Abstract
Aluminum foam-core sandwich panels combine flexural strength and energy absorption at low mass, but their performance depends on face-core load transfer. Previous studies mainly compared adhesive and metallurgical bonding or varied core and face sheet parameters; direct comparisons of stiff and elastic adhesives based on global bending, local strain, and damage morphology remain limited. To address this gap, panels comprising aluminum face sheets and a closed-cell aluminum foam core were bonded with either LOCTITE EA 9466 structural epoxy or TEROSON MS 939 elastic silane-modified polymer adhesive. Three panels per configuration were tested under quasi-static three-point bending at 6 mm/min. Load-deflection response, lower face sheet strain, load retention and energy absorption at a common deflection of 12 mm, and post-test damage morphology were evaluated. The epoxy-bonded panels achieved a 4.5% higher maximum load and absorbed 20.5% more energy to 12 mm. In contrast, TEROSON MS 939 increased the mean deflection at maximum load by 87.6% and carried a higher load at 12 mm. Both configurations developed localized foam crushing. Near-interface foam fracture was observed in the inspected epoxy-bonded specimen, whereas the TEROSON MS 939 specimen maintained visible adhesive continuity. Within the tested conditions, the adhesive system influenced maximum load, deformation capacity, and face-core integrity.
1. Introduction
Sandwich panels are made with thin and stiff face sheets and a lightweight core material to give high flexural stiffness and load-carrying capacity at low structural mass. Under bending, the face sheets carry the main longitudinal tensile and compressive stresses. The core keeps the faces apart, carries the transverse shear, and prevents local deformation of the compressed face [1,2,3,4]. This structural efficiency has led to the use of sandwich structures in aerospace, automotive, railway, marine, civil, and protective fields [1,2,5,6]. Aluminum foam is an attractive core material because of its low density, energy absorption, vibration damping, thermal resistance, and non-combustibility [7,8].
The mechanical behavior of closed-cell aluminum foam depends on relative density, cell size, wall thickness, anisotropy, and defects. Under compression, aluminum foam commonly exhibits an initial quasi-elastic response, followed by progressive cell collapse and a plateau region, and finally densification at higher strains [9,10,11,12,13]. Cell morphology can also influence the location and development of strain concentrations; cell-wall curvature, pore-size variation, and local imperfections can produce non-uniform deformation and specimen-to-specimen variability [12,13].
The flexural response of aluminum foam-core sandwich panels depends on the interaction between the face sheets, the cellular core, and the face-core connection. Possible deformation and failure modes include face yielding, face wrinkling, core shear, local indentation, progressive core crushing, and face-core separation [1,3,4,14,15,16,17,18]. These mechanisms can occur separately or interact as the load continues. Chen et al. [1] identified face yielding, indentation, and core shear as competing collapse modes in metallic foam-core sandwich beams. McCormack et al. [16] showed that the governing failure mode depends on the relative dimensions and strengths of the face sheets and core. Kabir et al. [17] also demonstrated that face sheet strength, core thickness, and support span affect both the failure load and the failure mode of the aluminum foam-core sandwich panels.
The face-core connection is important because it allows the constituent layers to act as an integrated sandwich section. Crupi and Montanini [14] studied the collapse behavior of aluminum foam sandwich panels and found that the face-core connection and the support configuration both influence it. Wang et al. [15] reported on the interacting modes of deformation in quasi-static three-point bending of aluminum foam sandwiches with CFRP face sheets, including failure modes: indentation, core shear, face sheet fracture, and debonding. For aluminum foam-based panels manufactured using powder compact melting, Formisano et al. [18] reported that the bending strength of the panels was affected by the panel thickness and skin reinforcement. The findings suggest that the interface condition and constituent geometry should be considered together when assessing flexural behavior.
Huang et al. [19] demonstrated the influence of interface bonding method on peak load, energy absorption and damage development of aluminum foam sandwich panels. The peak load of the metallurgically bonded panels was 24% higher than that of the glued panels. Premature separation of the glued panels also reduced the contribution of the foam core to progressive deformation. Studies of adhesive bonding in aluminum foam sandwiches have also found that the morphology of the foam, bonded area, surface preparation and quality of the bond influence the load transfer between the face sheets and core [20,21]. Flexural performance should therefore not be evaluated from maximum load alone. Deflection at maximum load, post-peak load, energy absorption, and residual face-core integrity are also relevant. Recent studies on metallurgically bonded aluminum foam sandwich panels have related pore structure uniformity, face sheet thickness, and interfacial microstructure to the mechanical response and failure modes [22,23].
Previous experimental studies have mainly examined the effects of core density, core thickness, face sheet material, support span, pore structure, and adhesive versus metallurgical bonding [14,15,17,18,19,24,25]. Fatigue studies have shown that adhesively bonded sandwich panels with lower-density aluminum foam cores are more likely to develop face-core debonding. Denser cores provide a larger bonded area and greater resistance to interface failure [26]. Experimental tests of initially damaged foam-core sandwich beams have also revealed that the face-core separation can alter the deformation path and induce fracture in the surrounding core material [27]. Structural adhesives differ considerably in stiffness, elongation, and deformation capacity, but studies often treat adhesively bonded aluminum foam panels as one group.
Adhesive compliance in the present study is the ability of the cured bond line to effectively deform, including the effect of the adhesive mechanical properties and thickness. The adhesive layer is therefore considered a structural part of the sandwich panel rather than only a joining material. A relatively stiff bond line can support initial composite action and load transfer, while a more compliant layer can accommodate greater relative rotation and displacement between the face sheets and core. Hunston et al. [28] demonstrated that the stiffness of sandwich beams is dependent on adhesive shear properties. The authors have also noted that the adhesive properties of the bond line in constrained specimens vary from those of bulk specimens.
Damage development and residual structural performance can also be influenced by the adhesive selection. Fatima et al. [29] reported that the modification of the skin-core adhesive affected the load transfer, energy dissipation and damage growth of the sandwich composites. Pereira and Fernandes [30] similarly reported that the adhesive layer influenced the bending performance of sandwich panels and should be considered in their structural design. These findings support the need to compare adhesive layers with strongly different stiffness and deformation capacities rather than treating all adhesively bonded panels as mechanically equivalent.
Fiber-metal laminates provide a related example of aluminum-based layered materials in which bonded interfaces affect structural performance. GLARE consists of alternating aluminum sheets and glass fiber reinforced polymer layers and combines low density with high specific strength, fatigue resistance, impact resistance, and damage tolerance [31,32]. Its mechanical response depends on fiber orientation, stacking sequence, aluminum layer thickness, manufacturing conditions, surface treatment, and interfacial adhesion [31,33,34]. Recent three-point bending studies showed that these factors influence flexural behaviour, energy absorption, and failure mode. GLARE configurations with predominantly 0° glass fiber layers were dominated by delamination, whereas those with predominantly 90° layers mainly developed central cracking [33]. Interfacial delamination at the aluminum/composite interfaces has also been reported as the dominant failure mechanism of GLARE 3/2 laminates, with its severity depending on fiber orientation and stacking sequence [35]. Although GLARE and aluminum foam-core sandwich panels have different internal structures, both depend on effective load transfer and continuity between bonded layers. In GLARE, the reinforced polymer layers contribute directly to the laminate response, whereas in the present panels the cellular foam core mainly transfers shear and undergoes indentation and crushing. GLARE is therefore considered only as a related example of the importance of bonded interfaces.
Despite the established importance of face-core integrity, previous studies on aluminum foam-core sandwich panels have mainly examined core density, core thickness, face sheet properties, support span, pore structure, or adhesive versus metallurgical bonding [14,15,17,18,19,20,21,24,25,26]. Latour et al. [36] compared adhesive properties with the ultimate behavior of steel face sheet/aluminum foam sandwich panels but, to the authors’ knowledge, no comparison has combined aluminum face sheets, local face sheet strain, and post-test interface morphology. Direct experimental comparisons between adhesive systems with significantly different stiffness and deformation capacity therefore remain limited. The specific contribution of the present study is a direct comparison of aluminum foam-core sandwich panels bonded with LOCTITE EA 9466 structural epoxy and TEROSON MS 939 elastic silane-modified polymer adhesive. Three panels were tested for each configuration using the same three-point bending arrangement. Rather than focusing only on maximum load or final failure mode, the present work combines group-level load deflection results, common-deflection load retention and energy absorption, local lower face sheet strain, residual-deflection assessment, and post-test digital microscope examination. This approach connects the global bending response with local strain development and damage in the foam core and face-core regions.
Based on this research gap, the study had three specific objectives: (i) to compare the maximum load, deflection at maximum load, post-peak load retention, and energy absorption of the two adhesive configurations at common deflection limits; (ii) to examine the relationship between local lower face sheet strain and the global load-deflection response during loading and post-peak deformation; and (iii) to identify and compare the post-test damage mechanisms in the foam core and face-core regions. These objectives were addressed through quasi-static three-point bending tests, strain-gauge measurements, residual-deflection assessment, and digital-microscope examination.
2. Materials and Methods
2.1. Constituent Materials
The sandwich panels consisted of a closed-cell aluminum foam core bonded between two aluminum face sheets with a nominal thickness of 2 mm. The face sheets were made of EN AW-2017A aluminum alloy, with a yield strength of approximately 382 MPa, an ultimate tensile strength of 480 MPa, and an elastic modulus of 72 GPa [37]. Two commercially available adhesives with contrasting mechanical characteristics were investigated: LOCTITE EA 9466, a two-component structural epoxy adhesive, and TEROSON MS 939, a one-component silane-modified polymer adhesive. LOCTITE EA 9466 was mixed at a resin-to-hardener volume ratio of 2:1, whereas TEROSON MS 939 was supplied as a single-component adhesive.
The manufacturer-reported properties relevant to the present investigation are summarized in Table 1. LOCTITE EA 9466 combines a high tensile modulus with low elongation at break, whereas TEROSON MS 939 exhibits substantially greater elongation. These contrasting properties provide the basis for evaluating the influence of adhesive-layer compliance on the flexural response and damage development of the sandwich panels.
Table 1.
Properties of the adhesive systems [38,39].
The two adhesives were selected because they have strongly contrasted mechanical and deformation characteristics. LOCTITE EA 9466 is a two-component structural epoxy with a tensile strength of 32 MPa, a tensile modulus of 1718 MPa, and an elongation at break of 3%. TEROSON MS 939 is a one-component, moisture-curing silane-modified polymer adhesive with an elongation at break of approximately 250%. The adhesives also differ in chemical composition, curing mechanism, and the final geometry of the bonded panels. These manufacturer-reported values are used only to describe the general differences between the two adhesive systems and should not be treated as measured properties of the cured bond lines. The present study therefore compares the response of two complete adhesive systems rather than isolating compliance as a single independent variable.
2.2. Sandwich-Panel Preparation and Three-Point Bending Test
The aluminum face sheets and closed-cell aluminum foam cores were cut to the dimensions given in Table 2. Before bonding, the face-core contact surfaces were abraded using P180-grit abrasive paper, degreased with acetone, and air-dried for 15 min.
Table 2.
Geometrical and testing parameters of the sandwich specimens used in the three-point bending tests.
The sandwich panels were assembled by hand lay-up using LOCTITE EA 9466 epoxy adhesive or TEROSON MS 939 elastic silane-modified polymer adhesive. For each configuration, the adhesive was distributed over the prepared face core contact surfaces before assembly. The panels were then placed in the same alignment fixture and clamped during curing. The same surface preparation, adhesive application, alignment, clamping, and curing-duration procedures were used for all specimens to maintain consistent manufacturing conditions within each configuration. Both adhesive configurations were maintained for 7 days at 22 ± 2 °C before mechanical testing. The TEROSON MS 939 panels were cured at a relative humidity of 50 ± 5%, consistent with the moisture-dependent curing mechanism of the silane-modified polymer adhesive [38]. The measured total panel thickness after manufacturing and curing was used to define the final geometry of each adhesive configuration.
The nominal constituent dimensions were the same for both configurations, comprising two 2 mm aluminum face sheets and a 20 mm foam core. After manufacturing and curing, the measured total panel thickness, d, was 24.78 mm for the LOCTITE EA 9466-bonded panels and 26.12 mm for the TEROSON MS 939-bonded panels. These values describe the final assembled geometry and include both face sheets, the foam core, and the two cured adhesive layers. The measured total panel thickness differed by 1.34 mm, corresponding to approximately 5.4%. Because the nominal face sheet and core thicknesses were the same, this difference reflects the final manufactured geometry, including the cured adhesive layers, adhesive penetration into the foam surface, local foam irregularity, and normal assembly variation. Local bond line thickness was not measured separately and was therefore not estimated from the total panel thickness.
The specimen dimensions and test parameters are summarized in Table 2, while the corresponding geometrical notation is shown in Figure 1. Here, L is the support span; L + 2H is the total specimen length; d is the measured total sandwich thickness; b is the specimen width; t is the face sheet thickness; c is the core thickness; P is the load applied by the testing machine; H is the overhang and a is the radius of the loading and support rollers. The main stages of specimen manufacture are shown in Figure 2.
Figure 1.
Three-point bending configuration and geometrical notation of the sandwich specimen.
Figure 2.
Manufacturing sequence of the aluminum foam-core sandwich specimens: (a) constituent materials cut to the required dimensions; (b) preparation of the face-core bonding surfaces; (c) finished specimen prepared for three-point bending.
The quasi-static three-point bending tests of the sandwich panels were conducted using an MTS Insight electromechanical testing system (MTS Systems Corporation, Eden Prairie, MN, USA) equipped with a 10 kN load cell. The three-point bending arrangement was based on the sandwich beam flexure principle of ASTM C393/C393M-20 [40]. The Flat sandwich specimens were simply supported on two cylindrical rollers and loaded mid-span through a central roller. The tests were carried out under displacement control at a crosshead speed of 6 mm/min, with continuous recording of load and mid-span deflection. The mid-span deflection of the specimen was measured directly with an MTS displacement gauge positioned at the centre of the panel, so it is independent of fixture and machine compliance.
Before loading, each specimen was positioned in contact with the loading and support rollers, and the load and displacement channels were zeroed. Loading continued beyond the maximum load until a clear post-peak response had been recorded. Because a fixed terminal deflection was not imposed, the tests ended at different final deflections. Load retention and absorbed energy were therefore evaluated at the common deflection of 12 mm reached by all specimens. The same fixture, loading procedure, and measurement method were used for both adhesive configurations. The samples were 200 mm long and 40 mm wide, with a support span of 160 mm. The loading and support rollers had a radius of 5 mm. Three specimens were tested for each configuration, and a strain gauge was installed in the middle of the sheet on the lower face. The method was used for a comparative evaluation of load deflection response, local strain, post-peak load retention, energy absorption, and damage development. The core shear strength, the core shear modulus, the facing strength, and the allowable standards of the design were not determined. The procedure is therefore described as an ASTM-based comparative bending method rather than a fully standard-compliant determination of sandwich material properties.
During the three-point bending test, the strain of the lower face sheet of each specimen was measured using a strain gauge located at the geometrical center of the face. Before installing the strain gauge, the aluminum surface was prepared according to the manufacturer’s recommended procedure. Micro-Measurements M-Prep Conditioner A, M-Prep Neutralizer 5A, and M-Line GC-6 isopropyl alcohol were used to remove contaminants and provide a clean surface for bonding. A Micro-Measurements CEA-06-240UZ-120 foil strain gauge with a resistance of 120 Ω, a nominal gauge factor of 2.08, and a gauge length of 6.1 mm was bonded to the lower aluminum face sheet at mid-span, directly beneath the central loading roller [41]. M-Bond 200 cyanoacrylate adhesive was used to attach the gauge.
After the adhesive had cured, the lead wires were soldered to the gauge terminals. The installation was then covered with M-Coat A protective coating to provide electrical insulation and protect the strain gauge and soldered connections from moisture and mechanical damage. The measuring axis was aligned with the longitudinal axis of the specimen to record the tensile strain developed in the lower face sheet during bending. Strain gauges were installed at the same position on all three specimens from each adhesive configuration using the same preparation and bonding procedure.
The strain-gauge and MTS recordings were acquired in parallel throughout the three-point bending tests. Data acquisition was started manually at the same time using MM01 MultiDAQ software (version 2.0.1.3; Micro-Measurements, Vishay Precision Group) and the MTS data-acquisition system. The strain-gauge signal was recorded at a sampling frequency of 100 Hz, providing the measurement time, bridge output in mV/V, and longitudinal strain.
The strain-gauge and MTS datasets were aligned using their recorded time histories. The first detectable increase in applied load was used as the common reference point. This procedure allowed the local longitudinal strain in the lower face sheet to be related to the load and deflection recorded by the MTS system. The strain-gauge measurement arrangement is shown in Figure 3.
Figure 3.
Strain-gauge measurement arrangement: (a) gauge location at mid-span on the lower aluminum face sheet; (b) instrumented specimen mounted in the three-point bending fixture.
2.3. Post-Test Assessment
Following unloading, the residual deformation and macroscopic damage of the tested specimens were documented by visual examination. The assessment included global panel curvature, localized indentation beneath the central loading roller, foam-core crushing and shear, face sheet deformation, and face-core separation. The observed damage modes were classified with reference to the failure mechanisms reported for metallic foam-core sandwich beams [1,16,17] and by Steeves and Fleck [3].
The location and extent of damage were compared with characteristic changes in the corresponding load-deflection and strain responses. The local morphology of the face-core regions and exposed damage surfaces was examined using a DVM6 digital 3D microscope (Leica Microsystems, Wetzlar, Germany). All three specimens from each adhesive configuration were examined for indentation, foam-cell deformation, localized core crushing, evidence of core shear deformation, adhesive-layer continuity, face-core opening, cohesive adhesive failure, and near-interface foam fracture.
The occurrence and approximate extent of core crushing, face-core opening, cohesive adhesive failure, and near-interface foam fracture were recorded for each specimen using three descriptive categories: not observed, localized, and extended. “Localized” indicates a feature limited to a small region of the inspected section, whereas “extended” indicates a feature continuing across a larger part of the inspected region. This classification was used as a semi-quantitative record of the observed morphology and not as a measured damage-area fraction. Indentation and evidence of core shear deformation were considered during the visual assessment but were not graded from the local microscope fields. One specimen from each configuration was selected for illustration in Section 3.3 because the selected fields clearly showed the main damage features observed within the corresponding group. After unloading, the residual mid-span deflection of each panel was measured using a Vernier caliper. The recovered deflection was calculated as the difference between the maximum deflection recorded by the MTS system and the residual mid-span deflection measured after unloading. Recovery was observed only for the TEROSON MS 939 panels.
3. Results and Discussion
3.1. Three-Point Bending Response
Load-deflection curves for the LOCTITE EA 9466 and TEROSON MS 939-bonded panels are shown separately in Figure 4 and Figure 5, respectively. Figure 4 presents the three LOCTITE EA 9466 specimen curves together with their average response, whereas Figure 5 presents the corresponding curves for TEROSON MS 939. Both configurations showed an initial increase in load, followed by a nonlinear transition toward the maximum load and a gradual post-peak reduction. The sustained load after the maximum indicates progressive deformation and redistribution within the sandwich structure rather than sudden collapse. The individual curves and average responses also show the repeatability and within-group variation in each adhesive configuration.
Figure 4.
Load-deflection responses of the three aluminum foam-core sandwich specimens bonded with LOCTITE EA 9466 and their average response.
Figure 5.
Load-deflection responses of the three aluminum foam-core sandwich specimens bonded with TEROSON MS 939 and their average response.
The LOCTITE EA 9466-bonded panels reached a mean maximum load of 1108.3 ± 3.2 N, with a coefficient of variation of 0.29% (Table 3). The mean deflection at maximum load was 5.84 ± 2.02 mm. The low variation in maximum load indicates consistent load-carrying capacity, whereas the larger variation in deflection indicates greater specimen-to-specimen variability in the deformation developed before the maximum load. Figure 6 compares the mean maximum loads of the two adhesive configurations. The individual observations, confidence intervals, and exploratory effect sizes for the main response measures are provided in Supplementary Tables S1–S4.
Table 3.
Load-deflection and energy-absorption parameters of aluminum foam-core sandwich panels under three-point bending.
Figure 6.
Mean maximum load of the sandwich panels bonded with LOCTITE EA 9466 and TEROSON MS 939. Error bars represent ± one sample standard deviation (n = 3).
The TEROSON MS 939-bonded panels reached a mean maximum load of 1060.6 ± 14.8 N, with a coefficient of variation of 1.39%. The mean deflection at maximum load was 10.95 ± 0.91 mm. Compared with the LOCTITE EA 9466 configuration, the TEROSON MS 939 panels showed lower variation in deflection at maximum load and reached maximum load at a greater deflection.
The mean maximum load of the LOCTITE EA 9466-bonded panels was 4.5% higher than that of the TEROSON MS 939-bonded panels. However, the mean deflection at maximum load was 87.6% greater for the TEROSON MS 939 configuration. The epoxy-bonded panels reached maximum load at a smaller deflection, whereas the TEROSON MS 939-bonded panels accommodated greater deformation before maximum load. The higher modulus and lower elongation reported for LOCTITE EA 9466 are consistent with a comparatively stiff bond line, while the much greater elongation of TEROSON MS 939 is consistent with greater deformation capacity. However, the adhesive systems also differ in tensile strength, chemistry, curing mechanism, and final panel geometry. The measured differences therefore represent the combined response of the two adhesive configurations and cannot be attributed to compliance alone.
During loading, both panel configurations developed increasing global curvature together with localized deformation beneath the central loading roller. The change from the initial load-deflection response is consistent with the progressive development of local face sheet indentation and cellular deformation within the foam core. As loading continued, the deformed region around mid-span expanded, indicating the involvement of neighbouring cells in deformation and load transfer. The combined occurrence of global bending and localized indentation agrees with the behavior reported for aluminum foam-core sandwich panels under concentrated transverse loading [17,42].
Both adhesive configurations maintained substantial load-carrying capacity beyond the maximum load. A common deflection of 12 mm was selected for comparison because all tested specimens reached this value. At 12 mm, the LOCTITE EA 9466 panels sustained 942.1 ± 33.0 N, corresponding to 85.0 ± 3.2% of their respective maximum loads. The TEROSON MS 939 panels sustained 1041.3 ± 17.0 N and retained 98.2 ± 2.7% of their maximum loads. At the common deflection, the TEROSON MS 939 configuration carried 10.5% more load and retained 13.2 percentage points more of its maximum load than the LOCTITE EA 9466 configuration.
The final thickness of the TEROSON MS 939-bonded panels was 5.4% greater than that of the LOCTITE EA 9466-bonded panels (Table 2). To evaluate the possible influence of this difference on the results, a first-order estimate was made using simple sandwich-beam theory. For thin face sheets, the bending rigidity of the face sheets is proportional to (d − t)2, and the load for face sheet yielding is proportional to (d − t), where d is the total panel thickness and t is the face sheet thickness. The thicker TEROSON MS 939 panels would therefore be expected to have about 12.12% higher face sheet bending rigidity and about 5.9% higher load if face yielding controlled the response. The measured results do not follow this trend, since the TEROSON MS 939 panels had a 4.5% lower mean maximum load and absorbed less energy up to 12 mm deflection. This estimate is approximate because it does not include core shear, local indentation, or shear deformation of the adhesive layers. The thickness difference therefore does not account for the measured trends, and the response of the two configurations is interpreted as the combined effect of panel geometry, adhesive properties and bond-line characteristics at the panel level.
In addition, because the total panel thickness differed between the configurations, the deflection at maximum load was normalized by the corresponding total thickness as expressed in Equation (1):
where is the normalized deflection, δmax is the deflection at maximum load, and d is the measured total panel thickness. The mean normalized values were 0.236 for LOCTITE EA 9466 and 0.419 for TEROSON MS 939, so the normalized deflection was approximately 77.8% greater for the TEROSON MS 939 configuration. This is much larger than the 5.4% difference in thickness. The observed behavior is therefore not governed by the geometrical difference alone. The total thickness difference is treated as part of the final manufactured panel geometry, and its separate contribution cannot be isolated from the adhesive and bond-line effects in the present study.
The post-peak curves showed a gradual reduction with only limited local fluctuations. This response is consistent with progressive foam-cell deformation and load redistribution within the sandwich section. However, the curves alone cannot identify individual damage events. The strain response and post-test condition of the face-core regions are therefore discussed separately in Section 3.2 and Section 3.3.
The energy absorbed up to 12 mm of deflection was determined in accordance with Equation (2) from the area beneath each load-deflection curve:
where E12 is the absorbed energy up to 12 mm, F is the measured load, and δ is the recorded deflection. The integral was evaluated numerically from the recorded data, with F in N and δ in mm, divided by 1000 to give joules.
The LOCTITE EA 9466-bonded panels absorbed 11.07 ± 0.44 J, compared with 9.19 ± 0.19 J for the TEROSON MS 939-bonded panels. The mean absorbed energy was therefore 20.5% higher for the LOCTITE EA 9466 configuration. The load and energy results at 12 mm deflection describe different aspects of the panel response. The load at 12 mm is the load carried at one selected deflection, whereas the absorbed energy is the area under the complete load-deflection curve from 0 to 12 mm. The LOCTITE EA 9466 panels carried a higher load over the initial and intermediate part of the interval, which produced a larger area under the curve. At 12 mm, however, these panels had already entered the post-peak stage, whereas the TEROSON MS 939 panels remained close to their maximum-load region. The TEROSON MS 939 configuration therefore carried a higher load and kept a greater proportion of its maximum load at 12 mm, although its accumulated energy was lower. These results indicate a trade-off between greater energy absorption over the selected deflection range and greater load maintained at its endpoint.
The coefficients of variation were approximately 4.0% for LOCTITE EA 9466 and 2.1% for TEROSON MS 939, indicating low variability in the integrated response. A common integration limit was used because the tests ended at different final deflections. The reported values therefore describe the energy absorbed by the complete panel up to a common deflection of 12 mm and should not be interpreted as an intrinsic material property or as the total energy absorption capacity. Figure 7 compares the retained load and absorbed energy at this common deflection, while Table 3 summarizes the main load-deflection and energy-absorption parameters. Table 4 reports the absorbed energy at several common limits. Because the tests ended at different final deflections, post-peak comparisons are limited to the common deflection of 12 mm.
Figure 7.
Response at the common deflection of 12 mm: (a) load retention relative to the maximum load and (b) absorbed energy up to 12 mm. Error bars represent ± one sample standard deviation (n = 3).
Table 4.
Energy absorbed up to common deflection limits (mean ± SD).
To test whether the energy comparison depends on the 12 mm limit, the absorbed energy was also evaluated at common limits of 4, 6, 8, 10 and 12 mm (Table 4). The energy absorbed by the LOCTITE EA 9466 panels was higher than that of the TEROSON MS 939 panels at every limit, by 80.8% at 4 mm and decreasing to 20.5% at 12 mm, so the ranking of absorbed energy was consistent across the chosen limits. These limits are related values from the same load–deflection curves and not independent tests (Section 2.2). Dividing the energy increments in Table 4 by the deflection increments gives approximate mean loads for each interval. Over the first 4 mm, the mean load was about 705 N for LOCTITE EA 9466 and about 390 N for TEROSON MS 939, and the LOCTITE EA 9466 panels remained higher up to about 10 mm. The difference in absorbed energy therefore increased from 1.26 J at 4 mm to about 2.0 J at 8–10 mm. Between 10 and 12 mm, the TEROSON MS 939 panels carried the higher mean load (about 1045 N compared with 970 N) and absorbed more energy (about 2.09 J compared with 1.94 J), so the difference narrowed. These values are approximate because they are calculated from group mean energies. A possible contribution to the lower early load of the TEROSON MS 939 panels is the greater shear deformation of its softer and thicker bond line, but this cannot be separated from the other differences between the configurations (Section 3.4). Because the tests ended at different deflections, the total energy-absorption capacity of the two configurations could not be compared.
3.2. Strain Response and Damage Development
Figure 8 and Figure 9 show load and deflection as functions of longitudinal strain for representative LOCTITE EA 9466 and TEROSON MS 939-bonded panels, respectively. The strain was measured at mid-span on the lower face sheet and therefore represents the local tensile response at the gauge position. The representative panels correspond to the adhesive groups shown in Figure 4 and Figure 5, while the group-level load-deflection statistics are summarized in Table 3.
Figure 8.
Load and deflection as functions of longitudinal strain for the representative LOCTITE EA 9466-bonded aluminum foam-core sandwich panel.
Figure 9.
Load and deflection as functions of longitudinal strain for the representative TEROSON MS 939-bonded aluminum foam-core sandwich panel.
For the LOCTITE EA 9466 bonded panel, the load increased rapidly with longitudinal strain during the first 1.0 × 10−3. The maximum load occurred at approximately 1.9 × 10−3 strain, and the load remained close to its maximum value up to approximately 2.1 × 10−3 strain. An abrupt load reduction of approximately 6–7% occurred at about 2.2 × 10−3 strain, with only a small simultaneous increase in strain. The load then recovered slightly and remained comparatively stable between approximately 2.4 × 10−3 and 3.2 × 10−3 strain. During the subsequent post-peak stage, the strain continued to increase as the load decreased gradually. A longitudinal strain of approximately 5.4 × 10−3 was reached near the end of the recorded response. At this point, the panel retained approximately 83% of its maximum load. The gradual load reduction over the remaining strain range shows that local deformation of the lower face sheet continued while the panel retained a substantial part of its load-carrying capacity.
The deflection of the LOCTITE EA 9466 bonded panel increased throughout loading and reached approximately 12.2 mm at the end of the recorded response. During the initial stage, the deflection reached approximately 1.4 mm at 1.0 × 10−3 strain, corresponding to an average increase of about 1.4 mm per 1.0 × 10−3 strain. The deflection then increased more rapidly, reaching approximately 5.3 mm at 2.3 × 10−3 strain, corresponding to an average increase of about 3.0 mm per 1.0 × 10−3 strain between 1.0 × 10−3 and 2.3 × 10−3. Beyond this point, the deflection increased at a relatively steady rate of approximately 2.2 mm per 1.0 × 10−3 strain, reaching approximately 12.2 mm at the final strain of 5.4 × 10−3. Strain accumulation therefore continued together with increasing deflection during the post-peak stage. This behavior reflects the combined development of global bending, local lower face sheet deformation, and progressive crushing of the foam core.
For the TEROSON MS 939-bonded panel, the load increased progressively with longitudinal strain during the initial loading stage. The maximum load occurred at approximately 3.8–4.0 × 10−3 strain, and the load remained close to its maximum value until approximately 4.2 × 10−3 strain. A moderate load reduction then occurred between approximately 4.2 × 10−3 and 4.5 × 10−3strain, followed by a slight recovery near 4.7–4.8 × 10−3 strain. A second load reduction occurred between approximately 4.9 × 10−3 and 5.4 × 10−3 strain. During the subsequent post-peak stage, the longitudinal strain continued to increase while the load decreased gradually. Between approximately 5.5 × 10−3 and 8.7 × 10−3 strain, the panel maintained a comparatively stable post-peak response with only a moderate reduction in load. A further decrease occurred near the end of the record, where a longitudinal strain of approximately 9.3 × 10−3 was reached. At this point, the panel retained approximately 79–80% of its maximum load. The gradual post-peak reduction indicates that local tensile deformation of the lower face sheet continued while the panel retained a substantial proportion of its load-carrying capacity.
The deflection of the TEROSON MS 939-bonded panel increased throughout loading and reached approximately 21.0 mm at the end of the recorded response. During the initial stage, the deflection reached approximately 4.1 mm at 2.0 × 10−3 strain, corresponding to an average increase of approximately 2.1 mm per 1.0 × 10−3 strain. The deflection then increased more rapidly, reaching approximately 10.7 mm at 4.0 × 10−3 strain, corresponding to an average increase of approximately 3.3 mm per 1.0 × 10−3 strain between 2.0 × 10−3 and 4.0 × 10−3 strain. A short region of slower deflection growth was observed between approximately 4.0 × 10−3 and 4.6 × 10−3 strain. Beyond this region, the deflection increased at a comparatively steady rate, reaching approximately 16.0 mm at 7.0 × 10−3 strain and approximately 21.0 mm at the final strain of 9.3 × 10−3. Strain accumulation therefore continued together with increasing deflection throughout the post-peak stage. This behavior reflects the combined development of global bending, local lower-face sheet deformation, and progressive crushing of the foam core.
The representative panels differed mainly in the strain and deflection at which the maximum load was reached. The LOCTITE EA 9466 panel reached its maximum at approximately 1.9 × 10−3 strain, whereas the TEROSON MS 939 panel reached its maximum at approximately 3.8–4.0 × 10−3 strain. Thus, the LOCTITE EA 9466 panel reached maximum load earlier in the local strain history, while the TEROSON MS 939 panel developed greater local strain and deflection before reaching maximum load. After the maximum load, both panels continued to accumulate lower face sheet strain while retaining substantial load. The LOCTITE response showed an earlier post-peak reduction and subsequent gradual softening, whereas the TEROSON response maintained a broader high-load region before gradually decreasing. These strain-based observations are consistent with the group load-deflection results in Section 3.1, particularly the larger deflection at maximum load and higher load retention at 12 mm for TEROSON MS 939.
The strain records describe local behavior at the gauge positions. The gauge response was influenced by the overall panel curvature, local bending of the lower face sheet, indentation beneath the central loading roller, and deformation of the adjacent foam cells. The measured strain should therefore not be interpreted as uniform strain across the complete sandwich section. To assess specimen-to-specimen variability, the strain at maximum load and the maximum recorded strain were determined for all three specimens in each adhesive configuration. The specimen-level values and descriptive group statistics are summarized in Table 5.
Table 5.
Lower face sheet longitudinal strain results for all tested specimens.
The specimen-level results are consistent with the trends shown by the representative curves. The mean strain at maximum load was 1.985 ± 0.069 × 10−3 for LOCTITE EA 9466 and 4.090 ± 0.450 × 10−3 for TEROSON MS 939, with coefficients of variation of 3.46% and 11.01%, respectively. The mean maximum recorded strain was 5.450 ± 0.116 × 10−3 for LOCTITE EA 9466 and 9.883 ± 0.506 × 10−3 for TEROSON MS 939, with coefficients of variation of 2.13% and 5.12%, respectively. All three TEROSON MS 939 specimens reached maximum load at a higher local strain and developed a higher maximum recorded strain than the LOCTITE EA 9466 specimens.
After unloading, the strain of the representative panels decreased by 27.4% for TEROSON MS 939 and 29.5% for LOCTITE EA 9466 relative to their maximum values. The remaining strain is consistent with permanent deformation of the panels. After unloading, the residual mid-span deflection was measured, and the recovered deflection was calculated as the maximum recorded deflection minus the residual deflection. Partial geometric recovery was observed for the TEROSON MS 939 panels, with a mean recovered deflection of 4.52 mm, although permanent curvature remained. The remaining curvature is consistent with the permanent foam-core crushing and face sheet deformation observed in the post-test assessment, and a residual dent caused by core crushing is typical for foam-core sandwich beams [43]. Measured recovery represents the combined response of the face sheets, foam core, and adhesive layers rather than the response of the adhesive alone.
3.3. Post-Test Damage Morphology
The post-test morphology of the adhesive and near-interface foam regions is presented in Figure 10. All three specimens from each adhesive configuration were examined, and the specimen-level observations are summarized in Table 6. The main damage features were similar within each group, although their exact location and extent varied because of the heterogeneous cellular structure. Images (a–c) show a representative TEROSON MS 939-bonded specimen, while images (d–f) show a representative LOCTITE EA 9466-bonded specimen. Both configurations exhibited permanent deformation of the cellular core, including bending, buckling, and localized collapse of the foam walls. These features agree with the indentation, cellular-collapse, and core-deformation mechanisms previously reported for aluminum foam sandwich panels under three-point bending [15,19].
Table 6.
Specimen-level post-test damage observations in the inspected regions.
In the representative TEROSON MS 939 specimen, the adhesive formed rounded fillets around the exposed foam-cell edges and remained visibly continuous along the inspected upper and lower face-core regions. Figure 10a shows bending and distortion of the foam walls near the upper face sheet, while Figure 10b shows more pronounced cellular collapse within the core. Despite this local damage, no continuous opening was observed along the examined face-core boundaries. At the lower interface shown in Figure 10c, the adhesive remained attached to the face sheet and extended around the neighbouring foam-cell edges.
These observations suggest that deformation developed through bond line deformation and progressive collapse of the adjacent cellular structure, while face-core continuity was maintained. The continuous TEROSON MS 939 bond line is consistent with the maximum load being reached at a larger deflection and strain (Section 3.2 and Figure 10).
Figure 10.
Digital-microscope images of the post-test face-core and foam-core regions: (a–c) TEROSON MS 939-bonded specimen and (d–f) LOCTITE EA 9466-bonded specimen. The selected specimens show the main damage characteristics observed within their corresponding adhesive groups. (a) section showing adhesive continuity at the upper and lower face-core regions and deformation of the adjacent foam cells; (b) localized cellular collapse within the foam core; (c) section showing preserved adhesive attachment at the lower face-core region; (d) deformation of the cellular structure adjacent to the upper face sheet; (e) buckling and collapse of foam walls within the core; and (f) opened region adjacent to the lower face sheet, with foam on both separated surfaces. The scale bar in each panel represents 7.5 mm.
The larger normalized deflection at maximum load was observed in all three TEROSON MS 939 panels. This is consistent with the much higher elongation of this adhesive and with the maintained bond line continuity observed after testing, which indicate a more compliant face core connection that allows greater relative movement between the face sheet and the core as the panel curvature increases. Because the bond line thickness and the cured adhesive properties were not measured independently, this behaviour is attributed to the complete panel configuration and not to a single adhesive property. Permanent foam damage was present in both configurations, and visible attachment of the TEROSON MS 939 bond line was maintained within the inspected regions.
The LOCTITE EA 9466 specimen exhibited a more localized damage pattern. Figure 10d shows deformation of the foam cells adjacent to the upper face sheet, including bent and partly collapsed walls beneath the loading region. Figure 10e shows extensive distortion of the cellular network, with irregular pore shapes and locally folded cell walls. These features indicate that indentation and progressive foam crushing contributed to the permanent deformation of the epoxy-bonded panel.
The main difference was observed in the lower face-core region in Figure 10f, where a wide opening developed adjacent to the lower face sheet. The opposing surfaces were irregular, and fragments of the near-interface cellular structure remained visible along the separated region. Foam cell walls are visible on both sides of the opening, indicating that the separation occurred predominantly within the near-interface foam, through tearing and fracture of the foam cell walls, rather than along the adhesive layer. This morphology indicates that the bonded connection remained attached to fragments of the adjacent cellular structure [20]. The opening reduced the load transfer between the lower face sheet and the foam core over the affected region.
Previous studies have also shown that the face-core bonding condition affects deformation and damage development in aluminum foam sandwich panels. Maintaining the face-core connection allows a larger region of the cellular core to participate in progressive deformation. In contrast, interface separation reduces composite action and changes the subsequent load-transfer path [19,44]. Debonding has also been reported in adhesively bonded aluminum foam sandwich panels under cyclic three-point bending, when the joining region becomes the controlling part of the structural response [44].
A similar dependence on interface continuity has been reported for GLARE, where fiber orientation, stacking sequence, and interfacial adhesion affect the development of delamination and cracking under bending [33,34,35]. Although the present panels have a different internal structure, both material systems suggest that local separation between bonded layers changes load transfer and damage development.
The strain measurements and digital-microscope observations showed different deformation and damage responses for the two adhesive configurations. In the representative LOCTITE EA 9466 panel, maximum load was reached at a lower local strain, and foam-core crushing was accompanied by an opened lower face-core region with near-interface foam fracture. In the representative TEROSON MS 939 panel, maximum load was reached at a higher local strain, while visible adhesive continuity was maintained throughout the inspected regions. These differences may reflect the combined influence of adhesive strength, deformation capacity, curing behaviour, final bond line geometry, and interaction with the adjacent cellular core. Local variations in foam-cell size, shape, wall thickness, and defects may also have affected the initiation and development of crushing, tearing, and near-interface fracture. Since these factors were not varied independently, the observed damage patterns are interpreted as responses of the complete adhesive-panel configurations rather than as the isolated effect of one adhesive or foam characteristic.
3.4. Scope and Interpretation of the Mechanical Response
The present study compares complete sandwich-panel configurations manufactured with two commercial adhesive systems. As described in Section 2.1, several adhesive characteristics differed between the configurations, and their separate effects were not isolated. The final manufactured geometry also differed, as shown by the measured total panel thicknesses. The results are therefore interpreted at the configuration level rather than as the isolated effect of one adhesive property.
The difference in total panel thickness was considered by normalizing deflection at maximum load by the measured thickness of each configuration. The normalized results confirmed that the greater deformation of the TEROSON MS 939 configuration remained clear after accounting for panel thickness. However, the present measurements do not separate the effects of local bond line geometry, adhesive penetration into the foam surface, and other local manufacturing variations.
The measured three-point bending response included global panel bending, core shear, local indentation, foam crushing, and face-core damage. These mechanisms developed together during loading and could not be separated reliably using the available crosshead-deflection measurements. The reported maximum load, normalized deflection, load retention, absorbed energy, lower face sheet strain, and damage observations therefore describe the response of the complete manufactured panels under the stated test conditions.
Further work using calibrated bond line spacers, controlled adhesive application, recorded clamping conditions, direct bond line measurements, and additional panel geometries would allow the effects of adhesive properties and bonded geometry to be examined separately.
4. Conclusions
This study compared the quasi-static flexural response and damage development of aluminum foam-core sandwich panels manufactured with LOCTITE EA 9466 and TEROSON MS 939 adhesive systems. The first objective concerned the global flexural and post-peak responses. The two configurations reached similar maximum loads, with a 4.5% higher mean value for LOCTITE EA 9466. A clearer difference was observed in deformation behaviour, as the TEROSON MS 939 panels reached maximum load at an 87.6% greater mean deflection and carried a higher load at the common deflection of 12 mm. In contrast, the LOCTITE EA 9466 panels absorbed 20.5% more energy up to 12 mm. The main result is therefore a trade-off between greater energy absorption within the selected deflection range and greater deformation before maximum load.
The second and third objectives concerned local strain development and post-test damage. Lower face sheet strain continued to increase during post-peak loading in both representative panels while substantial load-carrying capacity was maintained. The TEROSON MS 939 specimen developed greater local strain and deflection before maximum load, whereas the LOCTITE EA 9466 specimen reached maximum load at a lower local strain. Post-test examination showed foam-cell bending, buckling, and localized crushing in both configurations. Visible face-core continuity was maintained in the inspected TEROSON MS 939 specimen, while an opening with near-interface foam fracture developed in the inspected LOCTITE EA 9466 specimen. These observations connect the global bending response with local strain and damage location, but they are interpreted as configuration-level findings rather than effects caused by adhesive compliance alone.
The findings apply to the tested panel geometry, manufacturing conditions, support span, and quasi-static loading rate, with three specimens tested per adhesive configuration. The adhesive systems also differed in chemistry, curing mechanism, mechanical properties, and final bond line geometry, and the separate influence of these factors was not isolated. Within this scope, adhesive selection should consider deformation capacity, post-peak load retention, energy absorption, and face-core damage together with maximum load. Further validation should include additional specimens, controlled bond line thickness, direct characterization of the cured adhesives, and testing across other panel geometries and loading rates.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/ma19234988/s1, Table S1. Individual endpoint observations for all tested specimens. Table S2. Individual absorbed-energy values at the common deflection limits. Table S3. Group descriptive statistics for the main response measures. Table S4. Exploratory comparison of the main endpoint measures.
Author Contributions
Conceptualization, C.A.T., S.D. and S.S.; methodology, C.A.T.; software, C.A.T. and S.S.; validation, S.D., S.S. and C.A.T.; formal analysis, C.A.T., S.D. and S.S.; investigation, A.W., C.A.T., G.G., G.K., S.D., S.S. and T.M.; resources, A.W., C.A.T., G.G., G.K., S.D., S.S. and T.M.; writing—original draft preparation, C.A.T.; writing—review and editing S.D., S.S. and C.A.T.; visualization, C.A.T., S.S. and S.D.; supervision, S.D. and S.S.; funding acquisition, S.D. All authors have read and agreed to the published version of the manuscript.
Funding
This publication has been funded by the Polish Ministry of Science and Higher Education under the “Vectors of Science” programme, project number WNK/SN/0508/2025/01, with project funding of PLN 134,200.00 and total project value of PLN 174,200.00. The content of this article was presented during the 62nd Symposium “Modelowanie w mechanice” (Modelling in Mechanics), Szczyrk, Poland, 1–4 March 2026.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contribution of this research is included in the paper and Supplementary Material. For further inquiries, please contact the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Chen, C.; Harte, A.M.; Fleck, N.A. The plastic collapse of sandwich beams with a metallic foam core. Int. J. Mech. Sci. 2001, 43, 1483–1506. [Google Scholar] [CrossRef] [Scilit]
- Huo, X.; Sun, G.; Zhang, H.; Lv, X.; Li, Q. Experimental study on low-velocity impact responses and residual properties of composite sandwiches with metallic foam core. Compos. Struct. 2019, 223, 110835. [Google Scholar] [CrossRef] [Scilit]
- Steeves, C.A.; Fleck, N.A. Collapse mechanisms of sandwich beams with composite faces and a foam core, loaded in three-point bending. Part II: Experimental investigation and numerical modelling. Int. J. Mech. Sci. 2004, 46, 585–608. [Google Scholar] [CrossRef] [Scilit]
- Bart-Smith, H.; Hutchinson, J.W.; Evans, A.G. Measurement and analysis of the structural performance of cellular metal sandwich construction. Int. J. Mech. Sci. 2001, 43, 1945–1963. [Google Scholar] [CrossRef] [Scilit]
- Charkaoui, A.; Hassan, N.M.; Bahroun, Z. Enhancing mechanical properties of cellular core sandwich panels: A review of topological parameters and design improvements. Mater. Res. Express 2023, 10, 102001. [Google Scholar] [CrossRef] [Scilit]
- Castanie, B.; Bouvet, C.; Ginot, M. Review of composite sandwich structure in aeronautic applications. Compos. Part C Open Access 2020, 1, 100004. [Google Scholar] [CrossRef] [Scilit]
- Banhart, J.; García-Moreno, F.; Heim, K.; Seeliger, H.W. Light-Weighting in Transportation and Defence Using Aluminium Foam Sandwich Structures. In Light Weighting for Defense, Aerospace, and Transportation; Gokhale, A.A., Prasad, N.E., Basu, B., Eds.; Springer: Singapore, 2019; pp. 61–72. [Google Scholar]
- Tarlochan, F. Sandwich Structures for Energy Absorption Applications: A Review. Materials 2021, 14, 4731. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Novak, N.; Vesenjak, M.; Duarte, I.; Tanaka, S.; Hokamoto, K.; Krstulović-Opara, L.; Guo, B.; Chen, P.; Ren, Z. Compressive Behaviour of Closed-Cell Aluminium Foam at Different Strain Rates. Materials 2019, 12, 4108. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Guo, Q.; Li, W.; Yao, W.; Wang, X.; Huang, C. Mechanical Properties and Constitutive Model Applied to the High-Speed Impact of Aluminum Foam That Considers Its Meso-Structural Parameters. Materials 2021, 14, 6206. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sharma, V.; Zivic, F.; Grujovic, N.; Babcsan, N.; Babcsan, J. Numerical Modeling and Experimental Behavior of Closed-Cell Aluminum Foam Fabricated by the Gas Blowing Method under Compressive Loading. Materials 2019, 12, 1582. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wan, X.; Zhu, K.; Xu, Y.; Han, B.; Jing, T. Early Compressive Deformation of Closed-Cell Aluminum Foam Based on a Three-Dimensional Realistic Structure. Materials 2019, 12, 1792. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Costanza, G.; Giudice, F.; Sili, A.; Tata, M.E. Correlation Modeling between Morphology and Compression Behavior of Closed-Cell Al Foams Based on X-ray Computed Tomography Observations. Metals 2021, 11, 1370. [Google Scholar] [CrossRef] [Scilit]
- Crupi, V.; Montanini, R. Aluminium foam sandwiches collapse modes under static and dynamic three-point bending. Int. J. Impact Eng. 2007, 34, 509–521. [Google Scholar] [CrossRef] [Scilit]
- Wang, X.; Cao, Z.; Fu, G. Quasi-Static Three-Point Bending Behavior of Aluminum Foam Sandwich with CFRP Face-Sheets. Metals 2022, 12, 1393. [Google Scholar] [CrossRef] [Scilit]
- McCormack, T.M.; Miller, R.; Kesler, O.; Gibson, L.J. Failure of sandwich beams with metallic foam cores. Int. J. Solids Struct. 2001, 38, 4901–4920. [Google Scholar] [CrossRef] [Scilit]
- Kabir, K.; Vodenitcharova, T.; Hoffman, M. Response of aluminium foam-cored sandwich panels to bending load. Compos. Part B Eng. 2014, 64, 24–32. [Google Scholar] [CrossRef] [Scilit]
- Formisano, A.; Durante, M.; Viscusi, A.; Carrino, L. Mechanical behavior and collapse mechanisms of innovative aluminum foam-based sandwich panels under three-point bending. Int. J. Adv. Manuf. Technol. 2021, 112, 1631–1639. [Google Scholar] [CrossRef] [Scilit]
- Huang, P.; Sun, X.; Su, X.; Gao, Q.; Feng, Z.; Zu, G. Three-Point Bending Behavior of Aluminum Foam Sandwich with Different Interface Bonding Methods. Materials 2022, 15, 6931. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Neugebauer, R.; Lies, C.; Hohlfeld, J.; Hipke, T. Adhesion in sandwiches with aluminum foam core. Prod. Eng. 2007, 1, 271–278. [Google Scholar] [CrossRef] [Scilit]
- Badkul, A.; Saxena, S. Developing metallic bond in aluminum foam in-filled sandwich composite panels and comparing normal and in-plane shear strengths performance with polymeric binders. Sādhanā 2023, 48, 160. [Google Scholar] [CrossRef] [Scilit]
- Huang, W.; Wang, M.; Zhang, Y.; Li, H.; Liu, Q.; Liu, T. Fabrication and Bending Performance of Aluminum Foam Sandwich Panels via Powder Composite Rolling Method. J. Mater. Eng. Perform. 2026, 35, 19204–19214. [Google Scholar] [CrossRef] [Scilit]
- Li, Y.; Gao, Q.; Su, X.; Feng, Z.; Fan, J.; Huang, P.; Zu, G. Interfacial Microstructure Evolution and Compressive Behavior of Asymmetric Aluminum Foam Sandwich Fabricated by Coupling Two-Step Foaming With Vacuum Bonding. Adv. Eng. Mater. 2026, 28, e202502947. [Google Scholar] [CrossRef] [Scilit]
- Huang, P.; Gao, Q.; Su, X.; Feng, Z.; Sun, X.; Zu, G. Effect of Core Density on the Three-Point Bending Performance of Aluminum Foam Sandwich Panels. Materials 2023, 16, 7091. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lu, X.; Jing, L.; Zhou, W.; Yang, H.; Yuan, P.; Li, X. Pore Structure and Deformation Correlation of an Aluminum Foam Sandwich Subject to Three-Point Bending. Materials 2024, 17, 567. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yao, C.; Hu, Z.; Mo, F. Three-Point Bending Fatigue Behavior of Aluminum Foam Sandwich Panels with Different Density Core Material. Metals 2021, 11, 1542. [Google Scholar] [CrossRef] [Scilit]
- Dhaliwal, G.S.; Newaz, G.M. Flexural Response of Degraded Polyurethane Foam Core Sandwich Beam with Initial Crack between Facesheet and Core. Materials 2020, 13, 5399. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hunston, D.; Miyagi, Z.; Schultheisz, C.; Zaghi, S. The Sandwich Bending Specimen for Characterizing Adhesive Properties. Mech. Time-Depend. Mater. 2003, 7, 71–88. [Google Scholar] [CrossRef] [Scilit]
- Fatima, N.S.; Dhaliwal, G.S.; Newaz, G. Influence of interfacial adhesive on impact and post-impact behaviors of CFRP/end-grain balsawood sandwich composites. Compos. Part B Eng. 2021, 212, 108718. [Google Scholar] [CrossRef] [Scilit]
- Pereira, A.B.; Fernandes, F.A.O. Sandwich Panels Bond with Advanced Adhesive Films. J. Compos. Sci. 2019, 3, 79. [Google Scholar] [CrossRef] [Scilit]
- Vermeeren, C.A.J.R. An Historic Overview of the Development of Fibre Metal Laminates. Appl. Compos. Mater. 2003, 10, 189–205. [Google Scholar] [CrossRef] [Scilit]
- Sinmazçelik, T.; Avcu, E.; Bora, M.Ö.; Çoban, O. A review: Fibre metal laminates, background, bonding types and applied test methods. Mater. Des. 2011, 32, 3671–3685. [Google Scholar] [CrossRef] [Scilit]
- Anand, S.; Dighe, N.; Gupta, P.; Alderliesten, R.; Castro, S.G.P. Failure modes and energy absorption in Glass Reinforced aluminum (GLARE) hybrid laminates subjected to three-point bending. Compos. Part C Open Access 2025, 18, 100651. [Google Scholar] [CrossRef] [Scilit]
- Megahed, M.; Alsaeedy, A.M.; Alshorbagy, A.E.; Atta, M. Influence of curing pressure and surface treatment on mechanical properties of hybrid fiber metal laminates. Sci. Rep. 2026, 16, 22538. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Allah, M.M.A.; Almuflih, A.S.; Mahmoud, S.F.; Saleh, D.I.; El-baky, M.A.A. Orientation- and Stacking Sequence-Dependent Mechanical Response and Failure Mechanisms of GLARE 3/2 Laminates. Fibers Polym. 2026, 27, 3991–4001. [Google Scholar] [CrossRef] [Scilit]
- Latour, M.; D’Aniello, M.; Landolfo, R.; Rizzano, G. Experimental and numerical study of double-skin aluminium foam sandwich panels in bending. Thin-Walled Struct. 2021, 164, 107894. [Google Scholar] [CrossRef] [Scilit]
- Macek, W.; Branco, R.; Szala, M.; Marciniak, Z.; Ulewicz, R.; Sczygiol, N.; Kardasz, P. Profile and Areal Surface Parameters for Fatigue Fracture Characterisation. Materials 2020, 13, 3691. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Henkel AG & Co. KGaA. TEROSON MS 939 Technical Data Sheet. 2019. Available online: https://datasheets.tdx.henkel.com/TEROSON-MS-939-en_GL.pdf (accessed on 1 June 2026).
- Henkel AG & Co. KGaA, LOCTITE EA 9466 Technical Data Sheet. 2025. Available online: https://datasheets.tdx.henkel.com/LOCTITE-EA-9466-en_GL.pdf (accessed on 1 June 2026).
- ASTM C393/C393M-20; Standard Test Method for Core Shear Properties of Sandwich Constructions by Beam Flexure. ASTM International: West Conshohocken, PA, USA, 2020.
- Vishay Micro-Measurements. 240UZA General Purpose Strain Gages—Linear Pattern; Vishay Precision Group: Raleigh, NC, USA, 2020. [Google Scholar]
- Li, Z.; Chen, X.; Jiang, B.; Lu, F. Local indentation of aluminum foam core sandwich beams at elevated temperatures. Compos. Struct. 2016, 145, 142–148. [Google Scholar] [CrossRef] [Scilit]
- Zenkert, D.; Shipsha, A.; Persson, K. Static indentation and unloading response of sandwich beams. Compos. Part B Eng. 2004, 35, 511–522. [Google Scholar] [CrossRef] [Scilit]
- Yao, C.; Hu, Z.; Mo, F.; Wang, Y. Fabrication and Fatigue Behavior of Aluminum Foam Sandwich Panel via Liquid Diffusion Welding Method. Metals 2019, 9, 582. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.