Next Article in Journal
Simultaneous Dirac-like Cones at Two Energy States in Tunable Phononic Crystals: An Analytical and Numerical Study
Previous Article in Journal
A State-of-the-Art Review on Suitability of Granite Dust as a Sustainable Additive for Geotechnical Applications
Previous Article in Special Issue
The Influence of Ni-Added Fe-Based Pre-Alloy on Microstructure Evolution and Lifetime Extension of Diamond Tools
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of Sn and Mo on Microstructure and Electrochemical Property of TiZrTaNb High Entropy Alloys

Key Laboratory of Air-Driven Equipment Technology of Zhejiang Province, Quzhou University, Quzhou 324000, China
*
Authors to whom correspondence should be addressed.
Crystals 2021, 11(12), 1527; https://doi.org/10.3390/cryst11121527
Submission received: 4 November 2021 / Revised: 24 November 2021 / Accepted: 5 December 2021 / Published: 7 December 2021
(This article belongs to the Special Issue Advance in Alloy Materials)

Abstract

:
The effects of Sn and Mo alloying elements on the microstructure and electrochemical properties of TiZrTaNb high entropy alloys were studied by optical microscope (OM), scanning electron microscopy (SEM), X-ray diffraction (XRD) and electrochemistry. TiZrTaNb, TiZrTaNbMo and TiZrTaNbSn alloys with equal atomic ratio were prepared by the arc melting method. The results showed that the microstructure of the high entropy alloys was dendritic structure with single BCC structure. The addition of Mo and Sn elements promoted the growth of the dendritic structure and accelerated the interdendritic segregation of the TiZrTaNb alloy. The TiZrTaNbMo alloy exhibited excellent corrosion properties compared to TiZrTaNb and TiZrTaNbSn alloys based on corrosion parameters Icorr, φcorr, Ipass. The corrosion mechanism is discussed based on the corrosion morphology. The alloying elements have an important effect on the microstructure and electrochemical properties of a high entropy alloy.

Graphical Abstract

1. Introduction

A high entropy alloy is a new alloy proposed at the beginning of this century [1,2,3]. It is a multiprincipal element alloy with five or more main elements and each element’s content is between 5% and 35%, which breaks the design concept of the traditional alloy and creates a new idea for alloy design [4,5,6]. The unique composition characteristics of the high entropy alloy lead to excellent properties such as high strength, high wear resistance and excellent corrosion resistance compared to traditional alloys, showing wide application prospects in aerospace, nuclear power and biomedical fields [7,8,9,10,11]. Previous studies have shown that the elastic modulus of a high-entropy alloy with BCC structure is low, which can achieve a better match with the human body and is more suitable for implantation materials [12,13,14]. Todai et al. prepared a series of high-entropy alloys for use in bone repair (TiNbTaZrHf, TiNbTaZr, TiNbTaZrMo, etc.) by alloying safe elements without cytotoxicity and sensitization factors. The as-cast TiZrTaNb exhibited a single BCC phase and achieved a compressive yield strength of 1100 ± 90 MPa, strain of 48 ± 6%, and modulus of 116 ± 6 GPa [15]. Moreover, the mechanical properties were improved after the addition of Mo element, which showed better biocompatibility than pure titanium and stainless steel [16,17,18]. The effect of elements can not only affect the mechanical properties, but also the electrochemical property which is a key parameter for biological materials [19,20,21]. Alloying designation is still a hot topic in material research, especially for the high entropy alloy, due to the complex element interactions.
The Sn element is commonly used in Ti-based biological alloy, which has non-toxic effects. In this paper, the effects of Sn and Mo elements on a TiZrNbTa high entropy alloy were studied, and three high entropy alloys (TiZrTaNb, TiZrTaNbMo and TiZrTaNbSn) with equal atomic ratio were designed. The effects of alloying elements on microstructure and properties were studied by means of scanning electron microscope (SEM), X-ray diffractometer (XRD) and electrochemical workstation.

2. Materials and Methods

High purity metal particles Ti, Zr, Ta, Nb, Mo and Sn (purity ≥99.9%) were selected as raw materials(Tim(Beijing)New Material Technology Co.,LTD), and arc melting was carried out in a high vacuum arc melting furnace (Model DHL-500LL) (The origin is Shenyang, China, purchased from Shenyang Scientific Instrument Co., Ltd. of the Chinese Academy of Sciences) to obtain high entropy alloy ingots. Three high entropy alloys are TiZrTaNb, TiZrTaNbMo and TiZrTaNbSn (at. %). The high melting point metal was placed at the top of crucible and low melting point metal was placed at the bottom, and then different melting point metals can be completely melted. The ingot was remelted five times and homogeneous chemical composition was achieved. No wrinkles and black pits were observed on the surface of ingot.
The electrochemical corrosion performance was tested on the CHI604E electrochemical workstation. The electrochemical system was a standard three-electrode system. The samples were the working electrode and AgCl electrode was the reference electrode, and platinum electrode was the auxiliary electrode. Before the experiment, the samples were polished and cleaned using alcohol ultrasonic. NaCl solution with mass fraction of 3.5% was used during the experiment. The sample should be kept in 3600s before the test. The alternating current impedance and corrosion rate (Tafel curve) were tested after the open-circuit potential stabilized.
Hitachi SU8010 field emission scanning electron microscope (SEM) (The origin is Tokyo, Japan, purchased from Hitachi High Technologies Corporation) was used to observe the microstructure and electrochemical corrosion morphology. The energy dispersive spectrometer (EDS) was used to analyze element distribution. The samples were ground to 2000# with SiC sandpaper, and then mechanical polished. X-ray diffractometer (D8 Advance) (The origin is Germany and purchased from Bruker, Siegsdorf, Germany) was used to assess the crystal structure and for phase analysis. The scanning step was set as 4°/min and the diffraction angle 2θ was selected between 20° and 100°.

3. Results and Discussion

X-ray was used for phase analysis of the three high entropy alloys and the results are shown in Figure 1. Two kinds of BCC structures were identified and labeled BCC1 and BCC2. It can be seen that the position of the diffraction peak changed after the addition of Mo and Sn elements, but the crystal structure did not change, which was attributed to the lattice distortion.
The microstructure and element distribution of different high entropy alloys were analyzed by SEM and EDS as shown in Figure 2. The microstructure showed a bright region and dark region in BSE mode corresponding to the dendrite and interdendritic, which resulted from the element segregation. The Ti, Zr, Nb elements were mainly segregated as interdendritic and the Ta element segregated as dendrite. The distribution of Ti, Zr, Nb, Ta in TiZrTaNbMo alloy was similar with TiZrTaNb alloy, while the Mo element was distributed as dendrite as shown in Figure 2c,d. In the TiZrTaNbSn alloy, the Sn element were enriched in interdendritic, while the Nb element was distributed homogeneously comparing to the TiZrTaNbMo alloy as shown in Figure 2e,f. It can be concluded that Ta, Mo elements are mainly enriched in dendrite and Zr, Ti, Nb, Sn elements are mainly distributed in the interdendritic in high-entropy alloys, which is attributed to the different equilibrium distribution coefficients.
In order to study the influence of alloying elements on the corrosion resistance of high entropy alloys, the electrochemical corrosion tests were carried out and the results are shown in Figure 3. The electrochemical impedance can be used to describe the corrosion resistance, and the higher impedance value represents the better corrosion resistance. The electrochemical impedance spectra of high-entropy alloys in 3.5% NaCl solution are shown in Figure 3a. The radius of the capacitive reactance arc decreases significantly after the addition of Mo and Sn elements. It can be seen from Figure 3a, TiZrTaNbMo showed the best corrosion resistance, while TiZrTaNbSn showed the worst corrosion resistance among the three high-entropy alloys. The potentiodynamic polarization curves of the three high entropy alloys were similar and the redox reactions occurred as shown in Figure 3b. Anodic polarization is an activation–passivation process, and the electrochemical corrosion parameters are calculated according to Figure 3b listed in Table 1. At the beginning of corrosion, the current density is called Icorr, which can reveal the corrosion resistance. The corrosion resistance increased with the decrease of Icorr, then it can be concluded that the TiZrNbTaMo alloy has the best corrosion performance. The corrosion potential φcorr can reflect the thermodynamic properties and surface state of the electrode. The corrosion tendency increased with the decrease of φcorr, as a result, the corrosion tendency of TiZrTaNbMo alloy was lower than that of TiZrTaNb and TiZrTaNbSn alloys. The passivation current density Ipass can be used to evaluate the state of corroded system, and the activated state changes to a passivated state depending on the Ipass. The smaller Ipass indicates that the system is easier to keep the passivation state. It indicates that the alloys have entered the passivation stage, and a protective passivation film is formed on the surface. The Ipass of TiZrTaNb, TiZrTaNbMo and TiZrTaNbSn alloys were 4.12 × 10−2 a·cm−2, 1.02 × 10−3 a·cm−2 and 5.2 × 10−2 a·cm−2 respectively. The TiZrTaNiMo alloy showed the best corrosion resistance according the corrosion parameters listed in Table 1.
The surface morphology of the high entropy alloys after electrochemical corrosion is shown in Figure 4. The surface was etched after electrochemical corrosion for 60 min. The electrochemical corrosion behavior of the high entropy alloys was basically the same, the corrosion mainly occurred at the grain boundary due to interdendritic segregation. The corrosion degree of the three high entropy alloys was different from each other, which corresponds to different corrosion properties. A small number of corrosion particles were attached to the surface of TiZrTaNbMo alloy, and no obvious corrosion was observed, denoting excellent corrosion resistance as shown in Figure 4b. Severe corrosion occured on the surface of TiZrTaNbSn alloy, and there was a large number of corrosion pits and cracks on the surface as shown in Figure 4c. The deteriorative corrosion property of TiZrTaNbSn alloy was attributed to the interdendritic segregation of the Sn element. The corrosion property of TiZrTaNbSn alloy could be improved by eliminating segregation and further work will be carried out.

4. Conclusions

This paper systematically studied the effect of Mo and Sn elements on the microstructure and corrosion properties of TiZrTaNb alloy, and the main conclusions are as follows:
  • The microstructure of TiZrTaNb, TiZrTaNbMo and TiZrTaNbSn alloys is dendrite with single BCC structures. The addition of Mo and Sn elements promotes dendrite growth and interdendritic segregation.
  • The Ta, Mo elements are mainly enriched in dendrite and Zr, Ti, Nb, Sn elements are mainly distributed in the interdendritic in high entropy alloys, which is attributed to the different equilibrium distribution coefficients.
  • The TiZrTaNiMo alloy shows excellent corrosion property according to the corrosion parameters Icorr, φcorr, Ipass. The corrosion property of the TiZrTaNb alloy deteriorated after the addition of Sn element and this is attributed to the interdendritic segregation of Sn element.

Author Contributions

Conceptualization, T.M.; methodology, Q.L., Y.J. and D.D.; formal analysis, D.Z.; investigation, X.W., Y.J. and Q.L.; resources, D.Z., and T.M.; data curation, Q.L.; writing—original draft preparation, Q.L.; writing—review and editing, D.Z. and T.M. All authors have read and agreed to the published version of the manuscript.

Funding

The work was supported by National Natural Science of Foundation of China (Grant No. 52001262, 52071188, 52171120), Zhejiang Province Natural Science Foundation of China (Grant No.: ZY22E010293, LQ20E010003).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Informed consent was obtained from all subjects involved in the study.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhang, Y.; Zuo, T.T.; Tang, Z.; Gao, M.C.; Dahmen, K.A.; Liaw, P.K.; Lu, Z.P. Microstructures and properties of high-entropy alloys. Prog. Mater. Sci. 2014, 61, 1–93. [Google Scholar] [CrossRef]
  2. He, M.Y.; Shen, Y.F.; Jia, N.; Liaw, P.K. C and N doping in high-entropy alloys: A pathway to achieve desired strength-ductility synergy. Appl. Mater. Today 2021, 25, 101162. [Google Scholar] [CrossRef]
  3. Krishna, Y.V.; Jaiswal, U.K.; Rahul, M.R. Machine learning approach to predict new multiphase high entropy alloys. Scr. Mater. 2021, 197, 113804. [Google Scholar] [CrossRef]
  4. Zhou, N.X.; Jiang, S.C.; Huang, T.; Qin, M.D.; Hu, T.; Luo, J. Single-phase high-entropy intermetallic compounds (HEICs): Bridging high-entropy alloys and ceramics. Sci. Bull. 2019, 64, 856–864. [Google Scholar] [CrossRef] [Green Version]
  5. Long, Y.; Li, G.Q.; Liang, X.B.; Peng, H.Y. Fine-grained FeCoNi(CuAl)(x) high entropy alloys: Phase transformation, microstructure evolution and mechanical properties. Front. Mater. 2020, 7, 537812. [Google Scholar] [CrossRef]
  6. Ma, Y.J.; Ma, Y.; Wang, Q.S.; Schweidler, S.; Botros, M.; Fu, T.T.; Hahn, H.; Brezesinski, T.; Breitung, B. High-entropy energy materials: Challenges and new opportunities. Energy Environ. Sci. 2021, 14, 2883–2905. [Google Scholar] [CrossRef]
  7. Chuang, M.H.; Tsai, M.H.; Wang, W.R.; Lin, S.J.; Yeh, J.W. Microstructure and wear behavior of AlxCo1.5CrFeNi1.5Ti high-entropy alloys. Acta Mater. 2011, 59, 6308–6317. [Google Scholar] [CrossRef]
  8. Nong, Z.S.; Li, D.S.; Zhu, J.C.; Yu, H.L.; Lai, Z.H. Effect of aluminum content on microstructure and wear resistance of CuCrFeMnTiAlx high-entropy alloy. Rare Met. Mater. Eng. 2011, 40, 550–554. [Google Scholar]
  9. Xiao, J.K.; Tan, H.; Chen, J.; Martini, A.; Zhang, C. Effect of carbon content on microstructure, hardness and wear resistance of CoCrFeMnNiCx high-entropy alloys. J. Alloy. Compd. 2020, 847, 156533. [Google Scholar] [CrossRef]
  10. Yin, B.L.; Curtin, W.A. Origin of high strength in the CoCrFeNiPd high-entropy alloy. Mater. Res. Lett. 2020, 8, 209–215. [Google Scholar] [CrossRef] [Green Version]
  11. Shang, C.Y.; Axinte, E.; Ge, W.J.; Zhang, Z.T.; Wang, Y. High-entropy alloy coatings with excellent mechanical, corrosion resistance and magnetic properties prepared by mechanical alloying and hot pressing sintering. Surf. Interfaces 2017, 9, 36–43. [Google Scholar] [CrossRef]
  12. Wang, S.P.; Xu, J. (TiZrNbTa)-Mo high-entropy alloys: Dependence of microstructure and mechanical properties on Mo concentration and modeling of solid solution strengthening. Intermetallics 2018, 95, 59–72. [Google Scholar] [CrossRef]
  13. Eletia, R.R.; Stepanova, N.; Yurchenko, N.; Zherebtsov, S.; Marescab, F. Cross-kink unpinning controls the medium- to high-temperature strength of body-centered cubic NbTiZr medium-entropy alloy. Scr. Mater. 2021, 209, 114367. [Google Scholar] [CrossRef]
  14. Eleti, R.R.; Stepanov, N.; Yurchenko, N.; Klimenko, D.; Zherebtsov, S. Plastic deformation of solid-solution strengthened Hf-Nb-Ta-Ti-Zr body-centered cubic medium/high-entropy alloys. Scr. Mater. 2021, 200, 113927. [Google Scholar] [CrossRef]
  15. Nguyen, V.T.; Qian, M.; Shi, Z.; Song, T.; Huang, L.; Zou, J. A novel quaternary equiatomic Ti-Zr-Nb-Ta medium entropy alloy (MEA). Intermetallics 2018, 101, 39–43. [Google Scholar] [CrossRef]
  16. Liao, M.Q.; Liu, Y.; Min, L.J.; Lai, Z.H.; Han, T.Y.; Yang, D.N.; Zhu, J.C. Alloying effect on phase stability, elastic and thermodynamic properties of Nb-Ti-V-Zr high entropy alloy. Intermetallics 2018, 101, 152–164. [Google Scholar] [CrossRef]
  17. Todai, M. Novel TiNbTaZrMo high-entropy alloys for metallic biomaterials. Scr. Mater. 2017, 129, 65–68. [Google Scholar] [CrossRef] [Green Version]
  18. Raabe, D.; Tasan, C.C.; Springer, H.; Bausch, M. From high-entropy alloys to high-entropy steels. Steel Res. Int. 2015, 86, 1127–1138. [Google Scholar] [CrossRef]
  19. Raza, A.; Abdulahad, S.; Kang, B.; Ryu, H.J.; Hong, S.H. Corrosion resistance of weight reduced AlxCrFeMoV high entropy alloys. Appl. Surf. Sci. 2019, 485, 368–374. [Google Scholar] [CrossRef]
  20. Shang, C.Y.; Axinte, E.; Sun, J.; Li, X.T.; Li, P.; Du, J.W.; Qiao, P.C.; Wang, Y. CoCrFeNi(W1-xMox) high-entropy alloy coatings with excellent mechanical properties and corrosion resistance prepared by mechanical alloying and hot pressing sintering. Mater. Des. 2017, 117, 193–202. [Google Scholar] [CrossRef]
  21. Li, J.J.; Zhao, X.Y.; Hu, L.N.; Ma, L.Q.; Shen, X.D. Electrochemical properties of Co-S/x wt.% AB(5) composite materials. Sci. China-Technol. Sci. 2015, 58, 1355–1359. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of high entropy alloys.
Figure 1. XRD patterns of high entropy alloys.
Crystals 11 01527 g001
Figure 2. BSE images and corresponding EDS of high entropy alloys: (a,b) TiZrTaNb alloy; (c,d) TiZrTaNbMo alloy; (e,f) TiZrTaNbSn alloy.
Figure 2. BSE images and corresponding EDS of high entropy alloys: (a,b) TiZrTaNb alloy; (c,d) TiZrTaNbMo alloy; (e,f) TiZrTaNbSn alloy.
Crystals 11 01527 g002
Figure 3. (a) Nyquist diagram and (b) corresponding polarization curves of high entropy alloys.
Figure 3. (a) Nyquist diagram and (b) corresponding polarization curves of high entropy alloys.
Crystals 11 01527 g003
Figure 4. Surface morphologies of high entropy alloys after electrochemical etching: (a) TiZrTaNb alloy; (b) TiZrTaNbMo alloy; (c) TiZrTaNbSn alloy.
Figure 4. Surface morphologies of high entropy alloys after electrochemical etching: (a) TiZrTaNb alloy; (b) TiZrTaNbMo alloy; (c) TiZrTaNbSn alloy.
Crystals 11 01527 g004
Table 1. Parameters of electrochemical corrosion of high entropy alloy.
Table 1. Parameters of electrochemical corrosion of high entropy alloy.
AlloyIcorr/A·cm2φcorr/VIpass/A·cm2
TiZrTaNb7.08 × 107−0.874.12 × 102
TiZrTaNbMo5.5 × 107−0.4991.02 × 103
TiZrTaNbSn7.87 × 107−0.8285.2 × 102
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Li, Q.; Ma, T.; Jin, Y.; Wang, X.; Dong, D.; Zhu, D. Effect of Sn and Mo on Microstructure and Electrochemical Property of TiZrTaNb High Entropy Alloys. Crystals 2021, 11, 1527. https://doi.org/10.3390/cryst11121527

AMA Style

Li Q, Ma T, Jin Y, Wang X, Dong D, Zhu D. Effect of Sn and Mo on Microstructure and Electrochemical Property of TiZrTaNb High Entropy Alloys. Crystals. 2021; 11(12):1527. https://doi.org/10.3390/cryst11121527

Chicago/Turabian Style

Li, Qiaoyu, Tengfei Ma, Yuliang Jin, Xiaohong Wang, Duo Dong, and Dongdong Zhu. 2021. "Effect of Sn and Mo on Microstructure and Electrochemical Property of TiZrTaNb High Entropy Alloys" Crystals 11, no. 12: 1527. https://doi.org/10.3390/cryst11121527

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop