Skip to Content
MaterialsMaterials
  • Article
  • Open Access

26 November 2026

22 Pages

Ultrasonic-Assisted Brazing and Mechanical Behavior of Aluminum Foam Sandwiches with Al or Cu Face Sheets

,
,
and
1
School of Mechanical Engineering, Shandong Huayu University of Technology, Dezhou 253034, China
2
Faculty of Manufacturing and Mechatronic Engineering Technology, Universiti Malaysia Pahang Al-Sultan Abdullah, Pekan 26600, Pahang, Malaysia
3
School of Mechanical Engineering, Shandong University of Technology, Zibo 255000, China
4
Shandong Hongyu Ventilator Limited Company, Zibo 255300, China
Materials2026, 19(23), 5033;https://doi.org/10.3390/ma19235033 
(registering DOI)
This article belongs to the Section Metals and Alloys

Abstract

Aluminum foam sandwiches (AFSs) are of interest for lightweight transport structures. AFSs with 1060 Al or pure Cu face sheets (Al-AFS and Cu-AFS) were fabricated by pure-Zn precoating and ultrasonic-assisted brazing (UAB). Conventional brazing provided a reference for interfacial characterization and assembly tensile testing; quasi-static compression and three-point bending were evaluated for UAB structures. After 15 s of ultrasonication, Al-rich and Zn-rich regions became less clearly separated in the examined Al-AFS sections, whereas the Cu-side reaction region developed a wavy or scalloped boundary with less pronounced columnar extensions. Mean nominal assembly tensile strengths were 4.27–6.09 MPa, with failure within the foam core. In the five plotted compression specimens, plateau stress ranged from 8.00 to 24.33 MPa and increased with parent foam-core density within each face-sheet series. Across the five groups (three specimens each), mean cumulative volumetric energy absorption at a strain of approximately 0.70 ranged from 14.36 to 29.41 MJ/m3. Under short-span bending, photographs of three specimens documented prolonged indentation and cell collapse in Al-B1, tensile-face cracking in Al-B2, and core cracking with local lower-face separation in Cu-B3. The Cu-faced specimens carried the higher peak load in each core-density class. When normalized by total specimen mass, peak load was higher for the Al-faced specimens in the low- and medium-density pairs and for the Cu-faced specimen in the high-density pair. Each material–density combination was represented by one bending specimen.

1. Introduction

Lightweight transport structures must combine load-bearing capacity with energy absorption for impact protection. Closed-cell aluminum foams dissipate deformation energy through cell-wall bending and progressive collapse, with their mechanical response governed by relative density and pore architecture [1]. An aluminum foam sandwich (AFS) comprises a foam core bonded to two dense face sheets. The face sheets primarily carry the normal stresses induced by bending, while the core maintains their separation and transfers shear loads. Compression studies of integrally formed AFSs have shown that loading direction influences the interaction between cell-wall deformation and face-sheet constraint [2]. The potential use of AFSs in lightweight vehicle bodies has stimulated research into structural design and manufacturing routes [3]. Effective face-to-core bonding sustains local load transfer, whereas premature separation at the joint changes the subsequent damage path.
AFSs can be produced either by foaming a composite precursor into an integral sandwich or by joining face sheets to a prefabricated foam core. The latter route offers flexibility in face-sheet selection but requires stable contact between a dense sheet and discrete foam cell walls. Solid cell-wall sections and open pores alternate across the cut foam surface, where oxide films and irregular gaps restrict filler spreading. Surface abrasion and vibration assistance have been used for fluxless joining of AFSs [4], and the choice of Zn-based joining material affects the interlayer microstructure in aluminum-sheet/aluminum-foam joints [5]. Hot pressing can establish metallurgical face-to-core bonding [6], whereas the interfaces in integrally formed structures evolve during precursor processing and foaming [7]. Mechanical stirring can promote bonding to a prefabricated foam core by activating the surfaces during Zn-based joining [8]. Studies of AFSs with aluminized steel face sheets show that changing the face-sheet material also changes the interfacial reactions and local deformation in adjacent regions [9]. The precoating procedure therefore needs to accommodate the corresponding interfacial reaction conditions.
Ultrasonic excitation can modify liquid-filler spreading and renew interfacial contact. High-speed observations and acoustic-field analyses have shown that the local cavitation distribution affects droplet wetting on Al substrates [10], while cavitation erosion is closely associated with oxide-film fragmentation [11]. These effects enable fluxless joining in air using Zn–Al fillers [12]. Replacing an Al/Al configuration with Al/Cu introduces a Cu-side reaction region and a more complex interfacial evolution. Reaction products in Al/Cu joints vary with ultrasonic duration [13], and ultrasonic amplitude affects both oxide-film disruption and reaction-layer morphology in aluminum-foam/Cu joints made with a semimolten Zn–14Al filler [14]. These studies have mainly employed Al-containing fillers. With pure Zn precoating, however, the seam acquires Al from the substrates during precoating and remelting. The choice of Al or Cu face sheets therefore changes the solute supply and interfacial reaction conditions, which may affect the microstructure formed during subsequent ultrasonic-assisted joining.
At the structural level, the mechanical compatibility of the face sheets and core shapes the response to three-point bending. It influences the sequence of local indentation and core failure, as well as the subsequent development of face-sheet cracking or separation [15,16]. The face-sheet failure mode affects the post-peak load response, as shown in sandwich beams with composite face sheets [17]. Pore architecture and face-sheet thickness jointly influence peak load and sustained deformation [18,19]. In situ imaging has linked bending orientation to nonuniform deformation in integrally formed AFSs [20], while digital image correlation has resolved crack development in different core architectures during elevated-temperature bending [21]. Experimental and finite-element studies of metallurgically bonded steel-faced AFSs and composite beams likewise connect face-sheet constraint with core deformation [22]. For Al- and Cu-faced AFSs, changing the face-sheet material alters both the joint microstructure and specimen mass. Peak load describes the maximum load-bearing capacity. The post-peak response captures continued energy dissipation, and the complete load–displacement history, together with specimen mass, determines how specific energy absorption evolves.
This study examines Al supply and interfacial evolution during the remelting of pure Zn precoatings. AFSs with 1060 Al or pure Cu face sheets (Al-AFS and Cu-AFS, respectively) were fabricated by pure Zn precoating and ultrasonic-assisted brazing (UAB). The Al-AFS seam receives Al from both the face sheet and foam core, whereas the Cu-AFS seam receives Al mainly from the foam and develops a reaction region at the Cu interface. Cross sections of conventionally and ultrasonically brazed joints were compared to evaluate the distribution of Al-rich and Zn-rich constituents and the morphology of the Cu-side reaction region. Energy-dispersive X-ray spectroscopy (EDS) point analyses supplemented these comparisons; line scans characterized the precoated interfaces. Joint tensile tests examined fracture behavior. Compression and bending tests then characterized the UAB structures, with individual bending histories used to relate damage development to load retention and energy absorption.

2. Materials and Methods

2.1. Materials and Zn Precoating

The core material was closed-cell aluminum foam (AF) produced by melt foaming, using 1060 Al as the matrix, TiH2 (supplied by Beijing Xingrongyuan Technology Co., Ltd., Beijing, China) as the blowing agent, and Ca (supplied by Shanghai Hansi Chemical Co., Ltd., Shanghai, China) as the thickening agent.
Before use, the TiH2 blowing agent was pre-oxidized at 400–450 °C for 15–20 min. Ca particles (1.5 wt.%) were added to the aluminum melt at 730 °C and incorporated by mechanical stirring to increase the melt viscosity. Following thickening, TiH2 powder (1.5 wt.%) was introduced and dispersed by stirring at 1500 r/min. The foamable melt was held for 2 min in a furnace maintained at 700 °C, followed by cooling with ice water.
Foam blocks measuring 50 × 50 × 10 mm3 were cut by wire electrical discharge machining and had core densities of approximately 0.30–0.80 g/cm3. After cutting, the foam blocks were cleaned with ethanol (supplied by Baiyu Chemical Reagents and Glassware, Zibo, China) to remove residual machining fluid and surface debris. The face sheets were 1060 Al (supplied by Zibo Yuetao Metal Materials Company, Zibo, China) or pure Cu (supplied by Dongguan Tongrun Copper and Aluminum Materials Co., Ltd., Dongguan, China), each measuring 50 × 50 mm2 and 1 mm thick. Pure Zn (supplied by Hefei Shushan District Tehe Metal Materials Store, Hefei, China) was used as the filler metal. Each sandwich specimen contained two face sheets of the same metal; the Al-faced and Cu-faced specimens are designated Al-AFS and Cu-AFS, respectively.
Before joining, the foam core was weighed and its core density, ρc, was calculated as mass divided by the external volume. After joining and cutting, structural density, ρs, was calculated from the complete specimen mass and prescribed external volume: 1.2 cm3 for compression and 6.0 cm3 for AFS bending specimens. The mass included both face sheets, the foam core, and retained filler. Table 1 gives the low-, medium-, and high-core-density ranges used to classify the bending specimens; the compression results are identified by the pre-brazing densities of their parent foam blocks. Core porosity was estimated as (1 − ρc/2.70) × 100%, using 2.70 g/cm3 for the density of 1060 Al.
Table 1. Core-density and structural-density ranges used to classify the bending specimens, with estimated core porosity.
The Zn precoating procedure is illustrated in Figure 1. The mating surfaces of the aluminum foam and Al face sheets were abraded with 400-grit paper, ultrasonically cleaned in ethanol for 5 min, and dried. Each complete 50 × 50 mm2 face-sheet/core interface received 2 g of pure Zn before specimen cutting. Zn pieces were placed on the mating surfaces and heated from above with a butane torch. An infrared thermometer (DT8550FCT; Shenzhen Cheerman Technology Co., Ltd., Shenzhen, China), directed at the heated external surface, indicated approximately 430–460 °C during precoating. This is reported as an apparent surface temperature because substrate-specific emissivity calibration and the buried-interface thermal history were unavailable. Once the Zn melted, a steel blade was drawn across the surface to spread the liquid over the Al sheet and exposed solid cell walls. The Cu face sheets were also precoated with Zn before assembly. Representative precoated surfaces and a fabricated AFS specimen are shown in Figure 2. The two interfaces therefore received 4 g in total per full sandwich before cutting. The Zn retained in an individual test piece was not weighed separately.
Figure 1. Zn precoating by flame heating from above: (a) Al face sheet and (b) aluminum foam.
Figure 2. Representative surfaces and fabricated AFS: (a) Zn-precoated Al face sheet, (b) Zn-precoated aluminum foam, and (c) assembled sandwich structure.

2.2. Ultrasonic-Assisted Brazing

The face sheets and foam core were stacked with their precoated surfaces facing each other and flame-heated from above. Visible Zn remelting marked the start of 15 s of ultrasonic excitation using a GN-20Pro device (Shenzhen Quantum Acoustics Technology Co., Ltd., Shenzhen, China). Its nominal power and frequency were 100 W and 36 kHz, respectively, with a 20 mm-diameter sonotrode tip. The tip contacted the center of the exposed face sheet and remained at that position throughout the 15 s treatment, without lateral movement. Contact was maintained under the device self-weight of approximately 450 g, corresponding to a nominal static pressure of approximately 14 kPa if the full circular tip area is in contact. Heating continued for approximately 1 min from the onset of remelting, followed by air cooling to room temperature. Joining was performed in air without flux. Actual tip displacement and time-resolved temperature at the buried interface were not measured. The fixed tip position, nominal settings, and visible remelting criterion specify the procedure; local pressure and thermal histories were not measured for individual assemblies.
Conventional brazing and ultrasonic-assisted brazing are abbreviated as CB and UAB, respectively. The CB specimens underwent the same precoating and remelting procedure, without ultrasonic vibration during the second heating stage. Interfacial characterization and joint tensile testing were performed for both joining routes, whereas all compression and three-point bending specimens were fabricated by UAB. The labels Al–CB, Al–UAB, Cu–CB, and Cu–UAB identify the face-sheet material and joining route in the figures.

2.3. Microstructural Characterization

Cross sections were prepared from the precoated and joined specimens. AFS specimens for metallographic examination measured 10 × 10 × 12 mm3, with the observation plane passing through the face sheet, brazed seam, and foam core. The specimens were sequentially ground with 400-, 1000-, 1500-, and 2000-grit paper, polished, and etched in 4% nitric acid in ethanol (Guangzhou Pinyi Metallographic Technology Co., Ltd., Guangzhou, China) for 3–6 s. Interfacial morphology was examined using an SDPTOP XD30M optical microscope (Ningbo Sunny Instruments Co., Ltd., Yuyao, China) and a Quanta 250 scanning electron microscope (SEM; FEI, Hillsboro, OR, USA). An EDS system (EDAX, Mahwah, NJ, USA) provided local elemental compositions, and line scans were collected at the precoated interfaces. Point-analysis results are reported as mass fractions (wt.%) at the selected EDS sites. Cross-sectional contrast and composition were assessed together to describe Al-rich and Zn-rich constituents and the Cu-side reaction region in the examined fields. The overview images show the contact contour; higher magnifications show the face-sheet side, the foam side, and the seam center. EDS sites identify regions of contrasting appearance within those fields. These local observations do not establish how often a feature occurred across independently prepared joints.

2.4. Mechanical Testing

Joint tensile tests used the bridging configuration shown in Figure 3, in which a 40 × 10 × 10 mm3 aluminum foam block joined two coplanar metal sheets. The sheets were pulled apart in their plane using an MTS Exceed universal testing machine (MTS Systems (China) Co., Ltd., Shenzhen, China) at room temperature and a crosshead speed of 1 mm/min. The foam cores were not selected or allocated to CB and UAB on the basis of density. Their densities were determined after wire cutting; the two routes were not tested as density-matched pairs. Three specimens were tested per group, and the peak load and fracture location were recorded. The nominal assembly tensile strength was calculated as the peak load divided by the joining area. This value characterizes the foam-bridged assembly under the loading configuration in Figure 3. Tensile results are reported as the arithmetic mean ± sample standard deviation (SD) of three independent specimens; SD was calculated with a denominator of n − 1.
Figure 3. Geometry and loading direction of the tensile specimen, with aluminum foam bridging two coplanar metal sheets.
Compression specimens had nominal dimensions of 10 × 10 × 12 mm3 (Figure 4) and were loaded through the AFS thickness using an MTS Exceed universal testing machine at room temperature and 1 mm/min. Three Al-AFS groups and two Cu-AFS groups were tested, with three specimens per group (15 in total). The compression specimens were identified by the density of the parent foam block measured before joining; these groups were independent of the bending classes. The recorded curves extend to approximately ε = 0.70, the common endpoint for cumulative energy comparisons. For each plotted compression specimen, plateau stress, σpl, was defined as the mean stress over ε = 0.20–0.40. The volumetric energy absorbed within this interval, wp, was calculated using Equation (1); stress in MPa gives wp in MJ/m3. The two plateau quantities refer to these individual curves; the endpoint energy measures are reported as group means ± sample SD (three specimens per group).
σ pl = 1 0.20 ∫ 0.20 0.40 σ ( ε )   d ε ,   w p = 0.20 σ pl  
Figure 4. Al-AFS and Cu-AFS specimens prepared for compression testing.
Cumulative volumetric energy absorption under compression, Wc, was obtained by integrating the stress–strain curve. Multiplication by the initial nominal external volume, V0 = 1.2 cm3, gives the total energy absorbed by a specimen in joules (1 MJ/m3 = 1 J/cm3). Dividing by that specimen’s complete mass, m, gives compressive specific energy absorption, SEAc, in J/g (Equation (2)). Equivalently, SEAc = Wc/ρs when structural density is in g/cm3. For each plotted specimen, the complete specimen mass was calculated as m = ρsV0. The structural densities for Al-C1, Al-C2, Al-C3, Cu-C1, and Cu-C2 were 1.318, 1.406, 1.526, 2.211, and 2.352 g/cm3, respectively. For the other two specimens in each group, mass was recovered by dividing the recorded volumetric energy by the corresponding mass-normalized index. The individual specific energy values are reported as group means and sample SDs.
W c ( ε ) = ∫ 0 ε σ ( ξ )   d ξ ,   SEA c = W c V 0 m
Three-point bending specimens had nominal dimensions of 50 × 10 × 12 mm3; the specimens and loading arrangement are shown in Figure 5. Tests were performed at room temperature using an MTS Exceed universal testing machine, a support span L of 40 mm, a loading-nose diameter of 10 mm, and a crosshead speed of 1 mm/min. The support span divided by the total specimen thickness was 40/12 = 3.33. The analysis includes six AFS load–displacement records, one per face-sheet material and core-density class, together with one bare-foam reference. Fmax is the maximum load over the complete recorded 0–10 mm interval, including any later load recovery. Equation (3) gives a nominal flexural stress based on specimen width b and total thickness h. This homogeneous-beam expression gives a nominal index for specimens of the stated geometry. It does not give the actual stress in either face sheet or resolve the local stresses beneath the loading nose.
σ b = 3 F max L 2 b h 2  
Figure 5. Three-point bending specimens and test arrangement: (a) specimens and (b) loading setup.
Bending absorbed energy, Eb, was calculated by integrating the load–displacement record, and specific energy absorption, SEAb, was obtained as Eb/m (Equation (4)). For AFS, m = ρsV with V = 6.0 cm3 and includes both face sheets, the foam core, and retained filler. The bare-foam reference has a mass of 2.660 g. Integration started at the first recorded point near zero displacement and ended at 10 mm, with interpolation at the endpoint. With load in N and displacement in mm, the integral was multiplied by 10−3 to obtain Eb in J; division by mass in g gives SEAb in J/g. The same mass was used to calculate Fmax/m in N/g.
E b ( δ ) = 10 − 3 ∫ δ 0 δ F ( x )   d x ,   SEA b = E b m
Here, δ0 is the first recorded displacement, close to zero. Bending results are reported for individual specimens. Symbols in the mechanical curve plots identify selected points along the recorded histories; the complete datasets were used for integration. With one AFS specimen per material–density combination, within-condition variability in peak load, absorbed energy, and specific energy absorption could not be estimated. Experimental data were plotted using Origin 2026 (OriginLab Corporation, Northampton, MA, USA).

3. Results and Discussion

3.1. Microstructure and Interfacial Contact After Zn Precoating

Zn precoating produced different contact configurations on the Al face sheets and the cut foam surfaces. On the Al sheet, a relatively continuous Zn-based coating formed above a largely planar Al/Zn interface (Figure 6a,c). The filler spread along the solid cell walls of the foam, with the apparent width of the Zn-rich coating varying along inclined cell walls. Large exposed cell openings remained unfilled (Figure 6b,d). Contact was therefore established along a planar interface on the face-sheet side and through the wetted cell walls and surrounding filler on the foam side.
Figure 6. Microstructures after Zn precoating: (a,c) Al/Zn, (b,d) foam/Zn, and (e,f) Cu/Zn interfaces. Panels (a,b,e) are optical micrographs, and panels (c,d,f) are SEM images. Chemical formulas denote candidate phases inferred from local EDS compositions and phase-equilibrium information. The red dashed arrows indicate the EDS line-scanning paths, the numbered crosses indicate EDS point-analysis sites, and the white arrows identify the annotated microstructural features. The dotted guides in (f) delineate the reaction regions.
EDS point analyses revealed an interspersed distribution of Al-rich and Zn-rich constituents within the precoatings (Table 2). On the Al-sheet side, point 1 in a plate-like region was predominantly Zn, whereas the adjacent points 2 and 3 contained 36.95 and 43.50 wt.% Al, respectively (Figure 6c). On the foam side, points 5 and 6 contained 29.84 and 57.09 wt.% Al, respectively, while point 7 was Zn-rich, consistent with the contrast between the acicular and lamellar constituents in Figure 6d. Local dissolution of the Al substrate during precoating altered the composition of the initially pure Zn melt, resulting in compositionally distinct regions after solidification. Ubertalli et al. [5] likewise reported that the microstructure of Zn-based joints between Al sheets and aluminum foam varied with local composition. The irregular geometry of the cell walls also produced nonuniform contact during manual spreading, further contributing to spatial variations in Al content.
Table 2. Selected EDS point compositions at the Zn-precoated interfaces in Figure 6 (wt.%).
Zn precoating established continuous contact with the Cu substrate (Figure 6e). A layered reaction region formed near the interface, where local microcracks were also observed (Figure 6f). Toward the Cu substrate, the Cu content rose from 6.48 wt.% at point 8 to 15.99 and 16.36 wt.% at points 9 and 10, respectively, and then to 37.98 wt.% at point 11 (Table 2). Point 13 adjacent to the substrate was predominantly Cu. The composition gradient was consistent with the layered morphology of the reaction region. The CuZn5, Cu5Zn8, and CuZn labels in Figure 6 and Figure 7 are tentative assignments based on the local EDS compositions and Cu–Zn phase equilibria [23]. EDS measures elemental composition; the crystal structures of the labeled regions were not independently verified by diffraction.
Figure 7. EDS line profiles across the Zn-precoated interfaces: (a) Al/Zn, (b) foam/Zn, and (c) Cu/Zn. Phase annotations denote candidates only; the measured quantities are elemental signals along the indicated paths (see also Table 2). The vertical dashed lines delineate the regions associated with the annotated candidate phases along the EDS scanning paths.
EDS line profiles across the precoated Al/Zn and foam/Zn interfaces showed alternating Al and Zn signals (Figure 7), corresponding to the Al-rich and Zn-rich regions identified in Table 2. Across the Cu/Zn interface, the Cu signal increased and the Zn signal decreased toward the substrate, with these changes occurring across the layered reaction region (Figure 6f). Thus, the spatial separation of Al–Zn constituents and the formation of a Cu–Zn reaction region during precoating established different initial microstructures for subsequent remelting at the two types of interface.

3.2. Effect of Ultrasonic-Assisted Brazing on the Al-AFS Seam Microstructure

Conventional brazing brought both Al-AFS substrates into contact with the filler. Distinct Al-rich and Zn-rich regions remained in the brazed seam (Figure 8a–d). Near the face sheet, point 2 contained 80.33 wt. % Al, point 4 contained 96.16 wt. % Zn, and point 5 contained 63.27 wt. % Al, demonstrating the alternating distribution of compositionally distinct regions (Table 3). Foam-side points 6 and 7 contained 76.36 and 96.32 wt. % Zn, respectively. Points 8 and 9 were predominantly Al. At the seam center, the Al contents at points 11, 12, and 13 were 63.27, 31.65, and 3.46 wt. %, respectively. Reheating remelted the opposing precoatings and brought them into contact, but local compositional differences persisted after solidification.
Figure 8. Interfacial microstructures of Al-AFS after conventional brazing ((a–d), upper block) and ultrasonic-assisted brazing ((e–h), lower block): (a,e) overall cross sections, (b,f) Al-side interfaces, (c,g) foam-side interfaces, and (d,h) seam centers. Numbered sites correspond to Table 3. Label key: AF, aluminum foam; α-Al and η-Zn, candidate constituents in Al-rich and Zn-rich regions, respectively; Zn–Al eutectic, a tentative interpretation of the fine morphology. The red dotted line in (a) marks the approximate boundary between the two compositionally distinct regions of the brazed seam.
Table 3. Selected EDS point compositions for Al-AFS in Figure 8 (wt.%).
After 15 s of ultrasonic excitation, Al-rich regions were interspersed with a fine region with two levels of SEM contrast, and the separation between compositionally distinct regions became less pronounced in the examined sections from the face-sheet side to the seam center (Figure 8e–h). Points 15 and 16 in Figure 8f contained 81.41 and 84.28 wt.% Al, respectively, while point 17 contained 94.51 wt. % Zn. On the foam side, point 19 contained 73.64 wt.% Al (Figure 8g). At the seam center, point 22 was Zn-rich and point 23 was Al-rich (Figure 8h and Table 3), with less sharply defined boundaries between the Al-rich and Zn-rich regions. Large exposed cell openings remained on the foam side, and local cracks occurred where these openings intersected the bonded contour (Figure 8e).
Figure 9 illustrates the proposed microstructural evolution of the Al-AFS seam. Precoating established metallic contact on the face sheet and portions of the cell walls. After remelting, ultrasonic agitation can promote liquid exchange near the solid–liquid interfaces. Li et al. [10,11] linked local flow and cavitation to oxide-film disruption, while Zhao et al. [24] also observed oxide-film fragmentation when joining Al-alloy laminates with a Zn interlayer. Both the face sheet and the foam core can supply Al to the Zn melt. Liquid flow can facilitate compositional exchange between the two remelted precoatings, thereby changing the spatial distribution of the Al-rich constituents upon solidification. This interpretation is consistent with the less distinct compositional regions observed in Figure 8.
Figure 9. Proposed interfacial evolution in Al-AFS during ultrasonic-assisted brazing and cooling: (a) initial separation of compositionally distinct regions, (b,c) redistribution of Al-rich regions, and (d) less distinct separation of Al-rich and Zn-rich constituents. Schematic, not to scale. The red dotted line in (a) represents the initial boundary between the compositionally distinct regions.
In addition, the exposed cell openings on the cut foam surface affected the spreading paths of the molten filler. In an independent brazing study of aluminum foam sandwiches, Wang et al. [25] observed filler wrapping partway around exposed cell walls. In the present specimens, the filler extended along the solid cell walls, while large cell openings and local gaps at their edges remained after ultrasonic treatment. The surface cell geometry therefore continued to govern the contour of the bonded region. A polished section intersects curved walls at different angles and can cut through either a wetted wall or the mouth of a cell. A local filler width therefore depends on section position and inclination. Counting open cell mouths as interfacial defects would also confound native porosity with incomplete bonding.

3.3. Evolution of the Cu-Side Reaction Region and Cu-AFS Seam Microstructure

Conventionally brazed Cu-AFS exhibited microstructural variations across the seam thickness (Figure 10a–d). In the field shown in Figure 10b, a band adjacent to Cu had columnar extensions projecting into the seam. Points 2 and 3 in Figure 10b contained 25.88 and 16.78 wt.⁠% Cu, respectively, with Zn accounting for most of the balance (Table 4). Within the seam, point 4 was predominantly Al and point 5 was predominantly Zn; on the foam side, points 7 and 8 contained 34.19 and 76.51 wt.% Al, respectively. Points 10, 11, and 12 in the seam center spanned compositions from Zn-rich to Al-rich. Voids were visible on the Cu side, and cracks occurred near exposed cell openings on the foam side (Figure 10a).
Figure 10. Interfacial microstructures of Cu-AFS after conventional brazing ((a–d), upper block) and ultrasonic-assisted brazing ((e–h), lower block): (a,e) overall cross sections, (b,f) Cu-side reaction regions, (c,g) foam-side interfaces, and (d,h) seam centers. The inset in (f) is a local enlargement. Numbered sites correspond to Table 4. Label key: AF, aluminum foam; Cu5Zn8 and CuZn5, candidate Cu–Zn phases. The numbered crosses mark EDS sites; the dotted guides in (b) delineate the annotated regions. The red dotted rectangles indicate regions selected for higher-magnification observation, while the red dotted ellipses highlight regions containing voids and cracks.
Table 4. Selected EDS point compositions for Cu-AFS in Figure 10 (wt.%).
In the UAB field, the Cu-side reaction region had less prominent extensions and a wavy or scalloped outer boundary (Figure 10e,f). Local Al–Cu–Zn compositional variations were detected near this region. Point 14 contained 26.50 wt.% Al, 53.90 wt.% Cu, and 19.60 wt.% Zn, whereas the corresponding values at point 19 in the enlarged view were 57.67, 30.20, and 12.13 wt.% (Figure 10f and Table 4). The different Al/Cu ratios reflect compositional heterogeneity within the reaction region and adjacent interstices. On the foam side, points 20 and 21 contained 36.51 and 98.31 wt.% Al, respectively (Figure 10g). At the seam center, points 22 and 23 contained 72.26 and 42.26 wt.% Al, respectively, indicating an interspersed Al–Zn microstructure (Figure 10h).
During remelting, both the face sheet and foam core supply Al in Al-AFS, whereas the cell walls are the principal Al source in Cu-AFS. The Cu–Zn reaction region formed during precoating comes into contact with the liquid filler again upon reheating. Exchange of the adjacent liquid can alter the Al distribution near the Cu side, contributing to the local compositional variations shown in Figure 10f. The phase equilibria and solid-solubility ranges of the Al–Cu–Zn system [26] indicate that the reaction microstructure in this region is closely related to the local ternary composition. Local dissolution and subsequent growth at the outer boundary may reshape the reaction region, making its columnar extensions less pronounced. A distance from the Cu surface to the end of a column in Figure 10b includes the projection; a distance to the base of that column does not. The scalloped boundary in Figure 10f likewise gives different distances at a crest and at a trough. The selected fields do not provide comparable sampling across independent sections for a representative layer thickness. The observed difference thus concerns boundary shape. Zhao et al. [13] distinguished a Cu-side compound layer from an adjacent diffusion layer in dense Al/Cu joints brazed with a Zn–Al filler.
Figure 11 illustrates the proposed morphological evolution of the Cu-side reaction region under ultrasonic excitation. Using high-speed imaging during aluminum-foam/Cu brazing, Dong et al. [14] observed cavitation-induced oxide-film disruption and the associated enhancement of wetting and spreading. In the present pure-Zn precoating system, liquid agitation could redistribute Al from the foam side toward the region adjacent to the Cu sheet, altering the local composition at the reaction front. The Al–Cu–Zn compositional differences between points 14 and 19 in Figure 10f occur near the altered outer boundary of the reaction region, suggesting a link between compositional exchange and interfacial evolution. The CuZn5 label in Figure 11 follows the tentative assignment based on the compositional and phase-equilibrium analysis described above. The local compositions and boundary shape are consistent with this interpretation; liquid flow and cavitation were not observed directly in these joints.
Figure 11. Proposed evolution of the Cu-side reaction region under ultrasonic excitation. CuZn5 denotes a candidate phase; the liquid-motion arrows depict a proposed mechanism. Schematic, not to scale.

3.4. Tensile Response and Fracture of the Foam Core

All four joint groups fractured within the foam core (Figure 12). Cell-wall remnants remained attached to the face sheets, and the bonded region did not separate completely. The mean nominal assembly tensile strengths of the conventionally brazed and ultrasonically brazed Al-AFS joints were 4.27 ± 0.26 and 4.86 ± 0.11 MPa, respectively, at core densities of 0.34 and 0.46 g/cm3. For Cu-AFS, the corresponding strengths were 6.09 ± 0.38 and 5.62 ± 0.29 MPa at core densities of 0.56 and 0.53 g/cm3 (Figure 13 and Table 5; mean ± SD, n = 3). Across the four groups, higher foam-core density coincided with higher mean nominal assembly strength. Fracture within the foam shows that core failure limited the measured load. Because the core densities differed between joining routes, the data do not resolve a separate effect of ultrasound on tensile strength.
Figure 12. Fracture locations in the tensile specimens: (a,b) Al-AFS and (c,d) Cu-AFS. The circles indicate local fracture regions within the foam core.
Figure 13. Nominal assembly tensile strength versus foam-core density. Al and Cu identify the face sheets; CB and UAB denote conventional and ultrasonic-assisted brazing. The four group means are shown with sample standard deviations (n = 3); smaller points show individual strengths. Each horizontal coordinate denotes a group-level core density.
Table 5. Nominal assembly tensile strengths (mean ± sample SD). Core densities are group-level values; failure occurred within the foam core.
Load was transferred from the two coplanar plates through the brazed seams and bonded cell walls into the foam skeleton (Figure 3). Variations in cell-wall thickness and orientation produced nonuniform local deformation. The cracks in Figure 12 propagated through weak regions of the foam skeleton adjacent to the brazed seam, while the remaining cell walls stayed bonded to the face sheets after fracture. This progression from localized deformation to skeleton fracture is consistent with strain-band propagation in steel-faced AFSs under tension [9] and core failure in AFSs produced by vibration-assisted joining [4].

3.5. Compressive Deformation and Energy Absorption

The compression curves of the AFS specimens fabricated by UAB comprise an initial rise, sustained deformation, and subsequent densification (Figure 14a). During initial loading, the cell walls deform and progressively come into contact. Weak cell walls then buckle or fracture, and successive cell collapse produces a load-bearing plateau. Further compression increases contact among collapsed cell walls and reduces the space available for deformation, causing the curves to turn upward. This behavior is consistent with progressive crushing in closed-cell metal foams and integrally formed AFSs [1,2]. For the Al-faced specimens, plateau stress rose from 14.26 to 17.62 and 24.33 MPa as parent foam-core density increased from 0.62 to 0.68 and 0.79 g/cm3, respectively (Al-C1–Al-C3). The two Cu-faced specimens had plateau stresses of 8.00 and 19.66 MPa at parent foam-core densities of 0.54 and 0.70 g/cm3, respectively (Cu-C1 and Cu-C2). In each series the denser parent core corresponded to a higher plateau stress in the plotted coupon. Table 6 distinguishes the energy absorbed within the plateau interval, wp, from cumulative volumetric energy absorption, Wc, up to a strain of approximately 0.70. The two endpoint energy columns give means and sample SDs across the three specimens in each group.
Figure 14. Individual compression histories for UAB-fabricated AFSs: (a) stress–strain curves and (b) compressive specific energy absorption (J/g). Both panels show the same five specimens. The legend identifies the plotted specimens by parent foam-core density (g/cm3): Al-C1, 0.62; Al-C2, 0.68; Al-C3, 0.79; Cu-C1, 0.54; and Cu-C2, 0.70.
Table 6. Compression properties by parent foam-core density measured before joining. Plateau stress and plateau-interval energy refer to the specimen plotted in Figure 14a (ε = 0.20–0.40). The two cumulative energy measures are group means ± sample SD at ε ≈ 0.70 (n = 3 per group). For SEAc, each specimen was normalized by its own mass before the group mean and SD were calculated.
Figure 14b shows cumulative SEAc for the five individual compression curves. Its rise steepens as densification increases the stress. The mean cumulative Wc values are 18.47 ± 0.78, 24.14 ± 1.67, and 29.41 ± 2.19 MJ/m3 for Al-C1–Al-C3, and 14.36 ± 1.13 and 28.23 ± 2.06 MJ/m3 for Cu-C1 and Cu-C2 (Table 6). At the same endpoint, mean SEAc ranges from 6.66 to 18.21 J/g across these five groups. The increase in mean volumetric energy absorption within each face-sheet series followed the increase in parent foam-core density. Outer layers can constrain nearby cells during densification [27]; the plateau is principally associated with crushing of the cellular core. For the mass-specific energy, the denominator includes the complete sandwich, including the face sheets and retained filler.

3.6. Flexural Load-Bearing Behavior and Failure

3.6.1. Peak Load and Core Support

In Figure 15, both AFS configurations reach higher maximum loads than the bare-foam reference specimen with a density of 0.532 g/cm3. The reference specimen reaches a peak of 193.7 N. Further crack growth reduces the load. In the AFS specimens, the face sheets and core deform together during initial loading, producing a rapid increase in load. Beyond the peak, the curves show a sustained plateau, an abrupt load drop, or a stepwise decline, reflecting different damage processes governing load retention at large displacements.
Figure 15. Individual bending load–displacement histories: (a) Al-AFS and (b) Cu-AFS, each with the same bare-foam reference. Legends give the individual AFS structural densities and the bare-foam density. The corresponding AFS core-density classes are listed in Table 7.
Across the low-, medium-, and high-core-density classes, the individual maximum loads are 348.5, 748.5, and 1056.6 N for Al-B1–Al-B3, and 428.5, 942.6, and 2100.8 N for Cu-B1–Cu-B3 (Table 7). These values are maxima over the recorded 0–10 mm interval. In particular, the low-density Al-AFS record reaches its maximum after prolonged deformation; this maximum should not be equated with an initial damage threshold. The high-density Al-AFS and Cu-AFS records give nominal beam indices of 44.0 and 87.5 MPa, respectively (Equation (3)); neither is a measured face-sheet stress.
Table 7. Individual AFS bending results. Core-density intervals identify the bending classes in Table 1; structural density applies to the individual tested specimen. Mass m = ρsV, with V = 6.0 cm3, includes both face sheets, the foam core, and retained filler. The same mass is used for SEAb and Fmax/m. One specimen was tested per combination; the entries are individual values.
The onset of damage in a sandwich beam depends on the failure criterion reached first, whereas the maximum load over a longer displacement interval also depends on subsequent crushing and load recovery. McCormack et al. [28] incorporated face-sheet yielding and core failure into their analysis of three-point bending and evaluated the limit load for local indentation beneath the loading point. Chen et al. [29] investigated plastic collapse modes through four-point bending experiments and limit-load calculations. At the present span-to-thickness ratio of 3.33, the recorded load includes resistance to indentation and crushing beneath the nose as well as bending of the sandwich. Wan et al. [4] observed indentation, core shear, and plastic hinging at a 40 mm span; Huang et al. [16] also observed indentation and core shear in low-density specimens at a 120 mm span. Here the peak loads characterize the short-span configuration. Previous AFS studies likewise show that the mechanical compatibility of the core and face sheets affects the sequence of local indentation and core damage, as well as subsequent face-sheet failure [15,16,19].
In steel-faced aluminum foam sandwich beams, increasing core density can shift the dominant failure mode from core shear to face-sheet yielding [30]. For the two photographed Al-faced specimens, Al-B1 continued to indent, whereas the tensile face of Al-B2 cracked.
The Cu-faced specimens reached higher peak loads within each pair of overlapping foam-core density classes (Table 7), but their structural densities and masses were also higher. In the low-density pair, the Al and Cu structural densities were 0.821 and 2.239 g/cm3, respectively; Al-B1 and Cu-B1 reach 348.5 and 428.5 N, respectively, while their Fmax/m values are 70.75 and 31.89 N/g. The medium-density values are 119.15 and 63.02 N/g for Al-B2 and Cu-B2. At high density, Cu-B3 reaches 124.12 N/g, compared with 118.75 N/g for Al-B3. For these six specimens, the mass-normalized ranking depends on the core-density class, even though the Cu-faced record carries the higher absolute load in each class. Optimization studies of sandwich beams with dissimilar face sheets likewise consider material combinations and strain hardening at a prescribed mass [31]. Normalizing by the complete mass changes the comparison but does not isolate face-sheet stiffness or strength from foam-core support and retained filler. For example, Cu-B3 carried nearly twice the peak load of Al-B3 (2100.8 versus 1056.6 N), yet their peak loads per unit mass differed by only 5.37 N/g. Each value comes from one short-span specimen.

3.6.2. Failure Evolution and Energy Absorption

Al-B1 (core-density range 0.298–0.327 g/cm3; structural density 0.821 g/cm3) sustains loading through continued local indentation, allowing the absorbed bending energy to accumulate with deformation (Figure 16). At a displacement of 4 mm, the upper face sheet develops a pronounced indentation beneath the loading nose, with localized bending on either side (Figure 17a). At 8 mm, the underlying cells progressively close, and the deformation band extends along the indentation profile. By 10 mm, local shear cracks appear in the core, while the face sheets remain in contact with the core in the photographed region and adjacent cell walls continue to deform. Digital image correlation studies of metallurgically bonded AFSs have also identified concurrent deformation of the face sheets and core, together with the development of continuous strain bands within the core [32]. Retention of the connection allows energy dissipation through local indentation and cell-wall collapse to continue.
Figure 16. Individual bending energy histories up to 10 mm: (a) absorbed energy Eb and (b) specific energy absorption SEAb. For AFSs, m = ρsV with V = 6.0 cm3; the bare-foam reference uses m = 2.660 g.
Figure 17. Short-span bending of (a) Al-B1, (b) Al-B2, and (c) Cu-B3. The respective foam-core class ranges were 0.298–0.327, 0.514–0.538, and 0.754–0.783 g/cm3; the individual structural densities were 0.821, 1.047, and 2.821 g/cm3. The sequences show (a) local indentation and cell collapse, (b) tensile-face cracking extending through the core, and (c) core cracking and local separation of the lower face from the foam. The white dotted outlines highlight crack initiation, crack propagation, and local face-sheet separation during bending.
Al-B2 (core-density range 0.514–0.538 g/cm3; structural density 1.047 g/cm3) instead developed a crack in the tensile face followed by through-thickness failure (Figure 17b). A crack appears near the center of the lower face sheet at a displacement of approximately 2 mm. The damage extends into the core by 3 mm and develops into a large through-thickness opening by 6 mm. Cracking of the lower face sheet reduces the section’s capacity to transmit bending moment, causing a rapid load drop and slowing the increase in absorbed energy.
In Cu-B3 (core-density range 0.754–0.783 g/cm3; structural density 2.821 g/cm3), core cracking develops together with local separation of the lower face sheet (Figure 17c). The lower face sheet is already partially detached on the right side at a displacement of 4 mm. The separated region subsequently expands as cracks propagate through the core. The opening interrupted contact between the tensile face and the foam on that side. The Cu sheet continued to bend and the core beneath the nose continued to indent while the specimen still carried load. The photographs resolve the local gap but not whether the crack followed the brazed seam or the adjoining foam cell walls. Load redistribution following face-sheet/core separation has also been reported in bending studies of AFSs prepared using different joining methods [15]. The absorbed energy of this specimen continues to increase, although the slope of the curve decreases as the load falls.
The Al-B2 and Al-B3 curves show an early load drop; through-thickness damage was photographed for Al-B2 (Figure 17b). Al-B1 continued to indent and sustain load. Its specific energy absorption overtook the values for the other two Al-faced specimens at larger displacements (Figure 16b). This crossover reflects the combined influence of initial load-bearing capacity and sustained deformation on energy absorption per unit mass. At 10 mm, the recalculated SEAb values for Al-B1, Al-B2, and Al-B3 are 0.659, 0.358, and 0.327 J/g, respectively. Lu et al. [18] similarly related post-drop energy accumulation to continued pore collapse and compaction in specimens with different pore structures.
Tensile strength and cumulative compression energy are summarized for three specimens per group. Plateau values describe the five plotted compression curves, while bending is assessed from one specimen per face-sheet material and core-density class. Repeat tests at larger span-to-thickness ratios would show whether the observed load rankings and damage paths persist as the contribution of overall bending increases. The SEM/EDS interpretation is local and qualitative, with phase assignments remaining tentative. Both routes require Zn precoating and remelting. UAB adds a 15 s treatment and control of tip contact; it was associated with local differences in constituent distribution and boundary shape. A stationary 20 mm tip on a 50 × 50 mm assembly does not establish uniform treatment over a larger panel. Larger areas would require a coverage strategy and measurements of temperature and displacement across the joint. Liquid Zn can redistribute or be expelled during joining, and wire cutting removes material from the full sandwich. The cut specimens include any retained Zn; its separate contribution to structural density and its variation between specimens were not determined. Thermal cycling, corrosion, and fatigue tests would further assess service stability.

4. Conclusions

Compared with conventional brazing, ultrasonic-assisted brazing produced less sharply separated Al-rich and Zn-rich regions in the Al-faced joints examined. On the Cu side, columnar projections were less pronounced and the reaction-zone boundary was wavy.
All tensile specimens fractured in the foam core. Mean nominal assembly strength increased from 4.27 to 6.09 MPa across the four group core densities (0.34–0.56 g/cm3); the groups were not density-matched by joining route. Under compression, progressive core collapse produced a plateau. Within each face-sheet series, specimens from denser parent cores showed higher plateau stresses.
Under short-span bending, the low-density Al-faced specimen sustained local indentation and cell collapse; in the medium-density Al-faced specimen, a lower-face crack propagated into the core and opened through the section. In the high-density Cu-faced specimen, the lower face sheet separated locally as the core cracked. The Cu-faced specimen carried the higher peak load in each core-density class, but the peak load per unit mass was higher for Cu only in the high-density pair.

Author Contributions

Methodology, T.Q. and Y.A.; investigation, T.Q.; formal analysis, T.Q.; data curation, T.Q.; writing—original draft preparation, T.Q.; writing—review and editing, Y.A., M.N.O.Z. and X.Y.; supervision, Y.A., M.N.O.Z. and X.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the General Program of the National Natural Science Foundation of China (Grant No. 52471041), the General Program of the Shandong Provincial Natural Science Foundation (Grant No. ZR2023ME148), the Natural Science Foundation of Shandong Province (Grant No. ZR2025MS761), the Dezhou Key R&D Program (Grant No. ZD2025ZC017), and the Intelligent Manufacturing Engineering Laboratory of Shandong Huayu University of Technology (Grant No. PT2025KJS002).

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Acknowledgments

During manuscript preparation, the authors used DeepSeek-V3 to assist with drafting and revising the text and improving English-language expression. All AI-assisted text was checked and revised by the authors, who assume full responsibility for the scientific accuracy, originality, and integrity of the manuscript.

Conflicts of Interest

Author Yukun An was employed by the company Shandong Hongyu Ventilator Limited Company. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as potential conflicts of interest.

References

  1. Banhart, J. Manufacture, characterisation and application of cellular metals and metal foams. Prog. Mater. Sci. 2001, 46, 559–632. [Google Scholar] [CrossRef] [Scilit]
  2. Zhang, Z.; Feng, H.; Xu, T.; Xin, W.; Ding, J.; Liu, N.; Wang, Z.; Wang, Y.; Xia, X.; Liu, Y. Compression performances of integral-forming aluminum foam sandwich. Compos. Struct. 2022, 283, 115090. [Google Scholar] [CrossRef] [Scilit]
  3. Neu, T.R.; Heim, K.; Seeliger, W.; Kamm, P.H.; García-Moreno, F. Aluminum Foam Sandwiches: A Lighter Future for Car Bodies. JOM 2024, 76, 2619–2630. [Google Scholar] [CrossRef] [Scilit]
  4. Wan, L.; Huang, Y.; Lv, S.; Feng, J. Fabrication and interfacial characterization of aluminum foam sandwich via fluxless soldering with surface abrasion. Compos. Struct. 2015, 123, 366–373. [Google Scholar] [CrossRef] [Scilit]
  5. Ubertalli, G.; Ferraris, M.; Bangash, M.K. Joining of AL-6016 to Al-foam using Zn-based joining materials. Compos. Part A Appl. Sci. Manuf. 2017, 96, 122–128. [Google Scholar] [CrossRef] [Scilit]
  6. Yang, S.; Luo, H.; Wang, L.; Guang, Z.; Zhang, P.; Liu, Y. Interface structure and bonding strength of metallurgical bonded aluminum foam sandwich (AFS) fabricated by hot-pressing. Vacuum 2023, 211, 111987. [Google Scholar] [CrossRef] [Scilit]
  7. Yang, S.; Luo, H.; Wang, L.; Wu, J.; Mu, Y.; Wu, L. Interface microstructures and mechanical properties of foamable precursor sandwiches and aluminum foam sandwiches. Compos. Struct. 2024, 336, 117961. [Google Scholar] [CrossRef] [Scilit]
  8. Izadpanahi, A.; Mahdavi Shahri, M.; Jampour, A. A novel technique for stir soldering of aluminum plate to aluminum foam. Weld. Int. 2023, 37, 700–707. [Google Scholar] [CrossRef] [Scilit]
  9. Wang, L.; Luo, H.; Yang, S.; Cui, S.; Wu, L. Achieving metallurgical bonding in steel faceplate/aluminum foam sandwich via hot pressing and foaming processes: Interfacial microstructure evolution and tensile behavior. J. Mater. Process. Technol. 2024, 334, 118636. [Google Scholar] [CrossRef] [Scilit]
  10. Li, Z.; Xu, Z.; He, P.; Ma, Z.; Chen, S.; Yan, J. Dependence of wetting on cavitation during the spreading of a filler droplet on the ultrasonically agitated Al substrate. Ultrason. Sonochem. 2022, 82, 105893. [Google Scholar] [CrossRef] [Scilit]
  11. Li, Z.; Xu, Z.; Zhang, B.; Yan, J. Cavitation Characteristics in Ultrasonic Soldering and the Erosion Effect. Weld. J. 2024, 103, 260-s–274-s. [Google Scholar] [CrossRef] [Scilit]
  12. Liu, C.; Liu, A.; Su, Y.; Chen, Y.; Zhou, Z.; Liu, C. Ultrasonically enhanced flux-less bonding with Zn-5Al alloy under ambient condition for high-temperature electronics interconnects. J. Manuf. Process. 2022, 73, 139–148. [Google Scholar] [CrossRef] [Scilit]
  13. Zhao, D.; Li, D.; Xiao, Y.; Li, M.; Chen, W. Acoustic cavitation-induced microstructure evolution in ultrasonically brazed Al/Cu joints using Zn-Al alloy fillers. Ultrason. Sonochem. 2024, 109, 107001. [Google Scholar] [CrossRef] [Scilit]
  14. Dong, Y.; Chen, H.; Zhang, R.; Fu, Q.; Qiao, Y.; Zhao, J.; Chen, J.; Liu, C.; Zhou, Y. Overwhelming oxide films fragmentation and interfacial reaction mechanisms in ultrasonic-assisted brazing of Al-foam/Cu using semi-molten Zn–14Al filler. J. Mater. Res. Technol. 2025, 38, 3990–4004. [Google Scholar] [CrossRef] [Scilit]
  15. Huang, P.; Sun, X.; Su, X.; Gao, Q.; Feng, Z.; Zu, G. Three-Point Bending Behavior of Aluminum Foam Sandwich with Different Interface Bonding Methods. Materials 2022, 15, 6931. [Google Scholar] [CrossRef] [Scilit]
  16. Huang, P.; Gao, Q.; Su, X.; Feng, Z.; Sun, X.; Zu, G. Effect of Core Density on the Three-Point Bending Performance of Aluminum Foam Sandwich Panels. Materials 2023, 16, 7091. [Google Scholar] [CrossRef] [Scilit]
  17. Zhang, J.; Huang, W.; Yuan, H.; Wu, X. Failure behavior of a sandwich beam with GLARE face-sheets and aluminum foam core under three-point bending. Thin-Walled Struct. 2023, 183, 110438. [Google Scholar] [CrossRef] [Scilit]
  18. Lu, X.; Jing, L.; Zhou, W.; Yang, H.; Yuan, P.; Li, X. Pore Structure and Deformation Correlation of an Aluminum Foam Sandwich Subject to Three-Point Bending. Materials 2024, 17, 567. [Google Scholar] [CrossRef] [Scilit]
  19. Wang, L.; Luo, H.; Cui, S.; Wu, L.; Xu, J. Exploring three-point bending response of novel aluminum foam sandwich beams fabricated by melt route. J. Mater. Sci. 2025, 60, 10551–10563. [Google Scholar] [CrossRef] [Scilit]
  20. Zhang, Z.; Zhang, Z.; Liu, N.; Xia, X.; Wang, Z.; Wang, J.; Cui, L.; Qiu, Z.; Ding, J.; Wang, Y.; et al. Three-point bending performances of integral-forming aluminum foam sandwich. Mater. Des. 2023, 229, 111889. [Google Scholar] [CrossRef] [Scilit]
  21. Yang, S.; Luo, H.; Wang, L.; Mu, Y.; Wu, L. Effect of core structure on the quasi-static bending behaviors and failure mechanisms of aluminum foam sandwiches at elevated temperatures. Mater. Charact. 2024, 208, 113638. [Google Scholar] [CrossRef] [Scilit]
  22. Latour, M.; Sato, A.; D’Aniello, M.; Landolfo, R.; Rizzano, G. Flexural response of metallurgically bonded steel-aluminium foam-steel panels and composite beams. Eng. Struct. 2025, 322, 119114. [Google Scholar] [CrossRef] [Scilit]
  23. Lee, H.; Lee, I.; Xu, X.; Omori, T.; Kainuma, R. Revisiting the Phase Equilibria in the Cu-Zn Binary System. J. Phase Equilib. Diffus. 2024, 45, 304–317. [Google Scholar] [CrossRef] [Scilit]
  24. Zhao, P.; Li, Z.; Kuang, L.; Wang, S.; Xu, Z.; Yan, J. Deformation-free manufacturing Al alloy laminated structures by an ultrasonic-assisted diffusion bonding. Mater. Charact. 2024, 211, 113883. [Google Scholar] [CrossRef] [Scilit]
  25. Wang, X.; Cao, Z.; Liu, X.; Wang, H.; Shi, S. Fabrication and three-point bending behavior of aluminum foam sandwich via controlled atmosphere brazing. Adv. Eng. Mater. 2025, 27, 2500468. [Google Scholar] [CrossRef] [Scilit]
  26. Liang, S.-M.; Schmid-Fetzer, R. Thermodynamic assessment of the Al–Cu–Zn system, Part III: Al–Cu–Zn ternary system. Calphad 2016, 52, 21–37. [Google Scholar] [CrossRef] [Scilit]
  27. Wang, L.; Luo, H.; Yang, S.; Wu, L.; Wu, J. Compressive behavior and energy absorption analysis of casting skin-wrapped aluminum foams. Mater. Today Commun. 2023, 36, 106839. [Google Scholar] [CrossRef] [Scilit]
  28. McCormack, T.M.; Miller, R.; Kesler, O.; Gibson, L.J. Failure of sandwich beams with metallic foam cores. Int. J. Solids Struct. 2001, 38, 4901–4920. [Google Scholar] [CrossRef] [Scilit]
  29. Chen, C.; Harte, A.-M.; Fleck, N.A. The plastic collapse of sandwich beams with a metallic foam core. Int. J. Mech. Sci. 2001, 43, 1483–1506. [Google Scholar] [CrossRef] [Scilit]
  30. Wang, Z.; Hong, B.; Xian, G.; Xin, M.; Huang, S.; Shen, H. Quasi-static and low-velocity impact behaviors of steel-aluminum foam sandwich beams. Structures 2024, 64, 106549. [Google Scholar] [CrossRef] [Scilit]
  31. Wang, M.; Yu, X.; Zhang, J.; Qin, Q. Three-point bending of physically asymmetric metal sandwich beams with aluminum foam core: Failure behavior and optimal design. Compos. Struct. 2022, 280, 114873. [Google Scholar] [CrossRef] [Scilit]
  32. Wang, L.; Luo, H.; Cui, S.; Xu, J.; Wu, L. Thermo-mechanical indentation behavior of metallurgically bonded aluminum foam sandwich structures: Interface synergy and stress transfer mechanism. Arch. Civ. Mech. Eng. 2026, 26, 107. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.