Abstract
To develop a multifunctional system, novel hydrogel matrices based on poly(vinylpyrrolidone), carboxymethylcellulose, poly(ethylene glycol), and agar were crosslinked via 30 kGy electron beam (e-beam). The functionality of the hydrogels was achieved through physicochemical and structural characterization. Additionally, cumulative wet-mass loss in buffer media and 5-fluorouracil (5-FU) loading capacity/release profiles were evaluated and investigated using mathematical models employed in the design of pharmaceutical formulations. At 30 kGy, gel fractions reached 98.25% for H1 and 94.72% for H2. The calculated crosslinking-to-chain-scission yield ratios were 16.66 for H1 and 2.27 for H2, indicating that crosslinking predominated in both formulations. The swelling degree and 5-FU loading depended on pH, reaching higher swelling at neutral pH (1380–1580%) than in basic media (980–1090%). Under ambient conditions, the hydrogels showed a relative wet-mass retention of approximately 46% after 8 h. Optimal 5-FU loading (~30% at 200 mg/L) occurred at pH 5–6, while sustained release at pH 7.4 reached ~47–54% within 30 h. 5-FU release kinetics were best described by Weibull for H1 at pH 5.0, while Peppas–Sahlin performed comparably to Weibull for H2 at pH 5.0, and to Makoid–Banakar for both hydrogels at pH 7.4 (R2 = 0.99). The experimental profiles showed an initial rapid release phase followed by slower release. The experimental results demonstrate that hydrogels obtained through e-beam crosslinking support the loading and release of 5-FU.
1. Introduction
Wound-healing processes can be accelerated through the use of a suitable medical device that offers distinct therapeutic advantages over conventional adhesive dressings. Hydrogel-based dressings have received considerable attention due to their highwater content and soft, conformable architecture that promotes wound hydration, adheres to irregular anatomical contours, absorbs exudate, and provide a protective barrier against the external environment [1]. Their relevance in tissue engineering and localized drug delivery applications arises from their water-swollen polymer network that combines high aqueous swelling with sufficient network integrity for handling and application [2].
The choice of biocompatible and non-toxic component materials is highly crucial as hydrogel dressings are applied directly to the wound sites. An effective approach to equilibrate predictable mechanical behaviour with hydration capacity and biologically relevant material properties is the combination of synthetic and natural polymers. Poly(vinylpyrrolidone) (PVP) is commonly used in radiation-crosslinked dressings due to its hydrophilicity, biocompatibility and ability to form stable polymer networks following irradiation [3]. Dressings based only on pure PVP have pure poor swelling, but their combination with polysaccharides such as carboxymethylcellulose (CMC) or agar improves these properties. Natural polymers, including CMC [4,5] and agar [6], contribute to water uptake, viscoelasticity, conformability, and hydration-dependent interactions with the surrounding medium. Poly(ethylene glycol) (PEG) is used as a plasticizing and network-modifying component to increase matrix flexibility, water uptake, and solute transport [7]. The potential of multicomponent radiation-crosslinked hydrogel systems has been demonstrated in PVP/CMC/agar matrices containing self-assembled silver nanostructures, which showed high water uptake, acceptable cytocompatibility, and improved wound closure in a rabbit model. However, that study primarily focused on antimicrobial performance rather than controlled therapeutic release [8].
In aqueous polymer formulations, e-beam or γ-irradiation generates reactive species that can promote interchain bond formation and hydrogel network development without conventional low-molecular-weight initiators and, in suitable systems, without supplementary chemical crosslinkers [9]. Depending on the irradiation conditions, this approach may also support concurrent material sterilization; however, this outcome must be validated for the specific formulation, absorbed dose, packaging configuration, and intended application [10]. During irradiation, radical recombination promotes network formation, whereas polymer-chain cleavage counteracts gel development; consequently, sol–gel analysis and radiochemical-yield calculations are commonly used to assess the balance between these competing processes [9]. Previous work on e-beam-irradiated PVP/PEG/agar dressings has shown that the irradiation dose and polymer composition can markedly influence gel fraction, swelling capacity, and other functional characteristics of the resulting hydrogels [3].
Beyond their use as wound-contact materials, hydrogels can serve as local reservoirs for therapeutic agents incorporated within the polymeric matrices. The drug-release profile may be influenced by water penetration, the diffusion of the incorporated drug through the hydrated matrix, time-dependent polymer-segment relaxation, and, when relevant, gradual erosion or degradation of the network [11]. These systems are of particular interest for superficial cutaneous lesions accessible to topical treatment, where local administration may increase drug concentration at the target site while reducing systemic exposure. This approach may be relevant for selected non-melanoma skin cancers, precancerous lesions, or localized cutaneous lesions for which topical chemotherapy is clinically appropriate [12].
5-Fluorouracil (5-FU) is a fluorinated pyrimidine analogue whose antineoplastic activity is mainly associated with thymidylate synthase inhibition and the incorporation of active metabolites into nucleic-acid metabolic pathways [13]. However, its systemic use is constrained by dose-dependent toxicity in normal tissues with rapid cellular turnover [14]. Topical 5-FU formulations are already used in the management of selected precancerous and non-melanoma skin lesions, including actinic keratosis and certain superficial skin carcinomas. Consequently, controlled local delivery systems may prolong residence at the application site, regulate the release profile, and potentially reduce fluctuations in local drug exposure [15].
Several formulation approaches have been investigated to enhance local retention and/or skin permeation of 5-FU. For example, nanoemulsion-based gels have been reported to enhance cutaneous penetration relative to conventional formulations [16], whereas nanostructured lipid-carrier/hydrogel systems have been designed to improve drug flux through the skin [17]. Polymeric hydrogel networks have also been investigated as matrices for 5-FU loading and release. In one study, CMC/PVP-g-poly(acrylic acid) hydrogels were prepared by free-radical polymerization using N,N′-methylenebisacrylamide (MBA) as a crosslinking agent for potential colon-targeted 5-FU delivery. Drug release was evaluated under different pH conditions, while cytocompatibility, hemocompatibility, and acute oral toxicity assessments were used to investigate the safety of the developed matrices [18]. Radiation-crosslinked polymeric networks have also been explored for drug delivery. Ghobashy et al. prepared amphiphilic chitosan-grafted acrylic acid/2-acrylamido-2-methylpropane sulfonic acid hydrogels by gamma irradiation and evaluated their potential for controlled drug delivery [19]. More recently, a gamma-irradiated PVA/arginine/poly(methacrylic acid-co-acrylic acid)/zirconium composite hydrogel was developed for colon-targeted 5-FU administration, providing another example of radiation-engineered networks in stimulus-responsive drug-delivery systems [20].
Mathematical modeling is commonly used to describe drug-release kinetics and provide insight into the transport processes involved in hydrogel matrices [21]. The Korsmeyer–Peppas model can support the interpretation of release behavior in terms of Fickian diffusion, polymer relaxation, or anomalous transport [22]. The Peppas–Sahlin model can be used to estimate the relative contributions of diffusion and polymer relaxation to the overall release process [23].
While e-beam-crosslinked ternary PVP/PEG/agar hydrogels have previously been investigated strictly as physical moist as wound-dressing materials without therapeutic agents [3,24], their use as carriers for 5-FU delivery has not yet been reported. The present study introduces a quaternary multicomponent system by incorporating carboxymethylcellulose (CMC) into the PVP/PEG/agar matrix, crosslinked exclusively via electron-beam irradiation without low-molecular-weight chemical crosslinkers (such as glutaraldehyde or N,N′-methylenebisacrylamide). Combining radiation-induced network characterization with the evaluation of pH-dependent swelling, 5-FU loading, and in vitro release provides a necessary physicochemical foundation prior to biological and preclinical testing. A comparison with selected radiation-crosslinked hydrogels and hydrogel-based drug-delivery systems is provided in Table S1.
Two formulations were irradiated at an absorbed dose of 10–30 kGy to evaluate their sol–gel response and the parameters describing radiation-induced network formation. The hydrogels obtained at 30 kGy were subsequently characterized in terms of their physical, structural, viscoelastic, and swelling properties. Freeze-dried hydrogels were then loaded with 5-FU, and the effects of drug concentration and medium pH on loading efficiency were evaluated. Finally, in vitro 5-FU release at pH 5.0 and 7.4 was analyzed using Korsmeyer–Peppas, Peppas–Sahlin Makoid–Banakar and Weibull models to characterize the release kinetics.
2. Results and Discussion
2.1. Gel Fraction and E-Beam Radiation-Induced Network Formation
The gel fractions (GF) of H1 and H2 increased in a dose-dependent manner across the 10–30 kGy range (Figure 1a). The GF reached 98.25 ± 0.42% for H1 and 94.72 ± 0.58% for H2 at 30 kGy, indicating the formation of water-insoluble polymer networks. The rise in GF was more significant between 10 and 25 kGy, in contrast to 25–30 kGy, indicating that network formation approached a plateau at the highest dose. This observation aligns with our previous findings on multicomponent PVP-based hydrogels crosslinked by e-beam irradiation, where GF increased sharply up to 15–25 kGy and subsequently approached a plateau, suggesting increasing competition between chain scission and crosslinking at higher doses [25].
Figure 1.
Physicochemical properties of hydrogels: (a) GF as a function of e-beam irradiation doses; (b) relative wet-mass retention under ambient conditions, with representative photographs acquired at 0 and 24 h; (c,d) pH-dependent swelling behavior in buffer solutions at pH 4.0–8.0; and (e,f) cumulative wet-mass loss during 30 days of incubation in the corresponding buffer media. Panels (b–f) show data for hydrogels irradiated at 30 kGy. Data are presented as mean ± SD (n = 3).
The higher GF of H1 at 30 kGy suggests that the relative proportions of PVP, CMC, and PEG affected the overall balance between radiation-induced crosslinking and chain scission. Despite H2 having a greater concentration of PVP, its lower CMC content and different PEG amount could have influenced chain mobility, intermolecular interactions, and the efficiency of radical recombination during irradiation, ultimately resulting in a slightly lower insoluble fraction. Anwar et al. reported a direct relationship between GF and the concentrations of the constituent polymers (XG and PVP), acrylic acid monomer, and EGDMA crosslinker in chemically crosslinked XG/PVP-co-poly(acrylic acid) hydrogels. In contrast, despite its higher PVP content, H2 exhibited a slightly lower gel fraction than H1 at 30 kGy, indicating that, in the e-beam-irradiated PVP/CMC/PEG/agar systems, PVP concentration was not the exclusive factor of network formation [26]. The sol–gel results clearly demonstrate the successful formation of highly water-insoluble polymer networks in both pre-hydrogels formulations under e-beam irradiation. Wach et al. reported a dose-dependent increase in GF for e-beam-irradiated CMC-containing polysaccharide hydrogels, followed by a decrease at higher doses when chain scission increasingly competed with crosslinking. In the present study, the limited increase in GF between 25 and 30 kGy suggests that network formation approached a plateau; however, no degradation was detected within the investigated dose range [27].
The Charlesby–Rosiak analysis further confirmed that crosslinking predominated over degradation in both hydrogel compositions (Table 1). The calculated p0/q0 values were 0.03 (H1) and 0.22 (H2), both below the threshold value of 2, indicating a crosslinking-dominated radiation response. The markedly lower p0/q0 value of H1 indicates a more favourable crosslinking-to-scission ratio than that of H2. The Dg was 3.26 kGy for H1 and 0.59 kGy for H2, indicating that the onset of macroscopic gelation occurred at lower absorbed dose for H2. However, Dg and final GF describe distinct aspects of network formation and should not be interpreted as interchangeable measures of crosslinking efficiency [28]. While H2 gelled at a lower dose, H1 achieved the higher GF at 30 kGy. This interpretation is consistent with the findings of Pushpamalar et al., who reported that lower p0/q0 values in e-beam-irradiated carboxymethyl sago pulp hydrogels reflected the predominance of crosslinking over chain scission, while the maximum Dg values reported for their formulations ranged from 8.94 to 9.54 kGy. The lower gelation doses observed for the present multicomponent systems indicate that network formation was initiated at relatively low absorbed doses [29].
Table 1.
Charlesby–Rosiak parameters and radiation-chemical yields determined from dose-dependent sol–gel analysis of H1 and H2 hydrogels.
The calculated radiation-chemical yields also support the predominance of crosslinking. The GX/GS ratios were 16.66 for H1 and 2.27 for H2, confirming that the yield of crosslinking exceeded that of chain scission in both systems. Nevertheless, the lower model-estimated gelation dose of H2 (0.59 kGy versus 3.26 kGy for H1) indicates an earlier predicted onset of network formation, but does not necessarily imply a higher gel fraction at 30 kGy. The higher p0/q0 ratio of H2 (0.22 versus 0.03 for H1), together with its lower calculated GX/GS ratio, indicates a greater contribution of chain scission relative to crosslinking in H2 than in H1. This competition may limit the fraction of polymer retained in the insoluble network, consistent with the lower gel fraction of H2 at 30 kGy (94.72 ± 0.58% versus 98.25 ± 0.42% for H1). Taken together, the combination of high GF, lower p0/q0 ratios, and GX/GS > 1 demonstrated that 30 kGy was sufficient to produce stable radiation-crosslinked PVP/CMC/PEG/agar hydrogels. Therefore, the 30 kGy samples were selected for subsequent physicochemical characterization and 5-FU loading and release experiments based on the dose-dependent sol–gel analysis, particularly the gel-fraction results. Because we did not compare functional properties across irradiation doses, this study does not establish 30 kGy as the optimum dose for swelling, rheological properties, or 5-FU loading and release.
2.2. Relative Wet-Mass Retention Under Ambient Conditions
The relative wet-mass retention profiles of the hydrogels obtained at 30 kGy are shown in Figure 1b. Both formulations exhibited a progressive decrease in normalized wet mass during storage under ambient conditions (23 ± 0.5 °C and 55 ± 5% relative humidity), consistent with water evaporation from the hydrated hydrogels. After 8 h, both H1 and H2 retained ~46% of their initial wet mass. After 24 h, relative wet-mass retention decreased to 11.6% and 15.8%, respectively, with H2 retaining slightly more wet mass at the final measurement. The observed behaviour confirms that both radiation-crosslinked networks were able to preserve a substantial proportion of their initial hydrated mass during the first 8 h of exposure. Progressive water loss has also been reported for hydrogel wound dressings stored under ambient conditions, with evaporative loss increasing over the first 48 h before approaching a plateau, leaving approximately 15% of the initial water content after 4 days [30].
This may be relevant for applications in which the material is intended to provide a hydrated interface during the initial period of use. Nevertheless, the present experiment was performed in ambient air and therefore does not reproduce the thermal, fluidic, and biological conditions encountered at a wound surface. Electrolytes in wound exudate may alter hydrogel swelling through ionic screening [31], while proteins may change the physicochemical properties of the surrounding fluid and influence fluid uptake and retention [32]. Accordingly, these data should be interpreted as an assessment of relative wet-mass retention under controlled ambient conditions, rather than as a direct estimate of water content, in-use hydration, exudate-handling capacity, or dressing replacement time. The slightly greater retention observed for H2 may reflect compositional effects on water-polymer interactions and diffusion pathways, but the present measurements do not allow the individual roles of PVP, CMC, PEG, and agar to be determined. The higher PVP content of H2 may nevertheless have contributed to this trend, as PVP is a hygroscopic polymer that readily absorbs moisture from humid environments; this explanation remains tentative because the formulations also differed in CMC, PEG, and water contents [33]. Further assessment of exudate absorption, water vapor transmission, adhesion, mechanical integrity, and biocompatibility is needed before suitability as a wound dressing can be established.
2.3. Swelling Behavior and Stability in Buffer Media
The swelling profiles of H1 and H2 hydrogels in buffer solutions from pH 4.0 to pH 8.0 are shown in Figure 1c,d. Both formulations displayed rapid water uptake during the initial immersion period, followed by a gradual approach to an approximately constant swelling degree after about 30 h. The samples remained macroscopically intact throughout the 96-h experiment, indicating that the substantial water uptake did not result in visible disintegration of the radiation-crosslinked networks.
The highest swelling degree was obtained at pH 7.4, reaching 1385 ± 1.8% (H1) and 1577 ± 0.5% (H2). At pH 8.0, swelling decreased to 978 ± 2.1% (H1) and 1070 ± 0.4% (H2). Consequently, H2 exhibited a greater degree swelling compared to H1 in both neutral and slightly alkaline conditions, despite its higher elastic modulus and calculated effective network-chain density. The higher calculated effective crosslink density of H2 does not necessarily imply lower swelling, since swelling also depends on polymer–water interactions and ionic contributions [34]. Its higher PVP and PEG contents may favor hydration, whereas its lower CMC content would tend to reduce the ionic contribution to swelling. Changes in interpolymer interactions may also affect this balance. These competing effects may explain the greater swelling degree of H2, although their individual contributions cannot be isolated from the present comparison.
A related pH- and composition-dependent swelling response has been reported for PVP/CMC semi-IPN hydrogels, in which the CMC content and the pH of the swelling medium significantly influenced the network behavior [35]. In addition, Shah et al. reported maximum swelling ratios at pH 7 for biomineralized CaCO3/PVP-CMC hydrogels, followed by lower values at pH 8. Although the swelling degrees in the present study were substantially higher at near-neutral pH, both systems showed reduced swelling under mildly alkaline conditions [31].
Swelling reached a maximum at pH 7.4 rather than at pH 8.0, suggesting that factors other than pH may also have influenced water uptake. Changes in the ionization of CMC carboxyl groups may alter electrostatic repulsion and osmotic pressure within the network, affecting its swelling behaviour. A similar swelling maximum near neutral pH was reported for biomineralized PVP–CMC hydrogels, where enhanced water uptake at pH 7 was attributed to the presence of hydrophilic carboxylate and amide groups and hydrogen-bonding interactions with water [31]. Swelling may reflect the combined effects of pH, buffer ionic composition, and polymer-solvent interactions. At pH 7.4, both formulations showed high water uptake while maintaining macroscopic integrity, supporting their potential for local drug delivery. However, swelling alone cannot predict 5-FU loading or release, which also depends on drug–polymer interactions, drug ionization, and diffusion within the hydrated network.
The stability of H1 and H2 in the corresponding buffer media was evaluated in terms of cumulative wet-mass loss (Figure 1e,f). At the final measurement, the values for H1 were 2.59%, 1.29%, 1.26%, 2.73%, and 4.15% at pH 4.0, 5.0, 6.0, 7.4, and 8.0, respectively. The corresponding values for H2 were 1.57%, 1.98%, 1.74%, 1.68%, and 1.33%. H1 showed the largest numerical decrease at pH 8.0 and the smallest at pH 6.0, whereas H2 showed the largest decrease at pH 5.0 and the smallest at pH 8.0. Roy et al. reported dry-mass losses of approximately 10% after 2 weeks and 38% after 8 weeks for PVP-CMC hydrogel films incubated in Czapek–Dox medium containing microorganisms, attributed to microbial degradation [36]. Similarly, agar–carbomer hydrogels incubated in PBS at 37 °C exhibited progressive weight loss over 28 days, retaining 65% and 78% of their initial dry mass for the less- and more-highly crosslinked formulations, respectively [37]. These comparisons highlight that time-dependent mass loss is governed by network composition, crosslink density, incubation conditions, and the presence of biological degradation agents. Thus, the relatively wet-mass changes in H1 and H2 suggest stability in the tested buffers but do not establish biodegradability or resistance to biodegradation. Further assessment would require studies measuring dry-mass loss under enzymatic or other biologically relevant degradation conditions.
2.4. Dynamic Rheology Measurements and Network Characteristics
The frequency-dependent viscoelastic properties of H1 and H2 pre-hydrogels before e-beam crosslinking and the resulting hydrogels after crosslinking are shown in Figure 2. Before irradiation, both formulations exhibited relatively low storage and loss moduli and a marked dependence on frequency, indicating weak, predominantly physical associations within the polymer mixtures. These interactions may arise from thermoreversible associations of agar chains and hydrogen bonding among the hydrophilic components. This behavior is consistent with the established gelation mechanism of agar/agarose, in which cooling promotes coil-to-double-helix transitions followed by helix aggregation into hydrogen-bonded bundles, thereby forming a reversible physical network before covalent crosslinking [38].
Figure 2.
Frequency-dependent rheological properties of H1 and H2 formulations before irradiation (0 kGy) and after e-beam irradiation at 30 kGy: (a) storage modulus, G′; (b) loss modulus, G″; (c) loss tangent, tan δ = G″/G′; and (d) dynamic viscosity (η′). Data are presented as mean ± SD (n = 3).
E-beam crosslinking at 30 kGy led to a significant increase in both G′ and G″. In the crosslinked hydrogels samples, G′ consistently exceeded G″ across the investigated frequency range, with no crossover from G′ to G″. This behaviour is indicative of a predominantly elastic, gel-like response and supports the formation of stable radiation-crosslinked networks on the time scale demonstrated by oscillatory rheology (Figure 2a,b).
At 100 Hz, H1 exhibited a storage modulus of 36,709 ± 244 Pa and a loss modulus of 1584 ± 51 Pa, while H2 presented higher values of 54,095 ± 681 Pa and 3932 ± 176 Pa, respectively. The higher G′ of H2 indicates a greater resistance to reversible deformation under the applied oscillatory conditions. However, because the two formulations differ simultaneously in PVP, CMC, PEG, and water content, the difference in modulus cannot be attributed exclusively to a single compositional variable or to crosslink density alone.
The quality of a hydrogel chemically (covalently) crosslinked can be also assessed rheologically by considering a so-called power law equation of the storage modulus:
where K and n are two constant quantities and ω = 2πf (in rad/s) is the angular frequency of the strain (squeeze) applied. As a general rule, a covalently crosslinked gel exhibits a positive exponent value equal or close to zero [39,40]. In the case of the two hydrogels investigated, by linear fitting of the experimental data to the logarithmic form of Equation (1), the exponent values were found to be 0.016 for H1—30 kGy and 0.042 for H2—30 kGy (Figure S1), indicating a weak frequency dependence of the storage modulus in both hydrogels. The lower exponent obtained for H1 indicates a weaker frequency dependence of G′ compared with H2. However, the quality of covalently crosslinked hydrogel is slightly higher for H1—30 kGy hydrogel (n = 0.016) than that of H2—30 kGy hydrogel (n = 0.042).
G′ = Kωn,
This is in an agreement with what the frequency evolution exhibits (Figure 2c): (tanδ)H1gel < (tanδ)H2gel, which means that the gel-like property of H1—30 kGy hydrogel is superior to that of H2—30 kGy hydrogel. While characterizing true gels—such as radiation-induced hydrogels—by their viscosity is less common (flow is practically suppressed in these systems), the comparative assessment of apparent viscosity is a useful aspect from rheological standpoint for pre-hydrogel (non-irradiated) mixtures studied. This reduction in tan δ upon irradiation is consistent with observations for gamma-irradiated PVP/PEG hydrogels, in which increased PVP concentration and radiation processing promoted G′ ˃ G″ and tan δ ˂ 1, indicating a predominantly elastic network response [41]. Even though both H1 and H2 non-irradiated systems displayed a storage modulus higher than the corresponding loss modulus and as a result a less than unity value of the loss tangent over the entire frequency range (Figure 2a–c), a viscoelastic behavior was visually observed when the samples were poured between the plates of the rheometer.
Moreover, that the H1 and H2 pre-hydrogel are not real gels was supported rheologically by a strong frequency-dependence of G′ (Figure 2a) and the apparent viscosity (ηap), as a measure of the resistance to flow, taken at 37 °C, was obtained according to the following equation:
This apparent quantity is known as complex viscosity (in fact, modulus of complex viscosity), often called dynamic viscosity, ηdyn [42]. Thus, the rheograms shown in Figure 2d are practically superimposed which demonstrates a very similar viscoelastic behavior for the two mixtures—behavior that is almost independent of their composition.
The network parameters calculated from the plateau storage modulus are summarized in Table 2. H2 displayed a lower Mc of 4.15 kg/mol, compared with 4.84 kg/mol for H1. Correspondingly, H2 exhibited a higher Ve of 253 mol/m3, whereas the value for H1 was 211 mol/m3. The lower MC and higher Ve calculated for H2 are consistent with the higher storage modulus observed experimentally.
Table 2.
Rheological properties and calculated network parameters of hydrogels irradiated at 30 kGy. Data are presented as mean ± SD (n = 3).
Overall, both formulations formed predominantly elastic networks after irradiation at 30 kGy. H2 exhibited higher elastic stiffness and a higher apparent effective network-chain density, calculated from the plateau storage modulus, whereas H1 retained a slightly higher gel fraction and a more favourable GX/GS ratio. These results indicate that gel fraction, radiation-chemical yields, storage modulus, and rheologically derived network parameters describe complementary features of network formation. In particular, gel fraction quantifies the insoluble polymer fraction, whereas the modulus-derived Ve reflects the density of elastically active network chains; therefore, the two parameters are not necessarily expected to vary linearly [43].
2.5. Structural Analysis (ATR-FTIR)
The ATR-FTIR spectra of the uncrosslinked pre-hydrogel mixtures, unloaded hydrogels obtained at 30 kGy, and 5-FU-loaded hydrogels are shown in Figure 3e,f. The spectra of uncrosslinked H1 and H2 samples confirmed the characteristic absorption bands of the PVP/CMC/PEG/agar blends. The Broad bands at ~3405 cm−1 (H1) and 3391 cm−1 (H2) were attributed to O–H stretching vibrations of polysaccharide components and hydrogen-bonded water. The bands observed in the 2886–2888 cm−1 range corresponded to aliphatic C–H stretching vibrations. The absorption bands near 1655 and 1628 cm−1 were assigned to the C=O vibration PVP, potentially influenced by overlapping contributions from absorbed water and components containing CMC. The bands at 1493 and 1423 cm−1 are associated with C–H deformation and overlapping PVP/CMC vibrations, whereas the bands at 1373 cm−1 (H1) and 1317 cm−1 (H2) were linked to C–H deformation and vibrations of polymer backbone. The bands identified at 1287–1283 cm−1 corresponded to C–N stretching from PVP, while the bands around 1113 cm−1 (H1 and 1106 cm−1 (H2) indicated overlapping C–O–C/C–O vibrations from PEG and polysaccharide structures [44,45]. Following e-beam crosslinking at 30 kGy, the broad O–H stretching band within the 2850–3500 cm−1 region became wider and shifted to ~3420 cm−1 (H1) and 3410 cm−1 (H2). These changes are consistent with modification in the hydrogen-bonding environment and polymer-water or polymer-polymer interactions following hydrogel formation. The primary absorption bands remained present after irradiation, and no prominent new bands indicative to extensive degradation or novel functional groups were detected. In the fingerprint region, the C–O–C/C–O band shifted from 1113 to 1072 cm−1 (H1) and from 1061 to 1093 cm−1 (H2), suggesting changes in the local bonding environment and intermolecular interactions within this highly overlapping spectral region. Subsequent to the 5-FU loading, spectral contributions assigned to the drug were identified in the loaded hydrogels, including N–H stretching bands in the 3060–3350 cm−1 region, C=O bands near 1640–1660 cm−1, and a characteristic C–F vibration near 1235–1245 cm−1. Additional vibrations in the 800–950 cm−1 range may also originate from 5-FU [46]. For comparison, the spectrum of pure 5-FU is presented in Figure S7, showing bands at 3124, 3065, and 3032 cm−1, bands in the carbonyl region at 1770, 1720, and 1652 cm−1, a band at 1243 cm−1, and additional bands at 949, 935, 869, and 804 cm−1. A feature is also observed near 2417 cm−1. Moreover, following the loading of 5-FU into the hydrogels matrix, broad absorption bands were observed at 2393 cm−1 (H1) and 2384 cm−1 (H2). These bands may be associated with low-frequency vibrations of strongly hydrogen-bonded complexes formed between the pyrimidine ring of 5-FU and the functional groups of the polymeric blend (i.e., COOH and OH groups of CMC, PEG, agar, and the pyrrolidone C=O of PVP), enhanced by Fermi resonance in the 2600–2200 cm−1 region [47]. Another possible explanation of these absorption bands involves the formation of N-H+ species as a consequence of interactions between free COOH functional groups of CMC which can partially or totally transfer the H+ to the N atoms of 5-FU, generating a positively charged intermediate species [48]. The identification of 5-FU-related bands demonstrate incorporation of the drug into both e-beam crosslinked hydrogels. Minor shifts and intensity variations relative to unloaded networks are consistent with changes in the local chemical environment and possible non-covalent interactions between hydrophilic functional groups in the basic polymer matrix. Therefore, the results are consistent with drug incorporation through physical entrapment and possible reversible non-covalent interactions, including hydrogen bonding and van der Waals interactions [49].
Figure 3.
5-FU loading and ATR-FTIR characterization of H1 and H2 hydrogels. (a,b) Effect of initial 5-FU concentration (100–800 mg/L) and loading time (24, 48, and 72 h) on hydrogels in PBS at pH 7.4; (c) effect of loading-medium pH (4.0–8.0) on 5-FU loading capacity after 8 h of incubation with 200 mg/L 5-FU; (d) time-dependent 5-FU loading in PBS at pH 7.4 using an initial 5-FU concentration of 200 mg/L; (e,f) ATR–FTIR spectra of pre-hydrogel mixtures (0 kGy), unloaded crosslinked hydrogels at 30 kGy, and 5-FU-loaded hydrogels; (g) representative photographs of hydrogels after e-beam crosslinking and after freeze-dry; and (h) photographs of 5-FU-loaded hydrogels.
2.6. 5-FU Loading Capacity
Figures S2–S4 show the calibration curves for 5-FU over the concentration range of 0.125–50 mg/L in buffers at pH 5.0, 6.0, and 7.4. The effect of 5-FU concentration on the loading capacity of H1 and H2 is shown in Figure 3a,b. The amount of loaded 5-FU increased progressively as the drug concentration increased from 100 to 800 mg/L. Depending on loading time and 5-FU concentration, H1 loaded ~2.5–2.9 mg/g at 100 mg/L and 21.5–25.7 mg/g at 800 mg/L. Under the same conditions, H2 also showed an increase from ~2.0–2.2 mg/g to 19.0–20.3 mg/g.
Both hydrogels showed comparable loading at lower 5-FU concentrations, while H1 generally exhibited higher loading above 400 mg/L. This difference may partly reflect its higher CMC content, although the individual contributions of CMC, PVP, and PEG could not be isolated because their concentrations varied simultaneously. Drug loading increased across the entire tested concentration range, with no saturation observed even at 800 mg/L.
The effect of loading-medium pH was evaluated using 200 mg/L of 5-FU and an incubation time of 8 h (Figure 3c). H1 showed drug loading of ~5.7 mg/g at pH 6, while H2 reached its highest loading capacity of ~5.2 mg/g, at pH 5.0, followed by decrease in pH 6.0–8.0. At pH 8.0, both hydrogel formulations showed lower loading than in acidic or neutral media. The pH-dependent loading response likely reflects combined changes in 5-FU aqueous solubility, ionization of the CMC-containing network, hydrogel swelling, and drug-polymer interactions [50]. Based on the initial hydrogel mass, loading-solution volume, and quantified loading capacities, ~29% of the initially available 5-FU was incorporated into H1 at pH 6.0, whereas H2 incorporated ~30% at pH 5.0.
The time-dependent loading profiles obtained in PBS at pH 7.4 are presented in Figure 3d. For H1, drug uptake increased during the loading period and reached a maximum of ~5.1 mg/g after 8 h, while H2 reached a similar maximum loading capacity of ~5.2 mg/g after 12 h. At longer incubation times, no sustained increase in loading capacity was observed for either formulation. Based on the experimental results presented above, the selected hydrogels were loaded with 5-FU for subsequent release experiments using an initial drug concentration of 200 mg/L (Figure 3g,h). Loading at pH 6.0 for H1 and pH 5.0 for H2 was performed for 8 h, whereas loading in PBS at pH 7.4 was performed for 8 h for H1 and 12 h for H2.
2.7. In Vitro 5-FU Release
Figure 4 shows the cumulative in vitro 5-FU release profiles from crosslinked H1 and H2 hydrogels. As described in Section 3.5 regarding the selected loading parameters, hydrogels loaded with 5-FU in PBS 7.4 displayed a sustained release profile under both acidic and physiological pH conditions. As illustrated in Figure 4a, at pH 5.0 (over a 30-h period), both hydrogels exhibited an initial accelerated release phase within the first hour, reaching ~51% for H1 and ~38% for H2, followed by a more gradual release period, culminating in cumulative releases of ~63% and ~51% for H1 and H2, respectively.
Figure 4.
In vitro cumulative release of 5-FU from hydrogels in citric acid-Na2HPO4 buffer (pH 5.0) and phosphate-buffered saline (PBS, pH 7.4): release profiles in (a) pH 5.0 and (b) pH 7.4 for H1 and H2 hydrogels previously loaded in PBS at pH 7.4; release profiles in (c) pH 5.0 and (d) pH 7.4 for H1 hydrogel loaded at pH 6.0 and H2 hydrogel loaded at pH 5.0 (for 8 h). Data are expressed as apparent cumulative 5-FU release percentages relative to the depletion-derived loading amounts estimated before rinsing and are presented as mean ± SD (n = 2 independent hydrogel specimens per experimental condition).
Conversely, at pH 7.4 (Figure 4b), H1 and H2 showed more moderate initial rates and reached maximum cumulative releases of ~47% and ~54% over the 30-h observation experiment. The release profiles exhibited a biphasic pattern, characterized by an initially accelerated phase followed by a slower mass transport controlled by diffusion through the hydrated hydrogel matrix.
Furthermore, hydrogels H1 and H2 loaded with 5-FU at specific loading pH values of 6 and 5, respectively, showed sustained release profiles over the 12-h observation period (Figure 4c,d). Under these conditions, H2 released a slightly larger fraction of the drug compared to H1 in both media. Specifically, in the pH 5 release medium (Figure 4c), H1 reached a cumulative release of ~31%, whereas H2 reached ~38%. In the pH 7.4 release medium (Figure 4d), H1 released ~24% and H2 released ~41% of the loaded 5-FU.
H1 exhibited a storage modulus of ~36,700 Pa, a higher 5-FU loading capacity of 5.7 mg/g (29%), and a lower swelling degree of 1385% compared with H2. In contrast, H2 displayed a storage modulus of 54,095 Pa, a comparable 5-FU loading capacity of 5.2 mg/g (30%), and a swelling degree of 1577%. The higher crosslinking density of H2 was attributed to its higher PVP content (7%), while its higher swelling degree was associated with the presence of 1.2% PEG, which increases hydrogel hydrophilicity and consequently promotes 5-FU release.
The higher fractional release observed for H2 may be related to its superior swelling degree at pH 7.4, which exceeds 1500%, thereby facilitating water uptake and the subsequent diffusion of 5-FU through the hydrated polymer network. This variation between the release profiles should not be attributed solely to the intrinsic aqueous solubility of 5-FU. Since 5-FU is a weakly acidic compound with a reported pKa = 8, its solubility is expected to remain broadly similar below pH 7 and to increase substantially only as the pH approaches or exceeds its pKa [51]. Instead, the observed profiles likely reflect the synergic effects of drug distribution during loading, reversible interactions between 5-FU and the polymer chains, buffer composition, ionic strength, matrix hydration, and diffusion through the swollen hydrogel network. Because the surface-associated 5-FU fraction was not quantified separately, the initially faster release phase is described as an observed accelerated release phase rather than as definitive evidence of a burst-release mechanism [52,53]. It should be noted that the cumulative release percentages presented in Figure 4 were normalized to the drug-loading amounts indirectly estimated by solution depletion before rinsing. Since potential 5-FU loss during rinsing was not quantified, the reported values represent apparent cumulative release percentages rather than exact fractions of the drug retained immediately before release testing. This uncertainty does not affect the experimentally determined cumulative mass of 5-FU recovered in the receptor medium.
Based on the optimized loading capacities (5.7 mg/g for H1 at pH 6.0 and 5.2 mg/g for H2 at pH 5.0) and the observed fractional release percentages, the cumulative mass of 5-FU released across the monitored intervals, ranged from ~0.12 to 0.33 mg (120 to 330 μg).
Although the 5-FU loading capacities of the e-beam crosslinked developed hydrogels are relatively moderate compared to some highly porous alternative delivery systems, the amount of drug released provides a quantifiable baseline for localized administration strategies. The literature reports in vitro IC50 values for 5-FU ranging from 5–6 µg/L in selected colorectal cancer cell models to 100 µg/L for melanoma cells [54]. However, while these literature values offer a concentration context, the total mass released in a buffer system cannot be directly equated to actual drug concentration or therapeutic efficacy within target tissue. Factors such as topical permeability, local drug retention, bioavailability, and cellular exposure duration must be independently evaluated [55].
Overall, both H1 and H2 released quantifiable amounts of 5-FU over 12–30 h, with the observed release profiles varying according to hydrogel formulation, drug-loading conditions, and release-medium pH. Since the proportions of PVP, CMC, PEG, and water were varied simultaneously, the observed differences cannot be attributed to individual polymer components. Furthermore, given the number of experimental replicates (n = 2), comparisons between H1 and H2 are descriptive, and no statistical significance is inferred from the observed differences. From a theoretical drug-delivery perspective, the biphasic profile is characterized by an initial accelerated phase followed by slower release, could potentially provide early drug availability followed by sustained local exposure over 12–30 h. However, it should be emphasized that the present study was specifically designed to establish the synthesis, structural dynamics, and in vitro 5-FU transport behavior under defined buffer conditions, rather than to demonstrate antitumor efficacy. Whereas in vitro release assays isolate diffusion and matrix-hydration effects, in vivo models involve complex tissue interactions, local clearance, and pharmacodynamic responses that lie beyond the experimental scope of this work. Establishing these physicochemical and release parameters first provides a rational baseline for subsequent cellular cytotoxicity assays and in vivo therapeutic evaluations.
2.8. Mathematical Modeling of 5-FU Release
The 5-FU release profiles from H1 and H2 hydrogels in citric acid-Na2HPO4 buffer (pH 5.0) and PBS (pH 7.4) were fitted over the 0–12 h interval using the Korsmeyer–Peppas, Peppas–Sahlin, Makoid–Banakar, and Weibull models. The fitted parameters and goodness-of-fit criteria for all evaluated models are summarized in Table 3 and Table 4, while Figures S5 and S6 illustrate the fitted curves for the Korsmeyer–Peppas, Peppas–Sahlin, and Makoid–Banakar models.
Table 3.
Parameter estimates and goodness-of-fit criteria for the Korsmeyer–Peppas and Peppas–Sahlin models fitted to 5-FU release profiles from H1 and H2 hydrogels loaded in PBS (pH 7.4).
Table 4.
Parameter estimates and goodness-of-fit criteria for the Makoid–Banakar and Weibull models fitted to 5-FU release profiles from H1 and H2 hydrogels loaded in PBS (pH 7.4).
The Korsmeyer–Peppas model provided high R2 values, ranging from 0.98 to 0.99, with release exponents (n) ranging from 0.073 to 0.084. For cylindrical matrices, n values below 0.45 indicate quasi-Fickian diffusion, a transport mechanism highly characteristic of systems exhibiting a rapid initial release phase. However, because this mathematical model is primarily applicable for the initial release stage (typically up to ~ 60% cumulative release) and the experimental fractional release exceeded this threshold shortly after the first hour, the calculated n values serve primarily as empirical indicators of the early accelerated release rather than definitive mechanistic proof for the entire time interval. The experimental profiles showed substantial initial release, with approximately 39–52% of the depletion-derived loading amount released within the first hour. However, not all profiles exceeded 60% cumulative release during the investigated interval. Consequently, the fitted Korsmeyer–Peppas exponents should be interpreted cautiously and should not be considered definitive evidence of a particular release mechanism.
The Peppas–Sahlin model demonstrated superior statistical performance, yielding R2 values approaching 0.99 and lower AIC values. As shown in Figures S5 and S6, the model curves successfully captured the biphasic shape of the experimental data. The diffusional constant, kPS1, was consistently positive (51.44 to 72.00), whereas the nominal relaxation constant, kPS2, was negative for all profiles. The exponent m ranged from 0.248 to 0.321.
As previously established in the literature, negative kPS2 values prevent the direct quantitative decoupling of Fickian diffusion and polymer chain relaxation. Therefore, while statistically robust, the Peppas–Sahlin model was evaluated strictly for empirical fitting purposes over the analyzed time frame.
The Makoid–Banakar model also provided superior fits across the entire 0–12 h interval, accurately reflecting both the initial rapid phase and the subsequent plateau (Figures S5 and S6). The model yielded R2 values of 0.99, low AIC values (9.21–26.56) and high MSC values of 3.95–4.90. In both pH media, the statistical performance of the Makoid–Banakar and Peppas–Sahlin models was comparable and superior to the standard Korsmeyer–Peppas model, successfully describing the progressive reduction in the release rate over time.
The Weibull model showed varying performance depending on hydrogel composition and release medium. For H1 in citric acid-Na2HPO4 buffer at pH 5.0, Weibull yielded the lowest AIC (9.82) and highest MSC (5.24) among the evaluated models.
For H2 in the same medium, Weibull and Peppas–Sahlin showed nearly identical statistical performance, with AIC values of 4.85 and 4.82 and MSC values of 5.23 and 5.24, respectively. In PBS at pH 7.4, Weibull yielded higher AIC (40.92) and lower MSC (2.38) values than Peppas–Sahlin and Makoid–Banakar for both hydrogels. The Weibull shape parameter, β, ranged from 0.048 to 0.072. According to established kinetic interpretations, values of β < 0.75 are typically associated with Fickian diffusion in fractal or structurally disordered matrices, consistent with transport through a highly swollen polymeric network [56].
Overall, the statistical criteria indicate that the complete 12-h 5-FU release profiles were most accurately described by the Makoid–Banakar and Peppas–Sahlin models. The visual fits (Figures S5 and S6) confirm their ability to map the biphasic release behavior. Combined with the high macroscopic swelling and the negligible wet-mass loss of the hydrogels during incubation, the kinetic modelling supports a mechanism predominantly governed by molecular diffusion through the hydrated, disordered polymer network, preceded by an initial accelerated release phase. The kinetic models were fitted to the mean release profiles, and the goodness-of-fit criteria (R2, AIC, and MSC) were used to evaluate model performance rather than to establish statistically significant differences between H1 and H2. Given the number of experimental replicates, the kinetic interpretation should be considered descriptive and exploratory.
3. Materials and Methods
3.1. Materials
Poly(vinylpyrrolidone) (PVP, Mw = 3.6 × 105 g/mol), sodium carboxymethylcellulose (CMC, Mw = 2.5 × 105 g/mol), poly(ethylene glycol) (PEG, Mw = 2 × 104 g/mol), agar (sourced from Carl Roth for microbiological applications), and 5-fluoro-1H,3H-pyrimidine-2,4-dione (5-FU powder for HPLC, Mw = 130.08 g/mol, ≥99% purity) were purchased from Sigma-Aldrich (Merck KGaA, Darmstadt, Germany) and utilized without further modification. Analytical grade sodium hydroxide and buffer solutions were used for pH adjustment and preparation of swelling, loading, and release media, while Type I ultrapure water (18.2 MΩ·cm at 25 °C) was produced in-house and used in all experimental procedures. The buffer solutions utilized throughout the swelling, drug loading, and in vitro release experiments were prepared in-house using ultrapure water, following the standard chemical compositions specified by Sigma-Aldrich. Specifically, the acidic media (pH 4.0, 5.0, and 6.0) consisted of a citric acid-disodium hydrogen phosphate (C6H6O7⋅H2O-Na2HPO4), while the alkaline medium (pH 8.0) was prepared using a disodium hydrogen phosphate-sodium dihydrogen phosphate (Na2HPO4-NaH2PO4). The phosphate-buffered saline (PBS, pH 7.4) used as the physiological testing medium was prepared by dissolving PBS tablets (Sigma-Aldrich) in ultrapure water according to the manufacturer’s instructions.
3.2. Hydrogel Formulation and E-Beam Crosslinking
Two aqueous pre-hydrogel formulations, labelled H1 and H2, were prepared on a weight basis (w/w), as summarized in Table 5. Briefly, PVP, CMC, and PEG were sequentially dissolved in Type I water under magnetic stirring at 800 rpm and 23 ± 0.5 °C. The pH of each mixture was adjusted to 7.3–7.5 using 1M NaOH, followed by heating to 80–90 °C. Agar was subsequently added under continuous stirring until homogeneous mixtures were obtained. The mixtures were then subjected to ultrasound-assisted degassing (37 kHz, 30 min) in hot water, poured into sealed cylindrical molds (ϕ = 1.3 cm, h = 0.5 cm), and allowed to stabilize to room temperature prior to e-beam irradiation.
Table 5.
Composition of the pre-hydrogel formulations (wt%).
Electron-beam irradiation was performed using a linear electron accelerator (ALID-7 Accelerators Laboratory, National Institute for Laser, Plasma and Radiation Physics, Măgurele, Romania) operating at mean electron energy of 6 MeV, average beam current of 5 μA, pulse duration of 3.75 μs, repetition frequency of 50 Hz, and dose rate of 3.3 kGy/min. The samples were exposed to absorbed doses of 10, 15, 20, 25, and 30 kGy. The nominal absorbed dose was monitored using primary standard graphite calorimeters, while dose distribution and uniformity were verified with B3 radiochromic dosimeter films calibrated against alanine transfer dosimeters at the Risø High Dose Reference Laboratory (Roskilde, Denmark). Unless otherwise stated, hydrogels irradiated at 30 kGy were selected for subsequent physicochemical characterization and 5-FU loading and release assays. Prior to drug loading, the hydrogels were frozen at −90 °C for 3 h in the bottom condenser chamber of the freeze-dryer (BK-FD18P, Biobase, Jinan, China), lyophilized for 40 h, and stored in a desiccator until further use.
3.3. Characterization of Hydrogels
3.3.1. Gel Fraction and Radiation-Crosslinking Parameters
The gel fraction (GF) was determined gravimetrically to evaluate the e-beam crosslinking efficiency. Hydrogels were dried at 30 °C in a vacuum oven to constant mass (m0). The insoluble polymer fraction was then extracted in Type I ultrapure water for 48 h at room temperature (23 ± 1 °C) to remove uncrosslinked polymers; it was then dried again under the same conditions to constant mass (md). The gel fraction (GF) was calculated as follows [57]:
The sol fraction was calculated as s = 1 − GF/100. The dose-dependent sol-fraction data were analyzed using GelSol95 v.1.0 (Lodz University of Technology, Poland). The gelation dose (Dg), virtual dose (Dv), and the degradation-to-crosslinking ratio (p0/q0) were estimated from the Charlesby–Rosiak model using Equation (4) [58]. The radiation-chemical yields of crosslinking (GX) and chain scission (GS), were calculated for the 30 kGy samples using the MC values derived from rheological analysis, according to Equations (5) and (6) [59]:
Here, MC is the average molecular weight between consecutive cross-links (kg/mol), c is the total polymer concentration in the irradiated mixture (g/L), and ρ is the hydrogel density (kg/m3) [60]. Gel fraction measurements were performed in triplicate for each hydrogel formulation and irradiation dose.
3.3.2. Relative Wet-Mass Retention Under Ambient Conditions
The water retention capability was evaluated gravimetrically under ambient conditions (23 ± 0.5 °C and 55 ± 5% relative humidity). The hydrated hydrogels obtained at 30 kGy (650 ± 20 mg) were initially weighed (m0) and thereafter placed in open Petri dishes. The tare-corrected weight (mt) was recorded at predetermined time intervals. The relative wet-mass retention (MRC) was calculated according to Equation (7) [61]:
where m0 is the initial hydrated mass and mt is the mass at time t. Because the dry polymer fraction was not subtracted; this parameter reflects normalized wet-sample mass retention rather than absolute water content. All tests were performed in triplicate, and data are expressed as mean ± standard deviation (n = 3).
3.3.3. Swelling Behavior and Stability in Buffer Media
Freeze-dried hydrogels irradiated at 30 kGy were immersed in buffer solutions at pH 4.0, 5.0, 6.0, 7.4, and 8.0 and maintained at 37.0 °C. At predetermined time intervals, the samples were removed, gently blotted without compression, weighed, and returned to the same medium. The swelling degree (SD) was calculated using the following equation [62]:
where md is the initial dry mass, and ms is the swollen mass at time t.
After the swelling equilibrium had been reached, the hydrogels were maintained in the corresponding buffer solutions for an additional 30 days at 37 ± 0.5 °C. At predetermined intervals (10, 15, 20, and 30 days), the samples were removed, gently blotted to remove excess surface liquid, and weighed. The incubation medium was then completely replaced with fresh buffer of the same pH. The cumulative wet-mass loss was calculated according to Equation (9) [63]:
where ms is the wet mass of the hydrogel at swelling equilibrium and mt is the wet mass recorded at each subsequent sampling time t. This gravimetric assay evaluates changes in hydrated sample mass under the tested buffer conditions; it does not directly quantify dry-polymer loss or biodegradation. All measurements were performed in triplicate and the results are expressed as mean ± SD (n = 3).
3.3.4. Dynamic Rheology Measurements
To perform the dynamic rheology measurements, an instrument MFR 2100 (GBC, Dandenong, Victoria (VIC), Australia) was employed. In the case of non-irradiated systems (H1 and H2), a proper amount of semisolid sample of ca. 0.5 g was sandwiched between the two circular plates of rheometer with a horizontal orientation and parallel to each other. The thickness of the samples tested (equal to the gap between the upper and the bottom plates) was set at 300 µm. Briefly, the measurement procedure consisted in squeezing the sample by imparting a vertical oscillatory motion possessing a pseudorandom noise pattern to the upper plate, while the bottom plate was held stationary. Thus, the resulting oscillatory deformation through the sample led to a characteristic force exerted onto the bottom plate below which a proper sensor measured and continuously acquired this force signal. The signal of squeezing motion and that of the corresponding force were processed by a Fourier transform algorithm to find out the values of the storage (G′) and loss (G″) moduli at 400 discrete frequencies (0.25–100.00 Hz, step of 0.25 Hz) concomitantly. The measurement on the hydrogels (H1—30 kGy and H2—30 kGy) were carried out relatively similarly, but with some peculiarities related to their gel-like state. Accordingly, disc-shaped hydrogel samples were cut and placed one by one between the two plates of the instrument in a sandwich configuration. To perform the measurements, the samples were initially compressed from a thickness of 5000 µm to 2500 µm (40% compressive strain), and data acquisition was carried out in the same manner as described for the non-irradiated samples. Following the cited methodology [64], small oscillatory displacement amplitudes relative to the sample thicknesses were selected, to target the linear viscoelastic region (LVER): 0.03–0.04 µm for the non-irradiated samples and 0.3 µm for the hydrogel samples. Overall, the measurements were made at 37.0 ± 0.1 °C, in triplicate, with a mean standard deviation of max. 15%, every rheograms being an average of 20 successive scans.
3.3.5. ATR-FTIR
ATR-FTIR spectra were recorded for the pure 5-FU powder, non-irradiated polymer mixtures, unloaded hydrogels obtained at 30 kGy, and 5-FU-loaded hydrogels prepared under the formulation-specific loading conditions described in Section 2.6. Before analysis, the polymer mixtures and hydrogel samples were freeze-dried. Spectra were acquired in absorbance mode using Spectrum 100 spectrometer (PerkinElmer, Waltham, MA, USA) across the spectrum of 4000–400 cm−1, with a resolution of 4 cm−1, by averaging 48 scans. A background spectrum was recorded and used as the reference for calculating the absorbance spectra. The corresponding baseline correction and normalization procedure was applied to all spectra in order to allow for direct comparisons between samples.
3.4. 5-FU Loading Studies
To identify the maximum amount of 5-FU that could be loaded into the selected hydrogels, drug-loading experiments were performed to assess the influence of 5-FU concentration, pH media, and loading duration. These experiments followed an experimental approach adapted from that reported by Alfassam et al. [54], with modifications to tailor the hydrogel formulations and experimental conditions investigated in this research. Lyophilized H1 (66.0 ± 2.6 mg) and H2 (80.0 ± 1.5 mg) samples were immersed individually in 7 mL of 5-FU solution, under constant stirring at 400 rpm, and protected from light. Three loading series were performed: (i) 5-FU concentrations of 100–800 mg/L (PBS, pH 7.4, 37 °C and 24 to 72 h); (ii) 200 mg/L 5-FU in buffers at pH 4.0, 5.0, 6.0, 7.4, and 8.0 (8 h, 37 °C); and (iii) loading duration was tested using 200 mg/L 5-FU (PBS, pH 7.4, 37 °C and 2 to 72 h). At the end of each loading experiment, the hydrogel was removed and the final solution volume was recorded. The residual 5-FU concentration was quantified via UV-Vis spectrophotometry at 266 nm using a Jenway 6850 spectrophotometer (Cole-Parmer, Staffordshire, UK). The calibration curve was constructed across the concentration range of 0.125–50 mg/L (R2 = 0.999). To quantify loading capacity, Q (mg 5-FU/g dry hydrogel), aliquots beyond the calibration range were diluted in the blank medium and associated dilution factors were considered to express the amount of 5-FU loaded according to Equation (10) [65]:
where C5-FU,i is the initial concentration of the 5-FU standard solution (mg/L), C5-FU,f is the residual 5-FU concentration in solution after completion of the loading experiment (mg/L), Vi is the initial solution volume (7 mL), Vf is the final solution volume after loading (mL), and mhydrogel is the dry mass of the hydrogel (g). Following loading, the hydrogel samples intended for ATR–FTIR characterization and in vitro release testing were briefly rinsed with Type I ultrapure water to minimize residual loading solution and loosely surface-associated 5-FU. The drug-loading amounts calculated using Equation (10) represent indirect estimates of 5-FU uptake based on solution depletion before rinsing. Since the rinsing solutions were not analyzed, the actual amount of 5-FU retained after rinsing could not be determined.
3.5. In Vitro 5-FU Release
In vitro release experiments were carried out in vertical Franz diffusion cells using an HDT 1000 system (Copley Scientific, Nottingham, UK) having a receptor volume of 7 mL. Hydrated 5-FU-loaded hydrogels (H1: 1055 ± 0.55 mg; H2: 1215 ± 0.75 mg) were evaluated for drug release using either citric acid-Na2HPO4 buffer (pH 5.0) or PBS at (pH 7.4) as receptor medium. The receptor medium was maintained at 37 °C and stirred at 600 rpm, while the diffusion cells were protected from light throughout the experiment. Drug release from the hydrogels was monitored for up to 30 h in both release media PBS (pH 7.4 and citric acid-Na2HPO4 buffer, pH 5.0) for hydrogels previously loaded in PBS at pH 7.4, and for 12 h for hydrogels loaded at formulation-specific pH values (pH 6.0 for H1 and pH 5.0 for H2). Aliquots of 1.8 mL were withdrawn from the receptor compartment at 1 h intervals up to 12 h, with additional withdrawals at 24 and 30 h. Each aliquot was immediately replaced with an equal volume of fresh, preheated receptor medium. The amount of released 5-FU was quantified spectrophotometrically at 266 nm using corresponding calibration curves prepared separately in pH 5.0 (R2 = 0.998) and pH 7.4 (R2 = 0.999) media. The cumulative released mass and the apparent cumulative release percentage, normalized to the drug-loading amount estimated by solution depletion before rinsing, were calculated using Equations (11) and (12), respectively [66]:
where V = 7 mL is the total receptor cell volume, Vs = 1.8 mL is the sampling aliquot volume, Cn is the 5-FU concentration measured at time point n, and Ci represents the drug concentration at each preceding time point i. The percentage of cumulative release is expressed relative to the initial mass of drug loaded into the hydrogel (M0):
where Mt is the cumulative mass of 5-FU released at time t (mg), and M0 represents the initial drug-loading amount (mg) indirectly estimated by solution depletion (Equation (10)), before rinsing. As potential drug loss during rinsing was not quantified, the cumulative release percentages were calculated relative to this depletion-derived estimate rather than the actual post-rinsing retained drug mass. In vitro release experiments were performed using two separate hydrogel specimens per experimental condition (n = 2), and the results were expressed as mean ± standard deviation (SD).
3.6. Mathematical Modelling of 5-FU Release
The mean cumulative release profiles of 5-FU from hydrogels were fitted over the initial 0–12 h interval by nonlinear regression using DDSolver v1.0, a Microsoft Excel add-in for dissolution-data analysis [67]. Four kinetic models were evaluated: Korsmeyer–Peppas, Peppas–Sahlin, Makoid–Banakar, and Weibull [68,69].
The Korsmeyer–Peppas model was described by:
Ft = kKP · tn,
The Peppas–Sahlin model was expressed as follows:
Ft = kPS1 · tm + kPS2 · t2m,
The Makoid–Banakar model was described by:
Ft = kMB · tn · e−k · t,
The Weibull model was expressed as follows:
where Ft is the cumulative percentage of 5-FU released at time t; kKP is the Korsmeyer–Peppas release constant; kPS1 and kPS2 are the Peppas–Sahlin constants associated with the Fickian diffusion and polymer relaxation contributions, respectively; kMB, n, and k are empirical parameters of the Makoid–Banakar model; n and m are release exponents in the Korsmeyer–Peppas/Makoid–Banakar and Peppas–Sahlin models, respectively; α and β are the scale and shape parameters of the Weibull model, respectively; The Weibull location parameter, Ti, was fixed at 0.
Model performance was evaluated using the coefficient of determination (R2), Akaike information criterion (AIC), and model selection criterion (MSC). Among the candidate models, lower AIC and higher MSC values were considered indicative of improved goodness of fit. The parameters obtained from the Korsmeyer–Peppas and Peppas–Sahlin models were interpreted mechanistically only when they were physically meaningful and compatible with the assumptions underlying the respective models [70].
3.7. Statistical Analysis
Unless otherwise specified, experimental measurements were performed in triplicate, and the results were expressed as mean ± standard deviation (SD). In vitro 5-FU drug-release experiments were conducted using two independent hydrogel specimens per experimental condition (n = 2). Due to the number of replicates, differences between H1 and H2 release profiles were evaluated descriptively, without statistical significance testing. Drug-release kinetic models were fitted, and their parameters were estimated using DDSolver, as described above, while dose-dependent sol–gel analysis was performed using GelSol95 software (v1.0, Division of Applied Radiation Chemistry, Lodz University of Technology, Lodz, Poland).
4. Conclusions
E-beam crosslinking at 30 kGy produced PVP/CMC/PEG/agar hydrogel networks with high gel fractions (98.25 ± 0.42% for H1 and 94.72 ± 0.58% for H2). Under the aqueous conditions investigated, the hydrogels retained their macroscopic integrity during swelling and gravimetric stability experiments. Rheological measurements showed a predominantly elastic response (G′ > G″). Both formulations exhibited pH-dependent swelling, with the highest swelling degrees observed at pH 7.4 (1385 ± 1.8% for H1 and 1577 ± 0.5% for H2). Under ambient conditions, relative wet-mass retention decreased to approximately 46% after 8 h. ATR-FTIR spectra indicated that the principal functional groups of the constituent polymers were retained after e-beam crosslinking. In the loaded hydrogels, spectral bands associated with 5-FU were consistent with physical drug incorporation and showed non-covalent interactions between the drug and the polymer matrix. 5-FU loading depended on hydrogel composition, initial drug concentration, loading duration, and loading-medium pH. The highest loading capacities (~5.2–5.7 mg/g) were obtained at pH 6.0 for H1 and pH 5.0 for H2. Loading conditions also influenced subsequent drug release. Compared with samples loaded at the selected pH values, hydrogels loaded in PBS at pH 7.4 exhibited faster initial release, followed by continued release for up to 30 h. Among the tested kinetic models, the best-fitting model depends on the hydrogel formulation and release medium, with Makoid–Banakar and Peppas–Sahlin showing comparable statistical performance in PBS at pH 7.4. Taken together with the swelling behavior, negligible wet-mass changes during incubation, and biphasic release profiles, these results are consistent with a contribution of matrix hydration and drug diffusion through the hydrated polymer network to 5-FU release.
Overall, the e-beam-crosslinked PVP/CMC/PEG/agar hydrogels demonstrated 5-FU and release behavior that depended on hydrogel composition and loading conditions, without the use of chemical crosslinkers. Because the present investigation focused on physicochemical characterization and in vitro release kinetics in buffer media, the findings establish the baseline transport performance of these matrices without claiming demonstrated in vivo therapeutic efficacy. Consequently, further studies are needed to evaluate 5-FU retention and permeation in relevant skin models, preservation of drug bioactivity after release, cytocompatibility with healthy skin cells, and antitumor efficacy in appropriate cellular and in vivo models.
Supplementary Materials
The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/ijms272310614/s1. [7,15,18,19,20,71,72,73].
Author Contributions
Conceptualization, M.D. and I.C.C.; methodology, M.D., A.S. and I.C.C.; validation, M.D., A.S. and I.C.C.; formal analysis, M.D., A.S. and I.C.C.; investigation, M.D., A.S., M.M. and I.C.C.; data curation, M.D., A.S., M.M. and I.C.C.; writing—original draft preparation, M.D., A.S., M.M. and I.C.C.; writing—review and editing, M.D., A.S. and I.C.C.; project administration, I.C.C. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by a grant from the Ministry of Research, Innovation and Digitization, CNCS–UEFISCDI, project number PN-IV-P2-2.1-TE-2023-0453, within PNCDI IV, as well as by the Romanian Ministry of Education and Research under the Romanian National Core Program LAPLAS VII–Contract No. 30N/2023.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data presented in this study are available on request from the corresponding author.
Acknowledgments
We acknowledge the support of the National Interest Infrastructure Facility, IOSIN at INFLPR. During the preparation of this manuscript, the authors used Gemini and Grammarly exclusively for academic language translation, grammar correction, and stylistic editing. All scientific content, data analysis and interpretation were developed and verified by the authors.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Ahmed, E.M. Hydrogel: Preparation, Characterization, and Applications: A Review. J. Adv. Res. 2015, 6, 105–121. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Li, J.; Mooney, D.J. Designing Hydrogels for Controlled Drug Delivery. Nat. Rev. Mater. 2016, 1, 16071. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ajji, Z.; Mirjalili, G.; Alkhatab, A.; Dada, H. Use of Electron Beam for the Production of Hydrogel Dressings. Radiat. Phys. Chem. 2008, 77, 200–202. [Google Scholar] [CrossRef] [Scilit]
- Alfindee, M.; Sweah, Z.; Saki, T. Preparation and Characterization of Polymer Blends Based on Carboxymethyl Cellulose, Polyvinyl Alcohol, and Polyvinylpyrrolidone. Egypt. J. Chem. 2021, 64, 2679–2684. [Google Scholar] [CrossRef] [Scilit]
- Kaur, P.; Bohidar, H.B.; Nisbet, D.R.; Pfeffer, F.M.; Rifai, A.; Williams, R.; Agrawal, R. Waste to High-Value Products: The Performance and Potential of Carboxymethylcellulose Hydrogels via the Circular Economy. Cellulose 2023, 30, 2713–2730. [Google Scholar] [CrossRef] [Scilit]
- Beni, B.H.; Falahati, M.; Rostamabadi, M.M.; Navid, S.; Rostamabadi, H. Agar as a Natural Polymer: From Culture Media to Cutting-Edge Biomedical Applications. Carbohydr. Polym. 2025, 368, 124100. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ghosh, B.; Bhattacharya, D.; Kotal, A.; Kuila, A.; Mukhopadhyay, M. Cytocompatible, Thermostable Hydrogel with Utility to Release Drug over Skin. J. Sol-Gel Sci. Technol. 2020, 94, 616–627. [Google Scholar] [CrossRef] [Scilit]
- de Lima, G.G.; de Lima, D.W.F.; de Oliveira, M.J.A.; Lugão, A.B.; Alcântara, M.T.S.; Devine, D.M.; de Sá, M.J.C. Synthesis and in Vivo Behavior of PVP/CMC/Agar Hydrogel Membranes Impregnated with Silver Nanoparticles for Wound Healing Applications. ACS Appl. Bio Mater. 2018, 1, 1842–1852. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rosiak, J.M.; Yoshii, F. Hydrogels and Their Medical Applications. Nucl. Instrum. Methods Phys. Res. B 1999, 151, 56–64. [Google Scholar] [CrossRef] [Scilit]
- Demeter, M.; Scărișoreanu, A.; Călina, I. State of the Art of Hydrogel Wound Dressings Developed by Ionizing Radiation. Gels 2023, 9, 55. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Thang, N.H.; Chien, T.B.; Cuong, D.X. Polymer-Based Hydrogels Applied in Drug Delivery: An Overview. Gels 2023, 9, 523. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tököli, A.; Bodnár, B.; Bogár, F.; Paragi, G.; Hetényi, A.; Bartus, É.; Wéber, E.; Hegedüs, Z.; Szabó, Z.; Kecskeméti, G.; et al. Structural Adaptation of the Single-Stranded DNA-Binding Protein C-Terminal to DNA Metabolizing Partners Guides Inhibitor Design. Pharmaceutics 2023, 15, 1032. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Dart, A. Common Driver Gets New Oncogenic Mechanism. Nat. Rev. Cancer 2016, 16, 551. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wu, B.; Lu, X.; Shen, H.; Yuan, X.; Wang, X.; Yin, N.; Sun, L.; Shen, P.; Hu, C.; Jiang, H.; et al. Intratumoral Heterogeneity and Genetic Characteristics of Prostate Cancer. Int. J. Cancer 2020, 146, 3369–3378. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kasiński, A.; Zielińska-Pisklak, M.; Oledzka, E.; Nałęcz-Jawecki, G.; Drobniewska, A.; Sobczak, M. Hydrogels Based on Poly(Ether-Ester)s as Highly Controlled 5-Fluorouracil Delivery Systems—Synthesis and Characterization. Materials 2020, 14, 98. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ahmad, N.; Ahmad, R.; Mohammed Buheazaha, T.; Salman AlHomoud, H.; Al-Nasif, H.A.; Sarafroz, M. A Comparative Ex Vivo Permeation Evaluation of a Novel 5-Fluorocuracil Nanoemulsion-Gel by Topically Applied in the Different Excised Rat, Goat, and Cow Skin. Saudi J. Biol. Sci. 2020, 27, 1024–1040. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rajinikanth, P.; Chellian, J. Development and Evaluation of Nanostructured Lipid Carrier-Based Hydrogel for Topical Delivery of 5-Fluorouracil. Int. J. Nanomed. 2016, 11, 5067–5077. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hanan, H.; Pervaiz, F.; Ijaz, M.; Javaid, S.M.; Bukhari, A.N.; Arshad, T.; Akhtar, S.J.; Majeed, A.; Ain, Q. Revolutionizing Colon Cancer Therapy by Site-Specific 5-Fluorouracil Delivery with Novel Stimuli-Responsive Mucoadhesive Hydrogel: Optimization via Response Surface Methodology. J. Drug Deliv. Sci. Technol. 2024, 92, 105358. [Google Scholar] [CrossRef] [Scilit]
- Ghobashy, M.M.; Elbarbary, A.M.; Hegazy, D.E. Gamma Radiation Synthesis of a Novel Amphiphilic Terpolymer Hydrogel pH-Responsive Based Chitosan for Colon Cancer Drug Delivery. Carbohydr. Polym. 2021, 263, 117975. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hegazy, D.E.; Mohamed, M.M.; Sayed, A.; Sayed, F.A.; Abdel-Raouf, M.E. Gamma Radiation Synthesis and Characterization of PVA/Arginine/p(MAAc-co-AAc)/Zr Composite Hydrogels for Biomedical Drug Delivery. ChemistrySelect 2025, 10, e02281. [Google Scholar] [CrossRef] [Scilit]
- Vigata, M.; Meinert, C.; Hutmacher, D.W.; Bock, N. Hydrogels as Drug Delivery Systems: A Review of Current Characterization and Evaluation Techniques. Pharmaceutics 2020, 12, 1188. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Korsmeyer, R.W.; Gurny, R.; Doelker, E.; Buri, P.; Peppas, N.A. Mechanisms of Solute Release from Porous Hydrophilic Polymers. Int. J. Pharm. 1983, 15, 25–35. [Google Scholar] [CrossRef] [Scilit]
- Peppas, N.A.; Sahlin, J.J. A Simple Equation for the Description of Solute Release. III. Coupling of Diffusion and Relaxation. Int. J. Pharm. 1989, 57, 169–172. [Google Scholar] [CrossRef] [Scilit]
- Biazar, E.; Roveimiab, Z.; Shahhosseini, G.; Khataminezhad, M.; Zafari, M.; Majdi, A. Biocompatibility Evaluation of a New Hydrogel Dressing Based on Polyvinylpyrrolidone/Polyethylene Glycol. J. Biomed. Biotechnol. 2012, 2012, 343989. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Călina, I.; Demeter, M.; Scărișoreanu, A.; Sătulu, V.; Mitu, B. One Step E-Beam Radiation Cross-Linking of Quaternary Hydrogels Dressings Based on Chitosan-Poly(Vinyl-Pyrrolidone)-Poly(Ethylene Glycol)-Poly(Acrylic Acid). Int. J. Mol. Sci. 2020, 21, 9236. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Anwar, M.; Pervaiz, F.; Shoukat, H.; Noreen, S.; Shabbir, K.; Majeed, A.; Ijaz, S. Formulation and Evaluation of Interpenetrating Network of Xanthan Gum and Polyvinylpyrrolidone as a Hydrophilic Matrix for Controlled Drug Delivery System. Polym. Bull. 2021, 78, 59–80. [Google Scholar] [CrossRef] [Scilit]
- Wach, R.A.; Palmeri, G.; Adamus-Wlodarczyk, A.; Rokita, B.; Olejnik, A.K.; Dispenza, C.; Ulanski, P. Dual Stimuli-Responsive Polysaccharide Hydrogels Manufactured by Radiation Technique. Appl. Sci. 2022, 12, 11764. [Google Scholar] [CrossRef] [Scilit]
- Rosiak, J.; Olejniczak, J.; Charlesby, A. Determination of the Radiation Yield of Hydrogels Crosslinking. Int. J. Radiat. Appl. Instrum. Part C Radiat. Phys. Chem. 1988, 32, 691–694. [Google Scholar] [CrossRef] [Scilit]
- Pushpamalar, V.; Langford, S.J.; Ahmad, M.; Hashim, K.; Lim, Y.Y. Preparation of Carboxymethyl Sago Pulp Hydrogel from Sago Waste by Electron Beam Irradiation and Swelling Behavior in Water and Various pH Media. J. Appl. Polym. Sci. 2013, 128, 451–459. [Google Scholar] [CrossRef] [Scilit]
- Nuutila, K.; Eriksson, E. Moist Wound Healing with Commonly Available Dressings. Adv. Wound Care 2021, 10, 685–698. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Shah, R.; Saha, N.; Saha, P. Influence of Temperature, pH and Simulated Biological Solutions on Swelling and Structural Properties of Biomineralized (CaCO3) PVP–CMC Hydrogel. Prog. Biomater. 2015, 4, 123–136. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Svensby, A.U.; Nygren, E.; Gefen, A.; Cullen, B.; Ronkvist, Å.M.; Gergely, A.; Craig, M.D. The Importance of the Simulated Wound Fluid Composition and Properties in the Determination of the Fluid Handling Performance of Wound Dressings. Int. Wound J. 2024, 21, e14861. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Fitzpatrick, S.; McCabe, J.F.; Petts, C.R.; Booth, S.W. Effect of Moisture on Polyvinylpyrrolidone in Accelerated Stability Testing. Int. J. Pharm. 2002, 246, 143–151. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hoti, G.; Caldera, F.; Cecone, C.; Rubin Pedrazzo, A.; Anceschi, A.; Appleton, S.L.; Khazaei Monfared, Y.; Trotta, F. Effect of the Cross-Linking Density on the Swelling and Rheological Behavior of Ester-Bridged β-Cyclodextrin Nanosponges. Materials 2021, 14, 478. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lü, S.; Liu, M.; Ni, B.; Gao, C. A Novel pH- and Thermo-sensitive PVP/CMC semi-IPN Hydrogel: Swelling, Phase Behavior, and Drug Release Study. J. Polym. Sci. B Polym. Phys. 2010, 48, 1749–1756. [Google Scholar] [CrossRef] [Scilit]
- Roy, N.; Saha, N.; Kitano, T.; Saha, P. Biodegradation of PVP–CMC Hydrogel Film: A Useful Food Packaging Material. Carbohydr. Polym. 2012, 89, 346–353. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rossi, F.; Chatzistavrou, X.; Perale, G.; Boccaccini, A.R. Synthesis and Degradation of Agar-carbomer Based Hydrogels for Tissue Engineering Applications. J. Appl. Polym. Sci. 2012, 123, 398–408. [Google Scholar] [CrossRef] [Scilit]
- Roux, D.C.D.; Caton, F.; Jeacomine, I.; Maîtrejean, G.; Rinaudo, M. Reversibility in the Physical Properties of Agarose Gels Following an Exchange in Solvent and Non-Solvent. Polymers 2024, 16, 811. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Jampala, S.N.; Manolache, S.; Gunasekaran, S.; Denes, F.S. Plasma-Enhanced Modification of Xanthan Gum and Its Effect on Rheological Properties. J. Agric. Food Chem. 2005, 53, 3618–3625. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Staicu, T.; Iliş, M.; Cîrcu, V.; Micutz, M. Influence of Hydrocarbon Moieties of Partially Fluorinated N -Benzoyl Thiourea Compounds on Their Gelation Properties. A Detailed Rheological Study of Complex Viscoelastic Behavior of Decanol/ N -Benzoyl Thiourea Mixtures. J. Mol. Liq. 2018, 255, 297–312. [Google Scholar] [CrossRef] [Scilit]
- Alsarra, I.A.; Hamed, A.Y.; Alanazi, F.K.; Neau, S.H. Rheological and Mucoadhesive Characterization of Poly(Vinylpyrrolidone) Hydrogels Designed for Nasal Mucosal Drug Delivery. Arch. Pharm. Res. 2011, 34, 573–582. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mezger, T.G. The Rheology Handbook: For Users of Rotational and Oscillatory Rheometers; Coatings Compendia; Vincentz Network GmbH & Co. KG: Hannover, Germany, 2006; ISBN 9783878701743. [Google Scholar]
- Roca-Arroyo, A.F.; Gutierrez-Rivera, J.A.; Morton, L.D.; Castilla-Casadiego, D.A. Hydrogel Network Architecture Design Space: Impact on Mechanical and Viscoelastic Properties. Gels 2025, 11, 588. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ashames, A.; Pervaiz, F.; Al-Tabakha, M.; Khalid, K.; Hassan, N.; Shoukat, H.; Buabeid, M.; Murtaza, G. Synthesis of Cross-Linked Carboxymethyl Cellulose and Poly (2-Acrylamido-2-Methylpropane Sulfonic Acid) Hydrogel for Sustained Drug Release Optimized by Box-Behnken Design. J. Saudi Chem. Soc. 2022, 26, 101541. [Google Scholar] [CrossRef] [Scilit]
- El-Hag Ali, A.; Shawky, H.A.; Abd El Rehim, H.A.; Hegazy, E.A. Synthesis and Characterization of PVP/AAc Copolymer Hydrogel and Its Applications in the Removal of Heavy Metals from Aqueous Solution. Eur. Polym. J. 2003, 39, 2337–2344. [Google Scholar] [CrossRef] [Scilit]
- Cheralayikkal, S.; Manoj, K.; Safna Hussan, K.P. Formulation and Evaluation of a Smart Drug Delivery System of 5-Fluorouracil for pH-Sensitive Chemotherapy. Heliyon 2022, 8, e09926. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Khurshid, A.; Anwar, Z.; Usmani, M.; Altaf, R.; Awan, A.; Akram, Z.; Kazi, S.H.; Ahmed, S.; Sheraz, M.A.; Ahmad, I. Cyclodextrin-Assisted Photostabilization of 5-Fluorouracil: A Combined Kinetic and Computational Investigation. RSC Adv. 2025, 15, 31194–31209. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Balaban, A.T.; Banciu, M.; Pogany, I.I. Aplicații Ale Metodelor Fizice în Chimia Organică; Editura Științifică și Enciclopedică: Bucharest, Romania, 1983. [Google Scholar]
- Pandya, I.; Joshi, V.; Kumar, S.; Aswal, V.K.; Raje, N.; Kuddushi, M.; Zhang, X.; Malek, N. Multifunctional and Stimuli-Responsive Ionic Liquid-Polymeric Hydrogel: A Promising Platform for Co-Drug Delivery in Cancer Treatment. Nanoscale 2025, 17, 28091–28103. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Saadh, M.J.; Kyada, A.; Jyothi, S.R.; Kumar, M.R.; Allela, O.Q.B.; Nathiya, D.; Kaur, P.; Sead, F.F.; Kaur, J.; Ghafouriraz, S. DFT Investigation of 5-Fluorouracil Tautomerism and Non-Covalent Interactions with PLGA Nanoparticles for Enhanced Drug Delivery and Sensing. Spectrochim. Acta A Mol. Biomol. Spectrosc. 2025, 335, 125945. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wielińska, J.; Nowacki, A.; Liberek, B. 5-Fluorouracil—Complete Insight into Its Neutral and Ionised Forms. Molecules 2019, 24, 3683. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mohsin, M.E.A.; Siddiqa, A.J.; Mousa, S.; Shrivastava, N.K. Design, Characterization, and Release Kinetics of a Hybrid Hydrogel Drug Delivery System for Sustained Hormone Therapy. Polymers 2025, 17, 999. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Monnot, E.; Kindberg, C.; Johnson, T.; Riley, C.; Stobauch, J.; Slavik, M. Stability of Intravenous Admixtures of 5-Fluorouracil and Spirogermanium, a Novel Combination of Cytotoxic Agents. Int. J. Pharm. 1990, 60, 41–52. [Google Scholar] [CrossRef] [Scilit]
- Alfassam, H.E.; Othman, S.I.; Bin Jumah, M.N.; Al-Waili, M.A.; Allam, A.A.; Al Zoubi, W.; Abukhadra, M.R. Characterization of Chitosan-Hybridized Diatomite as Potential Delivery Systems of Oxaliplatin and 5-Fluorouracil Drugs: Equilibrium and Release Kinetics. ACS Omega 2023, 8, 38330–38344. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Xiao, Y.; Chen, C.; Zhang, Y.; Tsaoulidis, D.; Chen, T. A Modelling-Based Comparison of IVRT and Synthetic-Membrane Permeation for Early Formulation Screening. RSC Pharm. 2026, 3, 1034–1043. [Google Scholar] [CrossRef] [Scilit]
- Papadopoulou, V.; Kosmidis, K.; Vlachou, M.; Macheras, P. On the Use of the Weibull Function for the Discernment of Drug Release Mechanisms. Int. J. Pharm. 2006, 309, 44–50. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nagasawa, N.; Yagi, T.; Kume, T.; Yoshii, F. Radiation Crosslinking of Carboxymethyl Starch. Carbohydr. Polym. 2004, 58, 109–113. [Google Scholar] [CrossRef] [Scilit]
- Olejniczak, J.; Rosiak, J.; Charlesby, A. Gel/Dose Curves for Polymers Undergoing Simultaneous Crosslinking and Scission. Radiat. Phys. Chem. 1991, 37, 499–504. [Google Scholar] [CrossRef] [Scilit]
- Wach, R.A.; Mitomo, H.; Nagasawa, N.; Yoshii, F. Radiation Crosslinking of Methylcellulose and Hydroxyethylcellulose in Concentrated Aqueous Solutions. Nucl. Instrum. Methods Phys. Res. B 2003, 211, 533–544. [Google Scholar] [CrossRef] [Scilit]
- Charlesby, A. Past and Future Trends in Polymer Irradiation. Int. J. Radiat. Appl. Instrum. Part C Radiat. Phys. Chem. 1991, 37, 5–10. [Google Scholar] [CrossRef] [Scilit]
- Boonkaew, B.; Suwanpreuksa, P.; Cuttle, L.; Barber, P.M.; Supaphol, P. Hydrogels Containing Silver Nanoparticles for Burn Wounds Show Antimicrobial Activity without Cytotoxicity. J. Appl. Polym. Sci. 2014, 131, 40215. [Google Scholar] [CrossRef] [Scilit]
- Chen, J.; Park, H.; Park, K. Synthesis of Superporous Hydrogels: Hydrogels with Fast Swelling and Superabsorbent Properties. J. Biomed. Mater. Res. 1999, 44, 53–62. [Google Scholar] [CrossRef] [Scilit]
- Tanan, W.; Panichpakdee, J.; Saengsuwan, S. Novel Biodegradable Hydrogel Based on Natural Polymers: Synthesis, Characterization, Swelling/Reswelling and Biodegradability. Eur. Polym. J. 2019, 112, 678–687. [Google Scholar] [CrossRef] [Scilit]
- Goodwin, J.W.; Hughes, R.W. Linear Viscoelasticity I: Phenomenological Approach. In Rheology for Chemists; Royal Society of Chemistry: Cambridge, UK, 2008; pp. 92–134. [Google Scholar]
- Gao, F.; Wu, X.; Wu, D.; Yu, J.; Yao, J.; Qi, Q.; Cao, Z.; Cui, Q.; Mi, Y. Preparation of Degradable Magnetic Temperature- and Redox-Responsive Polymeric/Fe3O4 Nanocomposite Nanogels in Inverse Miniemulsions for Loading and Release of 5-Fluorouracil. Colloids Surf. A Physicochem. Eng. Asp. 2020, 587, 124363. [Google Scholar] [CrossRef] [Scilit]
- El-Zeiny, H.M.; Abukhadra, M.R.; Sayed, O.M.; Osman, A.H.M.; Ahmed, S.A. Insight into Novel β-Cyclodextrin-Grafted-Poly (N-Vinylcaprolactam) Nanogel Structures as Advanced Carriers for 5-Fluorouracil: Equilibrium Behavior and Pharmacokinetic Modeling. Colloids Surf. A Physicochem. Eng. Asp. 2020, 586, 124197. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.; Huo, M.; Zhou, J.; Zou, A.; Li, W.; Yao, C.; Xie, S. DDSolver: An Add-In Program for Modeling and Comparison of Drug Dissolution Profiles. AAPS J. 2010, 12, 263–271. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ibrahim, S.M.; Bin Jumah, M.N.; Othman, S.I.; Alruhaimi, R.S.; Al-Khalawi, N.; Salama, Y.F.; Allam, A.A.; Abukhadra, M.R. Synthesis of Chitosan/Diatomite Composite as an Advanced Delivery System for Ibuprofen Drug; Equilibrium Studies and the Release Profile. ACS Omega 2021, 6, 13406–13416, Correction in ACS Omega 2021, 6, 24296. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Arifin, D.Y.; Lee, L.Y.; Wang, C.-H. Mathematical Modeling and Simulation of Drug Release from Microspheres: Implications to Drug Delivery Systems. Adv. Drug Deliv. Rev. 2006, 58, 1274–1325. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bruschi, M.L. Mathematical Models of Drug Release. In Strategies to Modify the Drug Release from Pharmaceutical Systems; Bruschi, M.L., Ed.; Elsevier: Cambridge, MA, USA, 2015; pp. 63–86. ISBN 9780081000922. [Google Scholar]
- Demeter, M.; Călina, I.; Scărișoreanu, A.; Micutz, M. E-Beam Cross-Linking of Complex Hydrogels Formulation: The Influence of Poly(Ethylene Oxide) Concentration on the Hydrogel Properties. Gels 2022, 8, 27. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Suryavanshi, P.; Mahajan, S.; Banerjee, S.K.; Seth, K.; Banerjee, S. Synthesis and Characterization of a pH/Temperature-Dual Responsive Hydrogel with Promising Biocompatibility Features for Stimuli-Responsive 5-FU Delivery. J. Mater. Chem. B 2024, 12, 5098–5110. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chen, J.; Rong, L.; Lin, H.; Xiao, R.; Wu, H. Radiation Synthesis of pH-Sensitive Hydrogels from β-Cyclodextrin-Grafted PEG and Acrylic Acid for Drug Delivery. Mater. Chem. Phys. 2009, 116, 148–152. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.