Reviewer 1 Report
Comments and Suggestions for AuthorsThe manuscript addresses an interesting and relevant topic and presents potentially valuable experimental results concerning the plasma nitriding of high-speed steels. However, the paper requires substantial improvements, particularly in terms of methodological clarity, microstructural characterisation, and the depth of the discussion.
-
In my opinion, the title of the manuscript is not consistent with the actual scope of the study. The authors do not investigate abrasive wear, but rather the adhesion of the nitrided layer to the substrate. The technique used is, in my view, not appropriate for the evaluation of diffusion layers and is more typically applied to coatings deposited using PVD methods.
-
The manuscript lacks a clearly stated element of scientific novelty. Although the introduction provides a well-structured overview of the topic, the authors do not clearly indicate what new scientific contribution or innovative aspect the study is intended to demonstrate.
-
The microstructure of the substrate prior to and after the nitriding process is not presented.
-
Metallographic analysis is missing. The SEM images provided are difficult to interpret and do not add meaningful information to the discussion of the results.
-
Please verify the numerical notation used in the tables and figures and replace commas with decimal points where appropriate.
-
The manuscript would be significantly clearer if the authors reconsidered the order in which the results are presented. First, the microstructure of the substrate should be characterised using optical microscopy and scanning electron microscopy, complemented by EDS analysis. This should be followed by an analysis of the phase composition, supported by TEM investigations to provide a more detailed structural characterisation. Only after these analyses should the authors proceed to the evaluation of wear resistance, preferably using a method specifically intended for the assessment of diffusion layers
Author Response
We are pleased to submit the revised version of our manuscript, entitled:
“AEGD-Assisted Plasma Nitriding of AISI M2 Steel: Influence of Treatment Time on Microstructure and Scratch Resistance”
We sincerely thank you and the reviewers for the constructive feedback, which has significantly improved the quality, clarity, and scientific rigor of our manuscript. We have carefully considered all comments and have revised the manuscript accordingly.
In particular, we have:
- Clarified the novelty and scientific contributions of the work.
- Improved the presentation and interpretation of microstructural and mechanical characterization data.
- Revised figures, tables, and captions for consistency and clarity.
- Corrected typographical errors and standardized terminology throughout the manuscript.
- Provided additional explanations where needed to strengthen the scientific reasoning and interpretation of results.
A detailed, point-by-point response to each reviewer comment has been prepared and is attached for your consideration. We believe that the revised manuscript now fully addresses the reviewers’ concerns and is suitable for publication in [Journal Name].
We greatly appreciate your time and consideration and look forward to your favorable evaluation.
Sincerely,
Juan Manuel González Carmona PhD
SECIHTI, Center of Engineering and Industrial Development, CIDESI,
Querétaro, Av. Pie de la Cuesta 702, CP 76125
México
Tel: +(52) 1 442 748 0070
REVIEWER 1
- The manuscript addresses an interesting and relevant topic and presents potentially valuable experimental results concerning the plasma nitriding of high-speed steels. However, the paper requires substantial improvements, particularly in terms of methodological clarity, microstructural characterisation, and the depth of the discussion.
- In my opinion, the title of the manuscript is not consistent with the actual scope of the study. The authors do not investigate abrasive wear, but rather the adhesion of the nitrided layer to the substrate. The technique used is, in my view, not appropriate for the evaluation of diffusion layers and is more typically applied to coatings deposited using PVD methods.
R// We thank the reviewer for this valuable comment. We agree that the original title did not fully reflect the actual scope of the study. Accordingly, it has been revised to better represent the focus of the work.
This study is centered on the scratch resistance of plasma-nitrided layers rather than on abrasive wear. The scratch test was employed to evaluate the mechanical response and load-bearing capacity of the modified surface. It is important to note that, unlike PVD coatings, nitrided layers are diffusion zones without a well-defined interface; therefore, the test does not assess adhesion in the conventional sense.
Furthermore, the static scratch test was used to simulate, under controlled conditions, the interaction of a hard particle with the surface, representing a third-body abrasion scenario.
In addition, the thickness of the diffusion layer was characterized by SEM, enabling correlation with the observed mechanical behavior.
The manuscript has been revised accordingly. The proposed new title is:
“AEGD-Assisted Plasma Nitriding of AISI M2 Steel: Influence of Treatment Time on Microstructure and Scratch Resistance.”
- The manuscript lacks a clearly stated element of scientific novelty. Although the introduction provides a well-structured overview of the topic, the authors do not clearly indicate what new scientific contribution or innovative aspect the study is intended to demonstrate.
R// We thank the reviewer for this important observation. We agree that the novelty of the study was not sufficiently emphasized in the original version, and the manuscript has been revised accordingly to improve clarity.
The novelty of this work resides in: (i) the application of AEGD-assisted plasma nitriding, (ii) the achievement of comparable or improved mechanical performance with significantly reduced treatment times (1.5 h and 3.5 h) relative to conventional processes (> 4 h), and (iii) the comparative evaluation of substrates with and without prior heat treatment.
These aspects, combined with the systematic correlation between diffusion layer characteristics and scratch resistance, represent the main scientific contributions of the study.
Furthermore, the Introduction has been revised to explicitly highlight these contributions, thereby improving the overall clarity and positioning of the manuscript.
- The microstructure of the substrate prior to and after the nitriding process is not presented.
R// We thank the reviewer for this insightful observation. The manuscript has been revised to explicitly include the substrate microstructure in both the as-received and heat-treated conditions. This information is now presented in Figure 1, which shows representative SEM micrographs of both states.
A detailed description supported by SEM and EDS analyses has also been incorporated to characterize the initial microstructural features. This addition provides a clearer and more rigorous basis for understanding the starting condition of the material prior to the nitriding treatment, thereby strengthening the interpretation of the subsequent results.
- Metallographic analysis is missing. The SEM images provided are difficult to interpret and do not add meaningful information to the discussion of the results.
R// We thank the reviewer for this valuable observation. In response, we performed a complementary metallographic analysis and substantially strengthened the discussion by providing a more detailed interpretation of the SEM micrographs, supported by EDS results.
The revised analysis offers a clearer and more rigorous description of the morphology, spatial distribution, and chemical nature of the carbides. This improvement enhances the relevance of the microstructural characterization and its direct connection to the overall findings of the study.
- Please verify the numerical notation used in the tables and figures and replace commas with decimal points where appropriate.
R// We thank the reviewer for this observation. The manuscript has been carefully revised to ensure consistency in numerical notation, and decimal commas have been replaced with decimal points throughout the document, where appropriate.
These corrections have been implemented in the following sections:
- Table 1.
- Figure 1.
- Figure 6.
- Figure 7.
- The manuscript would be significantly clearer if the authors reconsidered the order in which the results are presented. First, the microstructure of the substrate should be characterised using optical microscopy and scanning electron microscopy, complemented by EDS analysis. This should be followed by an analysis of the phase composition, supported by TEM investigations to provide a more detailed structural characterisation. Only after these analyses should the authors proceed to the evaluation of wear resistance, preferably using a method specifically intended for the assessment of diffusion layers
R// We thank the reviewer for this constructive suggestion. The manuscript has been revised to enhance the clarity and logical progression of the Results section. In particular, the microstructural characterization of the substrate (SEM/EDS) is now presented prior to the phase analysis and discussion.
At the same time, the overall structure of the manuscript has been carefully preserved to maintain the coherence between the XRD and subsequent TEM analyses, which are closely interconnected and benefit from being discussed sequentially.
We believe that this revised organization improves readability while preserving the scientific rigor and internal consistency of the study.
Author Response File:
Author Response.pdf
Reviewer 2 Report
Comments and Suggestions for AuthorsThis manuscript examines the impact of the AEGD-Assisted Plasma Nitriding process on AISI M2 Steel and presents extensive data. To further enhance clarity in the discussion and presentation, the following suggestions are offered to strengthen the manuscript prior to publication.
- Table 1 – Two different decimal symbols are used - “,” and “.” Consider using only one symbol.
- Line 130 – “Φ = 5.08 cm, 99.5 %”. Please describe what ‘Φ’ and 99.5% referring to?
- Line 149 – “….Rwp < 3%, and normalized residual S < 1.09.” Please describe what ‘Rwp’ and ‘S’ are.
- Figure 1 – These figures are not labeled with (1a) or (1b).
- Line 199-200 – The sentence refers to TEM in Section 3.3; however, Section 3.3 is titled “Diffusion Layers.” Would it be more appropriate to combine the TEM and X-ray results in Section 3.1?
- Figure 2(a) – The legend lists a sample group labeled “VC”; however, this group is not referenced elsewhere in the manuscript. Should this be corrected to “MC”?
- Line 242 – “……while the γ′-Fe4N phase reached peak concentration of ~ 27 wt.% after 1.5 h and decreased to ~ 10 wt.% after 3.5 h of nitriding.” Please check if this statement is correct and matches the data shown in Figure 2a.
- Line 255 – “After 3.5 h of AEGD-PAN significant fractions of MC (21.3 wt. %) and M6C (7.9 wt. %), carbides were still detected…..” The results shown in Figure 2 do not seem to support this statement. Could the authors please provide additional information to clarify their argument?
- Line 273 – “…. PDF 79982…..” Is ‘PDF 79982’ a typo?
- Line 276 – “…….PDF 01-078-3750….” Is ‘PDF 01-078-3750’ a typo?
- Line 289 – “…consistent with PDF 79982.” Is ‘PDF 79982’ a typo?
- Figure 5 – Please clarify in the manuscript whether the dotted lines in Figure 5 indicate diffusion layers or their boundaries.
- Figure 7 – The figure presents hardness as a function of depth. Could the authors clarify which sample groups correspond to HT and non-HT? Additionally, what does the “TT” sample in the figure legend represent? The text refers to ‘TT’ only once, without providing a definition (Line 528).
- Figure 8 – Please clarify the meaning of the “TT” labels in the figures; should these be labeled as ‘HT’? Additionally, the image resolution requires improvement, as the cracks in Figure 8(b) are difficult to discern.
- Line 444 – “This behavior reflects the high hardness of the nitrided layer combined with a moderate reduction in toughness, allowing controlled microfracture for stress relief without catastrophic spalling.” The underlying factors contributing to this ‘moderate reduction in toughness’ are not clearly explained. Please provide further clarification.
- Line 439 – “….most of the groove, suggesting a plastic creep response and significant material drag,….” The role of “plastic creep response” in lateral crack formation is not clearly explained. Further clarification is needed. Typically, creep refers to a high-temperature, strain rate-dependent deformation process.
- Line 459 – What is “circumferential crack”? “Perpendicular cracks” labeled in Figure 9(a)?
- Line 474 – “It is noteworthy that nitriding times shorter than 3.5 h increase microhardness and resistance to plastic deformation,…” This statement appears to contradict the results presented in Figure 7, as samples treated for 1.5 and 3.5 hours demonstrate similar hardness.
- Figure 10 – Please check if the “TT” labels are typos.
Author Response
We are pleased to submit the revised version of our manuscript, entitled:
“AEGD-Assisted Plasma Nitriding of AISI M2 Steel: Influence of Treatment Time on Microstructure and Scratch Resistance”
We sincerely thank you and the reviewers for the constructive feedback, which has significantly improved the quality, clarity, and scientific rigor of our manuscript. We have carefully considered all comments and have revised the manuscript accordingly.
In particular, we have:
- Clarified the novelty and scientific contributions of the work.
- Improved the presentation and interpretation of microstructural and mechanical characterization data.
- Revised figures, tables, and captions for consistency and clarity.
- Corrected typographical errors and standardized terminology throughout the manuscript.
- Provided additional explanations where needed to strengthen the scientific reasoning and interpretation of results.
A detailed, point-by-point response to each reviewer comment has been prepared and is attached for your consideration. We believe that the revised manuscript now fully addresses the reviewers’ concerns and is suitable for publication in [Journal Name].
We greatly appreciate your time and consideration and look forward to your favorable evaluation.
Sincerely,
Juan Manuel González Carmona PhD
SECIHTI, Center of Engineering and Industrial Development, CIDESI,
Querétaro, Av. Pie de la Cuesta 702, CP 76125
México
Tel: +(52) 1 442 748 0070
REVIEWER 2
This manuscript examines the impact of the AEGD-Assisted Plasma Nitriding process on AISI M2 Steel and presents extensive data. To further enhance clarity in the discussion and presentation, the following suggestions are offered to strengthen the manuscript prior to publication.
- Table 1 – Two different decimal symbols are used - “,” and “.” Consider using only one symbol.
R// We thank the reviewer for this observation. The manuscript has been carefully revised to ensure consistency in numerical notation, and decimal commas have been replaced with decimal points throughout the document, where appropriate.
These corrections have been implemented in the following sections:
- Table 1.
- Figure 1.
- Figure 6.
- Figure 7.
- Line 130 – “Φ = 5.08 cm, 99.5 %”. Please describe what ‘Φ’ and 99.5% referring to?
R// We thank the reviewer for pointing out this ambiguity. The description has been clarified to explicitly indicate that Φ = 5.08 cm corresponds to the cathode diameter, while 99.5% refers to its purity.
The revised text now reads as follows: “…using a shielded Ti cathode (Φ = 5.08 cm in diameter, 99.5% purity) and a stainless steel anode…”.
- Line 149 – “….Rwp < 3%, and normalized residual S < 1.09.” Please describe what ‘Rwp’ and ‘S’ are.
R// We thank the reviewer for this observation. The original text has been revised to improve clarity and to explicitly define the refinement quality parameters.
The revised text reads as follows:
“Rigaku’s PDXL software was employed for the analysis, and correlation values were determined using the minimum method. The quality of the Rietveld refinement was evaluated using the weighted profile R-factor (Rwp) and the goodness-of-fit parameter (S). The obtained values (Rwp < 3% and S < 1.09) indicate excellent agreement between the experimental and calculated diffraction patterns.”
- Figure 1 – These figures are not labeled with (1a) or (1b).
R// We thank the reviewer for this observation. The comment has been addressed by renaming Figure 2 into two subfigures, now labeled as Figure 2a and Figure 2b (This takes into account that the numbering of the figures was modified), to improve clarity and facilitate interpretation.
- Line 199-200 – The sentence refers to TEM in Section 3.3; however, Section 3.3 is titled “Diffusion Layers.” Would it be more appropriate to combine the TEM and X-ray results in Section 3.1?
R// We thank the reviewer for this valuable suggestion. The reference has been corrected accordingly. The proposed reorganization was carefully considered; however, the current sequence (XRD, Rietveld refinement, and TEM) has been retained, as it provides a more coherent and logical progression of the results—from phase identification to quantitative analysis and subsequent microstructural validation. However, we have included an initial section with a detailed study of the material's microstructure before nitriding.
We believe this structure enhances the clarity and interpretability of the findings while maintaining the scientific rigor of the study.
- Figure 2(a) – The legend lists a sample group labeled “VC”; however, this group is not referenced elsewhere in the manuscript. Should this be corrected to “MC”?
R// We thank the reviewer for identifying this error. The phase name has been corrected accordingly, changing “VC” to “MC” to accurately reflect the analyzed material in figure 3.
- Line 242 – “……while the γ′-Fe4N phase reached peak concentration of ~ 27 wt.% after 1.5 h and decreased to ~ 10 wt.% after 3.5 h of nitriding.” Please check if this statement is correct and matches the data shown in Figure 2a.
R// We thank the reviewer for this observation. The reported data were carefully verified and found to be consistent with the comment. Accordingly, the text has been corrected and now reads:
“…the γ′-Fe₄N phase reached a peak concentration of ~55 wt.% after 1.5 h, increasing to approximately 68 wt.% after 3.5 h of nitriding, at the expense of the iron content.”
- Line 255 – “After 3.5 h of AEGD-PAN significant fractions of MC (21.3 wt. %) and M6C (7.9 wt. %), carbides were still detected…..” The results shown in Figure 2 do not seem to support this statement. Could the authors please provide additional information to clarify their argument?
R// We thank the reviewer for this comment. The statement regarding the carbide fractions after 3.5 h of AEGD-PAN resulted from a drafting error and was inconsistent with the data presented in Figure 3.
The original sentence:
“After 3.5 h of AEGD-PAN significant fractions of MC (21.3 wt. %) and M₆C (7.9 wt. %) carbides were still detected, suggesting concurrent carbide stability and possible carbon redistribution.”
has been replaced with:
“After 3.5 h of AEGD-PAN, only minor fractions of carbides were detected. MC was nearly absent, while M₆C was present in limited amounts, particularly in the HT condition (~5 wt.%). This behavior indicates partial destabilization of pre-existing carbides under high nitrogen activity, accompanied by possible carbon redistribution during the treatment.”
This correction now aligns accurately with the quantitative results shown in Figure 3.
- Line 273 – “…. PDF 79982…..” Is ‘PDF 79982’ a typo?
R// We thank the reviewer for this comment. The acronym PDF refers to the powder diffraction files used as reference diffraction charts. This clarification has been added to Section 3.3, Rietveld Analysis and Phase Quantification, to improve clarity.
- Line 276 – “…….PDF 01-078-3750….” Is ‘PDF 01-078-3750’ a typo?
R// We thank the reviewer for this comment. The acronym PDF refers to the powder diffraction files used as reference diffraction charts. This clarification has been added to Section 3.3, Rietveld Analysis and Phase Quantification, to improve clarity.
- Line 289 – “…consistent with PDF 79982.” Is ‘PDF 79982’ a typo?
R// We thank the reviewer for this comment. The acronym PDF refers to the powder diffraction files used as reference diffraction charts. This clarification has been added to Section 3.3, Rietveld Analysis and Phase Quantification, to improve clarity.
- Figure 5 – Please clarify in the manuscript whether the dotted lines in Figure 5 indicate diffusion layers or their boundaries.
R// We thank the reviewer for this comment. As described in Section 3.4, Diffusion Layers, the dotted lines represent the non-uniform boundary observed between the nitrided zone and the steel core. This boundary reflects the gradual transition in nitrogen concentration and microstructural changes from the hardened layer to the substrate, providing insight into the depth-dependent properties of the treated material.
- Figure 7 – The figure presents hardness as a function of depth. Could the authors clarify which sample groups correspond to HT and non-HT? Additionally, what does the “TT” sample in the figure legend represent? The text refers to ‘TT’ only once, without providing a definition (Line 528).
R// We thank the reviewer for this comment. The figure has been revised to more accurately represent the obtained data, and the sample labels have been updated to ensure consistency with the terminology used throughout the text, thereby improving clarity and interpretability.
- Figure 8 – Please clarify the meaning of the “TT” labels in the figures; should these be labeled as ‘HT’? Additionally, the image resolution requires improvement, as the cracks in Figure 8(b) are difficult to discern.
R// We thank the reviewer for this feedback. The sample notation has been revised to ensure consistency throughout the text. The designation TT was identified as a typographical error and has been corrected in both the text and figures. In addition, high-resolution images have been provided to facilitate more accurate analysis and interpretation of the results.
- Line 444 – “This behavior reflects the high hardness of the nitrided layer combined with a moderate reduction in toughness, allowing controlled microfracture for stress relief without catastrophic spalling.” The underlying factors contributing to this ‘moderate reduction in toughness’ are not clearly explained. Please provide further clarification.
R// We thank the reviewer for this comment. The observed moderate reduction in toughness is attributed to the formation of hard and relatively brittle nitride phases, as well as residual stresses and microstructural modifications induced during the AEGD-PAN treatment.
The original sentence:
“This behavior reflects the high hardness of the nitrided layer combined with a moderate reduction in toughness, allowing controlled microfracture for stress relief without catastrophic spalling.”
has been revised to:
“This behavior reflects the high hardness of the nitrided layer combined with a moderate reduction in toughness, which can be attributed to the formation of brittle nitride phases, residual stresses, and microstructural modifications, such as carbide destabilization. These factors facilitate controlled microfracture for stress relief without leading to catastrophic spalling.”
- Line 439 – “….most of the groove, suggesting a plastic creep response and significant material drag,….” The role of “plastic creep response” in lateral crack formation is not clearly explained. Further clarification is needed. Typically, creep refers to a high-temperature, strain rate-dependent deformation process.
R// We thank the reviewer for this important clarification. The term “plastic creep response” was deemed inappropriate in this context and has been replaced. The revised text now refers to “plastic deformation” to accurately describe the material behavior during scratching. Furthermore, additional clarification has been added to explain that the absence of lateral cracks reflects enhanced plastic accommodation and material flow, which delays crack initiation and contributes to the improved scratch resistance of the nitrided layer.
- Line 459 – What is “circumferential crack”? “Perpendicular cracks” labeled in Figure 9(a)?
R// We thank the reviewer for this comment. In the context of the scratch tests, “circumferential cracks” refer to cracks that form along the perimeter of the indenter track, approximately following the surface contour around the scratch direction. These cracks are typically associated with tensile stresses developing perpendicular to the scratch path due to elastic-plastic deformation.
Similarly, “perpendicular cracks” describe cracks oriented roughly orthogonal to the scratch direction, resulting from tensile stresses concentrated ahead of the indenter tip. Both types of cracks provide insight into the fracture behavior and stress distribution within the nitrided layer, allowing assessment of its toughness and deformation mechanisms under localized loading.
- Line 474 – “It is noteworthy that nitriding times shorter than 3.5 h increase microhardness and resistance to plastic deformation,…” This statement appears to contradict the results presented in Figure 7, as samples treated for 1.5 and 3.5 hours demonstrate similar hardness.
R// We thank the reviewer for this valuable feedback. In response, the text has been revised to avoid overgeneralization. While the surface hardness values for the 1.5 h and 3.5 h treatments are comparable, the data indicate that the 3.5 h condition exhibits a more gradual decrease in hardness with depth, reflecting a thicker diffusion layer. Accordingly, the text now clarifies that the enhanced mechanical performance observed at 3.5 h is associated with an increased load-bearing capacity rather than a significant increase in surface hardness.
- Figure 10 – Please check if the “TT” labels are typos.
R// We thank the reviewer for this feedback. The sample notation has been revised to ensure consistency throughout the text. The designation TT was identified as a typographical error and has been corrected in both the text and figures.
Additional notes:
- The affiliation of co-author Leonardo Bohorquez Santiago from the Universidad Tecnológica de Pereira was corrected (2 à 1), as well as the name of co-author Julián Felipe Villada Castillo (Juan à Julian), and his email address (jvillada@utp.edu.co à jfvillada@utp.edu.co).
- The acknowledgments have been adjusted, including at the end acknowledgments to the Universidad Tecnológica de Pereira for their support in the development of the project:
“Likewise, we thank the Universidad Tecnológica de Pereira for the support for the development of the project “influencia de los parámetros del plasma en las propiedades mecánicas y tribológicas del acero AISI M2 funcionalizado por nitruración asistida por plasma por el método AEGD” with code 3-25-8.”
Author Response File:
Author Response.pdf
Reviewer 3 Report
Comments and Suggestions for AuthorsThis manuscript presents a relatively systematic study on AEGD-assisted plasma nitriding of M2 steel. The experimental work covers multiple characterization techniques, enabling correlation between microstructure and properties across different scales. Overall, the study demonstrates certain engineering relevance and a solid academic foundation.
- The introduction involves several potential points of novelty, including low-temperature processing, short treatment duration, and AEGD assistance; however, it lacks a clear central focus. It is better to explicitly state the core innovation of this work compared with existing PAN or related studies at the end of the introduction. For example, the authors could emphasize the unique role of AEGD in short-time nitriding or its influence on diffusion behavior.
- The mechanism of AEGD is insufficiently explained. Although the manuscript emphasizes the AEGD process throughout, it does not clearly clarify its fundamental physical differences compared with conventional plasma nitriding. It is recommended to combine the existing results and provide a mechanistic interpretation from perspectives such as ion energy, plasma density, surface activation, and sputtering effects.
- The manuscript mentions that the growth of the diffusion layer deviates from the parabolic law, but the controlling mechanism is not further analyzed. It is recommended to use the existing thickness data to provide both qualitative and quantitative discussions, clarifying whether the diffusion process is governed by a mixed mechanism (diffusion combined with surface reaction).
- The discussion on the evolution of γ′-Fe₄N and ε-Fe₂–₃N remains largely at a phenomenological level, lacking a unified interpretation based on thermodynamics or nitrogen potential.
- The description of the crack types is relatively thorough, but it lacks support from the mechanical mechanisms. It is recommended to explain crack behavior by incorporating residual stress distribution, gradient structures, and the thickness of the diffusion layer.
- The text directly employs the modified form of the Archard model but does not specify its applicable conditions and limitations.
- The conclusion section is somewhat repetitive and could be appropriately streamlined to emphasize the key findings.
- The correspondence between the figures/tables and the text could be further strengthened. It is recommended to indicate the layers or key features within the figures and tables.
Author Response
We are pleased to submit the revised version of our manuscript, entitled:
“AEGD-Assisted Plasma Nitriding of AISI M2 Steel: Influence of Treatment Time on Microstructure and Scratch Resistance”
We sincerely thank you and the reviewers for the constructive feedback, which has significantly improved the quality, clarity, and scientific rigor of our manuscript. We have carefully considered all comments and have revised the manuscript accordingly.
In particular, we have:
- Clarified the novelty and scientific contributions of the work.
- Improved the presentation and interpretation of microstructural and mechanical characterization data.
- Revised figures, tables, and captions for consistency and clarity.
- Corrected typographical errors and standardized terminology throughout the manuscript.
- Provided additional explanations where needed to strengthen the scientific reasoning and interpretation of results.
A detailed, point-by-point response to each reviewer comment has been prepared and is attached for your consideration. We believe that the revised manuscript now fully addresses the reviewers’ concerns and is suitable for publication in [Journal Name].
We greatly appreciate your time and consideration and look forward to your favorable evaluation.
Sincerely,
Juan Manuel González Carmona PhD
SECIHTI, Center of Engineering and Industrial Development, CIDESI,
Querétaro, Av. Pie de la Cuesta 702, CP 76125
México
Tel: +(52) 1 442 748 0070
REVIEWER 3
- The introduction involves several potential points of novelty, including low-temperature processing, short treatment duration, and AEGD assistance; however, it lacks a clear central focus. It is better to explicitly state the core innovation of this work compared with existing PAN or related studies at the end of the introduction. For example, the authors could emphasize the unique role of AEGD in short-time nitriding or its influence on diffusion behavior.
R// We thank the reviewer for this suggestion. The Introduction has been revised to clearly highlight the core innovation of the study. The final paragraph now explicitly emphasizes the unique role of AEGD-assisted plasma nitriding in achieving short-time, low-temperature treatment while enhancing diffusion behavior and mechanical performance, distinguishing it from conventional PAN and related studies.
- The mechanism of AEGD is insufficiently explained. Although the manuscript emphasizes the AEGD process throughout, it does not clearly clarify its fundamental physical differences compared with conventional plasma nitriding. It is recommended to combine the existing results and provide a mechanistic interpretation from perspectives such as ion energy, plasma density, surface activation, and sputtering effects.
R// We appreciate the comment regarding mechanistic explanation. The manuscript now includes a detailed discussion of the fundamental differences between AEGD-assisted and conventional plasma nitriding. The revision considers ion energy, plasma density, surface activation, and sputtering effects, linking these factors to enhanced nitrogen incorporation and accelerated diffusion in the short-time AEGD process.
- The manuscript mentions that the growth of the diffusion layer deviates from the parabolic law, but the controlling mechanism is not further analyzed. It is recommended to use the existing thickness data to provide both qualitative and quantitative discussions, clarifying whether the diffusion process is governed by a mixed mechanism (diffusion combined with surface reaction).
R// The discussion of diffusion layer growth has been expanded. Using the measured thickness data, both qualitative and quantitative analysis now indicate that the growth deviates from parabolic law due to a mixed controlling mechanism, involving bulk diffusion combined with surface reaction kinetics. This interpretation clarifies the influence of treatment time and nitrogen activity on layer thickness and gradient formation.
- The discussion on the evolution of γ′-Fe₄N and ε-Fe₂–₃N remains largely at a phenomenological level, lacking a unified interpretation based on thermodynamics or nitrogen potential.
R// The manuscript has been revised to provide a unified interpretation of γ′-Fe₄N and ε-Fe₂–₃N evolution, incorporating thermodynamic considerations and nitrogen potential. This approach explains the preferential formation and relative stability of these phases during short-time AEGD-PAN treatments, moving beyond a purely phenomenological description.
- The description of the crack types is relatively thorough, but it lacks support from the mechanical mechanisms. It is recommended to explain crack behavior by incorporating residual stress distribution, gradient structures, and the thickness of the diffusion layer.
R// We agree that a mechanistic link was needed. The revised text now discusses crack formation in relation to residual stress distribution, gradient microstructure, and diffusion layer thickness. The analysis explains how these factors influence the initiation and propagation of circumferential and perpendicular cracks observed during scratch testing.
- The text directly employs the modified form of the Archard model but does not specify its applicable conditions and limitations.
R// The use of the modified Archard model has been clarified. The manuscript now specifies the applicable conditions and limitations of the model, ensuring proper interpretation of the wear analysis within the context of the study.
- The conclusion section is somewhat repetitive and could be appropriately streamlined to emphasize the key findings.
R// The Conclusion has been streamlined to emphasize the key findings: the effectiveness of short-time AEGD-assisted plasma nitriding, the correlation between diffusion layer characteristics and mechanical performance, and the enhanced scratch resistance. Redundant statements have been removed to improve readability and impact.
- The correspondence between the figures/tables and the text could be further strengthened. It is recommended to indicate the layers or key features within the figures and tables.
R// Figures and tables have been revised to strengthen their correspondence with the text. Layers and key features are now clearly indicated, and captions have been enhanced to facilitate interpretation of the microstructural and mechanical data in the context of the discussion.
Author Response File:
Author Response.pdf
Reviewer 4 Report
Comments and Suggestions for Authors1 The manuscript's title and introduction highlight the "Arc-Enhanced Glow Discharge (AEGD)" aspect as a key feature. However, the results and discussion do not explicitly compare the findings with a standard PAN process (without AEGD) conducted under similar parameters (350°C, 1.5/3.5 h). The unique advantage of AEGD—presumably higher plasma density leading to more efficient nitriding at lower temperatures—is asserted but not directly demonstrated within the study. The authors should strengthen the discussion by more explicitly linking the observed results to the proposed mechanisms of the AEGD process. A dedicated paragraph in the discussion comparing the achieved layer thicknesses/hardness with literature values for conventional PAN at similar temperatures and times would solidify the novelty claim.
2 section 1, the introduction is comprehensive but could be more focused. The paragraph beginning "Thermochemical surface engineering processes..." (lines 48-72) is repeated verbatim. This duplication should be removed. The research gap is well-identified (limited studies on PAN of annealed M2 and AEGD-PAN), but the final sentence of the introduction could more sharply state the specific objectives of this study.
3 section 2, Table 2: The gas flow is listed as "N2:Ar:H2 flow (sccm)" with the value "50:278:25". Please clarify if this is a ratio or the actual flow rates in sccm. The total seems high (353 sccm); confirming this or providing the ratio would avoid confusion.
4 section3.6, the analysis of the wear mechanism is somewhat brief. The authors conclude that wear occurs "predominantly by a plowing mechanism" but could provide deeper insight. It would be valuable to include higher-magnification SEM images of the scratch tracks, particularly showing the track bottom and edges. This could help identify micro-fracture events, plastic deformation features, or oxidative wear debris, providing a more nuanced understanding of how the nitride layer fails progressively under repeated loading. Relating the specific nitride phases (ε-Fe₂₋₃N vs. γ'-Fe₄N) to their propensity for micro-cracking or plastic deformation would enhance the discussion.
Author Response
We are pleased to submit the revised version of our manuscript, entitled:
“AEGD-Assisted Plasma Nitriding of AISI M2 Steel: Influence of Treatment Time on Microstructure and Scratch Resistance”
We sincerely thank you and the reviewers for the constructive feedback, which has significantly improved the quality, clarity, and scientific rigor of our manuscript. We have carefully considered all comments and have revised the manuscript accordingly.
In particular, we have:
- Clarified the novelty and scientific contributions of the work.
- Improved the presentation and interpretation of microstructural and mechanical characterization data.
- Revised figures, tables, and captions for consistency and clarity.
- Corrected typographical errors and standardized terminology throughout the manuscript.
- Provided additional explanations where needed to strengthen the scientific reasoning and interpretation of results.
A detailed, point-by-point response to each reviewer comment has been prepared and is attached for your consideration. We believe that the revised manuscript now fully addresses the reviewers’ concerns and is suitable for publication in [Journal Name].
We greatly appreciate your time and consideration and look forward to your favorable evaluation.
Sincerely,
Juan Manuel González Carmona PhD
SECIHTI, Center of Engineering and Industrial Development, CIDESI,
Querétaro, Av. Pie de la Cuesta 702, CP 76125
México
Tel: +(52) 1 442 748 0070
REVIEWER 4
- 1 The manuscript's title and introduction highlight the "Arc-Enhanced Glow Discharge (AEGD)" aspect as a key feature. However, the results and discussion do not explicitly compare the findings with a standard PAN process (without AEGD) conducted under similar parameters (350°C, 1.5/3.5 h). The unique advantage of AEGD—presumably higher plasma density leading to more efficient nitriding at lower temperatures—is asserted but not directly demonstrated within the study. The authors should strengthen the discussion by more explicitly linking the observed results to the proposed mechanisms of the AEGD process. A dedicated paragraph in the discussion comparing the achieved layer thicknesses/hardness with literature values for conventional PAN at similar temperatures and times would solidify the novelty claim.
R// We thank the reviewer for highlighting the need to explicitly link the observed results to the mechanisms of AEGD. A dedicated paragraph has been added in the Discussion, comparing the achieved diffusion layer thickness and surface hardness with literature values for conventional PAN under similar conditions (350 °C, 1.5–3.5 h). The revised text clarifies that the enhanced performance observed in AEGD-PAN—higher nitrogen incorporation and thicker diffusion layers at comparable or lower surface hardness—is attributable to the higher plasma density, increased ion energy, and more effective surface activation provided by the AEGD process. This comparison strengthens the novelty claim by demonstrating the mechanistic advantage of AEGD in short-time, low-temperature nitriding.
- 2 section 1, the introduction is comprehensive but could be more focused. The paragraph beginning "Thermochemical surface engineering processes..." (lines 48-72) is repeated verbatim. This duplication should be removed. The research gap is well-identified (limited studies on PAN of annealed M2 and AEGD-PAN), but the final sentence of the introduction could more sharply state the specific objectives of this study.
R// We thank the reviewer for pointing out the duplicated paragraph. The repeated text beginning “Thermochemical surface engineering processes…” has been removed. Furthermore, the final paragraph of the Introduction has been revised to sharpen the focus and explicitly state the specific objectives of this study: to evaluate the effect of AEGD-assisted plasma nitriding on the microstructure, diffusion layer growth, and mechanical performance of annealed AISI M2 steel under short-time, low-temperature treatments.
- 3 section 2, Table 2: The gas flow is listed as "N2:Ar:H2 flow (sccm)" with the value "50:278:25". Please clarify if this is a ratio or the actual flow rates in sccm. The total seems high (353 sccm); confirming this or providing the ratio would avoid confusion.
R// We appreciate the reviewer’s observation regarding gas flow rates. The values listed in Table 2 (50:278:25) correspond to the actual flow rates in sccm for N₂, Ar, and H₂, respectively. The total flow rate of 353 sccm is correct and has been clarified in the table caption to avoid ambiguity.
- 4 section3.6, the analysis of the wear mechanism is somewhat brief. The authors conclude that wear occurs "predominantly by a plowing mechanism" but could provide deeper insight. It would be valuable to include higher-magnification SEM images of the scratch tracks, particularly showing the track bottom and edges. This could help identify micro-fracture events, plastic deformation features, or oxidative wear debris, providing a more nuanced understanding of how the nitride layer fails progressively under repeated loading. Relating the specific nitride phases (ε-Fe₂₋₃N vs. γ'-Fe₄N) to their propensity for micro-cracking or plastic deformation would enhance the discussion.
R// We thank the reviewer for suggesting a more detailed analysis of the wear mechanisms. The discussion has been expanded to relate the observed wear features to plastic deformation, micro-cracking, and oxidative debris formation. Moreover, the analysis now explicitly links the wear behavior to the nitride phases present: ε-Fe₂₋₃N is associated with increased brittleness and micro-crack initiation, whereas γ′-Fe₄N exhibits higher plastic accommodation, explaining the progressive failure mechanisms of the nitrided layer under repeated loading.
Author Response File:
Author Response.pdf
Round 2
Reviewer 1 Report
Comments and Suggestions for AuthorsDear Authors,
Thank you for the revised version of the manuscript. Several technical issues still require clarification before the manuscript can be considered suitable for publication.
1. Crystallographic data (Figure 2):
The manuscript still lacks sufficient quantitative crystallographic information. Please provide a table listing the Miller indices (hkl) corresponding to the identified diffraction peaks for each phase, along with the calculated lattice parameters. The inclusion of these data is essential for a rigorous and verifiable discussion of phase identification and structural analysis.
2. Figure legibility:
High-resolution versions of Figures 1, 4, 5d, 5f, 6, and 9 are required. In the current submission, the magnification values and scale bars remain illegible, which prevents proper assessment and interpretation of the microstructural features.
These issues must be addressed to ensure the scientific clarity and robustness of the manuscript.
Author Response
- Crystallographic data (Figure 2):
The manuscript still lacks sufficient quantitative crystallographic information. Please provide a table listing the Miller indices (hkl) corresponding to the identified diffraction peaks for each phase, along with the calculated lattice parameters. The inclusion of these data is essential for a rigorous and verifiable discussion of phase identification and structural analysis.
Response// We appreciate the reviewer’s comment and fully agree on the importance of providing direct access to the crystallographic information obtained from the analysis. However, due to the large number of phases involved (α-Fe, ε-Fe₂–₃N, M₆C, γ′-Fe₄N, and MC) across four different conditions (with and without heat treatment, and nitriding times of 1.5 and 3.5 h), the resulting table becomes quite extensive.
While this information is valuable for validating the methodology, it does not substantially contribute to the discussion of the results. Therefore, we propose including it as Supplementary Material 1 (S1) and kindly request that it be incorporated into the article’s supplementary archive.
- Figure legibility:
High-resolution versions of Figures 1, 4, 5d, 5f, 6, and 9 are required. In the current submission, the magnification values and scale bars remain illegible, which prevents proper assessment and interpretation of the microstructural features.
Response// We thank the reviewer for this important observation. High-resolution versions of Figures 1, 4, 5d, 5f, 6, and 9 have been provided in the revised manuscript. The images have been replaced with versions of improved clarity, ensuring that magnification values and scale bars are clearly legible. These changes allow for proper assessment and interpretation of the microstructural features.
Author Response File:
Author Response.pdf
Reviewer 2 Report
Comments and Suggestions for AuthorsThere are a few more typos that need to be fixed prior to publications
Chemical formulas, such as N2, H2, M6C, Co3W3C, and others, need to be corrected in the manuscript.
Figures 3(a) and (b) – There are gray dashed lines in the figure that do not appear to be data.
Author Response
Response to Reviewer 2
Comment:
There are a few more typos that need to be fixed prior to publication.
Response:
We appreciate the reviewer’s observation. The manuscript has been thoroughly revised to correct typographical errors and improve overall consistency.
Comment:
Chemical formulas, such as N2, H2, M6C, Co3W3C, and others, need to be corrected in the manuscript.
Response:
Thank you for your observation. The chemical formulas throughout the manuscript have been carefully revised to ensure proper formatting and consistency. All species, including N₂, H₂, M₆C, Co₃W₃C, and others, are now presented using appropriate subscript notation in accordance with standard scientific conventions.
Comment:
Figures 3(a) and (b) – There are gray dashed lines in the figure that do not appear to be data.
Response:
We thank the reviewer for this valuable observation. The lines in question correspond to connectors between experimental data points in Figures 3a and 3b. We agree that the original use of solid lines could lead to misinterpretation as continuous data. Accordingly, Figure 3 has been revised by replacing these with dashed lines to clearly indicate that they represent trends between discrete experimental points rather than continuous datasets.
Author Response File:
Author Response.pdf
Reviewer 4 Report
Comments and Suggestions for AuthorsIt can be accepted.
Author Response
- It can be accepted.
Response// We appreciate the positive evaluation and the recommendation for acceptance. Thank you for your time and consideration.