Calcium/Phosphorus Ratio Changes in Demineralized Enamel and Dentin Adjacent to Ion-Releasing and Conventional Bulk-Fill Restorative Systems and Interfacial Micromorphology After Six Months in Artificial Saliva: An In Vitro SEM–EDX Study

,
,
and
1
Conservative Dentistry Department, Faculty of Dentistry, Mansoura University, Mansoura 35516, Egypt
2
College of Dentistry, Al-Farabi University, Baghdad P.O. Box 12083, Iraq
3
Specialized Medical Hospital, Mansoura University, Mansoura 35516, Egypt
4
Restorative Dentistry Department, Faculty of Oral and Dental Medicine, Alsalam University, Tanta 31511, Egypt

Abstract

Background: Recurrent demineralization at restoration margins threatens the longevity of Class I restorations, and restorative materials marketed as ion-releasing or “bioactive” are proposed to modify the mineral status of the adjacent tooth tissue. Objective: Our objective was to compare the calcium-to-phosphorus (Ca/P) weight ratio of demineralized enamel and dentin adjacent to three ion-releasing restorative systems and one conventional bulk-fill composite after six months of storage in artificial saliva, using energy-dispersive X-ray spectroscopy (EDX), and to describe the tooth–restoration interface by scanning electron microscopy (SEM). Methods: Standardized Class I cavities (3 mm × 3 mm × 2 mm) were prepared in 40 sound human molars, which were randomly allocated to four groups (n = 10): Beautifil-Bulk, Predicta® Bioactive Bulk, Stela self-cure composite, and Tetric® N-Power Fill 2 (reference comparator). Each tooth was sectioned from a region close to the prepared cavity to obtain two ≈2 mm slices: one served as the sound baseline reference, and the other one was obtained after tooth demineralization (acetic acid, pH 4.5, 7 days), analyzed by EDX, restored, and stored for six months in artificial saliva containing calcium and phosphate, and each specimen was re-sectioned for EDX (Ca/P at 50 µm from the interface) and SEM (interfacial gap width). Between-group differences at each stage and in per-tooth change scores were analyzed with Welch’s ANOVA and Games–Howell tests, and within-tooth changes were analyzed from the linked per-tooth measurements with paired tests (Holm-adjusted); gap widths were measured on representative micrographs and reported descriptively. Results: Ca/P ratios did not differ among groups at baseline (enamel p = 0.195; dentin p = 0.915) or after demineralization (p = 0.472 and p = 0.773). After storage, enamel Ca/P differed among groups (p < 0.001); recovery from the demineralized state was greater adjacent to Predicta® (+0.57 ± 0.18) than adjacent to Stela (+0.24 ± 0.08), Beautifil-Bulk (+0.11 ± 0.18), and Tetric® N-Power Fill 2 (+0.07 ± 0.27) (p ≤ 0.001). In dentin, post-storage Ca/P differed only between Predicta® and Tetric® N-Power Fill 2 (p = 0.006), and recovery did not differ significantly among groups (p = 0.235). On representative SEM micrographs, interfacial gaps were narrowest for Stela (no enamel gap; dentin 6.21 µm) and widest for Predicta® (enamel 11.18 µm; dentin 16.84 µm). Conclusions: Under static storage in mineral-containing artificial saliva, enamel adjacent to Predicta® showed the greatest recovery of the Ca/P ratio, whereas differences in dentin were small. On representative SEM micrographs, Stela showed the closest interfacial adaptation and Predicta® the widest gaps, with wider gaps at dentin than at enamel margins in all systems. Because ion release was not measured, no unrestored control was included, and the storage medium itself supplied calcium and phosphate, these findings describe Ca/P changes at the interface and should not be interpreted as direct evidence of material-driven ion release or of a clinical anticaries benefit.

1. Introduction

Modern restorative materials combine high clinical effectiveness and durability, and material development has gradually shifted from merely restoring lost mechanical function toward incorporating bioactive properties, so that restorations are increasingly designed to interact favorably with the surrounding biological environment [1,2].
Bioactive functioning includes both protective and promotive biological properties. The bioprotective role involves limiting bacterial infection and strengthening the dental substrate [2], whereas biopromotive activity supports remineralization [3], regulates inflammatory processes [4,5], and activates cellular mechanisms accompanied by tissue repair and regeneration [6,7]. Collectively, these biological effects represent a major shift in restorative dentistry, from extensive and invasive elimination of dental tissues toward conservative and minimally invasive techniques focused on preserving healthy tooth structure [8].
Remineralization restores both the mineral composition and structural integrity of dental structures, thereby counteracting demineralization [9]. Despite advancements in restorative dentistry, there is currently no restorative material that effectively combines lasting remineralization with strong antibacterial properties [10]. Resin composites are commonly employed as direct restoratives owing to their optical and mechanical characteristics [11]. The absence of inherent remineralization properties, combined with the deterioration of the bonding interface, could cause resin composite restorations to fail [12].
Compared with resin-based composites, glass-ionomer cement appears to offer a superior capacity to facilitate the repair of lesions. It is considered a bioactive substance that releases fluoride and bonds to dental structures through ion exchange [13]. However, the deterioration of these properties over time has led to further material development [14,15]. Consequently, researchers have developed innovative bioactive materials for caries management, which should be capable of releasing various ions, including fluoride, calcium, and phosphate (F−, Ca2+, and PO43−), along with additional active compounds that prevent biofilm formation, promote hydroxyapatite growth, or activate odontoblasts to encourage mineral deposition [16]. Their hydrophilic nature promotes interaction with saliva and other oral fluids, enabling ionic exchange and allowing the material to release and subsequently recharge its constituent ions in response to variations in pH [13,17].
New dental materials have been developed to reduce biofilm activity, prevent the demineralization of adjacent tissues, and promote the remineralization of previously carious regions [18,19]. Giomer, a “hybrid composite” that combines characteristics of resin composite and glass-ionomer cement, is produced by incorporating pre-reacted glass-ionomer filler particles in a resin matrix [17,20,21]. Further ion-releasing materials have since been introduced, such as Predicta® Bioactive (Parkell, Edgewood, NY, USA), a dual-cure resin composite claimed to release and recharge F−, Ca2+, and PO43− ions [22], and Stela (SDI, Victoria, Australia), a self-curing resin-based composite whose fillers include fluoroaluminosilicate glass and ytterbium fluoride [23]. Both are reported to counteract biofilm acids and create a more alkaline environment [24], and the gradual release of phosphate, calcium, and fluoride ions may help protect against demineralization at the tooth–restoration interface [25,26].
In this study, the term “bioactive” is used with the caution recommended by the FDI World Dental Federation, which advises that a bioactivity claim for a restorative material be substantiated by evidence of a specific beneficial effect on the adjacent tissues and that ion release or mineral deposition demonstrated in vitro does not, by itself, establish bioactivity [1]. Accordingly, the three test materials are classified here by composition and by the manufacturers’ claims rather than by an established biological effect: Beautifil-Bulk is a giomer whose surface pre-reacted glass-ionomer (S-PRG) filler releases fluoride, strontium, sodium, aluminum, borate, and silicate ions [17,20,21]; Predicta® Bioactive Bulk is a dual-cure composite designated by its manufacturer as bioactive and claimed to release and recharge calcium, phosphate, and fluoride ions [22]; and Stela is a self-cure composite containing fluoroaluminosilicate glass and ytterbium fluoride [23], for which ion release is claimed by the manufacturer but has not, to our knowledge, been independently quantified. These three are hereafter referred to as ion-releasing restorative materials. Tetric® N-Power Fill 2, a conventional light-cured nanohybrid bulk-fill composite without a claimed remineralizing mechanism [27], was included as a reference comparator; because it contains ytterbium fluoride and was bonded with an adhesive, it is not regarded as an inert negative control.
Changes in the mineral composition of tooth tissue can be characterized by energy-dispersive X-ray (EDX) spectroscopy [28], a technique that provides elemental analysis of the examined surface [29]. In the present research, EDX was used to determine the calcium and phosphorus contents, expressed as the Ca/P weight ratio, of enamel and dentin adjacent to the restorations [28]; it characterizes the tissue and does not quantify the ions released by the materials. The same combined EDX–SEM approach has been used to study the interface between ion-releasing restorations and tooth tissue. Raghip et al. found that an ion-releasing restorative material released significantly more calcium into demineralized dentin than a conventional bulk-fill composite and formed a thicker remineralized interfacial zone [30], and Sarhan et al. reported that the calcium and phosphorus contents at the interfaces of a giomer, an ion-releasing composite, and a resin-modified glass ionomer differed among materials and changed over 6 months of storage [31]; comparable EDX analyses of the Ca/P ratio of dentin adjacent to ion-releasing materials have been reported in other models [32,33]. None of these studies, however, examined the materials tested here or analyzed enamel and dentin separately. SEM micromorphological analysis was also performed to examine the stability and integrity of the tooth–restoration interface [34]. Interfacial failure can produce marginal gaps, permitting microorganisms, toxins, and food debris to penetrate through these microgaps [35].
Evidence remains limited regarding the comparative behavior of different restorative systems at the tooth–restoration interface [25]. Thus, the objective of the present research was to compare the Ca/P ratios of demineralized enamel and dentin adjacent to three ion-releasing restorative materials and a conventional bulk-fill composite after six months of storage in artificial saliva, and to describe the corresponding interfacial micromorphology. The following null hypotheses were tested: (H01) after six months of storage, there would be no differences among the four restorative systems in the Ca/P ratio of the adjacent demineralized enamel, or in its recovery from the demineralized state; and (H02) there would be no such differences in the adjacent demineralized dentin. In addition, interfacial gap width at the enamel and dentin margins was described by SEM on representative specimens; this component is descriptive, and no group-level hypothesis was tested.
This study evaluated Ca/P changes and interfacial micromorphological integrity over an extended 6-month in vitro period. The design uses a within-tooth reference: from each tooth, one slice sectioned before demineralization served as the sound baseline reference, and a second slice from the same tooth was analyzed after demineralization and again after restoration and storage. Finally, enamel and dentin at the interface were analyzed separately, and the Ca/P findings obtained by EDX were considered alongside the interfacial adaptation observed by scanning electron microscopy (SEM).

2. Materials and Methods

2.1. Materials

The research utilized four restorative materials: Beautifil-Bulk (Shofu Inc., Kyoto, Japan), Predicta® Bioactive Bulk dual-cure composite (Parkell, Edgewood, NY, USA), Stela self-cure composite (SDI, Bayswater, VIC, Australia), and Tetric® N-Power Fill 2 Bulk (Ivoclar Vivadent, Schaan, Liechtenstein). A universal adhesive (All-Bond Universal; Bisco, Inc., Schaumburg, IL, USA) was used in self-etch mode for the Beautifil-Bulk, Predicta®, and Tetric® N-Power Fill 2 groups, whereas Stela was used with its dedicated self-cure primer (Stela Primer, SDI), as instructed by its manufacturer. Each group therefore represents a restorative system (bonding agent plus restorative material) applied according to the respective manufacturer’s instructions, and interfacial outcomes are attributed to the system rather than to the restorative material alone. The materials are detailed in Table 1.
Table 1. Materials employed in this research.

2.2. Methods

2.2.1. Sample Size Calculation

The sample size was estimated from the differences between bioactive and conventional restorative materials reported by Kasraei et al. [24]. An a priori power analysis (G*Power, version 3.1.9.6; Heinrich Heine University, Düsseldorf, Germany) [36] for a two-tailed comparison of two independent means, with an anticipated effect size of d = 2.08, α = 0.05, and power = 0.95, indicated a minimum of 8 specimens per group. This was increased to 10 specimens per group (N = 40) to accommodate the four-group design and multiple pairwise comparisons: with n = 10, the power to detect d = 2.08 remains 0.94 at a Bonferroni-adjusted α of 0.0083 (six pairwise comparisons). A sensitivity analysis for the omnibus four-group comparison (one-way ANOVA, N = 40, α = 0.05) showed that the design could detect effects of Cohen’s f ≥ 0.55 with 80% power and f ≥ 0.69 with 95% power; smaller between-group differences may therefore have remained undetected.

2.2.2. Ethical Approval and Teeth Selection

Ethical approval for the present research was granted by the Ethics Committee of the Faculty of Dentistry, Mansoura University (protocol No. M0202025CD).
Forty freshly extracted, intact molars were obtained from the Oral and Maxillofacial Surgery Clinic, Faculty of Dentistry, Mansoura University, from patients aged 50–60 years with periodontal disease. Teeth exhibiting restorations, cracks, fractures, caries, or abrasion were excluded, and informed consent was secured for their use in the study. Following extraction, residual soft tissues and calculus were removed with a hand scaler (Zeffiro; Lascod, Florence, Italy). The teeth were disinfected in 0.5% chloramine at 4 °C and subsequently kept in distilled water at 37 °C in an incubator (BTC, Model: BT1020, Cairo, Egypt) until use. All specimens were used within 3 months after extraction [37].

2.2.3. Teeth Mounting and Preparation Procedures

Polyvinyl chloride cylinders were employed as molds to produce blocks of self-curing acrylic resin (Acrostone, Egypt), with the teeth positioned within the resin such that the resulting acrylic blocks extended approximately 1 mm beyond the cementum–enamel junction. Standardized Class I cavities measuring 3 mm × 3 mm × 2 mm were subsequently formulated utilizing a straight carbide bur mounted on a high-speed handpiece (Sirona T4, Bensheim, Germany), under continuous air–water irrigation. Cavity preparation was standardized using a specially fabricated cavity preparation machine developed by the Department of Mechanical Design and Production Engineering, Faculty of Engineering, Mansoura University [38]. After every five cavity preparations, the bur was replaced with a new one. To achieve a standardized smear layer, the cavity floor and axial surfaces were gently finished with a small piece of 600-grit silicon carbide abrasive paper in a circular movement with continuous water irrigation for 60 s [39,40]. After cavity preparation, digital periapical radiographs were obtained to assess the remaining dentin thickness. A minimum thickness of 1.0 mm between the floor of the cavity and the pulp chamber was considered adequate [41]. Teeth with pulp exposure were omitted.

2.2.4. Specimen Preparation and Study Workflow

The study design is shown in Figure 1, and the sequence of procedures is summarized in Figure 2. After cavity preparation, each tooth was sectioned longitudinally along its long axis from a region close to the prepared cavity with a low-speed diamond saw (Isomet 1000; Buehler, Lake Bluff, IL, USA) under continuous water cooling, yielding two standardized slices approximately 2 mm thick, each slice containing a portion of the enamel and dentin walls. The two slices from the same tooth were used as follows: (i) Slice 1 (sound reference) was not demineralized and was analyzed by EDX to obtain the baseline Ca/P ratio of the sound enamel and dentin of that tooth; (ii) Slice 2 (experimental slice) was subjected to artificial demineralization for 7 days, analyzed by EDX to obtain the post-demineralization Ca/P ratio. After restoration and storage in artificial saliva for six months, each specimen was sectioned again into two pieces: one was analyzed by EDX (post-storage Ca/P ratio) and the other was examined by SEM (interfacial micromorphology). Thus, each tooth contributed one baseline, one post-demineralization, and one post-storage Ca/P measurement for each tissue, as well as one SEM specimen. The sound slice served only as a within-tooth baseline reference; no separate unrestored control specimens were stored (see Section 6). The cut surfaces intended for EDX and SEM were manually ground with 600-, 1000-, 1200-, and 2000-grit SiC abrasive papers (Microcut™, Buehler, Lake Bluff, IL, USA) under water lubrication and polished with a polishing cloth and diamond pastes with particle sizes of 6 μm, 4 μm, and 1 μm, respectively (Diamat, Pace Technologies, Tucson, AZ, USA) [42]. Finally, the specimens were immersed in a digital ultrasonic cleaner (Guilin Woodpecker, Guilin, China) for 5 min to remove any remaining debris.
Figure 1. Study design. From each tooth, a sound slice (baseline reference) and an experimental slice were obtained; the experimental slice was analyzed by EDX after demineralization. After restoration and six months of storage in artificial saliva, each specimen was sectioned again into two pieces: one was analyzed by EDX, and the interface of the other one was examined by SEM.
Figure 2. Specimen preparation workflow: (1) mounting in acrylic resin; (2) standardized cavity preparation; (3) protection of the external surfaces with inlay wax; (4) sectioning of each tooth from a region close to the prepared cavity into two slices; (5) Slice 1, sound baseline reference; (6) Slice 2, was obtained after demineralization of specimens in acetic acid buffer (pH 4.5, 7 days); (7) creation of a standardized smear layer; (8) EDX analysis of Slices 1, 2; (9) restoration and six-month storage in artificial saliva; (10,11) re-sectioning of specimens into two pieces for EDX and SEM.

2.2.5. Artificial Demineralization of Samples

To protect the surrounding dental tissues from demineralization, all surfaces of the specimens were covered with an acid-resistant inlay wax, while the cavity areas were left uncovered [43]. With the exception of Slice 1 (sound reference), the cavity surfaces of each specimen were subjected to demineralization. Each specimen was submerged in a glass container comprising 40 mL of demineralizing solution (1.5 mM CaCl2, 0.9 mM KH2PO4, 50 mM acetic acid, and 0.02% NaN3; pH 4.5, adjusted with NaOH) and maintained at 37 °C for 7 days to promote demineralization [44]. This solution was manufactured in the Pharmaceutics Department, Faculty of Pharmacy, Mansoura University. The same demineralizing solution was stored in a refrigerator at 4 °C and renewed every 24 h to preserve a constant pH and ensure the ion-exchange process. The pH was regularly measured with a pH meter (STARTER 2100, Parsippany, NJ, USA). Afterward, the demineralized specimens were removed, and the acid-resistant inlay wax was carefully eliminated with a wax knife. The specimens were washed and stored in deionized purified water (Direct-Q UV; Molsheim, France) at 25 °C until use. Before restoration, specimens were manually polished with 600-grit silicon carbide paper (Fuji Star, Okegawa, Saitama, Japan) under running water for 30 s to establish a standardized smear layer. These procedures were performed by the same operator [30]. These procedures are presented in Figure 2.

2.2.6. Restorative Procedures

The specimens were randomly allocated into four equal groups (n = 10) according to the restorative material: Group R1 was restored with Beautifil-Bulk; Group R2 with Tetric® N-Power Fill 2 Bulk; Group R3 with Predicta® Bulk; and Group R4 with Stela Capsules (self-cure). To reduce operator-related variation and ensure procedural consistency, all restorative treatments were carried out by the same operator [45].
The universal adhesive (All-Bond Universal) was applied to the Beautifil-Bulk, Predicta®, and Tetric® N-Power Fill 2 specimens in two distinct coats, scrubbing for 10–15 s with each coat in self-etch mode, using a micro-brush. After adhesive application, the adhesive was gently air-dried for at least 10 s to facilitate solvent evaporation, ensuring that no visible adhesive movement remained. The adhesive was then light-cured for 10 s following the manufacturer’s recommendations, using a light-emitting diode curing unit (1200 mW/cm2; Bluephase 20i, Ivoclar Vivadent, Schaan, Liechtenstein). A standardized 1 mm curing distance was maintained, an orange light shield was used, and the light intensity was regularly assessed using a dental radiometer. Each restorative material was placed in a single increment to fill the cavity completely and was subsequently cured according to the manufacturer’s instructions. A gold-plated composite instrument (Sedra Dent, Cairo, Egypt) was used to insert the restorative materials into the prepared cavities. Transparent celluloid strips (TOR VM Ltd., Moscow, Russia) were then placed over the complete occlusal surfaces to ensure proper adaptation. The restorations were subsequently shaped and finished with a tungsten carbide bur (Okodent, Tautenhain, Germany), followed by sequential polishing with medium-, fine-, and extra-fine-grit Sof-Lex™ discs (3M ESPE, St. Paul, MN, USA).
For Beautifil-Bulk and Tetric® N-Power Fill 2 bulk restorative materials: The light-activated ingredients were placed into the cavity until it was somewhat overfilled. Then, excess material was eliminated. Finally, the material was irradiated for twenty seconds from each side (according to the manufacturer’s recommendation).
Predicta® Bulk Restorative is supplied in fine-needle automix tips with a bendable 19-gauge metal cannula to ensure an even mix of base and catalyst; it was introduced directly into the cavity. Each specimen was left undisturbed for 5 min to allow self-cure setting, followed by visible-light curing for 20 s per side with a dental curing unit according to the manufacturer’s guidelines. The light-curing intensity was verified, and the tip-to-specimen distance was standardized across all specimens and experimental groups.
For the Stela Capsules (Chemically cured composite), the Stela Primer was first distributed over the specimen surfaces and margins, left undisturbed for 5 s to dwell, and then gently air-dried for 2–3 s. The Stela capsule was activated by pressing the plunger, then mechanically mixed for 10 s utilizing an Ultramat 2 (SDI). The activated capsule was subsequently positioned in the SDI applicator, and the trigger was pressed until the material appeared at the transparent nozzle. The composite was then dispensed in one increment, with a slight overextension beyond the cavity and marginal boundaries, followed by careful anatomical contouring. Material at the margins was not removed until the setting was complete. The restoration was left undisturbed for 4 min after mixing to allow polymerization; the restoration procedure was subsequently completed, followed by final polishing to achieve a smooth surface.

2.2.7. Storage in Artificial Saliva

After the restoration procedure was completed, the specimens were immersed in 40 mL of artificial saliva and incubated at 37 ± 1 °C in an incubator (BTC, Model: BT1020, Cairo, Egypt) for 6 months [30]. The artificial saliva was formulated following the method of McKnight-Hanes and Whitford, with sorbitol excluded from the original formulation [46]. Its chemical composition was: sodium carboxymethyl cellulose (10 g/L), methyl-p-hydroxybenzoate (2 g/L), MgCl2·6H2O (0.059 g/L), CaCl2·2H2O (0.166 g/L), KH2PO4 (0.326 g/L), K2HPO4 (0.804 g/L), and KCl (0.625 g/L). The prepared solution was brought to pH 7, and the artificial saliva was renewed every week to ensure consistent pH conditions throughout the storage period. The storage medium therefore contained approximately 1.1 mM calcium and 7.0 mM total phosphate and constituted an external source of mineral ions common to all groups; its implications for interpretation are addressed in Section 4 and Section 6.

2.2.8. Elemental Analysis (EDX)

Elemental analysis was performed on uncoated specimens with an energy-dispersive X-ray spectrometer (X-Max 20; Oxford Instruments, High Wycombe, UK) coupled to a field-emission scanning electron microscope operated under high vacuum at an accelerating voltage of 30 kV, a working distance of 10–15 mm, and magnifications of ×1000 to ×2000. For adequate dehydration, the specimens were removed from distilled water 24 h before the EDX measurements. No gold sputter-coating was performed before EDX analysis to avoid interference with elemental determination. Elemental measurements were obtained, separately in enamel and dentin, from areas located 50 µm from the tooth–restoration interface (or, for Slice 1 and for Slice 2 before restoration, 50 µm from the corresponding cavity wall) [31,47]. Calcium and phosphorus contents were obtained as weight percentages by standardless quantification, and the Ca/P weight ratio was calculated. Standardless EDX quantification is semi-quantitative: its accuracy for major elements is influenced by surface topography, specimen charging, and matrix (ZAF) corrections [48]. The Ca/P ratio was therefore interpreted comparatively between groups and stages acquired under identical conditions, rather than as an absolute stoichiometric value.

2.2.9. Micromorphological Analysis

For micromorphological analysis, each specimen underwent an acid–base challenge following a standardized preparation protocol. The specimens were first treated with 10% orthophosphoric acid for 5 s to demineralize the dentin surface and expose the collagen matrix, followed by a 10 s rinse with water. The samples were subsequently immersed in 5% sodium hypochlorite for 5 min to remove remaining organic constituents [49]. After dehydration, the specimens were mounted on aluminum stubs and gold sputter-coated (SPI Module Sputter Carbon/Gold Coater; EDEN Instruments, Japan). The tooth–restoration interfaces were then examined with a field-emission scanning electron microscope (Quanta FEG 250; FEI Company, Hillsboro, OR, USA) using the backscattered-electron detector at 30 kV, a working distance of 10.9–15.0 mm, and a magnification of ×2000 [50].
Interfacial gap width (µm) was measured on the calibrated digital ×2000 micrographs as the distance between the restoration and the opposing cavity wall. For each restorative system, one representative micrograph of the enamel portion and one of the dentin portion of the interface were measured at three points along the gap; the measurement lines and values are displayed on the micrographs (in Section 3.4). Where no gap was visible (Stela, enamel), the gap width was recorded as 0 µm. Values are reported as the mean ± SD of the three measurements. Because they derive from a single micrograph per group and interface, they describe the representative specimen rather than the group, and no inferential comparison between groups was performed. Blinding of the examiner to group allocation was not documented. In addition, the acid–base challenge, dehydration, and high-vacuum conditions required for SEM can create or widen interfacial gaps and produce cracks in enamel and dentin [51]. The gap data are therefore regarded as semi-quantitative and are interpreted descriptively together with the micrographs.

2.2.10. Statistical Analysis

Ca/P ratios are presented as mean ± standard deviation (SD) for n = 10 teeth per group. The tooth was the unit of analysis, and the three Ca/P measurements of each tooth (baseline, after demineralization, after storage) were linked by tooth identity. Normality was examined with the Shapiro–Wilk test; because one of the 24 group–stage cells deviated from normality (enamel, Stela, after demineralization; Shapiro–Wilk p = 0.014) and group SDs differed by up to 3.6-fold, procedures that do not assume equal variances were used for between-group comparisons; with balanced groups of n = 10, these procedures are reasonably robust to moderate departures from normality [52]. (1) Between-group comparisons at each stage (baseline, after demineralization, and after storage) were performed with Welch’s ANOVA [53] followed by the Games–Howell post hoc test [54]; eta-squared (η2) is reported as the effect size. (2) The three Ca/P measurements of a tooth were obtained on different section planes (Slice 1, the surface of Slice 2 before restoration, and a new cut plane of Slice 2 after storage) and are therefore not repeated measurements of the same site, but they come from the same tooth and were not assumed to be independent. Within-group differences between stages were therefore estimated from the linked per-tooth differences as mean differences with 95% confidence intervals (CI, t distribution with 9 degrees of freedom) and paired t-tests, with Holm’s correction for the three comparisons within each group [55]; Wilcoxon signed-rank tests with the same correction were run as a sensitivity check, and Pearson’s r was used to describe the correlation between stages, pooled across all 40 teeth within each tissue. (3) Three per-tooth change scores were calculated: demineralization loss (ΔDemin = after demineralization − baseline), recovery during storage (ΔRecovery = after storage − after demineralization; primary outcome), and net change relative to sound tissue (ΔNet = after storage − baseline). Their means and SDs were calculated from the per-tooth values, and they were compared among groups with Welch’s ANOVA and Games–Howell tests. Because a change score does not by itself remove the influence of the starting value [56], two sensitivity analyses were added: post-storage Ca/P was analyzed by ANCOVA with group as the factor and the post-demineralization and baseline values as covariates (reported as F(3, 34): three numerator degrees of freedom for the four groups and 34 residual degrees of freedom, i.e., 40 teeth minus six estimated parameters—the intercept, three group terms, and two covariates), and all three stages were modelled together with a generalized estimating equation (exchangeable working correlation, tooth as the cluster, and robust standard errors) including a group × stage interaction. Percentage recovery [ΔRecovery/|ΔDemin| × 100] is reported descriptively. (4) Because the interfacial gap widths were obtained from a single representative micrograph per group and interface (three measurement points each), they were summarized descriptively and were not tested statistically, as doing so would have treated measurement points within one specimen as independent observations. All tests were two-sided, with significance set at p ≤ 0.05. Analyses were performed in Python 3.13 with SciPy 1.18, statsmodels 0.15, and pingouin 0.7; the per-tooth data (Supplementary File S1) and the analysis script (Supplementary File S2) are provided as Supplementary Materials.

3. Results

3.1. Enamel Ca/P Ratio

The enamel Ca/P ratios of the four groups at each stage are presented in Table 2 and Figure 3. The groups did not differ significantly at baseline (Welch’s F(3, 19.7) = 1.72, p = 0.195, η2 = 0.10) or after demineralization (F(3, 19.6) = 0.87, p = 0.472, η2 = 0.06). Demineralization reduced the enamel Ca/P ratio significantly in all groups (mean differences −0.31 to −0.49; Holm-adjusted p ≤ 0.021).
Table 2. Enamel Ca/P weight ratio (mean ± SD, n = 10) adjacent to the four restorative systems at each stage.
Figure 3. Enamel Ca/P weight ratio (mean ± SD, n = 10) adjacent to the four restorative systems at each stage. Uppercase letters compare groups within a stage (Games–Howell test); lowercase italic letters compare stages within a group (paired t-test with Holm correction). Bars sharing a letter do not differ significantly (p > 0.05).
After six months of storage, the groups differed significantly (F(3, 19.3) = 13.62, p < 0.001, η2 = 0.60). The enamel adjacent to Predicta® showed the highest Ca/P ratio (2.36 ± 0.16), which was significantly higher than that adjacent to Stela (2.10 ± 0.09; p = 0.003), Beautifil-Bulk (1.99 ± 0.14; p < 0.001), and Tetric® N-Power Fill 2 (1.92 ± 0.17; p < 0.001). Stela was significantly higher than Tetric® N-Power Fill 2 (p = 0.046) but did not differ from Beautifil-Bulk (p = 0.200), and Beautifil-Bulk did not differ from Tetric® N-Power Fill 2 (p = 0.749).
Within teeth, the post-storage Ca/P ratio was significantly higher than the post-demineralization value in the Predicta® (+0.57; 95% CI 0.44 to 0.70; p < 0.001) and Stela (+0.24; 95% CI 0.18 to 0.30; p < 0.001) groups and did not differ from baseline (p = 0.302 and p = 0.127, respectively). In the Beautifil-Bulk (+0.11; 95% CI −0.02 to 0.24; p = 0.089) and Tetric® N-Power Fill 2 (+0.07; 95% CI −0.12 to 0.26; p = 0.432) groups, the post-storage values did not differ significantly from the demineralized values and remained below baseline (p = 0.030 and p = 0.021, respectively).

3.2. Dentin Ca/P Ratio

The dentin Ca/P ratios are presented in Table 3 and Figure 4. No significant between-group differences were found at baseline (F(3, 19.3) = 0.17, p = 0.915, η2 = 0.02) or after demineralization (F(3, 18.0) = 0.37, p = 0.773, η2 = 0.03). After storage, a significant difference was detected (F(3, 18.6) = 6.43, p = 0.004, η2 = 0.29), which was confined to the comparison between Predicta® (2.15 ± 0.16) and Tetric® N-Power Fill 2 (1.92 ± 0.07; p = 0.006); Stela (2.05 ± 0.16) and Beautifil-Bulk (2.00 ± 0.14) did not differ from either material or from each other (p ≥ 0.139). Within teeth, the dentin Ca/P ratio decreased after demineralization in all groups, but no decrease remained significant after Holm correction (p ≥ 0.055; Predicta® −0.32, 95% CI −0.60 to −0.04, p = 0.056). It increased significantly during storage in the Predicta® (+0.35; 95% CI 0.15 to 0.55; p = 0.011) and Stela (+0.21; 95% CI 0.07 to 0.36; p = 0.029) groups, and not in the Beautifil-Bulk (+0.13; p = 0.281) and Tetric® N-Power Fill 2 (+0.12; p = 0.211) groups. No post-storage dentin value differed from its baseline (p ≥ 0.211). The large baseline variability of dentin (SD up to 0.37) limited the precision of these comparisons.
Table 3. Dentin Ca/P weight ratio (mean ± SD, n = 10) adjacent to the four restorative systems at each stage.
Figure 4. Dentin Ca/P weight ratio (mean ± SD, n = 10) adjacent to the four restorative systems at each stage. Letter conventions as in Figure 3.

3.3. Change Scores

The change scores, calculated from the per-tooth differences, are presented in Table 4. In enamel, the demineralization loss was comparable among groups (F(3, 19.4) = 2.07, p = 0.137), whereas recovery during storage differed significantly (F(3, 18.2) = 12.95, p < 0.001): ΔRecovery was greater for Predicta® (+0.57 ± 0.18) than for Stela (+0.24 ± 0.08; p = 0.001), Beautifil-Bulk (+0.11 ± 0.18; p < 0.001), and Tetric® N-Power Fill 2 (+0.07 ± 0.27; p = 0.001), with no significant differences among the latter three (p ≥ 0.221). The enamel net change relative to baseline also differed (F(3, 19.2) = 4.35, p = 0.017), being higher for Predicta® (+0.08 ± 0.23) than for Beautifil-Bulk (−0.24 ± 0.25; p = 0.039) and Tetric® N-Power Fill 2 (−0.25 ± 0.23; p = 0.023). In dentin, none of the change scores differed significantly among groups (Δ Demin, p = 0.848; Δ Recovery, p = 0.235; Δ Net, p = 0.457). The correlations between stages, pooled across all 40 teeth within each tissue, were weak and nonsignificant (|r| ≤ 0.20, all p ≥ 0.21); with 10 teeth per group, these pooled estimates are imprecise and do not exclude within-tooth dependence. In the sensitivity analyses, the group effect on post-storage Ca/P remained after adjustment for the post-demineralization and baseline values in enamel (ANCOVA, F(3, 34) = 17.18, p < 0.001) and in dentin (F(3, 34) = 4.63, p = 0.008), and the group × stage interaction in the cluster-robust model was significant in enamel (Wald χ2 = 51.6, 6 df, p < 0.001) but not in dentin (χ2 = 10.7, 6 df, p = 0.098). Wilcoxon signed-rank tests gave the same conclusions except for two borderline within-tooth comparisons (Stela dentin recovery and Tetric® N-Power Fill 2 enamel demineralization), which did not remain significant after Holm correction. Representative post-storage EDX spectra of enamel and dentin are shown in Figure 5 and Figure 6.
Table 4. Change scores of the Ca/P weight ratio (mean ± SD) by tissue and restorative system.
Figure 5. Representative EDX spectra of enamel 50 µm from the tooth–restoration interface after six months of storage: (a) Predicta®, (b) Stela, (c) Beautifil-Bulk, and (d) Tetric® N-Power Fill 2.
Figure 6. Representative EDX spectra of dentin 50 µm from the tooth–restoration interface after six months of storage: (a) Predicta®, (b) Stela, (c) Beautifil-Bulk, and (d) Tetric® N-Power Fill 2.

3.4. Interfacial Micromorphology and Gap Width

Representative micrographs are shown in Figure 7, Figure 8, Figure 9 and Figure 10, and the corresponding gap widths are shown in Table 5. In the representative micrographs, no gap was detected at the enamel margin of the Stela restoration (0.00 µm), whereas the enamel gaps measured 3.07 ± 0.51 µm for Tetric® N-Power Fill 2, 5.17 ± 1.84 µm for Beautifil-Bulk, and 11.18 ± 4.71 µm for Predicta®. At the dentin margin, the gaps measured 6.21 ± 3.34 µm for Stela, 13.45 ± 0.34 µm for Tetric® N-Power Fill 2, 14.49 ± 0.46 µm for Beautifil-Bulk, and 16.84 ± 1.16 µm for Predicta®. In every restorative system, the dentin gap was wider than the enamel gap. Because these values were obtained from one representative micrograph per group and interface, they are descriptive and were not compared statistically.
Table 5. Interfacial gap width (µm) at the enamel–restoration and dentin–restoration interfaces, measured on one representative micrograph per restorative system (mean ± SD of three measurement points).
Figure 7. Representative SEM micrographs (×2000) of the tooth–restoration interface in the Predicta® group. (A) Dentin–restoration interface showing a continuous interfacial gap (mean of three measurements, 16.84 ± 1.16 µm). (B) Enamel–restoration interface showing a wide, continuous marginal gap (mean of three measurements, 11.18 ± 4.71 µm); the crack visible in the enamel is consistent with a dehydration/high-vacuum preparation artifact, which cautions against interpreting gap width solely as a material property.
Figure 8. Representative SEM micrographs (×2000) of the tooth–restoration interface in the Stela group. (A) Dentin–restoration interface showing a localized interfacial gap (mean of three measurements, 6.21 ± 3.34 µm). (B) Enamel–restoration interface showing close adaptation, with no gap detectable at this magnification (0.00 µm).
Figure 9. Representative SEM micrographs (×2000) of the tooth–restoration interface in the Beautifil-Bulk group. (A) Dentin–restoration interface showing a continuous interfacial gap (mean of three measurements, 14.49 ± 0.46 µm). (B) Enamel–restoration interface showing an irregular marginal gap (mean of three measurements, 5.17 ± 1.84 µm).
Figure 10. Representative SEM micrographs (×2000) of the tooth–restoration interface in the Tetric® N-Power Fill 2 group. (A) Dentin–restoration interface showing a gap along the interface (mean of three measurements, 13.45 ± 0.34 µm). (B) Enamel–restoration interface showing a narrow linear gap (mean of three measurements, 3.07 ± 0.51 µm).

4. Discussion

The selection of a suitable restorative material for Class I cavities may be relevant to caries control, because ion-releasing materials are proposed to increase the local availability of calcium and phosphate ions and to buffer acidic challenges, which could favor remineralization and limit secondary caries [24,35]. These potential benefits, however, require direct demonstration.
The present investigation compared the Ca/P ratio of demineralized enamel and dentin adjacent to four restorative systems after six months in artificial saliva. It is important to state at the outset what this outcome represents. EDX characterizes the local elemental composition of the tooth tissue at a defined distance from the interface; it does not measure the quantity of ions released by a restorative material, which requires direct analysis of the storage medium (e.g., by ion chromatography, inductively coupled plasma spectrometry, or ion-selective electrodes) [57]. Furthermore, the Ca/P ratio describes the relative proportion of the two elements rather than the absolute mineral content: a tissue can retain a near-normal ratio while having lost mineral, and the ratio can increase through deposition of calcium-rich phases without recovery of mineral density [58]. The results are therefore interpreted as changes in the local Ca/P ratio adjacent to each restorative system, not as a ranking of the materials’ ion-releasing capacity.
Predicta® is described by its manufacturer as a bioactive material able to release and recharge ions and thereby promote hydroxyapatite formation; however, in an SEM–EDX study of the dentin–material interface, Kunert et al. observed no mineral precipitation on its surface and only sporadic precipitates on the adjacent dentin, and the interfacial seal present at 24 h deteriorated after 7–28 days [22]. Because it is not a self-adhesive material, it was used with an adhesive in self-etch mode, as recommended by the manufacturer; self-etch adhesives partially demineralize and modify the smear layer, allowing acidic monomers to infiltrate dentin and form a hybrid layer [59].
The adhesive strategy differed between groups: three materials were bonded with the same universal adhesive, whereas Stela was used with its proprietary self-cure primer (10-MDP and 4-methacryloxyethyl trimellitic anhydride), as required by its manufacturer. Interfacial adaptation, and possibly ion transport across the interface, therefore reflects the combined behavior of the bonding agent and the restorative material: a light-cured adhesive layer may act as a diffusion barrier, and self-cure primer–composite combinations differ in polymerization kinetics and stress development [60,61]. Differences between Stela and the other groups cannot be attributed to the restorative material alone.
Artificially demineralized teeth were used as a standardized substrate, because naturally carious lesions vary markedly in size, morphology, and depth [62,63,64,65]. Simple demineralization protocols, frequently using acetic acid, are among the most common methods for producing artificial lesions [66]; they are inexpensive, rapid, and reproducible and produce lesions approximating natural ones [67]. A smear layer was then created following Joves et al. [44].
Artificial saliva at 37 °C and pH 7 was used to simulate the oral environment during the six-month aging period [68,69]. However, a single static demineralization followed by static immersion does not reproduce the alternating acid challenges of the oral environment; pH-cycling models, which alternate demineralizing and remineralizing phases, more closely simulate the cariogenic challenge and would provide a more discriminating test of the protective potential of these materials [70].
This storage protocol has an important consequence. The artificial saliva contained approximately 1.1 mM calcium and 7.0 mM phosphate, renewed weekly for six months, and thus provided an external mineral source to all specimens; the Ca/P ratio increased numerically from the demineralized state in every group, including Tetric® N-Power Fill 2, which is consistent with a possible contribution from the medium. Without an unrestored control, or one restored with a non-ion-releasing material, stored under identical conditions, material-induced changes cannot be separated from mineral uptake from the saliva or from their interaction. The nonsignificant recovery adjacent to Tetric® N-Power Fill 2 (+0.07 in enamel; +0.12 in dentin) cannot be taken to show that the contribution of the artificial saliva was small: a nonsignificant change is not evidence of no change, particularly with 10 specimens per group, and Tetric® N-Power Fill 2 is a conventional comparator rather than an inert or unrestored control, since it contains ytterbium fluoride and was bonded with an adhesive. Whether the greater enamel recovery adjacent to Predicta® reflects the restorative system, the storage medium, or their interaction therefore cannot be determined from this design.
SEM–EDX was used because it evaluates elements directly at defined positions relative to the tooth–restoration interface [57,71] and reproducibly identifies the principal elements and their relative proportions [28], although standardless quantification is semi-quantitative [48].
The absolute Ca/P values should therefore be interpreted with caution. The weight ratio of stoichiometric hydroxyapatite is approximately 2.15, yet sound enamel yielded 2.17–2.28, and enamel adjacent to Predicta® reached 2.36 after storage. First, biological enamel is a calcium-deficient, carbonate-substituted apatite in which carbonate partially replaces phosphate, which raises the Ca/P ratio [72]. Second, standardless EDX on uncoated specimens can bias calcium and phosphorus estimates by several percent [48], an uncertainty similar to some of the observed differences. Third, calcium-rich non-apatitic deposits (e.g., calcium carbonate or calcium fluoride-like phases) and material debris near the interface cannot be excluded, because other elements were not quantified. The value of 2.36 should therefore not be read as “over-mineralization”; it did not differ significantly from baseline (2.28), and comparisons acquired under identical conditions are more informative than absolute ratios.
SEM is widely used to assess interfacial micromorphology in enamel and dentin [73]; the acid–base challenge removes non-infiltrated dentin and organic residues to reveal the hybrid-like layer [74,75], and gold sputter-coating prevents electrostatic charging [76]. However, the acid–base challenge, dehydration for high-vacuum observation, and sectioning can open or widen gaps and induce cracks, as seen in the enamel in Figure 7B [51]; gap widths obtained from such specimens are therefore semi-quantitative.
The first null hypothesis (H01), concerning enamel, was rejected: after storage, the enamel Ca/P ratio differed among the restorative systems (p < 0.001), as did its recovery from the demineralized state (p < 0.001). The second null hypothesis (H02), concerning dentin, was partially rejected: the post-storage dentin Ca/P ratio differed among the restorative systems (p = 0.004), whereas its recovery from the demineralized state did not (p = 0.235). The re-analysis showed no significant baseline differences among groups in either tissue (enamel p = 0.195; dentin p = 0.915), and recovery from the demineralized state, which is expressed relative to the post-demineralization level, was approximately 2.4- to 8-fold greater for Predicta® than for the other groups (+0.57 vs. +0.07 to +0.24); change scores alone, however, do not exclude an influence of the starting value (for example, regression toward the mean), so the finding is not claimed to be independent of it. In dentin, the post-storage Ca/P ratio adjacent to Predicta® (2.15 ± 0.16) exceeded only that adjacent to Tetric® N-Power Fill 2, and recovery did not differ significantly among groups; the dentin findings are therefore weaker and should be interpreted cautiously. A possible explanation for the enamel finding is the composition of Predicta®, which its manufacturer claims releases calcium, phosphate, and fluoride ions; in addition, the hydrophilic monomer HEMA may facilitate water uptake and ion exchange [77]. These mechanisms were not tested directly in the present study.
Predicta® contains titanium dioxide nanofiller, which may facilitate calcium phosphate formation [78,79]: at physiological pH, the negatively charged TiO2 surface attracts calcium ions, which then react with phosphate and carbonate to form a Ca–P-rich layer that can crystallize into hydroxyapatite [80,81], and nanoscale bioactive fillers show enhanced alkalizing and apatite-forming activity [82]. Predicta® has also been reported to release more calcium than other bulk-fill and glass-ionomer-based materials, favoring the supersaturation needed for apatite nucleation [83], and its phosphate release increases with time, possibly through hydrolytic degradation of bioactive glass promoted by hydrophilic monomers such as HEMA [24,84]; a higher phosphate glass content likewise increases apatite formation [85]. Conversely, Garoushi et al. reported negligible mineralization by an ion-releasing composite despite substantial calcium release [86].
An alternative, non-exclusive explanation must also be considered. Predicta® showed both the greatest enamel recovery and the widest gaps on the representative micrographs (11.18 µm in enamel; 16.84 µm in dentin). Wider gaps may allow more of the mineral-containing saliva to reach the demineralized tissue, independently of ion release, or may facilitate the outward diffusion of material-derived ions. Gap width alone does not explain the pattern—Stela had the narrowest gaps yet the second-highest enamel recovery, whereas Tetric® N-Power Fill 2, with wider gaps, showed the smallest recovery—but because gaps were measured on single representative specimens and could not be related to the Ca/P ratio at the specimen level, a contribution of saliva access cannot be excluded.
The Stela group showed the second-highest post-storage enamel Ca/P ratio (2.10 ± 0.09) and a significant recovery in both enamel (+0.24) and dentin (+0.21). Stela is a self-cure, ion-releasing composite used with a dedicated primer; it contains fluoroaluminosilicate glass and ytterbium fluoride [23]. Its reactive fillers and wettability may facilitate calcium and phosphate exchange with the surrounding medium [26,87], and its close adaptation, supported by its primer, which has been shown to enhance the polymerization of a self-cured composite [88], and slow self-cure polymerization, may have favored exchange with the adjacent tissue. Its lower recovery than Predicta® may reflect a less permeable, more hydrophobic resin matrix and different reactive fillers, as resin-based materials of similar composition (UDMA, GDMA, ytterbium fluoride) show low calcium and phosphate release [89].
The Beautifil-Bulk (giomer) group showed post-storage Ca/P ratios of 1.99 ± 0.14 in enamel and 2.00 ± 0.14 in dentin, with a small, non-significant recovery and enamel values that remained below baseline. Its surface pre-reacted glass-ionomer filler releases mainly sodium, strontium, aluminum, silicate, borate, and fluoride ions [17], so its calcium and phosphate supply is likely smaller than that of materials designed to release these ions [90], and its high filler loading (83.3 wt%) limits water sorption and ion exchange [91]. Glass-ionomer-based materials can supply calcium and phosphate when these ions are incorporated in their formulation [92], whereas giomers have shown only limited ion release [20,93]. In a demineralized-dentin model, Sajini et al. found no significant difference in the Ca/P ratio of dentin adjacent to a giomer, an ion-releasing composite, and a glass ionomer after 4 weeks [32], and Sarhan et al. found the lowest interfacial calcium content with a giomer, both after 24 h and after 6 months, among the three ion-releasing Class V restorations they compared [31]; both observations are consistent with the small recovery found adjacent to Beautifil-Bulk.
Tetric® N-Power Fill 2 showed the lowest post-storage Ca/P ratios (1.92 ± 0.17 in enamel; 1.92 ± 0.07 in dentin) and no significant recovery in either tissue, consistent with its formulation as a conventional bulk-fill composite without a claimed ion-releasing or pH-modulating mechanism [94]. Its ion release is considered negligible [95]; although it contains ytterbium fluoride, it is not designed to release calcium or phosphate, and its photocured, adhesively bonded resin matrix may further limit ionic exchange [96], as may the more complete polymerization achieved with β-allyl sulfone chain-transfer technology [97].
Taken together, the results indicate that, under static storage in a calcium- and phosphate-containing medium, the Ca/P ratio of demineralized enamel adjacent to Predicta® recovered to a greater extent than that adjacent to the other restorative systems, reaching values that did not differ significantly from baseline. Whether this reflects ions released by the material and diffusing across the adhesive interface, mineral uptake from the storage medium facilitated by interfacial gaps, or both, cannot be determined from the present design.
These findings can be compared with two earlier studies that used the same EDX–SEM approach at the tooth–restoration interface. Raghip et al. found that an ion-releasing restorative material (ACTIVA BioACTIVE-Restorative) released significantly more calcium into demineralized dentin than a conventional bulk-fill composite (Filtek One Bulk Fill) and formed a thicker remineralized interfacial zone [30]; likewise, in the present study, the conventional bulk-fill comparator, Tetric® N-Power Fill 2, showed the lowest post-storage Ca/P ratios and no significant recovery. Sarhan et al. compared a giomer, an ion-releasing composite, and a resin-modified glass ionomer in Class V cavities and found that the calcium and phosphorus contents at the interface differed among the materials and changed between 24 h and 6 months of storage, while SEM showed good adaptation of all three materials to the tooth [31]. Their conclusion that mineral exchange depends on both storage time and material composition agrees with the material-dependent recovery observed here. The present study extends these reports by testing four contemporary bulk-fill or ion-releasing systems that had not previously been compared, by using an artificially demineralized substrate, and by measuring enamel and dentin separately; unlike in Sarhan et al., who stored specimens in deionized water [31], it used a calcium- and phosphate-containing artificial saliva, which may itself have contributed to the recovery observed in all groups.
The tooth–restoration interface largely determines restoration longevity [35]: marginal gaps permit microleakage, which is associated with secondary caries and clinical failure [98], and bulk-fill and ion-releasing materials have been developed partly to improve adaptation and protect the interface [18,19,27].
Interfacial gap width was measured on a single representative micrograph per group and interface. Repeated measurements within one specimen are not independent replicates and cannot support a between-group statistical comparison [99,100]; this component of the study is therefore descriptive, and no group-level hypothesis conclusion is drawn from it. On the representative micrographs, no gap was detected at the enamel margin of the Stela restoration, whereas the enamel gap measured 11.18 µm with Predicta®, and the dentin gaps ranged from 6.21 µm (Stela) to 16.84 µm (Predicta®). Such differences are consistent with reports that interfacial gap formation depends on the viscosity, filler content, polymerization kinetics, and shrinkage stress of the restorative material [60,61,101,102,103]. The four representative micrographs differed in interfacial adaptation (Table 5). Stela showed the narrowest gaps, followed in ascending order of gap width by Tetric® N-Power Fill 2, Beautifil-Bulk, and Predicta®. Given the semi-quantitative nature of the gap measurements and the potential for preparation artifacts, and because each value derives from a single representative specimen, these differences are interpreted as differences in the pattern of adaptation rather than as estimates of group gap size, and they were not tested statistically.
In all representative micrographs, gaps were wider at the dentin margin than at the enamel margin, consistent with the less predictable bonding to dentin, particularly after demineralization [104], and with the greater susceptibility of the dentin–adhesive interface to dehydration shrinkage during SEM preparation [51].
Predicta®, a low-viscosity dual-cure bulk-fill material with comparatively low filler content, showed the widest gaps, consistent with the effect of polymerization shrinkage stress on marginal adaptation [101] and with the greater gap formation reported for low-viscosity bulk-fill composites [102]. Tetric® N-Power Fill 2 showed intermediate gaps, possibly because its pre-polymerized fillers act as stress-relieving “microscopic springs” with a lower elastic modulus (≈10 vs. ≈71 GPa for conventional glass fillers) [105,106] and because β-allyl sulfone produces a more controlled, step-growth-like polymerization [96,107]. Beautifil-Bulk showed moderate gaps, which may relate to its high filler content [87] and to hygroscopic swelling of giomer matrices [108]. Stela showed the narrowest gaps, likely owing to the slower polymerization and lower shrinkage stress of chemically activated composites [60], whose later gel point allows stress-relieving flow [61,103], together with its dedicated primer.

5. Conclusions

Within the limitations of this in vitro study, in which demineralized specimens were stored statically for six months in artificial saliva containing calcium and phosphate, we have the following: (1) the Ca/P weight ratio of demineralized enamel adjacent to Predicta® recovered to a greater extent than that adjacent to Stela, Beautifil-Bulk, and Tetric® N-Power Fill 2, reaching values that did not differ significantly from baseline, as did that adjacent to Stela; (2) in dentin, differences among the restorative systems were small, with a higher post-storage Ca/P ratio adjacent to Predicta® than adjacent to Tetric® N-Power Fill 2 but no significant differences in recovery; and (3) on the representative SEM micrographs, interfacial adaptation varied among the restorative systems: Stela showed close adaptation, with no detectable gap at the enamel margin and the narrowest gap at the dentin margin; Tetric® N-Power Fill 2 and Beautifil-Bulk showed intermediate gaps; and Predicta® showed the widest, continuous gaps at both margins. In every restorative system, the gap was wider at the dentin margin than at the enamel margin, and the system with the widest gaps (Predicta®) also showed the greatest enamel Ca/P recovery. Because ion release was not measured, no unrestored control was stored under identical conditions, interfacial gaps may have facilitated access of the mineral-containing medium, and the SEM observations are descriptive, derived from single representative specimens and potentially influenced by preparation artifacts, these findings describe Ca/P changes and interfacial adaptation at the tooth–restoration interface and do not establish material-driven ion release or remineralization. Their clinical relevance, including any benefit for patients at high caries risk, requires confirmation in pH-cycling, biofilm-based, and clinical studies.

6. Limitations and Recommendations for Future Research

This study has several limitations that directly affect the interpretation of its findings. First, and most importantly, no negative control was included: demineralized cavities left unrestored, or restored with a material with negligible ion release, were not stored under identical conditions. Because the artificial saliva contained calcium (≈1.1 mM) and phosphate (≈7.0 mM), the observed Ca/P changes cannot be partitioned between the effects of the restorative systems, mineral uptake from the storage medium, and their interaction. This control cannot be added retrospectively, and its absence is regarded as a major limitation.
Second, ion release from the restorative materials was not measured, and EDX characterizes only the elemental composition of the tissue at a single location 50 µm from the interface. The Ca/P ratio indicates the relative proportion of calcium and phosphorus rather than the absolute mineral content; transverse microradiography or micro-computed tomography, together with analysis of the storage medium, would be required to quantify mineral gain and its source [58]. Only calcium and phosphorus were quantified; other elements (F, Sr, Na, Cl, C, O, Mg) were not, and standardless EDX quantification is semi-quantitative.
Third, the groups differed not only in restorative material but also in bonding protocol (a universal adhesive in self-etch mode vs. a proprietary self-cure primer for Stela), so interfacial outcomes reflect the restorative system as a whole.
Fourth, the three Ca/P measurements of each tooth were obtained on different section planes rather than at the same site. They were analyzed as linked per-tooth observations; the correlations between stages, pooled across all 40 teeth within each tissue, were weak and nonsignificant, but they are imprecise and do not exclude within-tooth dependence. One group–stage cell (enamel, Stela, after demineralization) also deviated from normality, and group SDs differed by up to 3.6-fold. With 10 specimens per group, only large between-group effects (Cohen’s f ≥ 0.55 at 80% power) could be detected reliably, and several within-tooth comparisons in dentin were borderline.
Fifth, gap width was measured on a single representative micrograph per restorative system and interface (three measurement points each), so the values describe individual specimens and could not be compared statistically between groups; examiner blinding was not documented; and the acid–base challenge, dehydration, and high-vacuum conditions required for SEM may have created or widened gaps and produced cracks (Figure 7B). The gap data are therefore semi-quantitative and could not be related to the Ca/P ratio at the specimen level.
Finally, restorative materials were assessed under laboratory conditions. The dynamic conditions of the oral cavity, including salivary flow, plaque accumulation, oral hygiene practices, and dietary habits, may yield outcomes that diverge from those of the present study. A single static demineralization followed by static immersion does not simulate the cyclic cariogenic challenge represented by pH-cycling models [70], and artificially demineralized lesions differ from natural caries in structure and organic content [62,63,64,65]. In addition, a single demineralization period (7 days) was used, producing lesions of one severity; because baseline lesion characteristics influence subsequent de- and remineralization [109], the materials might behave differently in shallower or deeper lesions. Moreover, only a caries-like (acetic acid) challenge was simulated; erosive challenges, which cause surface softening and loss rather than subsurface lesions, were not assessed [110].
To overcome these limitations and expand on the present results, future studies should (i) include an unrestored demineralized control and a non-ion-releasing restorative control stored under identical conditions, and/or use a storage medium free of calcium and phosphate, to isolate the material-related effect; (ii) measure ion release directly in the storage medium (e.g., by inductively coupled plasma spectrometry or ion-selective electrodes) in parallel with tissue analysis; (iii) quantify mineral content by transverse microradiography or micro-computed tomography; (iv) extend interfacial elemental profiling beyond calcium and phosphorus (F, Sr, Na, Cl, C, O, Mg) using techniques such as wavelength-dispersive X-ray spectroscopy and X-ray photoelectron spectroscopy to elucidate chemical bonding states and ion-exchange dynamics within the hybrid layer; (v) employ pH-cycling and multispecies biofilm models and natural carious lesions; (vi) standardize bonding protocols or test each material with a common adhesive; (vii) measure interfacial gaps on all specimens, at predefined points, by a blinded examiner using non-destructive or low-vacuum imaging, such as environmental scanning electron microscopy, swept-source optical coherence tomography, or micro-computed tomography, to avoid dehydration artifacts; (viii) use several demineralization periods to produce lesions of different severity [109] and evaluate the materials under erosive challenges using established erosion models [110]; and (ix) conduct randomized controlled clinical trials with longitudinal follow-up to evaluate restoration longevity, the incidence of secondary caries, and clinical efficacy in relation to oral factors such as salivary flow, biofilm dynamics, diet, and oral hygiene.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/dj14120775/s1; Supplementary File S1: Per-tooth Ca/P weight ratios (baseline, after demineralization, and after six-month storage) of enamel and dentin for all 40 teeth; Supplementary File S2, the Python script used for all statistical analyses.

Author Contributions

Conceptualization and study design, M.H.A., N.M.Z., and H.A.E.-H.; methodology, M.H.A., M.M.A.E., and H.A.E.-H.; writing—original draft preparation, N.M.Z.; writing—review and editing, M.M.A.E. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

The study was approved by the Ethics Committee of the Faculty of Dentistry, Mansoura University, Mansoura, Egypt (protocol No. M0202025CD; approved on 6 April 2025).

Data Availability Statement

The per-tooth Ca/p values and the analysis script are provided as Supplementary Materials (Supplementary File S1: Per-tooth Ca/p values; Supplementary File S2: Analysis script); further data are available from the corresponding author upon reasonable request. Group-level summary statistics are reported in Table 2, Table 3, Table 4 and Table 5.

Acknowledgments

The authors thank the Department of Mechanical Design and Production Engineering, Faculty of Engineering, Mansoura University, for fabricating the cavity preparation machine, and the Pharmaceutics Department, Faculty of Pharmacy, Mansoura University, for preparing the demineralizing solution. During the preparation of this manuscript, the authors used language editing, consistency checking, and revision of the text in response to the reviewers’ comments, and Google Gemini 4 Argon (Google) was used to generate the graphic abstract from a text prompt describing the study workflow and outcomes. The authors reviewed and edited all AI-assisted output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Schmalz, G.; Hickel, R.; Price, R.B.; Platt, J.A. Bioactivity of Dental Restorative Materials: FDI Policy Statement. Int. Dent. J. 2023, 73, 21–27. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Abozaid, D.; Azab, A.; Bahnsawy, M.A.; Eldebawy, M.; Ayad, A.; Soomro, R.; Elwakeel, E.; Mohamed, M.A. Bioactive restorative materials in dentistry: A comprehensive review of mechanisms, clinical applications, and future directions. Odontology 2026, 114, 349–377. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  3. Wakamatsu, N.; Ogika, M.; Okano, T.; Murabayashi, C.; Kondo, T.; Iinuma, M. Effect of tooth surface coating material containing S-PRG filler on white spot lesions of young permanent teeth. Pediatr. Dent. J. 2018, 28, 40–45. [Google Scholar] [CrossRef] [Scilit]
  4. Inoue, H.; Lan, L.; Ke, Z.; Yan, Y.; Zheng, F.; Mao, D.; Goda, S. Effects of S-PRG filler eluate on MMP-1 and MMP-3 secretion by human gingival fibroblasts. Dent. Mater. J. 2022, 41, 159–166, Erratum in Dent. Mater. J. 2023, 42, 458. https://doi.org/10.4012/dmj.2021-062-e. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Thein, H.S.S.; Hashimoto, K.; Kawashima, N.; Noda, S.; Okiji, T. Evaluation of the anti-inflammatory effects of surface-reaction-type pre-reacted glass-ionomer filler containing root canal sealer in lipopolysaccharide-stimulated RAW264.7 macrophages. Dent. Mater. J. 2022, 41, 150–158. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  6. Moroto, H.; Inoue, H.; Morikawa, Y.; Tanimoto, H.; Yoshikawa, K.; Goda, S.; Yamamoto, K. Effects of a co-stimulation with S-PRG filler eluate and muramyl dipeptide (MDP) on matrix metalloproteinase-1 production by human dental pulp fibroblast-like cells. Dent. Mater. J. 2023, 42, 375–382. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  7. Nemoto, A.; Chosa, N.; Kyakumoto, S.; Yokota, S.; Kamo, M.; Noda, M.; Ishisaki, A. Water-soluble factors eluated from surface pre-reacted glass-ionomer filler promote osteoblastic differentiation of human mesenchymal stem cells. Mol. Med. Rep. 2018, 17, 3448–3454. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Frencken, J.E.; Peters, M.C.; Manton, D.J.; Leal, S.C.; Gordan, V.V.; Eden, E. Minimal intervention dentistry for managing dental caries—A review: Report of a FDI task group. Int. Dent. J. 2012, 62, 223–243. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Chen, L.; Shen, H.; Suh, B.I. Bioactive dental restorative materials: A review. Am. J. Dent. 2013, 26, 219–227. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Stewart, C.A.; Finer, Y. Biostable, antidegradative and antimicrobial restorative systems based on host-biomaterials and microbial interactions. Dent. Mater. 2019, 35, 36–52. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  11. Baroudi, K.; Rodrigues, J.C. Flowable Resin Composites: A Systematic Review and Clinical Considerations. J. Clin. Diagn. Res. 2015, 9, ZE18–ZE24. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  12. Bourgi, R.; Kharouf, N.; Cuevas-Suárez, C.E.; Lukomska-Szymanska, M.; Haikel, Y.; Hardan, L. A Literature Review of Adhesive Systems in Dentistry: Key Components and Their Clinical Applications. Appl. Sci. 2024, 14, 8111. [Google Scholar] [CrossRef] [Scilit]
  13. Sidhu, S.K.; Nicholson, J.W. A Review of Glass-Ionomer Cements for Clinical Dentistry. J. Funct. Biomater. 2016, 7, 16. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Dutra, G.C.; Kreve, S.; Reis, A.C. What is the current state of the art in incorporating antimicrobial agents into conventional glass ionomer cement? A systematic review. Dent. Rev. 2024, 4, 100149. [Google Scholar] [CrossRef] [Scilit]
  15. Senthil Kumar, R.; Ravikumar, N.; Kavitha, S.; Mahalaxmi, S.; Jayasree, R.; Sampath Kumar, T.S.; Haneesh, M. Nanochitosan modified glass ionomer cement with enhanced mechanical properties and fluoride release. Int. J. Biol. Macromol. 2017, 104, 1860–1865. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  16. Melo, M.A.; Mei, M.L.; Li, K.C.; Hamama, H.H. Editorial: The Use of Bioactive Materials in Caries Management. Front. Oral Health 2022, 3, 832285. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  17. Okuyama, K.; Murata, Y.; Pereira, P.N.; Miguez, P.A.; Komatsu, H.; Sano, H. Fluoride release and uptake by various dental materials after fluoride application. Am. J. Dent. 2006, 19, 123–127. [Google Scholar] [PubMed]
  18. Torres, C.R.G.; Balsamo, M.; Imazato, S. Composite Restoration on Posterior Teeth. In Textbooks in Contemporary Dentistry; Springer International Publishing: Cham, Switzerland, 2019; pp. 577–630. [Google Scholar]
  19. Chen, L.; Suh, B.I.; Yang, J. Antibacterial dental restorative materials: A review. Am. J. Dent. 2018, 31, 6b–12b. [Google Scholar] [PubMed]
  20. Francois, P.; Fouquet, V.; Attal, J.P.; Dursun, E. Commercially Available Fluoride-Releasing Restorative Materials: A Review and a Proposal for Classification. Materials 2020, 13, 2313. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Naoum, S.; Ellakwa, A.; Martin, F.; Swain, M. Fluoride release, recharge and mechanical property stability of various fluoride-containing resin composites. Oper. Dent. 2011, 36, 422–432. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  22. Kunert, M.; Piwonski, I.; Hardan, L.; Bourgi, R.; Sauro, S.; Inchingolo, F.; Lukomska-Szymanska, M. Dentine Remineralisation Induced by “Bioactive” Materials through Mineral Deposition: An In Vitro Study. Nanomaterials 2024, 14, 274. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  23. Thadathil Varghese, J.; Raju, R.; Farrar, P.; Prentice, L.; Prusty, B.G. Comparative analysis of self-cure and dual cure-dental composites on their physico-mechanical behaviour. Aust. Dent. J. 2024, 69, 124–138. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  24. Kasraei, S.; Haghi, S.; Valizadeh, S.; Panahandeh, N.; Nejadkarimi, S. Phosphate Ion Release and Alkalizing Potential of Three Bioactive Dental Materials in Comparison with Composite Resin. Int. J. Dent. 2021, 2021, 5572569. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  25. El-Adl, E.T.; Ebaya, M.M.; Habib, E.E.; Zaghloul, N.M. Comparative measurement of short-term fluoride release and inhibition of caries around restoration by ion releasing restorative materials: An in vitro study. Sci. Rep. 2025, 15, 1600. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Chou, Y.F.; Maciel Pires, P.; Alambiaga-Caravaca, A.M.; Spagnuolo, G.; Hibbitts, A.; Sauro, S. Remineralisation of mineral-deficient dentine induced by experimental ion-releasing materials in combination with a biomimetic dual-analogue primer. J. Dent. 2025, 152, 105468. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Van Ende, A.; De Munck, J.; Lise, D.P.; Van Meerbeek, B. Bulk-fill composites: A review of the current literature. J. Adhes. Dent. 2017, 19, 95–109. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  28. Scimeca, M.; Bischetti, S.; Lamsira, H.K.; Bonfiglio, R.; Bonanno, E. Energy Dispersive X-ray (EDX) microanalysis: A powerful tool in biomedical research and diagnosis. Eur. J. Histochem. 2018, 62, 2841. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Sacher, E.; França, R. Surface Analysis Techniques for Dental Materials; Dental Biomaterials; World Scientific: Singapore, 2019; pp. 1–31. [Google Scholar]
  30. Raghip, A.G.; Comisi, J.C.; Hamama, H.H.; Mahmoud, S.H. In vitro elemental and micromorphological analysis of the resin-dentin interface of bioactive and bulk-fill composites. Am. J. Dent. 2023, 36, 3–7. [Google Scholar] [PubMed]
  31. Sarhan, H.; Mehesen, R.; Hamama, H.; Mahmoud, S.H. Elemental analysis and micromorphological patterns of tooth/restoration interface of three ion-releasing class V restorations. BMC Oral Health 2024, 24, 1221. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  32. Sajini, S.I.; Alshawi, B.A.; Alharbi, L.M. Assessment of remineralisation potentials of bioactive dental composite using an in-vitro demineralised dentine model. J. Taibah Univ. Med. Sci. 2022, 17, 640–647. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  33. Al-Wakeel, R.E.; Hamama, H.H.; Farahat, D.S.; El-Negoly, S.A. Microhardness and elemental analysis of ion-releasing restoration/ dentin interface following enzymatic chemomechanical caries excavation. BMC Oral Health 2024, 24, 581. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  34. Breschi, L.; Mazzoni, A.; Ruggeri, A.; Cadenaro, M.; Di Lenarda, R.; De Stefano Dorigo, E. Dental adhesion review: Aging and stability of the bonded interface. Dent. Mater. 2008, 24, 90–101. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. Hamama, H. Characterization of Bioactive Restoration/Dentine Interface. Egypt. Dent. J. 2019, 65, 2731–2738. [Google Scholar] [CrossRef] [Scilit]
  36. Faul, F.; Erdfelder, E.; Lang, A.-G.; Buchner, A. G*Power 3: A flexible statistical power analysis program for the social, behavioral, and biomedical sciences. Behav. Res. Methods 2007, 39, 175–191. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  37. Ebaya, M.M.; Ali, A.I.; Mahmoud, S.H. Evaluation of Marginal Adaptation and Microleakage of Three Glass Ionomer-Based Class V Restorations: In Vitro Study. Eur. J. Dent. 2019, 13, 599–606. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  38. Soares, C.J.; Fonseca, R.B.; Gomide, H.A.; Correr-Sobrinho, L. Cavity preparation machine for the standardization of in vitro preparations. Braz. Oral Res. 2008, 22, 281–287. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  39. Armstrong, S.; Breschi, L.; Ozcan, M.; Pfefferkorn, F.; Ferrari, M.; Van Meerbeek, B. Academy of Dental Materials guidance on in vitro testing of dental composite bonding effectiveness to dentin/enamel using micro-tensile bond strength (muTBS) approach. Dent. Mater. 2017, 33, 133–143. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  40. Choi, A.N.; Lee, J.H.; Son, S.A.; Jung, K.H.; Kwon, Y.H.; Park, J.K. Effect of Dentin Wetness on the Bond Strength of Universal Adhesives. Materials 2017, 10, 1224. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  41. Murray, P.E.; Smith, A.J.; Windsor, L.J.; Mjor, I.A. Remaining dentine thickness and human pulp responses. Int. Endod. J. 2003, 36, 33–43. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  42. Hamama, H. Effect of Dentine Surface Treatment on Bonding of Bioactive RMGI-based Restorative Material to Dentine. Egypt. Dent. J. 2019, 65, 2999–3006. [Google Scholar] [CrossRef] [Scilit]
  43. Amaechi, B.T.; Higham, S.M.; Edgar, W.M. Techniques for the production of dental eroded lesions in vitro. J. Oral Rehabil. 1999, 26, 97–102. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  44. Joves, G.J.; Inoue, G.; Nakashima, S.; Sadr, A.; Nikaido, T.; Tagami, J. Mineral density, morphology and bond strength of natural versus artificial caries-affected dentin. Dent. Mater. J. 2013, 32, 138–143. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  45. Motevasselian, F.; Kermanshah, H.; Rasoulkhani, E.; Özcan, M. Comparison of microleakage of an alkasite restorative material, a composite resin and a resin-modified glass ionomer. Braz. J. Oral Sci. 2021, 20, e213981. [Google Scholar] [CrossRef] [Scilit]
  46. McKnight-Hanes, C.; Whitford, G.M. Fluoride release from three glass ionomer materials and the effects of varnishing with or without finishing. Caries Res. 1992, 26, 345–350. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  47. Hamdi, K.; Hamama, H.H.; Motawea, A.; Fawzy, A.; Mahmoud, S.H. Remineralization of early enamel lesions with a novel prepared tricalcium silicate paste. Sci. Rep. 2022, 12, 9926. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  48. Newbury, D.E.; Ritchie, N.W.M. Is scanning electron microscopy/energy dispersive X-ray spectrometry (SEM/EDS) quantitative? Scanning 2013, 35, 141–168. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  49. Ismail, H.S.; Elawsya, M.E.; Ali, A.I. Effect of light-, chemical-, and dual-cured universal adhesives on the internal adaptation of resin composites to pulpal and gingival internal walls. Am. J. Dent. 2024, 37, 91–100. [Google Scholar] [PubMed]
  50. Sauro, S.; Makeeva, I.; Faus-Matoses, V.; Foschi, F.; Giovarruscio, M.; Maciel Pires, P.; Moura, M.E.M.; Neves, A.A.; Faus-Llácer, V. Effects of Ions-Releasing Restorative Materials on the Dentine Bonding Longevity of Modern Universal Adhesives after Load-Cycle and Prolonged Artificial Saliva Aging. Materials 2019, 12, 722. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  51. Perdigão, J.; Lambrechts, P.; Van Meerbeek, B.; Vanherle, G.; Lopes, A.L.B. Field emission SEM comparison of four postfixation drying techniques for human dentin. J. Biomed. Mater. Res. 1995, 29, 1111–1120. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  52. Delacre, M.; Leys, C.; Mora, Y.L.; Lakens, D. Taking parametric assumptions seriously: Arguments for the use of Welch’s F-test instead of the classical F-test in one-way ANOVA. Int. Rev. Soc. Psychol. 2019, 32, 13. [Google Scholar] [CrossRef] [Scilit]
  53. Welch, B.L. On the comparison of several mean values: An alternative approach. Biometrika 1951, 38, 330–336. [Google Scholar] [CrossRef] [Scilit]
  54. Games, P.A.; Howell, J.F. Pairwise multiple comparison procedures with unequal N’s and/or variances: A Monte Carlo study. J. Educ. Stat. 1976, 1, 113–125. [Google Scholar] [CrossRef] [Scilit]
  55. Holm, S. A simple sequentially rejective multiple test procedure. Scand. J. Stat. 1979, 6, 65–70. [Google Scholar]
  56. Vickers, A.J.; Altman, D.G. Analysing controlled trials with baseline and follow up measurements. BMJ 2001, 323, 1123–1124. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  57. Rouessac, F.; Rouessac, A. Chemical Analysis: Modern Instrumentation Methods and Techniques; John Wiley & Sons: Hoboken, NJ, USA, 2013. [Google Scholar]
  58. Arends, J.; Ten Bosch, J.J. Demineralization and remineralization evaluation techniques. J. Dent. Res. 1992, 71, 924–928. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  59. Van Meerbeek, B.; Yoshihara, K.; Yoshida, Y.; Mine, A.; De Munck, J.; Van Landuyt, K.L. State of the art of self-etch adhesives. Dent. Mater. 2011, 27, 17–28. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  60. Burrer, P.; Par, M.; Furer, L.; Stubi, M.; Marovic, D.; Tarle, Z.; Attin, T.; Tauböck, T.T. Effect of polymerization mode on shrinkage kinetics and degree of conversion of dual-curing bulk-fill resin composites. Clin. Oral Investig. 2023, 27, 3169–3180. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  61. Ilie, N. Fracture and viscoelastic behavior of novel self-adhesive materials for simplified restoration concepts. J. Mech. Behav. Biomed. Mater. 2022, 125, 104970. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  62. Nicoloso, G.F.; Antoniazzi, B.F.; Lenzi, T.L.; Soares, F.Z.; Rocha, R.O. Is There a Best Protocol to Optimize Bond Strength of a Universal Adhesive to Artificially Induced Caries-affected Primary or Permanent Dentin? J. Adhes. Dent. 2016, 18, 441–446. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  63. de Azevedo, C.S.; Garbui, B.U.; Martins E Silva, C.; Simionato Lorenzetti, M.R.; de Freitas, A.Z.; Matos, A.B. Obtaining artificially caries-affected dentin for in vitro studies. J. Contemp. Dent. Pract. 2014, 15, 12–19. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  64. Al-Taee, L.; Banerjee, A.; Deb, S. In-vitro adhesive and interfacial analysis of a phosphorylated resin polyalkenoate cement bonded to dental hard tissues. J. Dent. 2022, 118, 104050. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  65. Al-Hasan, R.M.; Al-Taee, L.A. Interfacial Bond Strength and Morphology of Sound and Caries-affected Dentin Surfaces Bonded to Two Resin-modified Glass Ionomer Cements. Oper. Dent. 2022, 47, E188–E196. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  66. Salam, A.E.A.; Ismail, H.S.; Hamama, H. Evaluation methods of artificial demineralization protocols for coronal dentin: A systematic review of laboratory studies. BMC Oral Health 2025, 25, 621. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  67. Yu, O.Y.; Zhao, I.S.; Mei, M.L.; Lo, E.C.; Chu, C.H. A Review of the Common Models Used in Mechanistic Studies on Demineralization-Remineralization for Cariology Research. Dent. J. 2017, 5, 20. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  68. Badole, G.P.; Shenoi, P.R.; Bengal, S. Comparative Evaluation of Surface Roughness and Microhardness of Bulk-fill Composite Placed in Artificial Saliva at Three Different pH. World J. Dent. 2023, 14, 331–335. [Google Scholar] [CrossRef] [Scilit]
  69. Leung, V.W.; Darvell, B.W. Artificial salivas for in vitro studies of dental materials. J. Dent. 1997, 25, 475–484. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  70. Buzalaf, M.A.R.; Hannas, A.R.; Magalhães, A.C.; Rios, D.; Honório, H.M.; Delbem, A.C.B. pH-cycling models for in vitro evaluation of the efficacy of fluoridated dentifrices for caries control: Strengths and limitations. J. Appl. Oral Sci. 2010, 18, 316–334. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  71. Besinis, A.; De Peralta, T.; Tredwin, C.J.; Handy, R.D. Review of nanomaterials in dentistry: Interactions with the oral microenvironment, clinical applications, hazards, and benefits. ACS Nano 2015, 9, 2255–2289. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  72. LeGeros, R.Z. Calcium phosphates in oral biology and medicine. Monogr. Oral Sci. 1991, 15, 1–201. [Google Scholar] [PubMed]
  73. Joshi, M.; Joshi, N.; Kathariya, R.; Angadi, P.; Raikar, S. Techniques to Evaluate Dental Erosion: A Systematic Review of Literature. J. Clin. Diagn. Res. 2016, 10, ZE01–ZE07. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  74. Alebady, M.H.; Hamama, H.H.; Mahmoud, S.H. Effect of various surface coating methods on surface roughness, micromorphological analysis and fluoride release from contemporary glass ionomer restorations. BMC Oral Health 2024, 24, 504. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  75. Khaled, H.R.; Hammama, H.H.; Mahmoud, S.H. Evaluation of microtensile bond strength, microleakage pattern and micromorphological analysis of new functional Monomer-Based universal adhesive tooth interface. Man. J. Dent. 2022, 9, 198–204. [Google Scholar] [CrossRef] [Scilit]
  76. Paradella, T.C.; Bottino, M.A. Scanning Electron Microscopy in modern dentistry research. Braz. Dent. Sci. 2012, 15, 43–48. [Google Scholar] [CrossRef] [Scilit]
  77. Tiskaya, M.; Al-Eesa, N.A.; Wong, F.S.L.; Hill, R.G. Characterization of the bioactivity of two commercial composites. Dent. Mater. 2019, 35, 1757–1768. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  78. Nayak, P.P.; Kini, S.; Ginjupalli, K.; Pai, D. Effect of shape of titanium dioxide nanofillers on the properties of dental composites. Odontology 2023, 111, 697–707. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  79. Witkowska, J.; Borowski, T.; Kulikowski, K.; Wunsch, K.; Morgiel, J.; Sobiecki, J.; Wierzchoń, T. Structure and Properties of Bioactive Titanium Dioxide Surface Layers Produced on NiTi Shape Memory Alloy in Low-Temperature Plasma. Micromachines 2024, 15, 886. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  80. Ponomarev, V.A.; Popova, A.D.; Sheveyko, A.N.; Permyakova, E.S.; Kuptsov, K.A.; Ilnitskaya, A.S.; Slukin, P.V.; Ignatov, S.G.; Gloushankova, N.A.; Subramanian, B.; et al. Microstructure and biological properties of titanium dioxide coatings doped with bioactive and bactericidal elements. Appl. Surf. Sci. 2022, 575, 151755. [Google Scholar] [CrossRef] [Scilit]
  81. Wang, X.X.; Hayakawa, S.; Tsuru, K.; Osaka, A. Bioactive titania-gel layers formed by chemical treatment of Ti substrate with a H2O2/HCl solution. Biomaterials 2002, 23, 1353–1357. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  82. Vollenweider, M.; Brunner, T.J.; Knecht, S.; Grass, R.N.; Zehnder, M.; Imfeld, T.; Stark, W.J. Remineralization of human dentin using ultrafine bioactive glass particles. Acta Biomater. 2007, 3, 936–943. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  83. Phyo, W.M.; Saket, D.; da Fonseca, M.A.; Auychai, P.; Sriarj, W. In vitro remineralization of adjacent interproximal enamel carious lesions in primary molars using a bioactive bulk-fill composite. BMC Oral Health 2024, 24, 37. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  84. Porenczuk, A.; Jankiewicz, B.; Naurecka, M.; Bartosewicz, B.; Sierakowski, B.; Gozdowski, D.; Kostecki, J.; Nasiłowska, B.; Mielczarek, A. A comparison of the remineralizing potential of dental restorative materials by analyzing their fluoride release profiles. Adv. Clin. Exp. Med. 2019, 28, 815–823. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  85. O’Donnell, M.D.; Watts, S.J.; Hill, R.G.; Law, R.V. The effect of phosphate content on the bioactivity of soda-lime-phosphosilicate glasses. J. Mater. Sci. Mater. Med. 2009, 20, 1611–1618. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  86. Garoushi, S.; Vallittu, P.; Lassila, L. Development and characterization of ion-releasing fiber-reinforced flowable composite. Dent. Mater. 2022, 38, 1598–1609. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  87. Randolph, L.D.; Palin, W.M.; Leloup, G.; Leprince, J.G. Filler characteristics of modern dental resin composites and their influence on physico-mechanical properties. Dent. Mater. 2016, 32, 1586–1599. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  88. Guarneri, J.A.G.; Maucoski, C.; Ghaffari, S.; MacNeil, B.D.; Price, R.B.; Arrais, C.A.G. Ability of a novel primer to enhance the polymerization of a self-cured resin composite. Dent. Mater. 2025, 41, 42–50. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  89. Aliberti, A.; Garcia-Godoy, F.; Borges, A.L.S.; Tribst, J.P.M.; Gasparro, R.; Mariniello, M.; Ausiello, P. Calcium, phosphate and fluoride ionic release from dental restorative materials for elderly population: An in vitro analysis. Front. Oral Health 2025, 6, 1609502. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  90. Sonbul, H.M. Influence of Bioactive Restorative Materials on Secondary Caries Prevention: A Clinical and In Vitro Study. J. Pharm. Bioallied Sci. 2025, 17, S1787–S1789. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  91. Marovic, D.; Par, M.; Posavec, K.; Maric, I.; Stajdohar, D.; Muradbegovic, A.; Tauböck, T.T.; Attin, T.; Tarle, Z. Long-Term Assessment of Contemporary Ion-Releasing Restorative Dental Materials. Materials 2022, 15, 4042. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  92. Sobh, E.G.; Hamama, H.H.; Palamara, J.; Mahmoud, S.H.; Burrow, M.F. Effect of CPP-ACP modified-GIC on prevention of demineralization in comparison to other fluoride-containing restorative materials. Aust. Dent. J. 2022, 67, 220–229. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  93. Kelic, K.; Par, M.; Peros, K.; Sutej, I.; Tarle, Z. Fluoride-Releasing Restorative Materials: The Effect of a Resinous Coat on Ion Release. Acta Stomatol. Croat. 2020, 54, 371–381. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  94. Pallavi, S.; Devadathan, A.; Pampadykandathil, L.P.; Chandrababu, V.; Nagaraj, N.J.; Alexander, A.K. In vitro evaluation of the antimicrobial efficacy, antibiofilm effect, and resistance to biodegradation of a novel composite against Streptococcus mutans. J. Conserv. Dent. Endod. 2025, 28, 1001–1006. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  95. Dahiya, M. Investigating the Remineralisation and Apatite Formation Potential of a Bioactive Glass Composite and a Commercial Composite; Cention Forte; Queen Mary University of London: London, UK, 2023. [Google Scholar]
  96. Hayashi, J.; Tagami, J.; Chan, D.; Sadr, A. New bulk-fill composite system with high irradiance light polymerization: Integrity and degree of conversion. Dent. Mater. 2020, 36, 1615–1623. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  97. Klaric, N.; Macan, M.; Par, M.; Tarle, Z.; Marovic, D. Effect of Rapid Polymerization on Water Sorption and Solubility of Bulk-fill Composites. Acta Stomatol. Croat. 2022, 56, 235–245. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  98. Nedeljkovic, I.; De Munck, J.; Vanloy, A.; Declerck, D.; Lambrechts, P.; Peumans, M.; Teughels, W.; Van Meerbeek, B.; Van Landuyt, K.L. Secondary caries: Prevalence, characteristics, and approach. Clin. Oral Investig. 2020, 24, 683–691. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  99. Hurlbert, S.H. Pseudoreplication and the design of ecological field experiments. Ecol. Monogr. 1984, 54, 187–211. [Google Scholar] [CrossRef] [Scilit]
  100. Lazic, S.E. The problem of pseudoreplication in neuroscientific studies: Is it affecting your analysis? BMC Neurosci. 2010, 11, 5. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  101. Ferracane, J.L.; Lawson, N.C. Probing the hierarchy of evidence to identify the best strategy for placing class II dental composite restorations using current materials. J. Esthet. Restor. Dent. 2021, 33, 39–50. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  102. Han, S.H.; Sadr, A.; Tagami, J.; Park, S.H. Internal adaptation of resin composites at two configurations: Influence of polymerization shrinkage and stress. Dent. Mater. 2016, 32, 1085–1094. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  103. Braga, R.R.; Ferracane, J.L. Contraction stress related to degree of conversion and reaction kinetics. J. Dent. Res. 2002, 81, 114–118. [Google Scholar] [CrossRef] [Scilit]
  104. Nakajima, M.; Kunawarote, S.; Prasansuttiporn, T.; Tagami, J. Bonding to caries-affected dentin. Jpn. Dent. Sci. Rev. 2011, 47, 102–114. [Google Scholar] [CrossRef] [Scilit]
  105. Salem, H.N.; Hefnawy, S.M.; Nagi, S.M. Degree of Conversion and Polymerization Shrinkage of Low Shrinkage Bulk-Fill Resin Composites. Contemp. Clin. Dent. 2019, 10, 465–470. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  106. Negovetic Mandic, V.; Par, M.; Marovic, D.; Rakic, M.; Tarle, Z.; Klaric Sever, E. Blue Laser for Polymerization of Bulk-Fill Composites: Influence on Polymerization Kinetics. Nanomaterials 2023, 13, 303. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  107. Watts, D.C.; Algamaiah, H. Characterizing surface viscoelastic integrity of ultra-fast photo-polymerized composites: Methods development. Dent. Mater. 2020, 36, 1255–1265. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  108. Cimpean, S.-I.; Ambrosie, I.; Moldovan, M.; Delean, A.; Prodan, D.; Prejmerean, C.; Moldovan, M.; Tomoaia-Cotisel, M.; Colceriu-Burtea, L. Testing of New Experimental Giomers: Water Sorption, Conversion Degree, Radiopacity, Microstructure and Biological Behavior. Stud. Univ. Babeș-Bolyai Chem. 2022, 67, 177–194. [Google Scholar] [CrossRef] [Scilit]
  109. Lynch, R.J.M.; Ten Cate, J.M. The effect of lesion characteristics at baseline on subsequent de- and remineralisation behaviour. Caries Res. 2006, 40, 530–535. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  110. Shellis, R.P.; Ganss, C.; Ren, Y.; Zero, D.T.; Lussi, A. Methodology and models in erosion research: Discussion and conclusions. Caries Res. 2011, 45, 69–77. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.