 116. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  41. Zheng, M.; Liu, Y.; Zhang, G.; Yang, Z.; Xu, W.; Chen, Q. The Antioxidant Properties, Metabolism, Application and Mechanism of Ferulic Acid in Medicine, Food, Cosmetics, Livestock and Poultry. Antioxidants 2024, 13, 853. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  42. Raafat, D.; von Bargen, K.; Haas, A.; Sahl, H.G. Insights into the mode of action of chitosan as an antibacterial compound. Appl. Environ. Microbiol. 2008, 74, 3764–3773. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  43. Hou, Z.; Yang, M.; Huang, L.; Xin, S.; Yang, H.; Hou, J. Polydopamine-based nanospheres as nanoplatforms to kill Staphylococcus aureus and to promote wound healing by photothermal therapy. Front. Chem. 2022, 10, 1111701. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  44. Zhang, B.; Wang, M.; Tian, H.; Cai, H.; Wu, S.; Jiao, S.; Zhao, J.; Li, Y.; Zhou, H.; Guo, W.; et al. Functional hemostatic hydrogels: Design based on procoagulant principles. J. Mater. Chem. B 2024, 12, 1706–1729. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  45. Allen, J.E. IL-4 and IL-13: Regulators and Effectors of Wound Repair. Annu. Rev. Immunol. 2023, 41, 229–254. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  46. Hao, Y.; Li, H.; Guo, J.; Wang, D.; Zhang, J.; Liu, J.; Yang, C.; Zhang, Y.; Li, G.; Liu, J. Bio-Inspired Antioxidant Heparin-Mimetic Peptide Hydrogel for Radiation-Induced Skin Injury Repair. Adv. Healthc. Mater. 2023, 12, 2203387. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.