Next Article in Journal
Injectable Hydrogels in Cardiovascular Tissue Engineering
Next Article in Special Issue
Research Progress of Natural Rubber Wet Mixing Technology
Previous Article in Journal
Transparent Superhydrophobic and Self-Cleaning Coating
Previous Article in Special Issue
Investigation of Macroscopic Mechanical Behavior of Magnetorheological Elastomers under Shear Deformation Using Microscale Representative Volume Element Approach
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Novel Reactive Polyhedral Oligomeric Silsesquioxane-Reinforced and Toughened Epoxy Resins for Advanced Composites

1
Key Laboratory for Specially Functional Polymeric Materials and Related Technology of (Ministry of Education), School of Materials Science and Engineering, East China University of Science and Technology, Shanghai 200237, China
2
HuaChang Polymers Co., Ltd., East China University of Science and Technology, Shanghai 200241, China
3
Manufacturing Center of Composite Materials for Commercial Aircraft, Shanghai Aircraft Manufacturing Co., Ltd., COMAC, Shanghai 201324, China
*
Author to whom correspondence should be addressed.
Polymers 2024, 16(13), 1877; https://doi.org/10.3390/polym16131877
Submission received: 22 April 2024 / Revised: 17 June 2024 / Accepted: 25 June 2024 / Published: 1 July 2024
(This article belongs to the Special Issue Advances in Functional Rubber and Elastomer Composites II)

Abstract

:
Most toughening methods for epoxy resins are usually used at the expense of other properties. Some polyhedral oligomeric silsesquioxanes (POSSs) with both a rigid Si-O-Si structure and flexible organic chain segments could be expected to be effective toughening agents. In this study, three reactive polyhedral oligomeric silsesquioxanes with a thiol group (OMPPS), a carboxyl group (OCOPS), and an epoxy group (OGCPS) were synthesized and characterized. They were utilized as modifiers to toughen 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline (AFG-90MH)/4,4′-methylenebis(2-ethylaniline) (MOEA) (epoxy resin) with different molar ratios to obtain hybrid resins named OMPPS-EP-i, OCOPS-EP-j, and OGCPS-EP-k. The effects of the amount of modifier added and the length of the organic chain on the cage structure on various properties of the hybrid resins were investigated. The results show that all three modifiers show good compatibility with the epoxy resin. The hybrid resins have a low viscosity at 45~85 °C and can be cured at a low temperature (110 °C). The cured hybrid resins display improved toughness. Typically, the critical stress intensity factor (KIC) and impact strength of OGCPS-EP-0.6-C are 2.54 MPa∙m−1/2 and 19.33 kJ∙m−2, respectively, which increased by 58.75% and 22.48% compared with the pristine epoxy resin, respectively. In addition, the glass transition temperature and flexural strength of the hybrid resins are basically unchanged.

Graphical Abstract

1. Introduction

Aerospace technology, being a highly sophisticated and state-of-the-art field, serves as a significant emblem of advancements in modern science and technology. The realization of this technology is inseparable from the support of advanced materials. In the aerospace field, due to its extremely harsh operating environment, the material requirements of performance are more stringent. High-performance epoxy resins have found extensive applications as matrix resins in aerospace component composites owing to their good thermal stability [1], high glass transition temperature, excellent mechanical properties, and low curing shrinkage [2,3,4,5,6]. However, the high crosslinking density of the epoxy resins also results in low toughness, which significantly limits their usage in some situations. Therefore, enhancing the toughness of the epoxy resins has always been one of the key subjects for high-performance epoxy resins.
There are organic and inorganic toughening agents for toughening epoxy resins. Organic toughening agents include liquid rubbers [7,8], thermoplastic polymers [9,10,11], hyperbranched polymers [12,13], and liquid crystal polymers [14]. They have a good toughening effect, but usually at the expense of the mechanical and thermal properties of the epoxy resins. In addition, because the load amount of the agents is generally high, the viscosity of the modified epoxy resins will increase, which is not conducive to the processing of the resins. Inorganic toughening agents include graphene oxide [15,16,17,18], carbon nanotubes [19,20], nano-silica [21,22], and nano-clay [23]. They can maintain good mechanical properties while toughening epoxy resins. However, they are easy to aggregate in the resins because of the small size and large specific surface area of the nanoparticles, which form stress concentration points and reduce the performance of the resins.
Polyhedral oligomeric silsesquioxane (POSS), a kind of nano organic–inorganic hybrid molecule, is composed of a silicon and oxygen skeleton and has attracted extensive attention from researchers in recent years [24,25]. The general molecular formula of POSS can be abbreviated as (RSiO1.5)n (where R stands for an organic group and n could be 8, 10, or 12). The center of POSS is a rigid inorganic Si-O-Si core and the exterior is connected to soft organic groups. POSS can be diversified through different chemical reactions, which can make POSS meet various application requirements. According to different external organic groups, POSSs can be divided into reactive POSSs and non-reactive POSSs. As a toughening agent for an epoxy resin, reactive POSSs can participate in the curing reaction of the epoxy resin through organic groups [26,27,28,29,30,31], and non-reactive POSSs can be uniformly dispersed in the resin by physical blending [32]. The molecular dispersion of reactive POSSs can be achieved through participation in the curing reaction of the epoxy resin, thereby enhancing the compatibility between POSSs and the epoxy resin.
Liu et al. [25] toughened an epoxy resin with POSS-grafted polyurethane (POSS-PU). The impact strength of the toughened epoxy resin increased by 115%, but the viscosity of the resin increased and the glass transition temperature decreased. Yang et al. [33] mixed octavinyl polyhedral oligomeric silsesquioxane (EPOSS)-modified vinyl resin with epoxy resin to form an interpenetrating network structure to toughen the epoxy resin. The impact strength of the resin increased by 139.6%, but the glass transition temperature decreased. Mishra et al. [28] incorporated trisilanol phenyl POSS and glycidyl POSS separately into an epoxy resin (EPON 862). Obviously, the trisilanol phenyl POSS is a non-reactive POSS and the glycidyl POSS is a reactive POSS. The toughness of the incorporated epoxy resins is increased by 30% and 130%, respectively. The toughening efficiency of the reactive POSS is much higher than that of the non-reactive POSS. Han et al. [26] modified an epoxy resin with octa-glycidyl POSS (OG-POSS) as a toughening agent. OG-POSS participated in the curing reaction and was evenly dispersed in the epoxy resin. The modified resin not only maintained the original glass transition temperature, flexural strength, and thermal stability but also increased the impact strength by 56%.
In this study, in view of the nano-sized hollow structure of polyhedral oligomeric silsesquioxanes and their good compatibility with a resin, three reactive polyhedral oligomeric silsesquioxanes with a thiol group (OMPPS), a carboxyl group (OCOPS), and an epoxy group (OGCPS) were synthesized and incorporated into the blend of 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline/4,4′-methylenebis(2-ethylaniline) (epoxy resin) to obtain OMPPS-EP-i, OCOPS-EP-j, and OGCPS-EP-k hybrid resins with good comprehensive properties. The effect of the structure and content of the three modifiers on the curing behavior of the hybrid resins, as well as the thermal and mechanical properties of the cured resins, was investigated and compared.

2. Experimental

2.1. Materials

(3-Mercaptopropyl) trimethoxysilane (analytical purity), 10-undecylenoic acid (analytical purity), and 2,2′-azobis(2-methylpropionitrile) (AIBN) (analytical purity) were purchased from Shanghai Titan Technology Co., Ltd. 4-Hydroxybenzaldehyde (analytical purity) was bought from Jiangsu Anhuai Chemical Technology Co., Ltd. (Nantong, China). Methyl triphenyl phosphonium bromide (analytical purity) was supplied by Shanghai Zhonghe Chemical Technology Co., Ltd. (Shanghai, China). Potassium tert-butanol (analytical purity) was purchased from Shanghai XINBO Chemical Technology Co., Ltd. (Shanghai, China). Sodium hydride (analytical purity), epichlorohydrin (analytical purity), tetrabutylammonium bromide (analytical purity), and sodium hydroxide (analytical purity) were bought from Shanghai Boer Chemical Technology Co., Ltd. (Shanghai, China). Hydrochloric acid was bought from Sinopharm Chemical Reagent Co., Ltd. (Shanghai, China). Epoxy resin AFG-90MH (industrial grade) was supplied by Shanghai Huayi Resin Co., Ltd. (Shanghai, China). 4,4″-Methylenebis(2-ethylbenzenamine) (MOEA) (analytical purity) was purchased from Shanghai Bide Pharmaceutical technology Co., Ltd. (Shanghai, China). The release agent (909A 45) was supplied by Dongguan Jiadan lubricating oil Co., Ltd. (Dongguan, China). All solvents (analytical purity) were purchased from Shanghai Titan Technology Co., Ltd. (Shanghai, China).

2.2. Synthesis of Octa (Mercaptopropyl) Polyhedral Oligomeric Silsesquioxane (OMPPS)

The synthetic route of OMPPS is shown in Scheme 1. First, 20 g of (3-Mercaptopropyl) trimethoxysilane (0.1 mol) and 25 mL of concentrated hydrochloric acid (36%) were added to a 1 L three-necked flask which contained 500 mL of methanol and stirred at 65 °C for 24 h under a N2 atmosphere. At the end of the reaction, the precipitate at the bottom of the flask was collected, washed three times with methanol, and dissolved in dichloromethane. Then, the obtained solution was washed three times with deionized water and dried to remove the solvent, followed by vacuum drying in a vacuum oven at 40 °C for 8 h to obtain OMPPS with a yield of 75%.

2.3. Synthesis of Octa (Carboxyl Decyl Thiopropyl) Polyhedral Oligomeric Silsesquioxane (OCOPS)

The synthetic route of OCOPS is shown in Scheme 2. First, 18.4 g of undecylenic acid (0.1 mol) and 1.0 g of 2,2′-azobis(2-methylpropionitrile) (AIBN) (6 mmol) were added to a 250 mL three-necked flask which contained 70 mL of dried tetrahydrofuran. The mixture in the flask was stirred until the solids were completely dissolved and heated up to 60 °C under N2. Then, a tetrahydrofuran solution (50 mL) containing 10.2 g (0.01 mol) OMPPS was added dropwise to the flask while stirring, and the addition time was controlled at 10~15 min. The reaction was stopped after maintaining at 60 °C for 6 h. After the reaction, the solution was concentrated and poured into 300 mL of methanol for sedimentation, and a white precipitate product was obtained. The product was placed in a vacuum oven and dried at 60 °C for 8 h to obtain OCOPS with a yield of 57%.

2.4. Synthesis of Octa (Glycidyl Phenyl Ethyl Thiopropyl) Polyhedral Oligomeric Silsesquioxane (OGCPS)

The synthetic route of OGCPS is shown in Scheme 3. 4-Vinyl phenyl glycidyl ether (DGHDS) was synthesized from 4-hydroxy styrene (HDS) and epichlorohydrin, which is shown in the supporting information.
First, 17.6 g of DGHDS (0.1 mol) and 1.0 g of 2,2′-azobis(2-methylpropionitrile) (AIBN) (6 mmol) were added to a 250 mL three-necked flask which contained 100 mL of dried tetrahydrofuran. The mixture was stirred until the solids were completely dissolved and heated up to 60 °C under N2. Then, a tetrahydrofuran solution (50 mL) containing 10.2 g (0.01 mol) OMPPS was added dropwise to the flask while stirring, and the addition time was controlled at 10~15 min. The reaction was stopped after maintaining at 60 °C for 6 h. After the reaction, the solution was concentrated and poured into 300 mL of methanol for sedimentation, and a light-yellow oily precipitate was obtained. After washing with methanol three times, the light-yellow oily precipitate was placed in a vacuum oven and dried at 60 °C for 8 h to obtain OMPPS with a yield of 52%.

2.5. Preparation of Hybrid Resins

The epoxy resin used in this study is 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline (AFG-90MH), and the curing agent is 4,4′-methylenebis(2-ethylaniline) (MOEA). The structural formulas of AFG-90MH and MOEA are shown in Figure 1. The pristine epoxy resin (EP) used as the control group consisted of AFG-90MH and MOEA. The obtained reactive polyhedral oligomeric silsesquioxanes (OMPPS, OCOPS, and OGCPS) were separately mixed into the EP to obtain the hybrid resins. The molar ratio of active hydrogen to the epoxy group in the hybrid resins was controlled at 1:1.

2.5.1. Preparation of OMPPS- or OGCPS-Modified Epoxy Hybrid Resins

AFG-90MH, MOEA, and OMPPS were dissolved in THF in a flask under stirring. After removing THF using a vacuum at 60 °C, the OMPPS-modified epoxy hybrid resins were obtained and named as OMPPS-EP-i (i = 0.3, 0.8, 1.4, 1.9, 2.8). The OGCPS-modified epoxy resins were made in the same way and named as OGCPS-EP-j (j = 0.1, 0.3, 0.6, 0.8, 1.2). The i and j are the molar percentage of OMPPS and OGCPS in the hybrid resins, respectively.

2.5.2. Preparation of OCOPS-Modified Epoxy Hybrid Resins

First, OCOPS was dissolved in DMF in a flask, and the produced solution was mixed with AFG-90MH and prepolymerized at 110 °C for 0.5 h. Then, DMF was removed using a vacuum, and a homogeneous resin was obtained. Finally, MOEA was added to the resin to obtain the OCOPS-modified epoxy hybrid resins, named OCOPS-EP-k (k = 0.1, 0.3, 0.6, 0.8, 1.2, 1.6, 1.9), in which k is the molar percentage of OCOPS in the OCOPS-modified epoxy resins.

2.6. Preparation of Cured Hybrid Resins

The obtained hybrid resins were poured into the treated molds, respectively, and then the molds containing the resins were placed in a vacuum oven and evacuated at 90 °C for 0.5 h to remove the residual solvent. Afterward, the resins with molds were moved to an oven and heated to 110 °C, then kept at 110 °C for 2 h and 150 °C for another 2 h to obtain the cured resins. The obtained cured resins were abbreviated as EP-C, OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C, respectively.

2.7. Instruments and Measurements

The 1H NMR spectrum was obtained on the AVANCE 400 Ⅲ spectrometer (Bruker, Switzerland) at an operating frequency of 400 MHz with chloroform-D (CDCl3) or DMSO-d6 as the deuterated solvent and tetramethylsilane as the internal standard. The FT-IR spectrum was obtained using a Nicolet iS10 infrared spectrometer (Thermo Scientific, Madison, WI, USA). Elemental analysis tests were conducted on the VARIO EL CUBE elemental analyzer (ELEMENTAR, Hanau, Germany). The relative molecular masses of POSSs were obtained by 4800 plus time-of-flight mass spectrometry (ABS, MAS Building, Singapore). The 29Si NMR spectrum was obtained on the Ascend 600 spectrometer at an operating frequency of 600 MHz with CDCl3 or DMSO-d6 as the deuterated solvent and chromium acetylacetonate as the relaxation reagent. Differential scanning calorimetry (DSC) was run on a DSC214 (NETZSCH, Selb, Germany) instrument at the heating rate of 10 °C/min under nitrogen flow from 40 °C to 300 °C. Dynamic thermomechanical analysis (DMA) was performed on a DMA 1 mechanical analyzer (Mettler Toledo, Greifensee, Switzerland) by using the three-point bending mode at a heating rate of 5 °C/min with a frequency of 1 Hz under nitrogen flow. The flexural performance and fracture toughness of the cured resin were measured using a SANS CMT 4204 universal testing machine (Sansi Material Testing Co., Ltd., Shenzhen, China) at a speed of 2.00 mm/min and 1.5 mm/min, respectively, at room temperature with the three-point bending method. The impact performances of the cured resins were obtained by a CEAST 9050 cantilever beam impact testing machine (CEAST, Torino, Italy). The fracture surface of the cured resins was characterized by S-4800/S-3400 scanning electron microscopy (HITACHI, Tokyo, Japan).

3. Results and Discussion

3.1. The Structural Characterization of OMPPS, OCOPS, and OGCPS

The structures of OMPPS, OCOPS, and OGCPS were characterized by FT-IR spectroscopy, and the spectra are shown in Figure 2a. The absorption peaks around 1100 cm−1 are the Si-O-Si stretching vibration peaks in OMPPS, OCOPS, and OGCPS. The peak at 2554 cm−1 corresponds to the -SH of OMPPS. The absorption peak of -SH disappears and the peak of -COOH at 1703 cm−1 for OCOPS appears, indicating that OCOPS has been successfully synthesized. In the FT-IR spectrum of OGCPS, the absorption peak of -SH also disappeared, and the absorption peak of the epoxy group appeared at 915 cm−1, indicating that the -SH at the eight corners of OMPPS has completely reacted with the vinyl group of DGHDS to form OGCPS. Figure 2b shows the 1H NMR spectra of OMPPS, OCOPS, and OGCPS. The solvent of the 1H NMR analysis for OMPPS and OGCPS is CDCl3 and the solvent for OCOPS is DMSO-d6. In the 1H NMR spectrum of OMPPS, the resonance peaks for the hydrogens of three methylene in the mercaptopropyl group are found at chemical shifts of 0.77 ppm(a1), 1.72 ppm(b1), and 2.57 ppm(c1), respectively, and the resonance peak of sulfhydryl hydrogen is found at chemical shift of 1.38 ppm(d1). The area ratio of the peaks for the hydrogens at a1, b1, c1, and d1 is 2.07:2.14:1.98:1.0. In the 1H NMR spectrum of OCOPS, the chemical shifts of the methylene hydrogens at a2, b2, and c2 move to the high field under the influence of the long-chain alkane group, compared to those of the hydrogens of OMPPS at a1, b1, and c1, which are 0.73 ppm, 1.60 ppm, and 2.50 ppm, respectively. The resonance peak of sulfhydryl hydrogen disappears, indicating that the sulfhydryl group has completely participated in the reaction, and the eight corners of POSS have become carboxyl-terminated groups. Under the influence of the thioether group, the chemical shifts of hydrogens for methylene-connected sulfur atoms are close, at about 2.50 ppm. The chemical shift of methylene hydrogens at d2 is influenced by the thioether group and moves to the lower field, at 1.47 ppm, while the chemical shift of methylene hydrogens at e2 is less affected and is 1.24 ppm. Due to the influence of the carboxyl group, the resonance peak of methylene hydrogens connected with the carboxyl group moves to the lower field and is 2.17 ppm. The peak area ratio is 2.00:2.05:4.07:3.98:12.14:2.0 for hydrogens at a2, b2, c2, d2, e2, and f2, respectively. In the 1H NMR spectrum of OGCPS, the resonance peaks at a3, b3, and c3 are slightly shifted to the lower field as compared to the hydrogens of OMPPS at a1, b1, and c1, with chemical shifts of 0.74 ppm, 1.68 ppm, and 2.53 ppm, respectively. The resonance peak of sulfhydryl hydrogen disappears, indicating that the sulfhydryl group has completely reacted, and the eight corners of POSS have become hydrocarbon chains with a terminal epoxy group. In addition, the chemical shifts of other hydrogen atoms in OGCPS can also correspond with each other in the spectrum. The peak area ratio of the hydrogens at a3, b3, (c3 + d3 + j3 + e3), i3, h3, g3, and f3 is 2.14:2.18:7.92:1.00:2.14:2.08:2.0.
The 29Si NMR spectra of OMPPS, OCOPS, and OGCPS are shown in Figure 3. The solvent of the 29Si NMR analysis of OMPPS and OGCPS is CDCl3 and the solvent for OCOPS is DMSO-d6. The 29Si NMR spectra of OMPPS, OCOPS, and OGCPS show a large single peak, indicating that the purity is high. In addition, the relative molecular masses of OMPPS, OCOPS, and OGCPS were determined by using MALDI-TOF-MS, and the results are shown in Figure S2. The analysis results are as follows: OMPPS (product + Na+): 1039.20 Da (calculated: 1039.14), OCOPS (product + Na+): 2512.33 Da (calculated: 2512.33), and OGCPS (product + Na+): 2447.30 Da (calculated: 2447.27). These results show that the molecular weights of OMPPS, OCOPS, and OGCPS are 1016, 2489, and 2424, respectively. The above test results demonstrate that OMPPS, OCOPS, and OGCPS were successfully synthesized.
The solubility of OMPPS, OCOPS, and OGCPS has an influence on the subsequent application. The dissolution behaviors of OMPPS, OCOPS, and OGCPS in common organic solvents are listed in Table 1. OMPPS and OGCPS have good solubility and can be dissolved in dichloromethane, tetrahydrofuran, ethyl acetate, N,N-dimethylformamide, and dimethyl sulfoxide. However, OCOPS has poor solubility and can be dissolved in tetrahydrofuran, N,N-dimethylformamide, and dimethyl sulfoxide.

3.2. The Processability of Hybrid Resins

Viscosity has an important effect on the processability of the epoxy resin. Figure 4 shows the viscosity of different resins as a function of the temperature. Obviously, the addition of OMPPS, OCOPS, and OGCPS has no significant effect on the viscosity of the epoxy resin. The viscosity of hybrid resins is lower than 500 mPa∙s at 45~85 °C, which is suitable for the liquid molding (RTM) process of composite materials.

3.3. Thermal Curing Behaviors of Hybrid Resins

In order to investigate the curing behavior of the hybrid resins, a differential scanning calorimeter (DSC) was used. Figure 5a–c shows the DSC curves of the OMPPS-EP-i, OCOPS-EP-j, and OGCPS-EP-k hybrid resins, and the detailed analysis data are listed in Table S1. It can be seen that the addition of OMPPS and OGCPS has no effect on the curing behaviors of the epoxy resin, but the addition of OCOPS can slightly reduce the curing temperature. This may be due to the fact that the carboxyl groups in OCOPS have a higher reactivity with epoxy resin than active groups in OMPPS and OGCPS. In order to compare the effects of different modifiers on the thermal curing behavior of the epoxy resin, we selected three hybrid resins with a modifier addition amount of 0.8 mol% for comparison. Figure 5d shows the DSC curves of the epoxy resin and hybrid resins with a 0.8 mol% load of the modifier. It can be seen that under conditions where the same molar amount is added, OCOPS is beneficial in promoting the thermal cross-linking reaction of epoxy resin.
The Ti (initial curing temperature) and Tp (top curing peak temperature) of the modified resins usually vary with the heating rate. The higher the heating rate, the higher the Ti and Tp. We conducted DSC tests for the pristine epoxy resin at various heating rates. The Ti0 and Tp0 at the heating rate of zero are obtained through the linear extrapolation of the Ti and Tp with the heating rate (Figure S4), and are 110 °C and 155 °C, respectively. Therefore, 110 °C/2 h + 150 °C/2 h was selected as the curing process of the epoxy resin. Figure 6 shows the DSC curves of OMPPS-EP-0.8, OCOPS-EP-0.8, and OGCPS-EP-0.8 before and after curing. There is no obvious exothermic peak in the cured epoxy resins, indicating that the epoxy resins have been completely cured.
FT-IR spectroscopy was adopted to investigate the structural changes in the hybrid resins during the curing process. The FT-IR spectra of the hybrid resins with 0.8 mol% modifier content before and after curing are shown in Figure 7. As shown in Figure 7a, the absorption peaks at 3400~3500 cm−1 are assigned to the stretching vibration peak of the amino group in the curing agent (MOEA). The absorption bands at 2554 cm−1 and 1703 cm−1 are attributed to the stretching vibration of -SH and -COOH, respectively, indicating that the modifiers have been introduced into the epoxy resin. After curing, the absorption peaks of -NH2 for the curing agent and the absorption peaks of the epoxy group (915 cm−1) disappeared, and a new absorption peak of -OH appeared, indicating that the amino group and epoxy group have completely reacted. In addition, the absorption peak of -SH in OMPPS-EP-0.8 and the absorption peak of -COOH in OCOPS-EP-0.8 disappeared after curing, indicating that OMPPS and OCOPS have participated in the curing reaction of the epoxy resins.

3.4. Mechanical Properties of Cured Hybrid Resins

3.4.1. Flexural and Impact Properties of Cured Hybrid Resins

The toughness and strength of resins have a significant influence on the performance of terminal fiber reinforced composites. The flexural properties of the cured hybrid resins were tested and the results are shown in Figure 8. When the amount of modifier added is small, the flexural properties of the cured hybrid resins increase slightly and then reach a peak value. However, as the amount of modifier added increases, the flexural properties begin to decline slightly. The reason for this phenomenon may be that at low loading, the rigid inorganic nano-scale Si-O-Si core is uniformly dispersed, which can disperse the stresses concentrated on the crack tip and thus increase the flexural properties of the cured hybrid resins. However, with the continuous addition of the POSS modifiers, POSS molecules self-assemble and aggregate to form the so-called “hard-core soft-shell particles”, which play a plasticizing role, resulting in a decline in the flexural properties of cured hybrid resins [28].
As shown in Figure 8, the flexural strength of OMPPS-EP-0.3-C reaches 138 MPa, compared with the flexural strength of 136 MPa for EP-C. Compared with OMPPS, OCOPS has longer and more flexible alkyl chain segments, the distance between the molecular chains is increased, and the free volume fraction in the cured resin is increased. Thus, the flexural strength of OCOPS-EP-0.6-C increases to 149 MPa, which is 10% higher than that of EP-C. As for OGCPS-EP-0.6-C with the same modifier addition ratio, the flexural strength of OGCPS-EP-0.6-C reaches 137 MPa, which is close to that of the pristine resin. This is mainly due to OGCPS’s molecular structure, which contains rigid benzene rings, increasing the rigidity of the cured resins (flexural modulus: OGCPS-EP-0.6-C > OCOPS-EP-0.6-C) and restricting the movement of the molecular chain. In summary, these results show that OMPPS, OCOPS, and OGCPS can effectively maintain or improve the flexural properties of epoxy resins at a certain dosage.
Impact performance tests were conducted on the cured resins, and the results are shown in Figure 9. It can be seen that the impact strength of OMPPS-EP-i-C and OGCPS-EP-j-C increases first and then decreases with an increase in the amount of modifier added, while the impact strength of OCOPS-EP-k-C increases with an increase in the amount of OCOPS added.
OMPPS, OCOPS, and OGCPS contain functional groups that can participate in the curing reactions of the epoxy resin, which can cause them to become better dispersed in the resin. POSSs, with rigid -Si-O-Si- cage-like structures, are uniformly distributed in the epoxy networks. When the cured epoxy structures are subjected to impact, POSSs play a dual role. On the one hand, they are able to absorb some energy as stress concentration points and thereby facilitate the dispersion of the stress. On the other hand, they also prevent the formation and propagation of micro-cracks, while forming shear bands within the resins to absorb another portion of the impact energy [26,28,34]. Organic soft segments in POSSs can also increase the flexibility of the polymer chain [35,36,37] and thus increase the impact strength of the epoxy resins. However, the impact strength decreases with the further loading of the amount of POSSs. The decline is possibly related to the assembling of POSSs.
In order to further analyze the relationship between the impact strength of the hybrid resins and the type and amount of modifier added, the micromorphology of the cured resins was investigated. The fracture surfaces of cured resins were observed by scanning electron microscopy (SEM), and the results are shown in Figure 10. As can be seen from Figure 10, EP-C presents a smooth fracture surface, indicating that the break of the resin is a brittle fracture. With the addition of OMPPS, OCOPS, and OGCPS, the fracture surfaces of the cured resins become rough, indicating that the fracture mode changes from brittleness to toughness [25,38,39]. For OMPPS-modified epoxy resins and OGCPS-modified epoxy resins, the roughness of the fracture surfaces first increases and then decreases with increases in POSS load amount. For OCOPS-modified epoxy resins, the roughness of the fracture surfaces increases with the increase in POSS load amount. The results demonstrate the change in impact strength.

3.4.2. Fracture Toughness of Cured Hybrid Resins

Fracture toughness refers to the ability of a material to prevent the unstable propagation of macro cracks, which can generally be represented by the critical stress intensity factor (KIC). The larger the KIC, the better the fracture toughness of the material. Figure 11 shows the KIC of OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
As shown in Figure 11, the KIC of OMPPS-EP-i-C and OGCPS-EP-k-C increases first and then decreases with the increase in the amount of modifier added, but the toughening effect of OGCPS is much better than that of OMPPS. The KIC of the pristine epoxy resin is 1.60 MPa∙m−1/2. When the addition amounts of OMPPS and OGCPS were 1.4 mol% and 0.6 mol%, respectively, the KIC of the cured resin reached the maximum, which was 1.98 MPa∙m−1/2 and 2.54 MPa∙m−1/2. Compared with the KIC of EP-C, it increased by 23.75% and 58.75%. The fracture toughness of OCOPS-modified epoxy resin increases with the increase in OCOPS addition. When the addition amount is 1.9 mol%, the KIC of OCOPS-EP-1.9-C is 2.53 MPa∙m−1/2, which is increased by 58.13% and close to the toughness of the OGCPS-EP-0.6-C resin.
There are two factors that affect the fracture toughness of the hybrid resins. One is the load capacity of OMPPS, OCOPS, and OGCPC in the epoxy resin, and the other is the different organic chain segments and functional groups in OMPPS, OCOPS, and OGCPC. When OMPPS or OGCPS is added to the epoxy resin, the fracture toughness of the hybrid resins first increases and then decreases, and there is a maximum value. After reaching the maximum value, further addition of OMPPS or OGCPS leads to a decrease in fracture toughness. This probably results from the aggregation of modifiers at a high load amount, which form stress concentration points within the resin when the resin is stressed [29,40]. The aggregation of the modifiers was observed by SEM, and the results are shown in Figure S5. Unlike OMPPS and OGCPS, the fracture toughness of the OCOPS-modified epoxy resins increases with the increase in OCOPS load amount. This may probably result from the long and flexible aliphatic chains at the eight corners of OCOPS.
In addition to the load capacity of OMPPS, OCOPS, and OGCPC, the difference in the organic segments of OMPPS, OCOPS, and OGCPC also leads to different toughening effects on the epoxy resin. OCOPS and OGCPS exhibit superior performance in enhancing the toughness of epoxy resins compared to OMPPS. This is primarily attributed to the longer molecular chain segments of OCOPS and OGCPS than those of OMPPS. These long flexible chain segments allow them to easily move and absorb more energy when the resins are subjected to stress. In addition, OGCPS exhibits better toughening effects on the epoxy resins compared to OCOPS before OGCPS agglomerates in the resin. This is possibly due to the presence of benzene rings in the organic chain segments and the glycidyl groups of OGCPS [36].

3.5. Thermal Properties of Cured Hybrid Resins

Dynamic mechanical analysis (DMA) was used to analyze the thermal mechanical properties of the cured resins, and the results are shown in Figure 12. As can be seen from Figure 12, OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C have a lower storage modulus (E’) than EP-C. All three modifiers have a caged hollow structure and flexible organic chain segments on the outside. Introducing them into the epoxy resin will lead to an increase in the free volume of the hybrid resin, causing a decrease in the storage modulus. The crosslinking density of the cured resins can be calculated using the data from the DMA curves, and the results are shown in Table S2. The results show the crosslinking density of the cured hybrid resins is lower than that of the cured pristine epoxy resin, which indicates the toughness contribution. The presence of a single peak in all tanδ curves indicates good compatibility between OMPPS, OCOPS, OGCPC, and the epoxy resin. The temperature corresponding to the peak is the glass transition temperature (Tg) of the cured resin. The Tg values of all epoxy resins are listed in Table 2. The introduction of OMPPS and OGCPS had no significant effect on the Tg of the cured hybrid resin. This is because OMPPS and OGCPS both have rigid internal Si-O-Si structures and external flexible organic chain segments, and the effects of the two on the Tg offset each other. However, the Tg of OCOPS-EP-j-C had a significant decreasing trend with increase in OCOPS addition. This may be because the external organic chain segments of OCOPS are longer or more flexible than those of OMPPS and OGCPS. At a lower loading, the effect of the rigid Si-O-Si structure on the Tg and the effect of flexible chain segments on the Tg offset each other, so the Tg of OCOPS-EP-0.1-C is close to that of EP-C. However, at higher addition amounts, due to the longer molecular chain of OCOPS, OCOPS has a stronger plasticizing effect, which exceeds the effect of the rigid Si-O-Si structure on the Tg of the modified epoxy resin [41]. Therefore, the Tg of OCOPS-EP-j-C decreases.
Thermogravimetric (TGA) analysis was used to determine the thermal stability of the resins, and the results are shown in Figure 13. The Td5 values of the cured hybrid resins are listed in Table 2. As shown in Table 2, we can see that the introduction of OMPPS and OGCPS can improve the thermal stability of the cured hybrid resins. Due to the short arms of OMPPS, most of which are composed of high energy Si-O and Si-C bonds [42,43], this is the key to the improvement of the thermal stability of OMPPS-EP-i-C. In contrast, OGCPS has a longer molecular chain segment than OMPPS, but the molecular chain of OGCPS contains a benzene ring structure, which also ensures that OGCPS-EP-k-C has high thermal stability [44]. However, for OCOPS-EP-j-C, the thermal stability is much lower than that of EP-C. There may be two reasons. Firstly, the presence of long flexible chains in the arms of OCOPS enhances the flexibility of the cross-linked structure when incorporated into the epoxy resin, subsequently compromising the thermal stability of the epoxy resin. Secondly, the reactive groups of OCOPS are carboxyl groups, and the ester groups formed during the curing reaction with epoxy groups may lead to a further reduction in the thermal stability of OCOPS-EP-j-C.

4. Conclusions

Three reactive polyhedral oligomeric silsesquioxanes with a thiol group (OMPPS), a carboxyl group (OCOPS), and an epoxy group (OGCPS) are utilized to modify 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline/4,4′-methylenebis(2-ethylaniline) (epoxy resin) and obtain hybrid resins with good thermal and mechanical properties. The hybrid resins display low viscosity in the temperature range of 45~85 °C and a low curing temperature (110 °C), which is beneficial for the liquid molding of the resin composites. The addition of OMPPS, OCOPS, and OGCPS greatly improves the toughness of the epoxy resin without sacrificing the mechanical and thermal properties of the epoxy resin. The critical stress intensity factor (KIC), impact strength, and Td5 of OGCPS-EP-0.6-C reach 2.54 MPa∙m−1/2, 19.33 kJ/m2, and 357 °C, showing increases of 58.75%, 22.48%, and 12.62%, respectively, compared to EP-C. The toughness of cured hybrid resins first increases and then decreases with the increase in the addition amount of OMPPS or OGCPS, reaching the maximum value when the addition amount is 1.4 mol% and 0.6 mol%, respectively. The toughness of OCOPS-EP-j-C increases with the increase in OCOPS addition. OCOPS, with long and flexible chain arms, exhibits a better toughening effect. This study provides a strategy for the design of polyhedral oligomeric silsesquioxane toughening agents and application in an epoxy resin, demonstrating an effective toughening method for the resin matrices of advanced composites.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/polym16131877/s1, Scheme S1: Synthetic route of HDS; Scheme S2: Synthetic route of DGHDS; Figure S1: (a) FT-IR spectra of HDS and DGHDS and (b) 1H NMR spectra of HDS and DGHDS; Figure S2. MALDT-TOF-MS spectra of OMPPS, OCOPS, and OGCPS; Figure S3. The sample diagram of four mechanical properties tests; Figure S4: Linear fitting of Ti and Tp vs. heating rate for the pristine resin; Figure S5: SEM images of the fracture surface of OMPPS-EP-0.8-C (a1), OMPPS-EP-1.9-C (a2), OGCPS-EP-0.6-C (b1), and OGCPS-EP-1.2 (b2); Table S1: DSC analysis data of OMPPS-EP-i, OCOPS-EP-j, and OGCPS-EP-k hybrid resins; Table S2: The cross-linking density of cured epoxy resins. Reference [45] is cited in the supplementary materials.

Author Contributions

Conceptualization, F.H. and W.L. (Weibo Liu); methodology, C.W., W.L. (Weibo Liu) and F.H.; validation, F.H., C.W. and W.L. (Weibo Liu); formal analysis, J.Q., W.L. (Weiping Liu); investigation, L.W., Y.C. and Y.F.; writing—original draft preparation, W.L. (Weibo Liu); writing—review and editing, F.H.; supervision, Z.L.; project administration, J.Q. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National KeyR&D Program of China (No. 2022YFB3709201) and the Fundamental Research Funds for the Central Universities (No. JKD01241701).

Institutional Review Board Statement

Not applicable.

Data Availability Statement

Data are contained within the article.

Conflicts of Interest

Zuozhen Liu and Jianhua Qian were employed by the company HuaChang Polymers Co., Ltd. Weiping Liu was employed by the company Manufacturing Center of Composite Materials for Commercial Aircraft, Shanghai Aircraft Manufacturing Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Paolillo, S.; Bose, R.K.; Santana, M.H.; Grande, A.M. Intrinsic self-healing epoxies in polymer matrix composites (PMCs) for aerospace applications. Polymers 2021, 13, 2073–4360. [Google Scholar] [CrossRef]
  2. Xu, N.; Zhu, T.; Yang, Z.; Han, M. Fabrication and optimization of La0.4Sr0.6Co0.2Fe0.7Nb0.1O3-δ electrode for symmetric solid oxide fuel cell with zirconia based electrolyte. J. Mater. Sci. Technol. 2017, 33, 1329–1333. [Google Scholar]
  3. Zhao, Y.S.; He, Y.H.; Yang, K.R.; Wang, X.P.; Bai, J.H.; Du, B. Improving the surface insulating performance of epoxy resin/Al2O3 composite materials by extending chain of liquid epoxy resin with Me-THPA. High Volt. 2020, 5, 472–481. [Google Scholar] [CrossRef]
  4. Zhao, Y.X.; Xu, R.; Xiao, Y.; Wang, H.L.; Zhang, W.; Zhang, G.Y. Mechanical performances of phenolic modified epoxy resins at room and high temperatures. Coatings 2022, 12, 643. [Google Scholar] [CrossRef]
  5. Zhang, X.L.; Liu, M.; Chen, Y.; He, J.C.; Wang, X.L.; Xie, J.; Li, Z.W.; Chen, Z.M.; Fu, Y.H.; Xiong, C.X.; et al. Epoxy resin/hollow glass microspheres composite materials with low dielectric constant and excellent mechanical performance. J. Appl. Polym. Sci. 2022, 139, E52787. [Google Scholar] [CrossRef]
  6. Qin, J.Y.; Zhao, H.P.; Qin, Z.L.; Zhang, W.C.; Yang, R.J. Effect of polyhedral oligomeric silsesquioxanes with different structures on dielectric and mechanical properties of epoxy resin. Polym. Compos. 2021, 42, 3445–3457. [Google Scholar] [CrossRef]
  7. Neves, R.M.; Ornaghi, H.L., Jr.; Zattera, A.J.; Amico, S.C. Toughening epoxy resin with liquid rubber and its hybrid composites: A systematic review. J. Polym. Res. 2022, 29, 340. [Google Scholar] [CrossRef]
  8. Thomas, R.; Yumei, D.; Yuelong, H.; Le, Y.; Moldenaers, P.; Weimin, Y.; Czigany, T.; Thomas, S. Miscibility, morphology, thermal, and mechanical properties of a DGEBA based epoxy resin toughened with a liquid rubber. Polymer 2008, 49, 278–294. [Google Scholar] [CrossRef]
  9. Jones, A.R.; Watkins, C.A.; White, S.R.; Sottos, N.R. Self-healing thermoplastic-toughened epoxy. Polymer 2015, 74, 254–261. [Google Scholar] [CrossRef]
  10. Wu, Z.J.; Yi, X.S.; Wilkinson, A. Interlaminar fracture toughness of carbon fibre/RTM6-2 composites toughened with thermoplastic-coated fabric reinforcement. Compos. Part B 2017, 130, 192–199. [Google Scholar] [CrossRef]
  11. Bekeshev, A.; Mostovoy, A.; Shcherbakov, A.; Zhumabekova, A.; Serikbayeva, G.; Vikulova, M.; Svitkina, V. Effect of Phosphorus and Chlorine Containing Plasticizers on the Physicochemical and Mechanical Properties of Epoxy Composites. J. Compos. Sci. 2023, 7, 178. [Google Scholar] [CrossRef]
  12. Eissa, M.M.; Samy, M.; Ramadan, A.M.; Amin, A. Amino-terminated hyperbranched polymer for toughness improvement of epoxy/clay nanocomposites. Polym. Bull. 2015, 72, 3147–3168. [Google Scholar] [CrossRef]
  13. Shiravand, F.; Ascione, L.; Persico, P.; Carfagna, C.; Brocks, T.; Cioffi, M.O.H.; Puglisi, C.; Samperi, F.; Ambrogi, V. A novel hybrid linear-hyperbranched poly(butylene adipate) copolymer as an epoxy resin modifier with toughening effect. Polym. Int. 2016, 65, 308–319. [Google Scholar] [CrossRef]
  14. Qi, Y.; Fan, Q.; Li, J.; Cao, Q.; Pan, X.; Pan, Y.; Jian, X.; Weng, Z. Toughened and reinforced the petroleum-based epoxy resin via thermotropic liquid crystal bio-based counterpart. Compos. Commun. 2023, 44, 101771. [Google Scholar] [CrossRef]
  15. Wang, T.T.; Huang, P.; Li, Y.Q.; He, N.; Fu, S.Y. Epoxy nanocomposites significantly toughened by both poly(sulfone) and graphene oxide. Compos. Commun. 2019, 14, 55–60. [Google Scholar]
  16. Xu, Z.G.; Song, P.G.; Zhang, J.; Guo, Q.P.; Mai, Y.W. Epoxy nanocomposites simultaneously strengthened and toughened by hybridization with graphene oxide and block ionomer. Compos. Sci. Technol. 2018, 168, 363–370. [Google Scholar] [CrossRef]
  17. Park, Y.T.; Qian, Y.Q.; Chan, C.; Suh, T.; Nejhad, M.G.; Macosko, C.W.; Stein, A. Epoxy toughening with low graphene loading. Adv. Funct. Mater. 2015, 25, 575–585. [Google Scholar] [CrossRef]
  18. Wang, F.Z.; Drzal, L.T.; Qin, Y.; Huang, Z.X. Enhancement of fracture toughness, mechanical and thermal properties of rubber/epoxy composites by incorporation of graphene nanoplatelets. Compos. Part A 2016, 87, 10–22. [Google Scholar] [CrossRef]
  19. Wang, Y.T.; Wang, C.S.; Yin, H.Y.; Wang, L.L.; Xie, H.F.; Cheng, R.S. Carboxyl-terminated butadiene-acrylonitrile-toughened epoxy/carboxyl-modified carbon nanotube nanocomposites: Thermal and mechanical properties. Express. Polym. Lett. 2012, 6, 719–728. [Google Scholar] [CrossRef]
  20. Rahman, M.M.; Hosur, M.; Ludwick, A.G.; Zainuddin, S.; Kumar, A.; Trovillion, J.; Jeelani, S. Thermo-mechanical behavior of epoxy composites modified with reactive polyol diluent and randomly-oriented amino-functionalized multi-walled carbon nanotubes. Polym. Test. 2012, 31, 777–784. [Google Scholar] [CrossRef]
  21. Dharmavarapu, P.; Reddy, M. Mechanical, low velocity impact, fatigue and tribology behaviour of silane grafted aramid fibre and nano-silica toughened epoxy eomposite. Silicon 2021, 13, 1741–1750. [Google Scholar] [CrossRef]
  22. Pham, T.D.; Vu, C.M.; Choi, H.J. Enhanced fracture toughness and mechanical properties of epoxy resin with rice husk-based nano-silica. Polym. Sci. Ser. A 2017, 59, 437–444. [Google Scholar] [CrossRef]
  23. Sahoo, S.K.; Mohanty, S.; Nayak, S.K. Study of thermal stability and thermo-mechanical behavior of functionalized soybean oil modified toughened epoxy/organo clay nanocomposite. Prog. Org. Coat. 2015, 88, 263–271. [Google Scholar] [CrossRef]
  24. Li, S.; Liu, Y.; Liu, Y.; Wang, Q. Synergistic effect of piperazine pyrophosphate and epoxy-octavinyl silsesquioxane on flame retardancy and mechanical properties of epoxy resin. Compos. Part B Eng. 2021, 223, 109115. [Google Scholar] [CrossRef]
  25. Liu, H.; Liu, M.; Zhang, P.; Xue, K.; Yao, T.; Liu, L.; Huang, Y. POSS-polyurethane prepolymer strengthened and toughened CF/epoxy resin composites for room and simulated arctic ambient temperature. Polymer 2024, 294, 126692. [Google Scholar] [CrossRef]
  26. Han, R.; Ma, X.; Cai, L.; Zhang, Z.; Fang, Y.; Wang, J. Low viscosity and low temperature curing reactive POSS/epoxy hybrid resin with enhanced toughness and comprehensive thermal performance. RSC Adv. 2024, 14, 7263–7275. [Google Scholar] [CrossRef] [PubMed]
  27. Ni, C.; Ni, G.; Zhang, L.; Mi, J.; Yao, B.; Zhu, C. Syntheses of silsesquioxane (POSS)-based inorganic/organic hybrid and the application in reinforcement for an epoxy resin. J. Colloid Interface Sci. 2011, 362, 94–99. [Google Scholar] [CrossRef] [PubMed]
  28. Mishra, K.; Pandey, G.; Singh, R.P. Enhancing the mechanical properties of an epoxy resin using polyhedral oligomeric silsesquioxane (POSS) as nano-reinforcement. Polym. Test. 2017, 62, 210–218. [Google Scholar] [CrossRef]
  29. Zhang, C.X.; Li, T.X.; Song, H.; Han, Y.Q.; Su, H.B.; Wang, Y.M.; Wang, Q. Epoxy Resin/POSS Nanocomposites with Toughness and Thermal Stability. J. Photopolym. Sci. Technol. 2017, 30, 25–31. [Google Scholar] [CrossRef]
  30. Cao, J.; Fan, H.; Li, B.-G.; Zhu, S. Synthesis and evaluation of Double-Decker Silsesquioxanes as modifying agent for epoxy resin. Polymer 2017, 124, 157–167. [Google Scholar] [CrossRef]
  31. Konnola, R.; Parameswaranpillai, J.; Joseph, K. Mechanical, thermal, and viscoelastic response of novel in situ CTBN/POSS/epoxy hybrid composite system. Polymer. Compos. 2016, 37, 2109–2120. [Google Scholar] [CrossRef]
  32. Zhang, C.; Li, T.; Song, H.; Han, Y.; Dong, Y.; Wang, Y.; Wang, Q. Improving the thermal conductivity and mechanical property of epoxy composites by introducing polyhedral oligomeric silsesquioxane-grafted graphene oxide. Polymer. Compos. 2018, 39, E1890–E1899. [Google Scholar] [CrossRef]
  33. Yang, J.; Zhang, Y.; Hao, M.; Zhi, J.; Qian, X. Synergistically toughened epoxy resin based on modified-POSS triggered interpenetrating network. Polymer 2023, 268, 125719. [Google Scholar] [CrossRef]
  34. Misasi, J.M.; Jin, Q.; Knauer, K.M.; Morgan, S.E.; Wiggins, J.S. Hybrid POSS-hyperbranched polymer additives for simultaneous reinforcement and toughness improvements in epoxy networks. Polymer 2017, 117, 54–63. [Google Scholar] [CrossRef]
  35. Kopesky, E.T.; Haddad, T.S.; McKinley, G.H.; Cohen, R.E. Miscibility and viscoelastic properties of acrylic polyhedral oligomeric silsesquioxane–poly(methyl methacrylate) blends. Polymer 2005, 46, 4743–4752. [Google Scholar] [CrossRef]
  36. Hao, N.; Böhning, M.; Schönhals, A. Dielectric properties of nanocomposites based on polystyrene and polyhedral oligomeric phenethyl-silsesquioxanes. Macromolecules 2007, 40, 9672–9679. [Google Scholar] [CrossRef]
  37. Ke, F.; Zhang, C.; Guang, S.; Xu, H. POSS Core star-shape molecular hybrid materials: Effect of the chain length and POSS content on dielectric properties. J. Appl. Polym. Sci. 2013, 127, 2628–2634. [Google Scholar] [CrossRef]
  38. Robertson, R.E.; Mindroiu, V.E.; Cheung, M.-F. Fracture in epoxy matrix resins. Compos. Sci. Technol. 1985, 22, 197–207. [Google Scholar] [CrossRef]
  39. Sahagun, C.M.; Morgan, S.E. Thermal control of nanostructure and molecular network development in epoxy-amine thermosets. ACS Appl. Mater. Inter. 2012, 4, 564–572. [Google Scholar] [CrossRef]
  40. Zhang, W.; Huang, J.; Guo, X.; Zhang, W.; Qin, Z.; Yang, R. Preparation and mechanism of toughening and flame retardance of epoxy resin using novel silsesquioxane molecules. React. Funct. Polym. 2023, 190, 105645. [Google Scholar] [CrossRef]
  41. Turan, D.; Sirin, H.; Ozkoc, G. Effects of POSS particles on the mechanical, thermal, and morphological properties of PLA and plasticised PLA. J. Appl. Polym. Sci. 2011, 121, 1067–1075. [Google Scholar] [CrossRef]
  42. Abbasi, A.; Salimi, A.; Bouhendi, H.; Karimi, M. A study of the thermal properties of alumina/glycidoxy propyl POSS/epoxy adhesives. Int. J. Adhes. Adhes. 2023, 124, 103368. [Google Scholar] [CrossRef]
  43. Lian, Q.; Chen, H.; Luo, Y.; Li, Y.; Cheng, J.; Liu, Y. Toughening mechanism based on the physical entanglement of branched epoxy resin in the non-phase-separated inhomogeneous crosslinking network: An experimental and molecular dynamics simulation study. Polymer 2022, 247, 124754. [Google Scholar] [CrossRef]
  44. Zeng, K.; Zheng, S. Nanostructures and surface dewettability of epoxy thermosets containing hepta(3,3,3-trifluoropropyl) polyhedral oligomeric silsesquioxane-capped poly(ethylene oxide). J. Phys. Chem. B 2007, 111, 13919–13928. [Google Scholar] [CrossRef]
  45. Ohashi, S.; Kilbane, J.; Heyl, T.; Ishida, H. Synthesis and characterization of cyanate ester functional benzoxazine and its polymer. Macromolecules 2015, 48, 8412–8417. [Google Scholar] [CrossRef]
Scheme 1. Synthetic route of OMPPS.
Scheme 1. Synthetic route of OMPPS.
Polymers 16 01877 sch001
Scheme 2. Synthetic route of OCOPS.
Scheme 2. Synthetic route of OCOPS.
Polymers 16 01877 sch002
Scheme 3. Synthetic route of OGCPS.
Scheme 3. Synthetic route of OGCPS.
Polymers 16 01877 sch003
Figure 1. Structural formulas of AFG-90MH and MOEA.
Figure 1. Structural formulas of AFG-90MH and MOEA.
Polymers 16 01877 g001
Figure 2. (a) FT-IR spectra of OMPPS, OCOPS, and OGCPS and (b) 1H NMR spectra of OMPPS, OCOPS, and OGCPS.
Figure 2. (a) FT-IR spectra of OMPPS, OCOPS, and OGCPS and (b) 1H NMR spectra of OMPPS, OCOPS, and OGCPS.
Polymers 16 01877 g002
Figure 3. 29Si NMR spectra of OMPPS, OCOPS, and OGCPS.
Figure 3. 29Si NMR spectra of OMPPS, OCOPS, and OGCPS.
Polymers 16 01877 g003
Figure 4. Viscosity of pristine epoxy resin, OMPPS-EP-0.8, OCOPS-EP-0.8, and OGCPS-EP-0.8.
Figure 4. Viscosity of pristine epoxy resin, OMPPS-EP-0.8, OCOPS-EP-0.8, and OGCPS-EP-0.8.
Polymers 16 01877 g004
Figure 5. DSC curves of the OMPPS-EP-i (a), OCOPS-EP-j (b), and OGCPS-EP-k (c) hybrid resins. (d) The pristine epoxy resin and hybrid resins with the same load amount of modifier.
Figure 5. DSC curves of the OMPPS-EP-i (a), OCOPS-EP-j (b), and OGCPS-EP-k (c) hybrid resins. (d) The pristine epoxy resin and hybrid resins with the same load amount of modifier.
Polymers 16 01877 g005
Figure 6. DSC curves of OMPPS-EP-0.8 (a), OCOPS-EP-0.8 (b), and OGCPS-EP-0.8 (c) before and after curing.
Figure 6. DSC curves of OMPPS-EP-0.8 (a), OCOPS-EP-0.8 (b), and OGCPS-EP-0.8 (c) before and after curing.
Polymers 16 01877 g006
Figure 7. FT-IR spectra of the hybrid resins with 0.8 mol% modifier content before (a) and after (b) curing.
Figure 7. FT-IR spectra of the hybrid resins with 0.8 mol% modifier content before (a) and after (b) curing.
Polymers 16 01877 g007
Figure 8. Flexural properties of OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c).
Figure 8. Flexural properties of OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c).
Polymers 16 01877 g008
Figure 9. Impact strength of OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
Figure 9. Impact strength of OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
Polymers 16 01877 g009
Figure 10. SEM images of the fracture surfaces of EP-C (a), OMPPS-EP-i-C (a1e1), OCOPS-EP-j-C (a2e2), and OGCPS-EP-k-C (a3e3).
Figure 10. SEM images of the fracture surfaces of EP-C (a), OMPPS-EP-i-C (a1e1), OCOPS-EP-j-C (a2e2), and OGCPS-EP-k-C (a3e3).
Polymers 16 01877 g010
Figure 11. KIC of OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
Figure 11. KIC of OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
Polymers 16 01877 g011
Figure 12. DMA curves of EP-C, OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c) in nitrogen.
Figure 12. DMA curves of EP-C, OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c) in nitrogen.
Polymers 16 01877 g012
Figure 13. TGA curves of EP-C, OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c), and modifier-EP-0.8-C (d) in nitrogen.
Figure 13. TGA curves of EP-C, OMPPS-EP-i-C (a), OCOPS-EP-j-C (b), and OGCPS-EP-k-C (c), and modifier-EP-0.8-C (d) in nitrogen.
Polymers 16 01877 g013
Table 1. Solubility of OMPPS, OCOPS, and OGCPS.
Table 1. Solubility of OMPPS, OCOPS, and OGCPS.
SolventSolubility
OMPPSOCOPSOGCPS
Methanol
Ethanol
Tetrahydrofuran+++
Ethyl acetate++
Dimethylformamide+++
Dimethyl sulfoxide+++
Dichloromethane++
Petroleum ether
Chloroform++
+ soluble, − insoluble.
Table 2. Tgs and Td5s of EP-C, OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
Table 2. Tgs and Td5s of EP-C, OMPPS-EP-i-C, OCOPS-EP-j-C, and OGCPS-EP-k-C.
SampleTg (°C)Td5 (°C)
EP-C169317
OMPPS-EP-0.3-C170341
OMPPS-EP-0.8-C173347
OMPPS-EP-1.4-C173348
OMPPS-EP-1.9-C171349
OMPPS-EP-2.8-C170345
OCOPS-EP-0.1-C174356
OCOPS-EP-0.3-C156333
OCOPS-EP-0.6-C155204
OCOPS-EP-0.8-C157136
OCOPS-EP-1.2-C158125
OGCPS-EP-0.1-C166355
OGCPS-EP-0.3-C168356
OGCPS-EP-0.6-C167357
OGCPS-EP-0.8-C167356
OGCPS-EP-1.2-C170353
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Liu, W.; Wang, C.; Feng, Y.; Chen, Y.; Wan, L.; Huang, F.; Liu, Z.; Qian, J.; Liu, W. Novel Reactive Polyhedral Oligomeric Silsesquioxane-Reinforced and Toughened Epoxy Resins for Advanced Composites. Polymers 2024, 16, 1877. https://doi.org/10.3390/polym16131877

AMA Style

Liu W, Wang C, Feng Y, Chen Y, Wan L, Huang F, Liu Z, Qian J, Liu W. Novel Reactive Polyhedral Oligomeric Silsesquioxane-Reinforced and Toughened Epoxy Resins for Advanced Composites. Polymers. 2024; 16(13):1877. https://doi.org/10.3390/polym16131877

Chicago/Turabian Style

Liu, Weibo, Caiyun Wang, Yu Feng, Yongfeng Chen, Liqiang Wan, Farong Huang, Zuozhen Liu, Jianhua Qian, and Weiping Liu. 2024. "Novel Reactive Polyhedral Oligomeric Silsesquioxane-Reinforced and Toughened Epoxy Resins for Advanced Composites" Polymers 16, no. 13: 1877. https://doi.org/10.3390/polym16131877

APA Style

Liu, W., Wang, C., Feng, Y., Chen, Y., Wan, L., Huang, F., Liu, Z., Qian, J., & Liu, W. (2024). Novel Reactive Polyhedral Oligomeric Silsesquioxane-Reinforced and Toughened Epoxy Resins for Advanced Composites. Polymers, 16(13), 1877. https://doi.org/10.3390/polym16131877

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop