Next Article in Journal
Towards Functional Parts by Binder Jetting Calcium-Sulphate with Thermal Treatment Post-Processing
Next Article in Special Issue
The Thermal Parameters of Mortars Based on Different Cement Type and W/C Ratios
Previous Article in Journal
Fabrication of Superhydrophobic Ti–6Al–4V Surfaces with Single-Scale Micotextures by using Two-Step Laser Irradiation and Silanization
Previous Article in Special Issue
The Effect of Aggregate Shape on the Properties of Concretes with Silica Fume
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Moisture Influence on Compressive Strength of Calcium Silicate Masonry Units–Experimental Assessment and Normative Calculations

by
Halina Garbalińska
,
Jarosław Strzałkowski
* and
Agata Stolarska
Department of Building Physics and Building Materials, Faculty of Civil Engineering and Architecture, West Pomeranian University of Technology Szczecin, al. Piastów 50, 70-311 Szczecin, Poland
*
Author to whom correspondence should be addressed.
Materials 2020, 13(17), 3817; https://doi.org/10.3390/ma13173817
Submission received: 6 August 2020 / Revised: 20 August 2020 / Accepted: 26 August 2020 / Published: 29 August 2020

Abstract

:
This paper primarily assesses the scale of adverse changes to the compressive strength of different types of silicates due to the influence of moisture. The study covers three groups of silicate units of different strength classes—15, 20 and 25—obtained from three different manufacturers. It was demonstrated that in all studied groups, moisture significantly decreased the compressive strength by about 30–40%. In addition, microstructural studies were conducted to analyze the relationship between the specific porosity structure of each group of silicate bricks and their compressive strength. On the basis of SEM (Scanning Electron Microscopy) and EDS (Electron Dispersive Spectroscopy) analysis, the elemental composition of individual silicates was determined and the contact zone between the aggregate and the binder was determined, which largely influenced the obtained compressive strength of each silicates. Next, the study referred to the utility of the normative procedure used to determine the strength class of samples with different geometries and at different moisture concentrations. The results of the calculations showed the high accuracy of the normative-based assessment of strength class, regardless of the manufacturer and the moisture values during examination.

1. Introduction

The calcium silicate brick was invented in Great Britain, and it was patented there in 1866. However, as with many other British inventions, it was first practically applied out of its borders: in Germany at the end of the 19th century. Some years later, at the start of the 20th century, the invention returned to the UK [1]. In Germany, Holland and the former Soviet Union, where sand is widely distributed, this class of brick became a main structural building material. It was so popular that a special law was introduced in Holland to protect the clay brick. At present, the calcium silicate brick is dominant in the Netherlands and Germany, and used extensively throughout Europe [1].
For example, in Polish climate conditions, the three most popular materials for wall construction are autoclaved aerated concrete, ceramics and silicates. Their respective shares of the wall material market in 2017 were 39.0%, 28.6% and 15.1%. While the share of autoclaved aerated concrete has remained near 40% for many years, the share of ceramics has dropped from 37% to 28.6% in the past decade, and the silicate share has increased from 9% to 15.1% [2].
The reason for the growing interest in silicate products is their numerous technical, health and environmental benefits, which are largely due to the use of only natural materials, such as sand (88–92%), lime (8–12%) and water (3–5%) [3]. Silicate bricks are considered to be a “green building material” and can be used as a substitute for burnt clay bricks by offering advantages for agricultural land protection, environmental protection and energy saving [4].
As is mentioned in [5], the production of clay bricks consumed huge amounts of clay in China. In the last 50 years, approximately a 1.3 billion m2 cultivated area has been destroyed, and about 70 million tons of coal has been consumed in the process of clay brick production.
The data given in work [6] show how many harmful substances appear in clay brick production, which contributes largely to environmental damage. A brick kiln emits 70–282 g of carbon dioxide, 0.001–0.29 g of black carbon, 0.29–5.78 g of carbon monoxide and 0.15–1.56 g of particulate matter per kilogram of clay brick, depending on the type of kiln and fuel used for the firing process. Moreover, depending on the technology, the production consumes about 0.54–3.14 MJ of specific energy per kilogram of clay brick.
Considering the negative environmental impact of the conventional brick production process, researchers and brick manufacturers all over the world have been trying to come up with alternative materials that will be more eco-friendly, but also durable and relatively cheap and have sustainability potential. Unquestionable environmental advantages result from the application of unfired bricks and the adoption of suitable stabilization techniques [7,8,9,10].
At the same time, numerous attempts are being made to partially replace clay with recycled waste materials in the production of bricks [5] (e.g., slag [11], pumice [12], waste marble [13], paper waste [14], waste glass [15]).
Having considered ecological aspects, autoclaved lime–sand brick, also known as calcium silicate brick, is a much more environmental-friendly sustainable material. Firstly, harmful substances are not emitted in its production process. Secondly, it is possible to recycle numerous waste materials by adding them into the silicate brick manufacturing process. Some researchers assess the influence of waste material addition into the silicate brick, analyzing, amongst other things, the microstructure and strength parameters [16,17,18,19,20,21,22,23].
Over the last few decades, pure calcium silicate bricks (made from sand, lime and water) have been produced. Pure silicate products are included in the safest building materials in terms of natural radioactivity [24]. They feature excellent acoustic parameters and a very good heat capacity.
They are also characterized by high resistances to both chemical and biological corrosion, and are non-combustible, so no harmful compounds will be emitted if a fire occurs. Undoubtedly, their growing popularity is also a result of their relatively high compressive strength, which is comparable to the strength of lower-class concretes. In practice, this means that this class of material can be used to construct walls in multi-storied buildings. Its relatively high strength parameters enable it to be used in structural elements that are subjected to higher loads, such as pillars, bay window corners, support areas for long lintel beams, etc.
Unfortunately, the properties of silicate products deteriorate significantly when heavy wall moisture occurs. This is especially a problem for the lower wall parts if, for example, they are exposed to flooding or groundwater, or if waterproofing is incorrectly applied or absent entirely. The technical characteristics provided by manufacturers are most often only for dry materials, while most of their parameters tend to deteriorate with increasing moisture content [25].
The problem of strength deterioration as a result of moistness has been analyzed in many articles. The researchers dealt with techniques of moisture content measurement (e.g., [26]) and assessed its impact on masonry units, mortar and wall strengths (e.g., [27]). In [28], the compressive strength of fired-clay bricks, cement mortar and hydraulic lime mortar are investigated in dry and saturated conditions. Masonry triplets (cement-based mortar) were tested in dry, moist and saturated conditions. The results were correlated with the microstructural parameters of the materials, i.e., total voids amount and pores size distribution. The fundamental mechanical properties of autoclaved sand–lime brick masonry were studied in [29], and selected properties of autoclaved bricks in [30]. The effect of sorption capacity on the mechanical properties of unfired clay bricks was investigated in [31]. The validation of selected non-destructive techniques of determining the compressive strength of masonry units was described in [32]. The researchers dealt with semi-non-destructive, non-destructive and ultrasonic methods used for autoclaved aerated concrete, in the four density classes of 400, 500, 600 and 700 kg/m3, tested at various moisture contents.
In particular, the influence of moisture on the strength properties of calcium silicate units was examined in [33]. The experiments were conducted on high precision calcium silicate units, which were assigned to strength class 20 and density class 2.0. The calcium silicate units were firstly adjusted to three different moisture contents: (a) oven dry, (b) 4% by weight and (c) 10% by weight. The highest mean compressive strength values were reached by the oven dry units—31.9 MPa. Related to the compressive strength in the oven dry state, the strength in the wet state amounted to between 0.67 (10% by weight) and 0.71 (4% by weight).
The problem of the negative influence of moisture concerns the majority of masonry units. Scientists from the Building Research Institute in Warsaw have recently conducted a number of experiments concerning the most popular masonry units in Poland [34]. The smallest decrease in compressive strength caused by moisture was recorded in the case of clay masonry units. This parameter has been reduced by 5–11% in relation to the dry material. A substantial percentage loss of compressive strength, caused by water saturation, occurred with autoclaved aerated concrete units, and it oscillated between 37% and 40%. By contrast, clearly the highest percentage of strength decrease was observed in the case of silicate components. The compressive strength of silicate units saturated with water showed a decrease of 42–51% relative to analogous dry products.
The problem is technically significant because, while the negative effects associated with autoclaved aerated concrete softening are widely known, it is also possible to associate silicates with relatively water-resistant materials that do not show such significant compressive strength changes. Due to the moisture resulting from the lack of waterproofing or incorrect assembly, or caused by the action of, e.g., flood waters, such changes can have a very negative impact on the safety of the building construction.
The problem of a significant deterioration in strength caused by moisture is not sufficiently highlighted in the literature—even in extensive review papers, e.g., [35].
To diagnose the extent to which moisture adversely affects the properties of silicate products, comprehensive diagnostic studies were carried out within the framework of [25]. To extend the diagnosis to include a wider range of commercially-available silicate products, the study was conducted on three groups of silicate units obtained from three different manufacturers. In a comprehensive multi-stage experiment, different basic material parameters were determined.
Another problem related to masonry is its thermal performance in fire. Harmathy et al. [36] researched the influence of moisture content in masonry walls on its fire endurance. The presence of moisture usually benefits fire endurance. In general, a 1% increase in moisture (by volume) is capable of increasing the fire endurance by 4% to 5%. However, above a certain critical level, moisture may cause explosive spalling in the case of fire. An extensive elaboration has been prepared by Naser [37,38] about the properties of common construction materials at elevated temperatures. The proposed material models have the potential to regulate and modernize structural design under extreme loading conditions, i.e., fire. The results of this investigation demonstrate the value of utilizing artificial intelligence (AI) in comprehending the impact of the complex nature of temperature-induced effects on building materials.
Manufacturers of calcium–silicate blocks ensure that these materials offer excellent acoustic insulation. This is due to their large weight. For example, in order for a wall to fulfil its acoustic requirements [39], a silicate wall with a thickness of 12 cm is sufficient. In terms of energy efficiency, silicate walls are a very advantageous solution due to their heavy weight, and thus their high heat capacity and thermal inertia.
Nurzyński in [40] searched for dependencies in the thermal and acoustic behaviours of various building elements, including silicate bricks. He showed that finding a simple relationship between acoustic and thermal insulation is quite difficult, and that massive homogeneous walls made of concrete, ceramic bricks or silicate blocks usually have good acoustic insulation and poor thermal resistance.
As noted in [41,42] the correlation between thermal resistance and sound insulation is possible for monolithic, homogenous and relatively thick walls of similar structure, but the thermal transmittance of such walls is so high that if they are used for an exterior shell they need additional insulation. Massive walls with additional lining behave, in acoustic terms, differently from bare homogeneous structures. Therefore, any correlation derived for heavy bare walls is of little practical use, when for multilayer and more complex partitions finding any correlation appears unlikely.
The results of strength studies were presented in the article [43]. They were linked to the absorbency analysis, density, and the distinct microstructures of individual silicate products, expressed by their varied pore distribution differential curves.
This article focuses on the compressive strengths of the three groups of silicates that were tested within [25]. At the beginning, all silicate specimens were exposed to water, which spread height-wise, carried up by capillary suction. Then, all specimens were cut horizontally into two pieces. The lower part was saturated with water, and the upper part was subjected to drying. Strength studies were carried out in order to discuss the two goals of the research.
The first objective concerns the influence of moisture on the reduction of the compressive strength of silicates of various strength classes. The second goal was to assess the accuracy of the normative procedures used to determine the compressive strength class of samples of different geometries and different moisture contents.

2. Materials and Methods

Three groups of calcium silicate products from different manufacturers were evaluated. Manufacturer names have been replaced by the symbols “E”, “X” and “B”, whereas masonry units categorized into particular groups were marked with CS-E, CS-X and CS-B symbols.
Each of these were rectangular solid units with the following dimensions [44] (lu length, wu width and hu height): CS-E: 240 × 115 × 71 mm; CS-X: 250 × 120 × 65 mm; CS-B: 240 × 120 × 80 mm, according to the manufacturer’s declaration.
Calcium silicate units, as well as other masonry units (in accordance with EN 771, Parts 1–6 [45,46,47,48,49,50]), were divided into four groups, according to the percentage, size and orientation of holes in the units when laid. Due to the fact that the masonry units chosen for the research did not feature any holes, all of them belonged to Group 1.
However, it was assumed that the particular groups of calcium silicate units CS-E, CS-X and CS-B should be differentiated via classification based on compressive strength. Calcium silicate masonry units are classified according to the normalized compressive strength classes given in EN 771-2 [46] (Annex D). The products from the manufacturers chosen for the research represented the most common compressive strength classes, 15 (CS-E), 20 (CS-X) and 25 (CS-B), with normalized compressive strengths of 15.0 N/mm2, 20.0 N/mm2 and 25.0 N/mm2, respectively.
Before conducting the strength tests, all samples were exposed to water which was introduced into the tested elements by capillary suction, to obtain a diverse distribution among the tested specimens. The idea was to reproduce in laboratory conditions a situation in which an element of an external wall is directly exposed to liquid water for a prolonged time.
Six units from each manufacturing plant (CS-E, CS-X and CS-B) were vertically placed in water-containing trays to orient the front surface at the suction surface. The water level was regularly replenished so that it reached a constant height of approx. 2 mm, measured from the bottom of each specimen.
The changes in the mass of individual samples were systematically recorded to determine the water sorption coefficient A, assigned to each of the 18 tested samples. This parameter describes the behavior of the porous material in contact with liquid water introduced into the porous material during the first period of capillary suction. It is defined in the EN ISO 9346:2007 standard [51] using the following formula:
m s = A × t
where ms is the specimen mass, divided by its bottom surface in contact with water, while t is the duration of the process. The average values of the water sorption coefficients, A, were then calculated.
The studies of capillary action were conducted over six weeks (about 1000 h), after which all samples were lifted from the trays and cut into halves. The upper halves were dried to a constant mass in a laboratory dryer with a gradual increase in temperature from 40 °C → 70 °C → 105 °C. In turn, the bottom halves were placed in a water bath, where they remained until they were completely saturated.
Figure 1 gives a schematic representation of these successive stages of preliminary experimental research: I—calcium silicate masonry unit during capillary suction testing; II—masonry unit on completion of the capillary test (varied redistribution of moisture along lu); III—masonry unit after cutting into two specimens (top (no. 1) with lower moisture content and bottom (no. 2) with a higher moisture content); IV—sample no. 1 after conditioning to the oven dry state and sample no. 2 after conditioning by immersion in water bath.
A total of 18 samples in the dried state (6 upper halves of each series) and a total of 18 samples in the saturated state (6 lower halves of each series) were used for strength tests. The load-bearing surfaces were not subjected to additional treatment because they were flat and even. The processes of specimen preparation and their numbering were in accordance with EN 772-1 [52]. Furthermore, the placing of specimens in the testing machine, as well as the settings of the loading rate, were in accordance with the recommendations included in the EN 772-1 standard [52].
First, compressive strength values were determined for all specimens no. 1 (dried to a constant mass), and then for all specimens no. 2 (conditioned by water immersion).
The maximum load obtained for each specimen was recorded, and then its compressive strength was calculated by dividing the measured compressive force value (N) by the load-bearing area (mm2). In all cases the gross area of the loaded surface was calculated in square millimeters by multiplying the length (≈½ lu) by the width (wu) of each specimen determined in accordance with EN 772-16 [44].
The obtained values from the compressive strength tests are summarized in tabular form in [43]. In each of the 36 samples (18 dry and 18 saturated), the determined value of the compression strength fc rounded to 0.1 N/mm2 was given. Based on these values, graphic comparisons of the results were prepared.

3. Results and Discussion

3.1. Results of Strength Tests in Terms of Moisture and Microstructure Effect

Figure 2, Figure 3 and Figure 4 show how the determined strength values of the specimens varied between the dry and water-saturated states. The specimens are grouped by producer and, to avoid presenting manufacturers’ names, they were described with symbols: CS-E, CS-X and CS-B. In each case, the strength values are quoted for two moisture states; firstly for six specimens dried to a constant mass, and then for six water-saturated specimens. Additionally, in Figure 2, Figure 3 and Figure 4 the average compressive strength values for the dry state (fC1) and for the saturated state (fC2) are shown.
A clear tendency of compression strength decrease was observed as a result of water saturation. In case of the CS-E group of silicates the drop fC2/fC1 was 66.9%, and in the case of groups CS-X and CS-B, the drops were 63.2% and 68.9%, respectively.
As noted in [43], this is an issue of great technical importance, since the most significant deterioration of mechanical parameters due to strong moisture occurs mainly in the lower parts of the wall exposed to groundwater or floods. The lower parts of the masonry construction carry a much greater load than the walls of higher floors, and are therefore subjected to much higher stress levels, and the moisture-induced strength decrease can jeopardize the safety of the entire structure.
It is commonly accepted that the properties of a porous material (including strength parameters) are determined by its internal structure—the skeletal structure and specificity of pores, particularly those that can be filled with water in the liquid phase.
For this reason, in the compilation in Table 1, additional data characterizing the tested silicates were included. For the three groups CS-E, CS-X and CS-B, the average compressive strength values in the dry state fC1 and in the saturated state fC2, and the water sorption coefficients, A, are shown in Table 1. The average density in the dry state, ρp, and average water absorption by weight, nw, and volume, nv, were obtained from [25,43], which provides detailed data for all the studied silicates.
An analysis of the data collected shows that the CS-E and CS-B products have similar water absorptions by weight nw (13.4% and 14.3%) and volume nv (24.7% and 26.1%), as well as similar apparent densities ρp (1.840 kg/dm3 and 1.830 kg/dm3). However, their compressive strength parameters are significantly different. While the CS-E products have the lowest compressive strength values, the CS-B products exhibit the highest parameters in this respect. For CS-E, CS-X and CS-B, the values of fC1 (in the dry state) and fC2 (in the saturated state) are the following: fC1 = 26.6 MPa < 34.9 MPa < 39.6 MPa and fC2 = 17.8 MPa < 22.0 MPa < 27.3 MPa. Similar trends were found in the case of the sorption coefficient, A = 3.6 < 5.2 < 8.3 kg/m2h0.5. It should be noted, however, that the highly different A values also have no direct connection to the other physical parameters (ρp, nw, nv) shown in Table 1.
Therefore, it can be concluded that the macroscopically-determined physical parameters of the materials (density, water absorption and water sorption coefficient) do not provide useful information for drawing conclusions regarding the potential compressive strength of given material groups.
Therefore, additional microstructural studies were carried out using mercury porosimetry and scanning electron microscopy (SEM), to clarify the differences in the porosity structures of individual groups of silicates.
Figure 5 and Figure 6 show integral and differential curves, which respectively represent the pore distribution.
The integral curves for CS-E and CS-X silicates show a significant increase in porosity at a pore diameter of about 30 µm. Such a situation does not occur in the case of the CS-B silicate, which generally has a more homogeneous porosity distribution. By analyzing the CS-B integral curve, a more pronounced deflection in its course can be observed in the pore diameter region of about 0.05 µm.
Differences in the distribution of pores can be assessed more clearly on the basis of differential curves assigned to individual materials. These curves are all characterized by the bimodal pore distribution of the tested silicates. Two areas with increased pore contents, but with a different proportion of pores, are clearly visible on all differential graphs. For CS-E and CS-X specimens, there are clear porosity peaks with diameters of 42 µm and 23 µm, respectively. For CS-B silicate, no dominant diameters are observed in this range. The pores of more than 3 µm in diameter are more evenly distributed, and their contents are maintained at significantly lower levels than in the CS-E and CS-X silicates. The second concentration range of pores appears between 0.01 and 0.07 µm. The highest amount of pores in this range of diameters is found in the CS-X silicate, and it is slightly lower in the CS-B silicate. The CS-E silicate shows clearly the lowest content of these small pores. No dominant diameter has shown its presence in any case, and the concentration range always extends with a wider spectrum of pores.
Based on the determined values and the tested relationships, it can be stated that density and water absorption do not provide useful information for predicting potential strength characteristics. It was shown that it is not so much the total volume of pores but rather their specific geometry, determined by additional tests, that is the most important. The analysis of the obtained integral and differential pore distribution curves indicates the different porosity characteristics of each of the tested silicates. Even if a material contains many pores, if they have small diameters, the material will possess relatively high strength parameters. Therefore, large capillary pores and air voids have the most negative impact on the strength characteristics. A comparative analysis of the integral curves shows that the CS-E silicate units contain the largest fraction of pores in the range from 0.3 μm to 300 μm. In CS-X, this value is lower, while CS-B clearly shows the lowest amount of such pores. This is also confirmed by the differential curve analysis, which indicates that the CS-E silicate brick has the largest amount of pores that range from 3 μm to 300 μm, compared with CS-X and CS-B. The last two, in turn, demonstrated the highest share in terms of the smallest pore content that did not negatively affect the strength. The determined specific redistribution of the largest pores was shown to have a direct impact on the macroscopic strength relationships, in the order fCS-E < fCS-X < fCS-B.
Figure 7 shows the SEM images of three silicates at ×200 magnification. They depict the quantitative fractions of large pores (responsible for decreased strength) within the second peak, covering the range from 3 to 300 μm.
The scanning electron microscopy (SEM) images in Figure 7 confirm the results obtained using mercury porosimetry. Photos a) and b) for, CS-E and CS-X respectively, show a large number of pores with diameters ranging from about 5 to 50 µm, which are not visible at all in photo c) for the CS-B silicate.
The figures on the right present the EDS results, showing only the silicon, representing the aggregate location and the calcium as the binder. In the case of CS-E, numerous voids are visible, which are most likely responsible for reducing the strength of this material. The binder is not evenly distributed.
In the specimen CS-X, the used aggregate is definitely of smaller diameter than the CS-B specimens. In CS-X, the binder content also represents a greater share than that in CS-B. The CS-B specimen has certainly the smallest share of visible voids between the grains of the aggregate and the calcium binder. This translated into a higher compressive strength compared to the remaining specimens.
In the Table 2, the proportions of the weights of the main elements are presented for the tested types of silicates. The differences in proportions do not appear to be large. However, it is clearly visible that the most silicon occurs in CS-B, and the least in CS-E, which exactly corresponds to the strength classes. This shows that the most silicon-based aggregate was in CS-B, hence its greater compressive strength.
In the case of calcium, the highest value was observed in CS-X, which is confirmed by the EDS photos in Figure 7. In the case of CS-B, the amount of calcium (and thus the binder) is the lowest. This, too, may result in the increased strength of this type of silicate compared to the others.

3.2. Results of Strength Tests in the Context of Normative Regulations

Masonry walls are composed of units that must meet the requirements contained in the documents of PN-EN 771-1–PN-EN 771-6 [45,46,47,48,49,50]. Their subsequent parts involve clay masonry units, calcium silicate masonry units, aggregate and autoclaved aerated concrete masonry units, and manufactured and natural stone masonry units. The second part of this regulation, PN-EN 771-2 [46], describes the properties of calcium silicate masonry units.
Eurocodes have set unified methods for testing the strength of masonry units. The PN-EN 772-1 [45] recommends that the average compressive strength of masonry units be determined and then recalculated to obtain a normalized compressive strength, using the formula [53]:
fb = ηw d fC
where fb—normalized compressive strength—is the compressive strength of masonry units converted into the air dry compressive strength of an equivalent 100 mm wide and 100 mm high masonry unit (MPa); fC—average compressive strength—is the arithmetic mean of the compressive strength values of particular specimens (MPa); ηw—is the coefficient that includes the moisture state of the masonry units (using the following values: ηw = 1.0 for specimens conditioned to air dry condition and conditioned to 6% moisture content, ηw = 0.8 for specimens conditioned to the oven dry condition, and ηw = 1.2 for specimens conditioned by immersion in water); and d—is the shape factor that considers the impact of the “scale effect” of tested masonry units.
Table 3 shows the values of the shape factor d taken from EN 772-1 [52] (Annex A), whereby the width and height of specimens should be determined in accordance with EN 772-16 [44].
Thus, the specimen’s compressive strength depends on its size, relative proportions and moisture content. For construction calculations, the normalized compressive strength fb was used. Formula (2) has been applied to establish the fb value. In accordance with the procedure described above, the average compressive strength is first converted to an equivalent compressive strength relevant to the air-dry conditioning regime. In order to obtain the normalized strength fb, the air-dry compressive strength is multiplied by a shape factor d, given in Table 3.
The procedure in Formula (2) was applied in [25] in relation to the results obtained with respect to the CS-E, CS-X and CS-B silicates.
The compressive strength fC for each of the tested materials was calculated as the average strength of individual specimens obtained from each manufacturer. Then, to standardize the compressive strength values, the average fC values obtained for individual groups of specimens were multiplied by the shape factor d and the moisture content coefficient ηw.
The particular results are given in Table 4, Table 5 and Table 6 for the CS-E, CS-X and CS-B silicates, respectively. The obtained results for the normalized compressive strength of specimens in dry and wet conditions have similar values. For all three types of silicates, the results obtained confirm the classes given by the manufacturers. The coefficients ηw have properly accounted for the effect of moisture on compressive strength. The proposed formula for normalized strength allows the product class to be determined with high accuracy.

4. Conclusions

The results of the studies carried out on samples in dry and saturated states show a clear trend whereby the compressive strength decreases as the result of the water saturation of the tested silicates. The determined variability ranges for individual products are as follows: CS-E—fC1(dry) = 26.6 MPa → fC2(wet) = 17.8 MPa; CS-X—fC1(dry) = 34.8 MPa → fC2(wet) = 22.0 MPa; and CS-B—fC1(dry) = 39.6 MPa → fC2(wet) = 27.3 MPa. The obtained quantitative relationships fC2(wet)/fC1(dry) in the case of each material were CS-E—0.67, CS-X—0.63, and CS-B—0.69.
The collected results indicate a significant percentage decrease for each of the studied strength classes. In the cases of the CS-E (strength class 15), CS-X (strength class 20) and CS-B (strength class 25) silicate units, the strength reductions exceeded 30%.
The goal of this article was to assess the physical and microstructural conditions of silicate products, and also to discuss the compatibility of normative procedures for determining the strength class of various kinds of silicates in differently-conditioned specimens. A comparative analysis of the results (Table 4, Table 5 and Table 6) shows that for all products, a very high correspondence of the data to the class provided by each of the manufacturers was obtained. Thus:
  • For CS-E units, a strength class of 15 was determined for both dry (fb1 = 18.3 MPa) and water-saturated (fb2 = 18.4 MPa) samples;
  • For CS-X units, a strength class of 20 was determined, both in dry (fb1 = 22.6 MPa) and water-saturated samples (fb2 = 21.4 MPa);
  • For CS-B units, a strength class of 25 was determined based on both dry (fb1 = 27.5 MPa) and water-saturated samples (fb2 = 28.5 MPa).
Thus, it can be assumed that the proposed formula for normalized strength allows the product class to be determined with high accuracy, while considering the actual size of the tested samples and their specific moisture contents.
However, taking into account the fact that a strength drop of over 30% was noted for all tested types of silicates, every effort should be made to protect the masonry elements against moisture. This applies both to the stage of designing building components (checking the requirements of internal and surface condensation) and the stage of erecting the building (the application of properly selected and properly made waterproofing).

Author Contributions

Conceptualization, H.G.; methodology, H.G.; validation, H.G., J.S.; formal analysis, H.G., J.S.; investigation, H.G., A.S.; resources, A.S.; data curation, J.S.; writing—original draft preparation, H.G.; writing—review and editing, J.S., A.S.; visualization, J.S.; supervision, H.G.; All authors have read and agreed to the published version of the manuscript.

Funding

This work was carried out as a part of the project UPB-DZS-51Tab-032-3126-01/18 supported by West Pomeranian University of Technology, Szczecin, Poland.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Bowley, B. Calcium Silicate Bricks. Struct. Surv. 1994, 12, 16–18. [Google Scholar]
  2. Misiewicz, L. The market of wall construction materials in Poland in 2017. Mater. Bud. 2018, 4, 4–5. (In Polish) [Google Scholar]
  3. Calcium Silicate Bricks or Sand Lime Bricks for Masonry Construction. Available online: https://theconstructordotorg.wpcomstaging.com/building/calcium-silicate-bricks-masonry-construction/17256/ (accessed on 20 August 2020).
  4. Fang, Y.; Gu, Y.; Kang, Q.; Wen, Q.; Dai, P. Utilization of copper tailing for autoclaved sand–lime brick. Constr. Build. Mater. 2011, 25, 867–872. [Google Scholar] [CrossRef]
  5. Ling, T.-C.; Mo, K.H.; Qu, L.; Yang, J.; Guo, L. Mechanical strength and durability performance of autoclaved lime-saline soil brick. Constr. Build. Mater. 2017, 146, 403–409. [Google Scholar] [CrossRef]
  6. Murmu, A.L.; Patel, A. Towards sustainable bricks production: An overview. Constr. Build. Mater. 2018, 165, 112–125. [Google Scholar] [CrossRef]
  7. Walker, P.J. Strength, durability and shrinkage characteristics of cement stabilised soil blocks. Cem. Concr. Compos. 1995, 17, 301–310. [Google Scholar] [CrossRef]
  8. Venkatarama Reddy, B.V.; Hubli, S.R. Properties of lime stabilised steam-cured blocks for masonry. Mater. Struct. 2002, 35, 293. [Google Scholar] [CrossRef]
  9. Degirmenci, N. The using of waste phosphogypsum and natural gypsum in adobe stabilization. Constr. Build. Mater. 2008, 22, 1220–1224. [Google Scholar] [CrossRef]
  10. Maskell, D.; Heath, A.; Walker, P. Geopolymer stabilisation of unfired earth masonry units. Key Eng. Mater. 2014, 600, 175–185. [Google Scholar] [CrossRef] [Green Version]
  11. Gencel, O.; Sutcu, M.; Erdogmus, E.; Koc, V.; Cay, V.V.; Gok, M.S. Properties of bricks with waste ferrochromium slag and zeolite. J. Clean. Prod. 2013, 59, 111–119. [Google Scholar] [CrossRef]
  12. Gencel, O. Characteristics of fired clay bricks with pumice additive. Energy Build. 2015, 102, 217–224. [Google Scholar] [CrossRef]
  13. Sutcu, M.; Alptekin, H.; Erdogmus, E.; Er, Y.; Gencel, O. Characteristics of fired clay bricks with waste marble powder addition as building materials. Constr. Build. Mater. 2015, 82, 1–8. [Google Scholar] [CrossRef]
  14. Sutcu, M.; del Coz Díaz, J.J.; Álvarez Rabanal, F.P.; Gencel, O.; Akkurt, S. Thermal performance optimization of hollow clay bricks made up of paper waste. Energy Build. 2014, 75, 96–108. [Google Scholar] [CrossRef] [Green Version]
  15. Phonphuak, N.; Kanyakam, S.; Chindaprasirt, P. Utilization of waste glass to enhance physical–mechanical properties of fired clay brick. J. Clean. Prod. 2016, 112, 3057–3062. [Google Scholar] [CrossRef]
  16. Stepien, A.; Kostrzewa, P.; Dachowski, R. Influence of barium and lithium compounds on silica autoclaved materials properties and on the microstructure. J. Clean. Prod. 2019, 236, 117507. [Google Scholar] [CrossRef]
  17. Dachowski, R.; Komisarczyk, K. Determination of microstructure and phase composition of sand-lime brick after autoclaving process. Procedia Eng. 2016, 161, 747–753. [Google Scholar] [CrossRef] [Green Version]
  18. Jasińska, I. Effect of foam glass granules fillers modification of lime-sand products on their microstructure. Open Eng. 2019, 9, 299–306. [Google Scholar] [CrossRef] [Green Version]
  19. Pytel, Z.; Maŀolepszy, J. Effect of mineral admixtures on some properties of sand-lime bricks. In Waste Management Series; Elsevier: Amsterdam, New Zealand, 2000; Volume 1, pp. 371–382. [Google Scholar]
  20. Pytel, Z.; Małolepszy, J. Effect of grain size composition of the calcium-sulphate fly ashes on the properties of autoclaved building materials. In Studies in Environmental Science; Elsevier: Amsterdam, The Netherlands, 1994; Volume 60, pp. 909–915. [Google Scholar]
  21. Dachowski, R.; Stępień, A. The impact of barium aggregate on the microstructure of sand-lime products. Adv. Mater. Res. 2011, 250–253, 618–621. [Google Scholar] [CrossRef]
  22. Stępień; Dachowski, R. Structural modification of sand-lime blocks regarding their physical and mechanical features. In Proceedings of the 8th PhD Symposium in Kgs., Copenhagen, Denmark, 20–23 June 2010; pp. 413–418. [Google Scholar]
  23. Jasińska, I. Effect of modification of sand-lime products on their basic functional properties. Tech. Trans. Civ. Eng. 2014, 1-B/2014, 39–45. [Google Scholar]
  24. Zhou, C.; Du, B.; Wang, N.; Chen, Z. Preparation and strength property of autoclaved bricks from electrolytic manganese residue. J. Clean. Prod. 2014, 84, 707–714. [Google Scholar] [CrossRef]
  25. Głowacka, A. Research and Analysis of Basic Technical Parameters of Silicate Bricks Exposed to the Capillary Water. Engineer’s Thesis, West Pomeranian University of Technology, Szczecin, Poland, March 2016. (In Polish). [Google Scholar]
  26. Maierhofer, C.h.; Wöstmann, J. Investigation of dielectric properties of brick materials as a function of moisture and salt content using a microwave impulse technique at very high frequencies. NDT E Int. 1998, 31, 259–263. [Google Scholar] [CrossRef]
  27. Sathiparan, N.; Rumeshkumar, U. Effect of moisture condition on mechanical behavior of low strength brick masonry. J. Build. Eng. 2018, 17, 23–31. [Google Scholar] [CrossRef]
  28. Franzoni, E.; Gentilini, C.; Graziani, G.; Bandini, S. Compressive behaviour of brick masonry triplets in wet and dry conditions. Constr. Build. Mater. 2015, 82, 45–52. [Google Scholar] [CrossRef]
  29. Zhang, Z.J. Experimental study on fundamental mechanical properties of autoclaved sand-lime brick masonr. Adv. Mater. Res. 2011, 168–170, 345–350. [Google Scholar] [CrossRef]
  30. Komisarczyk, K.; Dachowski, R. A study of selected properties of autoclaved bricks. Matec Web Conf. 2018, 174, 02017. [Google Scholar] [CrossRef]
  31. El Fgaier, F.; Lafhaj, Z.; Chapiseau, C.; Antczak, E. Effect of sorption capacity on thermo-mechanical properties of unfired clay bricks. J. Build. Eng. 2016, 6, 86–92. [Google Scholar] [CrossRef]
  32. Jasiński, R.; Drobiec, Ł.; Mazur, W. Validation of selected non-destructive methods for determining the compressive strength of masonry units made of autoclaved aerated concrete. Materials 2019, 12, 389. [Google Scholar] [CrossRef] [Green Version]
  33. Graubohm, M.; Brameshuber, W. Influence of the suction behavior of calcium silicate units on the properties of masonry under compressive load. In Brick and Block Masonry—Trends, Innovations and Challenges; Modena, C., Da Porto, F., Valluzzi, M.R., Eds.; Taylor & Francis Group: London, UK, 2016; pp. 495–502. [Google Scholar]
  34. Rzeszutko, M. Dampening of wall materials and safety of erected constructions. Ceram. Bud. 2017, 1–2, 4–6. (In Polish) [Google Scholar]
  35. Hendry, A.W. Masonry walls: Materials and construction—Review Article. Constr. Build. Mater. 2001, 15, 323–330. [Google Scholar] [CrossRef]
  36. Harmathy, T.Z.; Allen, L.W. Thermal performance of concrete masonry walls in fire. Fire Technol 1972, 8, 142–148. [Google Scholar] [CrossRef] [Green Version]
  37. Naser, M.Z. Properties and material models for common construction materials at elevated temperatures. Constr. Build. Mater. 2019, 215, 192–206. [Google Scholar] [CrossRef]
  38. Naser, M.Z.; Uppala, V.A. Properties and material models for construction materials post exposure to elevated temperatures. Mech. Mater. 2020, 142, 103293. [Google Scholar] [CrossRef]
  39. PN-B-02151-3:2015-10. Building Acoustics—Protection Against Noise in Buildings—Part 3: Requirements Concerning Sound Insulation of Partitions in Buildings and of Building Elements; PKN: Warsaw, Poland, 2015. [Google Scholar]
  40. Nurzyński, J. Is Thermal resistance correlated with sound insulation? Energy Procedia 2015, 78, 152–157. [Google Scholar] [CrossRef] [Green Version]
  41. Di Bella, A.; Granzotto, N.; Pavarin, C. Comparative Analysis of Thermal and Acoustic Performance of Building Elements; The Polish Acoustical Society: Kraków, Poland, 2014. [Google Scholar]
  42. Semprini, G.; Cocchi, A.; Marinosci, C. Possible correlation between acoustic and thermal performances of building structures. J. Acoust. Soc. Am. 2008, 123, 3609. [Google Scholar] [CrossRef]
  43. Garbalińska, H.; Głowacka, A.; Strzałkowski, J. Evaluation of dampness-induced strength reduction of calcium silicate blocks. E3S Web Conf. 2018, 49, 00028(1)–00028(7). [Google Scholar]
  44. PN-EN 772-16. Methods of Test for Masonry Units—Part 16: Determination of Dimensions; PKN: Warsaw, Poland, 2006. [Google Scholar]
  45. PN-EN 771-1. Specification for Masonry Units—Part 1: Clay Masonry Units; PKN: Warsaw, Poland, 2018. [Google Scholar]
  46. PN-EN 771-2:2011+A1:2015. Specification for Masonry Units—Part 2: Calcium Silicate Masonry Units; PKN: Warsaw, Poland, 2015. [Google Scholar]
  47. PN-EN 771-3. Specification for Masonry Units—Part 3: Aggregate Concrete Masonry Units (Dense and Lightweight Aggregates); PKN: Warsaw, Poland, 2015. [Google Scholar]
  48. PN-EN 771-4. Specification for Masonry Units—Part 4: Autoclaved Aerated Concrete Masonry Units; PKN: Warsaw, Poland, 2015. [Google Scholar]
  49. PN-EN 771-5. Specification for Masonry Units—Part 5: Manufactured Stone Masonry Units; PKN: Warsaw, Poland, 2011. [Google Scholar]
  50. PN-EN 771-6. Specification for Masonry Units—Part 6: Natural Stone Masonry Units; PKN: Warsaw, Poland, 2006. [Google Scholar]
  51. PN-EN ISO 9346. Hygrothermal Performance of Buildings and Building Materials—Physical Quantities for Mass Transfer; PKN: Warsaw, Poland, 2007. [Google Scholar]
  52. PN-EN 772-1:2011+A1:2015. Methods of Test for Masonry Units—Part 1: Determination of Compressive Strength; PKN: Warsaw, Poland, 2015. [Google Scholar]
  53. Drobiec, Ł.; Jasiński, R.; Piekarczyk, A. Wall Constructions in Accordance with the Eurocode 6 and Associated Regulations; PWN: Warszawa, Poland. (In Polish)
Figure 1. The scheme developed in-house showing the successive stages of preliminary experimental work, marked with symbols I, II, III and IV.
Figure 1. The scheme developed in-house showing the successive stages of preliminary experimental work, marked with symbols I, II, III and IV.
Materials 13 03817 g001
Figure 2. Overview of compressive strength values designated for silicate specimens CS-E-1–CS-E-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Figure 2. Overview of compressive strength values designated for silicate specimens CS-E-1–CS-E-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Materials 13 03817 g002
Figure 3. Overview of compressive strength values designated for silicate specimens CS-X-1–CS-X-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Figure 3. Overview of compressive strength values designated for silicate specimens CS-X-1–CS-X-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Materials 13 03817 g003
Figure 4. Overview of compressive strength values designated for silicate specimens CS-B-1–CS-B-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Figure 4. Overview of compressive strength values designated for silicate specimens CS-B-1–CS-B-6 (6 dry and 6 water-saturated), with fC1 (for dry state) and fC2 (for saturated state) averages.
Materials 13 03817 g004
Figure 5. Integral pore distribution curves of the three tested silicates.
Figure 5. Integral pore distribution curves of the three tested silicates.
Materials 13 03817 g005
Figure 6. Differential pore distribution curves of the three tested silicates.
Figure 6. Differential pore distribution curves of the three tested silicates.
Materials 13 03817 g006
Figure 7. SEM (Scanning Electron Microscopy) images (left) of individual silicate samples at ×200 magnification: (a) CS-E, (b) CS-X, (c) CS-B and the EDS (Electron Dispersive Spectroscopy) results (right).
Figure 7. SEM (Scanning Electron Microscopy) images (left) of individual silicate samples at ×200 magnification: (a) CS-E, (b) CS-X, (c) CS-B and the EDS (Electron Dispersive Spectroscopy) results (right).
Materials 13 03817 g007
Table 1. Comparison of the average values of the main parameters characterizing individual groups of tested silicate products.
Table 1. Comparison of the average values of the main parameters characterizing individual groups of tested silicate products.
Product NamefC1 (MPa)fC2 (MPa)A (kg/(m2·h0.5)ρp (kg/m3)nw (%)nv (%)
CS-E26.617.83.6184013.424.7
CS-X34.922.05.2163818.830.7
CS-B39.627.38.3183014.326.1
Table 2. The proportions of the weights of main elements in the tested specimens.
Table 2. The proportions of the weights of main elements in the tested specimens.
ElementElement Weight (%)
CS-ECS-XCS-B
O58.1656.0556.15
Si25.8226.3128.47
Ca14.8715.6614.15
Al0.881.120.86
Fe0.270.860.37
Total (%)100.00
Table 3. The values of the shape factor d, [52].
Table 3. The values of the shape factor d, [52].
Height (mm)Width (mm)
50100150200≥250
400.800.70---
500.850.750.70--
650.950.850.750.700.65
1001.151.000.900.800.75
1501.301.201.101.000.95
2001.451.351.251.151.10
≥2501.551.451.351.251.15
Table 4. The results obtained from the compressive strength tests carried out on the CS-E specimens used to convert to the strength class of the product.
Table 4. The results obtained from the compressive strength tests carried out on the CS-E specimens used to convert to the strength class of the product.
Samplefc1 (MPa)fc2 (MPa)ηw1ηw2 Averaged   h a v ,   1   ( mm ) Averaged   h a v ,   2   ( mm ) d (Interpolation)fb1 = ηwdfC1 (MPa)fb2 = ηwdfC2 (MPa)Class
CS-E-126.418.10.81.2711150.8618.318.415
CS-E-226.318.3
CS-E-328.418.2
CS-E-424.916.8
CS-E-527.518.3
CS-E-626.317.1
Table 5. The results obtained from the compressive strength tests carried out on the CS-X specimens used to convert to the strength class of the product.
Table 5. The results obtained from the compressive strength tests carried out on the CS-X specimens used to convert to the strength class of the product.
Samplefc1 (MPa)fc2 (MPa)ηw1ηw2 Averaged   h a v ,   1   ( mm ) Averaged   h a v ,   2   ( mm ) d (Interpolation)fb1 = ηwdfC1 (MPa)fb2 = ηwdfC2 (MPa)Class
CS-X-134.420.00.81.2641200.8122.621.420
CS-X-241.421.8
CS-X-329.021.7
CS-X-435.323.2
CS-X-536.821.6
CS-X-632.523.7
Table 6. The results obtained from the compressive strength tests carried out on the CS-B specimens used to convert to the strength class of the product.
Table 6. The results obtained from the compressive strength tests carried out on the CS-B specimens used to convert to the strength class of the product.
Samplefc1 (MPa)fc2 (MPa)ηw1ηw2 Averaged   h a v ,   1   ( mm ) Averaged   h a v ,   2   ( mm ) d (Interpolation)fb1 = ηwdfC1 (MPa)fb2 = ηwdfC2 (MPa)Class
CS-B-136.425.70.81.2791200.8727.628.525
CS-B-241.627.0
CS-B-334.927.9
CS-B-441.926.6
CS-B-541.429.3
CS-B-641.227.1

Share and Cite

MDPI and ACS Style

Garbalińska, H.; Strzałkowski, J.; Stolarska, A. Moisture Influence on Compressive Strength of Calcium Silicate Masonry Units–Experimental Assessment and Normative Calculations. Materials 2020, 13, 3817. https://doi.org/10.3390/ma13173817

AMA Style

Garbalińska H, Strzałkowski J, Stolarska A. Moisture Influence on Compressive Strength of Calcium Silicate Masonry Units–Experimental Assessment and Normative Calculations. Materials. 2020; 13(17):3817. https://doi.org/10.3390/ma13173817

Chicago/Turabian Style

Garbalińska, Halina, Jarosław Strzałkowski, and Agata Stolarska. 2020. "Moisture Influence on Compressive Strength of Calcium Silicate Masonry Units–Experimental Assessment and Normative Calculations" Materials 13, no. 17: 3817. https://doi.org/10.3390/ma13173817

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop