Next Article in Journal
Applications of Artificial Intelligence in the Study and Diagnosis of Orbital Pathologies: State of the Art and Future Directions
Previous Article in Journal
Multiscale Evaluation System for Cold Patch Asphalt Mixtures: Integrating Macro-Performance Tests and Meso-Structural CT Analysis
Previous Article in Special Issue
Performance Enhancement of Second-Life Lithium-Ion Batteries Based on Gaussian Mixture Model Clustering and Simulation-Based Evaluation for Energy Storage System Applications
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Probing Solid-State Interface Kinetics via Alternating Current Electrophoretic Deposition: LiFePO4 Li-Metal Batteries

Department of Materials Science and Engineering, Hongik University, 72-1, Sangsu-dong, Mapo-gu, Seoul 04066, Republic of Korea
*
Author to whom correspondence should be addressed.
Appl. Sci. 2025, 15(13), 7120; https://doi.org/10.3390/app15137120 (registering DOI)
Submission received: 8 May 2025 / Revised: 21 June 2025 / Accepted: 23 June 2025 / Published: 24 June 2025

Abstract

This work presents a comprehensive investigation into the interfacial charge storage mechanisms and lithium-ion transport behavior of Li-metal all-solid-state batteries (ASSBs) employing LiFePO4 (LFP) cathodes fabricated via alternating current electrophoretic deposition (AC-EPD) and Li1.3Al0.3Ti1.7(PO4)3 (LATP) as the solid-state electrolyte. We demonstrate that optimal sintering improves the LATP–LFP interfacial contact, leading to higher lithium diffusivity (~10−9 cm2∙s−1) and diffusion-controlled kinetics (b ≈ 0.5), which directly translate to better rate capability. Structural and electrochemical analyses—including X-ray diffraction, scanning electron microscopy, cyclic voltammetry, and rate capability tests—demonstrate that the cell with LATP sintered at 900 °C delivers the highest Li-ion diffusivity (~10−9 cm2∙s−1), near-ideal diffusion-controlled behavior (b-values ~0.5), and superior rate capability. In contrast, excessive sintering at 1000 °C led to reduced diffusivity (~10−10 cm2∙s−1). The liquid electrolyte system showed higher b-values (~0.58), indicating the inclusion of surface capacitive behavior. The correlation between b-values, diffusivity, and morphology underscores the critical role of interface engineering and electrolyte processing in determining the performance of solid-state batteries. This study establishes AC-EPD as a viable and scalable method for fabricating additive-free LFP cathodes and offers new insights into the structure–property relationships governing the interfacial transport in ASSBs.

1. Introduction

The development of all-solid-state Li-metal batteries (ASSLBs) has gained significant attention as a promising route toward next-generation energy storage systems with enhanced energy density, safety, and longevity [1,2,3,4]. Traditional Li-ion batteries (LIBs) are limited by flammable liquid electrolytes and low-capacity graphite anodes, which pose risks of leakage, dendrite formation, and thermal runaway [5,6]. In contrast, replacing the liquid electrolyte with a solid-state electrolyte (SSE) and utilizing Li metal as the anode offer substantial improvements in volumetric and gravimetric energy density while greatly reducing safety concerns [7,8]. ASSLBs are particularly appealing for high-demand applications such as electric vehicles and grid-level storage, where both energy density and safety are paramount.
Among various solid-state configurations, the LFP/Li1.3Al0.3Ti1.7(PO4)3 (LATP)/Li system presents a highly attractive platform [9,10,11]. LFP is a widely studied cathode material due to its exceptional thermal stability, flat voltage profile, long lifecycle, and compatibility with solid-state architectures [12,13,14]. LATP, a NASICON-type solid electrolyte, offers high Li-ion conductivity and relatively good stability against LFP [15,16]. Furthermore, Li metal as an anode maximizes energy density. This tri-layer system combines safety, cost-effectiveness, and electrochemical performance, making it a suitable model to explore the fundamental and practical aspects of ASSLBs.
A key challenge in solid-state battery development lies in the solid–solid interface between the electrolyte and electrodes [17,18]. Unlike liquid electrolytes that get wet and conform to electrode surfaces, solid electrolytes require intimate physical and chemical contact to enable efficient Li-ion transfer. Interfacial resistance, mechanical mismatch, and chemical reactivity can all hinder ion transport and degrade performance over time. Therefore, understanding and controlling the electrode/electrolyte interface are critical to improving ionic conductivity, cycling stability, and overall device performance in ASSLBs [19,20].
Compared to previous reports on Li/LATP/LFP solid-state batteries, the present study offers a distinct approach in both material processing and mechanistic understanding. In contrast to the work by He et al. [21], which employed a mesoporous LFP–LATP scaffold filled with the MEEP polymer to achieve high areal capacities, our study eliminates the use of polymer fillers entirely, instead relying on a dense LATP pellet with mechanically stable contact. This polymer-free design not only simplifies the cell architecture but also mitigates issues such as polymer degradation or dendrite formation within polymer-rich regions.
While Yao et al. explores Li/LATP/LFP ASSLBs using high-temperature sintered LATP and slurry-cast cathodes with polyvinylidene fluoride (PVDF) binders [22], our study utilizes an alternative fabrication method—alternating current electrophoretic deposition (AC-EPD)—which enables the uniform and binder-integrated deposition of LFP electrodes directly onto current collectors. This approach simplifies processing while ensuring strong adhesion and consistent morphology. In contrast to the tape-casting or manual mixing methods used in prior studies, AC-EPD offers better control over electrode thickness and composition, contributing to improved interface formation and mechanical integrity—critical factors for solid-state battery performance. Moreover, our study extends beyond the electrochemical testing emphasized in previous studies [22] by providing a quantitative correlation between Li-ion diffusivity, b-value analysis (from cyclic voltammetry), and morphological evolution [22,23,24]. For instance, while Mazor et al. focuses on enhancing interfacial contact via chemical strategies [23], such as coating LFP with ionic conductors or interlayers, our approach addresses interface engineering through controlled electrolyte sintering and the detailed analysis of its impact on ion transport.
In addition, Yan et al. investigates the influence of electrode porosity and processing conditions but lacks a comprehensive discussion of charge storage mechanisms [24]. Our work bridges this gap by using b-value analysis to distinguish between diffusion-limited and capacitive charge storage processes across different cell architectures, including comparisons with a liquid electrolyte control system. These insights establish a framework for understanding how interfacial morphology governs charge storage mechanisms in solid-state batteries, further distinguishing this study from the existing literature. While numerous studies focus on maximizing performance in Li/LATP/LFP batteries [21,22,23,24], the objective of this work is to elucidate the interfacial charge storage mechanism and lithium-ion transport kinetics. The electrochemical performance obtained in this study is on par with or superior to comparable systems reported in the literature with similar cathode mass loading, validating the reliability of our system for interface-sensitive analysis.
Here, we compared three battery systems: (a) LFP/LATP sintered at 900 °C, (b) LFP/LATP sintered at 1000 °C, and (c) LFP/LiPF6 liquid electrolyte. This comparison enables a systematic investigation of how the interfacial environment affects the microstructure and ionic pathways of LATP and how these changes translate to differences in electrochemical performance. The inclusion of a liquid-electrolyte-based system provides a practical benchmark, highlighting the performance and interfacial characteristics of conventional systems relative to solid-state architectures. In this study, we employed AC-EPD to fabricate uniform LFP composite cathodes for all three battery types. The AC-EPD technique allows for the controlled, reproducible deposition of active materials with consistent film morphology and thickness. Its ability to form uniform cathodes across different substrates (LATP and metal current collectors) enables the direct comparison of electrochemical performance with minimal variation in electrode architecture. This platform is particularly well suited for interface-sensitive studies, as it ensures that differences in performance can be primarily attributed to the electrolyte and interface characteristics rather than inconsistencies in cathode preparation.

2. Experimental Methods

2.1. Fabrication of AC-EPD LFP Cathode

To prepare the AC-EPD suspension, 108 mg of LFP, 6 mg of carbon black, and 6 mg of PVDF were combined in 40 mL of acetone, yielding a total solid concentration of 3 mg∙mL−1. The mixture was ultrasonicated and stirred to ensure a uniform dispersion. The resulting suspension was then used for AC-EPD, where an AC voltage of 50 V at a frequency of 4 Hz was applied for 10 min to deposit the LFP composite onto a stainless steel (SS) foil substrate, as shown in Figure 1a. The AC-EPD deposition parameters (50 V, 4 Hz) were optimized through preliminary experiments. Frequencies above 4 Hz resulted in negligible deposition due to rapid polarity switching, while lower frequencies (e.g., 2 Hz) caused particle agglomeration and non-uniform films. DC-EPD (0 Hz) led to uncontrolled thickness and poor film integrity. Therefore, 4 Hz was selected to balance deposition efficiency and particle stability, and 50 V was chosen to ensure sufficient electric field strength without inducing breakdown or solvent decomposition. This process produced a thin electrode film with a mass loading of approximately 0.5~0.7 mg∙cm−2. Prior to AC-EPD, the SS substrates were cleaned by sequential ultrasonication in acetone, methanol, and deionized water (1 min each), then dried at 80 °C to remove residual solvents and ensure a clean deposition surface. After deposition, the coated substrate underwent five cycles of roll pressing to improve particle connectivity and electrode cohesion. The electrode was subsequently annealed under an argon atmosphere at 400 °C for one hour, using a temperature ramp rate of 5 °C per minute. This thermal treatment enhanced structural integrity and ensured good adhesion before cell assembly.

2.2. Preparation of LATP Solid Electrolyte and Assembly of Li-Metal/AC-EPD LFP Batteries (Sample 1 and Sample 2) and Li-Metal/LiPF6/AC-EPD LFP (Sample 3)

To prepare the LATP solid electrolyte, 850 mg of the LATP powder was first compacted into a green pellet using uniaxial pressing at 7 MPa for 10 min. The resulting pellet was then vacuum-sealed and subjected to cold isostatic pressing (CIP) at 40 MPa for 30 min to enhance its mechanical strength and bulk density. The densified pellet was subsequently sintered in an argon atmosphere with a two-step thermal process: an initial stage at 650 °C for 30 min, followed by high-temperature sintering at 900 °C (Sample 1) or 1000 °C (Sample 2) for 5 h with a controlled heating rate of 10 °C per minute. After sintering, the LATP pellet was mechanically polished to achieve a uniform thickness of ~350 µm, making it suitable for cell integration. Ionic conductivity measurements using electrochemical impedance spectroscopy showed a value of 1.9 × 10−4 S∙cm−1, indicating sufficient ionic transport for solid-state applications. The ionic conductivity of the synthesized LATP was measured to be ~1.9 × 10−4 S∙cm−1, which lies within the well-reported optimized range for undoped LATP ceramics (typically 2–7 × 10−4 S∙cm−1). While values as high as 1.3 × 10−3 S∙cm−1 have been achieved in certain highly doped or glass–ceramic LATP variants, our result represents stable, reproducible conductivity obtained under conventional sintering conditions without additives. This conductivity is suitable for evaluating the electrochemical interface in all-solid-state batteries, and further enhancement through compositional tuning is planned in future studies.
For liquid-based Li-metal/LiPF6/AC-EPD LFP batteries (Sample 3), a standard 1 M LiPF6 electrolyte dissolved in a 1:1 volume mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) was used. CR2032 coin cells were assembled in an argon-filled glove box to prevent contamination from air or moisture. LFP cathodes were prepared via AC-EPD, and Li metal (250 μm foil) was used as both the counter and reference electrodes. In the solid-state configuration for Samples 1 and 2, LATP served as the primary electrolyte, and to enhance interfacial contact, a small volume (30 μL) of liquid electrolyte was added at the interface. Although a small amount of liquid electrolyte (30 µL of 1 M LiPF6 in EC/DEC) was introduced at the LFP/LATP interface to improve interfacial contact, this quasi-solid-state design is widely adopted to reduce interfacial resistance and better simulate realistic operating conditions. Previous studies have shown that such hybrid configurations do not significantly impair ionic conductivity or structural stability of the solid electrolyte [25,26]. Moreover, the low volume of electrolyte used in this study is unlikely to compromise the long-term solid-state nature of the system, while enabling the accurate evaluation of interface-sensitive charge storage behavior.

2.3. Electrochemical Evaluation of Li-Metal/LFP Cells and Structural Characterization

To investigate electrochemical performance, galvanostatic charge–discharge measurements were performed using a Neware battery cycler across a voltage window of 2.8–4.2 V vs. Li/Li+. Cells were tested at multiple current rates ranging from 1C (170 mA∙g−1) to 5C to evaluate the rate capability. Additionally, cyclic voltammetry (CV) was carried out at various scan rates—0.1, 0.3, 0.5, 0.8, and 1.0 mV∙s−1—to assess the redox behavior and kinetic response of the LFP electrodes, focusing on Li-ion insertion/extraction dynamics within the same voltage range. X-ray diffraction (XRD) and scanning electron microscopy (SEM) were utilized to investigate the crystal structure of the AC-EPD-deposited LFP on an SS foil, as well as to analyze the morphological evolution of the electrodes under varying interfacial conditions and cycling states.

3. Results and Discussion

The LFP cathode was deposited on the SS foil using the AC-EPD method using the setup in Figure 1a. The crystallinity of the LFP film on the SS was confirmed using XRD in Figure 1b. (Sample 1: Li/LATP (900 °C)/LFP, Sample 2: Li/LATP (1000 °C)/LFP, and Sample 3: Li/LiPF6 (liquid electrolyte/LFP.) The XRD pattern corresponds to the LFP electrode fabricated by AC-EPD onto an SS foil substrate under the conditions of 50 V and 4 Hz for 10 min. The diffraction peaks match well with the orthorhombic olivine structure of LFP, confirming the successful deposition of phase-pure crystalline LFP on the substrate. The sharp and intense peaks suggest a high degree of crystallinity in the deposited LFP film, with no evidence of secondary phases such as Fe2O3 or Li3PO4, which could form during improper processing. The absence of significant peak broadening also indicates that the crystallite size is relatively large, and that the EPD process did not degrade the structural integrity of the LFP particles.
The inset image in Figure 1a shows the surface of the EPD-deposited LFP film, which appears dense and uniform, further supporting the effectiveness of the AC-EPD method in forming a high-quality electrode layer. Overall, the XRD analysis in Figure 1b confirms that the AC-EPD process preserved the crystal structure of LFP and enabled its direct deposition onto conductive substrates for solid-state or conventional LIB applications.
The rate performance of the three samples was compared across a range of current densities from 1 C to 5 C in Figure 2, demonstrating its excellent high-rate capability in Sample 1. The rate performance of the three LFP-based cells—each interfaced with a different electrolyte environment—is presented in Figure 2a, with the corresponding charge–discharge voltage profiles shown in Figure 2b–d. These results clearly highlight the effect of the electrolyte interface and LATP sintering temperature on the electrochemical behavior of the LFP electrodes under various current rates. Sample 1, using LATP sintered at 900 °C, demonstrates the best rate performance and stability among the three configurations. As shown in Figure 2a, it maintains a specific capacity of approximately 80–120 mAh∙g−1 across a wide range of current rates (1 C to 5 C), and nearly full capacity is recovered upon returning to 1 C. The corresponding voltage profiles in Figure 2b display well-defined charge–discharge plateaus, even at high rates, suggesting low interfacial resistance and effective Li+ transport across the LFP/LATP interface. This performance indicates favorable interfacial contact and mechanical compliance between the LFP and LATP processed at this temperature.
In contrast, Sample 2, which used LATP sintered at 1000 °C, shows significantly lower capacity and poor rate capability. The capacity drops below 50 mAh∙g−1 at high rates and exhibits abnormal decay in the charging capacity when cycled back to 1 C. This is further supported by the voltage curves in Figure 2c, which reveal distorted and less-defined plateaus, indicating sluggish kinetics and possible interfacial degradation. The higher sintering temperature likely led to a denser LATP microstructure with reduced surface compliance, impairing interfacial contact and increasing resistance during cycling, which will be discussed later.
Sample 3, which employed a liquid electrolyte (1 M LiPF6), exhibits moderate performance. The initial capacity is around 100 mAh·g−1 at 1 C and gradually declines with the increasing rate, but the capacity largely recovers when the current is reduced back to 1 C. Figure 2d shows smoother voltage profiles than Sample 2. While the liquid electrolyte allows better wetting and ion transport than poorly sintered LATP, it still falls short of the well-optimized solid interface seen in Sample 1. Overall, these results demonstrate that the sintering condition of LATP has a substantial impact on the performance of all-solid-state batteries, with optimized conditions (900 °C) enabling superior rate capability and cycling stability through improved electrode–electrolyte interfacial contact.
From the comparison of the cycling performance in the Supporting Information (Figure S1), the LATP 900 °C and 1000 °C samples both exhibit stable cycling behavior over repeated cycles (500 cycles), although the 900 °C sample shows a higher initial capacity. This difference is likely due to better interfacial contact and lower resistance in the 900 °C-sintered LATP, which enhances lithium-ion transport. In contrast, the 1000 °C sample, while more densely sintered, may have poorer interfacial compliance, resulting in lower capacity. However, both samples maintain similar long-term stability, suggesting that their bulk structures remain intact and chemically stable throughout cycling.
The comparison of b-values for the three LFP-based samples, derived from CV at various scan rates, provides insight into the dominant charge storage mechanisms operating in each system [27,28]. The b-value, obtained from the slope of log(current) versus log(scan rate), indicates whether the process is diffusion-controlled (b ≈ 0.5) or surface-capacitive (b ≈ 1.0). Sample 1, which uses LATP sintered at 900 °C, shows b-values of 0.53 (anodic) and 0.52 (cathodic), as seen in Figure 3a,b. These values are very close to 0.5, indicating that the redox process is predominantly diffusion-controlled. The near-symmetric CV curves and stable peak separation further suggest efficient Li+ intercalation/deintercalation and good electrode–electrolyte interfacial contact. This result aligns well with the excellent rate performance observed earlier, confirming the favorable ion transport dynamics in this solid-state configuration.
Sample 2, paired with LATP sintered at 1000 °C, exhibits similar b-values of 0.51 (anodic) and 0.57 (cathodic) in Figure 3c,d. Although still diffusion-dominated, the cathodic value is marginally higher, indicating a slightly more capacitive contribution during discharge. In contrast, Sample 3, using a liquid electrolyte (1 M LiPF6), shows the highest b-values—0.58 (anodic) and 0.56 (cathodic)—as shown in Figure 3e,f. These values reflect a more significant contribution from surface capacitive processes, likely due to enhanced ion mobility and electrolyte wetting at the interface. The sharper, more symmetric CV peaks support this interpretation, pointing to fast surface redox activity and a more pronounced pseudocapacitive effect. In other words, all three systems show charge storage predominantly governed by diffusion, but to varying extents. Sample 1 demonstrates the most ideal solid-state interfacial kinetics, Sample 2 reveals limitations due to high-temperature sintering, and Sample 3 benefits from surface-dominated processes in liquid electrolytes. This comparison underscores how electrolyte type and interface quality critically influence the charge storage behavior in LFP electrodes.
It is also important to note that the broader redox peaks observed in CV curves for the solid-state cells (Samples 1 and 2) relative to the liquid electrolyte cell (Sample 3) arise from a combination of factors including higher interfacial resistance, lower ionic conductivity of LATP, and limited solid–solid contact at the LFP/LATP interface. These factors result in slower ion transport and more distributed electrochemical reactions, leading to peak broadening and increased polarization
The diffusivity analysis presented in Figure 4 compares the Li-ion diffusion behavior of three LFP-based electrodes interfaced with different electrolytes and processing conditions. The current response at anodic and cathodic peaks plotted against the square root of the scan rate (Figure 4a–c) was used to extract diffusion coefficients based on the Randles–Sevcik equation. The resulting diffusivity values are summarized in the bar graph shown in Figure 4d, providing insights into how interface characteristics affect Li-ion transport kinetics.
Sample 1, which uses LATP sintered at 900 °C, exhibits the highest diffusivity values for both anodic and cathodic processes, in the order of ~10−9 cm2∙s−1. This suggests that the interface between LFP and LATP is well formed, likely due to optimal sintering that balances densification and ionic conductivity. The high diffusion coefficient is consistent with the previously observed strong rate capability and minimal polarization in Sample 1, indicating efficient Li+ transport across the electrode–electrolyte interface. In contrast, Sample 2, based on LATP sintered at 1000 °C, shows the lowest diffusivity among the three. Both anodic and cathodic values drop significantly, approaching ~10−10 cm2∙s−1. This reduction reflects poor Li+ transport, which may be attributed to excessive grain growth or reduced surface compliance in the over-sintered LATP, leading to inferior contact with the LFP cathode. The compromised interface in Sample 2 results in sluggish ion kinetics, which aligns with its poor capacity retention and distorted voltage profiles seen in rate performance measurements. Sample 3, using a liquid electrolyte (1 M LiPF6), shows intermediate diffusivity values between Samples 1 and 2. Although not as high as Sample 1, the liquid electrolyte provides sufficient ion mobility and wetting, facilitating moderate diffusion (~10−9 cm2∙s−1). This is reflected in the CV symmetry and decent capacity recovery in rate cycling tests. However, limitations such as SEI formation and side reactions may hinder performance at higher current rates. The diffusivity results reinforce that interfacial quality is a critical factor in determining Li-ion transport in LFP electrodes. Properly sintered LATP at 900 °C (Sample 1) yields the most favorable conditions for fast and reversible diffusion, whereas excessive sintering (Sample 2) degrades ion transport. The liquid system (Sample 3) performs reasonably well, but lacks the structural robustness and long-term stability of an optimized solid-state interface.
The relationship between diffusivity and b-value across the three LFP-based samples reveals how ion transport kinetics and charge storage mechanisms are closely interconnected. In Sample 1, which uses LATP sintered at 900 °C, the b-values are close to 0.5 for both anodic and cathodic peaks, indicating a diffusion-controlled charge storage process. This is consistent with the high Li-ion diffusivity measured for this sample (~10−9 cm2∙s−1), suggesting efficient Li+ transport through the electrode and across the solid-state interface. The well-sintered LATP structure likely enables good contact and facilitates rapid bulk diffusion, which dominates the electrochemical behavior. In Sample 2, where LATP was sintered at a higher temperature of 1000 °C, the diffusivity is the lowest among the three samples (~10−10 cm2∙s−1), reflecting sluggish Li-ion transport. Although the b-values still hover near 0.5–0.57, indicating primarily diffusion-controlled behavior, the slightly higher cathodic b-value suggests a minor increase in surface-related contributions, potentially due to the poor interfacial contact that limits bulk diffusion. The degraded diffusivity is likely the result of reduced interface compliance and increased resistance, caused by excessive LATP grain growth or densification at elevated sintering temperatures. Sample 3, which uses a liquid electrolyte (1 M LiPF6), shows the highest b-values (~0.58) for both anodic and cathodic peaks, pointing to a stronger contribution from surface capacitive mechanisms. The liquid electrolyte facilitates faster ion movement at the electrode–electrolyte interface, enhancing pseudocapacitive and non-faradaic processes. Although its diffusivity is not as high as Sample 1, it remains sufficient (~10−9 cm2∙s−1) to support fast surface redox reactions. The relatively higher b-values in this case reflect the dominance of interfacial kinetics over bulk diffusion, which is typical in liquid systems.
The electrochemical performance of the three LFP-based systems can be comprehensively understood by analyzing the correlation between rate capability, b-values, and Li-ion diffusivity. Sample 1, which incorporates LATP sintered at 900 °C, exhibits the highest specific capacity across all tested C-rates, maintaining stable performance even at 5 C. This excellent rate capability is supported by b-values close to 0.5, indicating a diffusion-controlled charge storage mechanism. The high Li-ion diffusivity (~10−9 cm2∙s−1) measured in this sample further confirms efficient bulk ion transport and low interfacial resistance, enabling fast and reversible electrochemical reactions during high-rate cycling.
In contrast, Sample 2, based on LATP sintered at 1000 °C, shows significantly poorer rate performance, with lower capacities at all current densities and incomplete capacity recovery when the current returns to 1 C. Although the b-values (~0.51 anodic, ~0.57 cathodic) suggest the process is still largely diffusion-controlled, the much lower diffusivity (~10−10 cm2∙s−1) indicates sluggish ion transport. The compromised interface due to over-sintering likely results in poor contact between LFP and LATP, which hinders Li-ion movement and reduces the cell’s ability to perform under high current conditions.
Sample 3, which uses a liquid electrolyte (1 M LiPF6), demonstrates intermediate rate performance—better than Sample 2 but slightly inferior to Sample 1 at higher C-rates. This behavior is consistent with its relatively higher b-values (~0.58), suggesting a greater contribution from surface capacitive processes. The measured diffusivity (~10−9 cm2∙s−1) is sufficient to support fast interfacial reactions, though it does not fully compensate for limitations in bulk ion transport. The liquid electrolyte provides good ionic conductivity and wetting, which enhances surface-driven processes but may still be constrained by interfacial stability or side reactions during extended cycling. Sample 1 achieves superior rate performance due to its high diffusivity and well-formed solid-state interface that supports diffusion-controlled kinetics. Sample 2 is limited by low diffusivity and poor interfacial contact, while Sample 3 benefits from surface capacitive effects and moderate diffusivity but lacks the structural stability of an optimized solid-state system. These findings collectively demonstrate that high-rate capability in LFP electrodes depends on a delicate balance between bulk diffusion, interfacial contact, and surface kinetics, as summarized in Table 1.
The SEM images in Figure 5a–d illustrate the morphological evolution of AC-EPD LFP electrodes under various cycling and interfacial conditions. In Figure 5a, the as-deposited LFP electrode before cycling shows a loosely packed morphology with distinguishable primary particles. The structure appears porous, with noticeable interparticle spacing, indicating a typical surface formed by AC-EPD without compaction from cycling-induced stress or interface interactions.
After cycling in contact with a liquid electrolyte (1 M LiPF6), as shown in Figure 5b, the morphology significantly changes. The surface becomes smoother and more compact, suggesting surface reconstruction and particle merging likely caused by electrolyte-induced side reactions or binder/electrolyte degradation. The reduction in contrast and particle definition may also point to the formation of a surface film or decomposition products, such as SEI-like layers, which can passivate the electrode surface.
In contrast, LFP electrodes cycled in contact with solid-state LATP electrolytes sintered at different temperatures show distinct morphological behavior. In Figure 5c, the interface with LATP sintered at 900 °C preserves a relatively granular texture, with LFP particles still visible and partially interconnected. This suggests moderate interfacial contact and mechanical pressure during cycling, likely promoting Li transport while avoiding extensive surface degradation.
However, in Figure 5d, where LATP was sintered at 1000 °C, the LFP morphology becomes more densely packed and featureless. The clear particle boundaries visible in Figure 5a,c are significantly diminished, implying enhanced densification or possible interfacial reactions at elevated sintering-induced interface conditions. The higher sintering temperature likely increased LATP grain boundary conductivity and mechanical stiffness, leading to stronger physical contact and potentially more intense interfacial stress or reactions during cycling. The dense and featureless morphology observed in Figure 5d for LFP cycled with LATP sintered at 1000 °C may be attributed to mechanical stress accumulation at the rigid LATP interface, leading to particle compaction. Additionally, potential interfacial reactions—such as elemental diffusion from LATP (e.g., Ti or P)—could chemically modify the LFP surface, suppressing the original granular texture. These mechanisms, though not directly confirmed here, are consistent with the reported degradation pathways in high-temperature-processed solid-state interfaces and warrant further investigation using post-mortem structural and compositional analyses.
Although cross-sectional SEM/EDS analysis would provide the direct evidence of the LFP/LATP interface structure, attempts to prepare intact cross-sections were hindered by interfacial delamination and cracking during mechanical polishing, due to the brittle nature of sintered LATP. The surface SEM images indicate significant grain coarsening in LATP sintered at 1000 °C, consistent with excessive densification. This structural evolution is likely to reduce interfacial compliance and limit Li-ion transport, as also supported by the reduced diffusivity values. These findings align with those of the previous reports which state that excessive sintering can suppress beneficial grain boundary conduction and lead to brittle interfaces [29,30]. Further investigation using cross-sectional SEM or focused ion beam analysis is planned to validate this hypothesis.
In summary, the SEM images reveal that a moderately porous, well-adhered interface (Sample 1) supports fast Li-ion diffusion and diffusion-limited kinetics, leading to high-rate performance. Excessively dense morphology (Sample 2) impairs interfacial transport, lowering diffusivity and electrochemical efficiency. Meanwhile, surface smoothing and interphase formation (Sample 3) encourage surface-driven kinetics, reflected in higher b-values and acceptable diffusivity, albeit with less structural integrity than solid-state counterparts. Thus, morphology is a direct indicator of electrochemical performance, especially in systems where solid–solid interfaces govern charge transport.
Overall, these images highlight the critical role of the electrode/electrolyte interface—whether liquid or solid—and processing temperature on the structural integrity and surface stability of LFP electrodes. Solid-state interfaces, especially with optimized LATP processing, may offer improved morphological stability compared to liquid electrolytes, though high-temperature sintering can also induce unintended surface modifications. In this study, LATP pellets were sintered at 900 °C and 1000 °C to intentionally produce two distinct interfacial microstructures for comparative analysis. The lower temperature (900 °C) typically leads to less-densified LATP with higher interfacial resistance, while the higher temperature (1000 °C) may result in coarsened grains and potential interface degradation. These boundary conditions were selected to represent limiting cases rather than an exhaustive sintering profile, aiming to elucidate the impact of interface quality on electrochemical performance. Further work including intermediate sintering temperatures (e.g., 950 °C) is ongoing to extend the observed trends.
The electrochemical performance of our AC-EPD-fabricated LFP electrode is comparable to previously reported Li/LATP/LFP systems with similar mass loading [21,22,23,24]. This validates that our system offers a suitable performance baseline for probing interfacial kinetics and charge storage mechanisms, which is the central focus of this study. Further, to evaluate the scalability of the AC-EPD method, we also tested LFP electrodes with a mass loading of ~2 mg∙cm−2 using a liquid electrolyte, as shown in Figure S2 (Supporting Information). These higher-mass-loading electrodes demonstrated stable cycling and good rate performance, confirming that the interface-sensitive design remains effective under more practical loading conditions. Unlike prior works that primarily emphasized performance optimization, our platform enables mechanistic analysis by combining a reproducible AC-EPD fabrication process with interface-sensitive evaluation methods.
It is also important to emphasize that, in the liquid electrolyte configuration, the EC/DEC solvent system can decompose on the LFP surface to form a cathode–electrolyte interphase (CEI), typically composed of LiF, Li2CO3, and organic moieties. While this CEI can protect the electrode, it may also increase interfacial resistance over time. In contrast, the solid-state LATP interface does not undergo similar solvent-driven decomposition; however, it is subject to mechanical and chemical interfacial instability, especially under high-temperature sintering or prolonged cycling. For example, interfacial reactions such as Ti reduction or phosphate interdiffusion can occur, which degrade ionic conductivity and cycle stability. Therefore, although solid-state systems can suppress solvent-driven SEI formation, maintaining interfacial integrity requires the careful control of interface chemistry and processing conditions.

4. Conclusions

In this work, we systematically investigated the charge storage mechanisms and Li-ion transport behavior in three battery systems: Li/LATP (900 °C)/LFP, Li/LATP (1000 °C)/LFP, and Li/LiPF6 (liquid electrolyte)/LFP. Through scan rate-dependent CV and diffusivity analysis, we demonstrated that the all-solid-state battery with LATP sintered at 900 °C exhibited the highest Li-ion diffusivity and the most pronounced diffusion-controlled charge storage behavior, attributed to its optimized microstructure and strong interfacial contact. In contrast, the 1000 °C-sintered LATP suffered from degraded ionic transport due to microstructural instability, while the liquid electrolyte system showed a greater contribution from surface capacitive processes. The use of AC-EPD to fabricate uniform LFP cathodes enabled direct and reliable comparison across different electrolyte systems. These findings highlight the critical role of solid electrolyte processing and interface engineering in achieving high-performance, diffusion-dominated ASSLBs.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/app15137120/s1, Figure S1: Long-term cycling performance of Li/LATP/LFP all-solid-state cells, Figure S2: Rate performance of an AC-EPD-fabricated LFP electrode with a higher mass loading of ~2 mg cm−2.

Author Contributions

Methodology, S.J.L.; Software, S.J.L.; Formal analysis, B.P.; Investigation, B.P.; Data curation, S.J.L.; Writing—original draft, B.P.; Writing—review & editing, B.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the Basic Science Research Program through the National Research Foundation of Korea (NRF) funded by the Ministry of Education (NRF-2015R1A6A1A03031833, NRF-2019R1F1A1060042 and NRF-2020R1A2C1007258). This work was supported by 2025 Hongik University Innovation Support Program Fund.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The raw data supporting the conclusions of this article will be made available by the authors on request.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Xia, S.; Wu, X.; Zhang, Z.; Cui, Y.; Liu, W. Practical challenges and future perspectives of all-solid-state lithium-metal batteries. Chem 2019, 5, 753–785. [Google Scholar] [CrossRef]
  2. Schnell, J.; Günther, T.; Knoche, T.; Vieider, C.; Köhler, L.; Just, A.; Keller, M.; Passerini, S.; Reinhart, G. All-solid-state lithium-ion and lithium metal batteries–paving the way to large-scale production. J. Power Sources 2018, 382, 160–175. [Google Scholar] [CrossRef]
  3. Park, B. Pseudocapacitive charge storage in ultrathin NiCo-metal organic framework-derived NiCo2O4 Li-metal batteries. Mater. Lett. 2025, 394, 138654. [Google Scholar] [CrossRef]
  4. Wang, C.; Yu, R.; Hwang, S.; Liang, J.; Li, X.; Zhao, C.; Sun, Y.; Wang, J.; Holmes, N.; Li, R. Single crystal cathodes enabling high-performance all-solid-state lithium-ion batteries. Energy Storage Mater. 2020, 30, 98–103. [Google Scholar] [CrossRef]
  5. Kim, T.; Song, W.; Son, D.-Y.; Ono, L.K.; Qi, Y. Lithium-ion batteries: Outlook on present, future, and hybridized technologies. J. Mater. Chem. A 2019, 7, 2942–2964. [Google Scholar] [CrossRef]
  6. Galushkin, N.; Yazvinskaya, N.; Galushkin, D. Mechanism of thermal runaway in lithium-ion cells. J. Electrochem. Soc. 2018, 165, A1303. [Google Scholar] [CrossRef]
  7. Duan, S.; Qian, L.; Zheng, Y.; Zhu, Y.; Liu, X.; Dong, L.; Yan, W.; Zhang, J. Mechanisms of the Accelerated Li+ Conduction in MOF-Based Solid-State Polymer Electrolytes for All-Solid-State Lithium Metal Batteries. Adv. Mater. 2024, 36, 2314120. [Google Scholar] [CrossRef]
  8. Lim, H.; Jun, S.; Song, Y.B.; Baeck, K.H.; Bae, H.; Lee, G.; Kim, J.; Jung, Y.S. Rationally Designed Conversion-Type Lithium Metal Protective Layer for All-Solid-State Lithium Metal Batteries. Adv. Energy Mater. 2024, 14, 2303762. [Google Scholar] [CrossRef]
  9. Xia, Q.; Yuan, S.; Zhang, Q.; Huang, C.; Liu, J.; Jin, H. Designing the Interface Layer of Solid Electrolytes for All-Solid-State Lithium Batteries. Adv. Sci. 2024, 11, 2401453. [Google Scholar] [CrossRef]
  10. Yang, K.; Chen, L.; Ma, J.; He, Y.B.; Kang, F. Progress and perspective of Li1+xAlxTi2-x(PO4)3 ceramic electrolyte in lithium batteries. InfoMat 2021, 3, 1195–1217. [Google Scholar] [CrossRef]
  11. Choi, S.K.; Cho, I.W.; Myung, Y.; Cho, S.Y.; Choi, J.; Yang, M. Stabilizing the Interface between Lithium Metal Anode and Li1.5Al0.5Ti1.5(PO4)3 Electrolyte Using Ion-Conductive Polymers. ACS Appl. Energy Mater. 2025, 8, 6222–6231. [Google Scholar] [CrossRef]
  12. Xu, Y.; Zhang, B.; Ge, Z.; Zhang, S.; Song, B.; Tian, Y.; Deng, W.; Zou, G.; Hou, H.; Ji, X. Advances and perspectives towards spent LiFePO4 battery recycling. J. Clean. Prod. 2024, 434, 140077. [Google Scholar] [CrossRef]
  13. Suttison, S.; Pengpat, K.; Intatha, U.; Fan, J.; Zhang, W.; Eitssayeam, S. Preparation of LFP-based cathode materials for lithium-ion battery applications. Mater. Today Proc. 2022, 65, 2347–2350. [Google Scholar] [CrossRef]
  14. Lee, J.; Park, B.-N. Inducing and Understanding Pseudocapacitive Behavior in an Electrophoretically Deposited Lithium Iron Phosphate Li-Metal Battery as an Electrochemical Test Platform. J. Phys. Chem. Lett. 2024, 15, 7095–7102. [Google Scholar] [CrossRef] [PubMed]
  15. DeWees, R.; Wang, H. Synthesis and properties of NaSICON-type LATP and LAGP solid electrolytes. ChemSusChem 2019, 12, 3713–3725. [Google Scholar] [CrossRef]
  16. Luo, C.; Yi, M.; Cao, Z.; Hui, W.; Wang, Y. Review of ionic conductivity properties of NASICON type inorganic solid electrolyte LATP. ACS Appl. Electron. Mater. 2024, 6, 641–657. [Google Scholar] [CrossRef]
  17. Chai, S.; He, Q.; Zhou, J.; Chang, Z.; Pan, A.; Zhou, H. Solid-State Electrolytes and Electrode/Electrolyte Interfaces in Rechargeable Batteries. ChemSusChem 2024, 17, e202301268. [Google Scholar] [CrossRef]
  18. Jiang, Y.; Lai, A.; Ma, J.; Yu, K.; Zeng, H.; Zhang, G.; Huang, W.; Wang, C.; Chi, S.S.; Wang, J. Fundamentals of the Cathode-Electrolyte Interface in All-solid-state Lithium Batteries. ChemSusChem 2023, 16, e202202156. [Google Scholar] [CrossRef]
  19. Xi, L.; Zhang, D.; Xu, X.; Wu, Y.; Li, F.; Yao, S.; Zhu, M.; Liu, J. Interface Engineering of All-Solid-State Batteries Based on Inorganic Solid Electrolytes. ChemSusChem 2023, 16, e202202158. [Google Scholar] [CrossRef]
  20. Park, B. Mg-Composition Dependent Cycle Stability in Zn1-xMgx O Li-ion Battery: Transition from Electronic Transport-Limited to Ionic Transport Limited Cycles. Korean J. Met. Mater. 2024, 62, 377–384. [Google Scholar] [CrossRef]
  21. Ihrig, M.; Dashjav, E.; Laptev, A.M.; Ye, R.; Grüner, D.; Ziegner, M.; Odenwald, P.; Finsterbusch, M.; Tietz, F.; Fattakhova-Rohlfing, D. Increasing the performance of all-solid-state Li batteries by infiltration of Li-ion conducting polymer into LFP-LATP composite cathode. J. Power Sources 2022, 543, 231822. [Google Scholar] [CrossRef]
  22. Yao, S.; Kalami, S.; Nam, S.; Goodenough, J.B.; Khani, H. Development of an Electrophoretic Deposition Method for the In Situ Fabrication of Ultra-Thin Composite-Polymer Electrolytes for Solid-State Lithium-Metal Batteries. Small 2023, 19, 2208252. [Google Scholar] [CrossRef] [PubMed]
  23. Mazor, H.; Golodnitsky, D.; Burstein, L.; Gladkich, A.; Peled, E. Electrophoretic deposition of lithium iron phosphate cathode for thin-film 3D-microbatteries. J. Power Sources 2012, 198, 264–272. [Google Scholar] [CrossRef]
  24. Yan, S.; Guo, J.; Tong, Y.; Du, X. Electrophoresis study on carbon cloth loaded with LiFePO4 for integrated flexible cathodes in lithium-ion batteries. J. Appl. Electrochem. 2025, 55, 595–602. [Google Scholar] [CrossRef]
  25. Tang, J.; Wang, L.; You, L.; Chen, X.; Huang, T.; Zhou, L.; Geng, Z.; Yu, A. Effect of organic electrolyte on the performance of solid electrolyte for solid–liquid hybrid lithium batteries. ACS Appl. Mater. Interfaces 2021, 13, 2685–2693. [Google Scholar] [CrossRef]
  26. Wang, C.; Sun, Q.; Liu, Y.; Zhao, Y.; Li, X.; Lin, X.; Banis, M.N.; Li, M.; Li, W.; Adair, K.R. Boosting the performance of lithium batteries with solid-liquid hybrid electrolytes: Interfacial properties and effects of liquid electrolytes. Nano Energy 2018, 48, 35–43. [Google Scholar] [CrossRef]
  27. Schötz, T.; Gordon, L.W.; Ivanov, S.; Bund, A.; Mandler, D.; Messinger, R.J. Disentangling faradaic, pseudocapacitive, and capacitive charge storage: A tutorial for the characterization of batteries, supercapacitors, and hybrid systems. Electrochim. Acta 2022, 412, 140072. [Google Scholar] [CrossRef]
  28. Park, B.-N. An Electrochemical-Cycling-Induced Capacitive Component on the Surface of an Electrophoretic-Deposited Lithium Iron Phosphate Cathode. Crystals 2024, 14, 658. [Google Scholar] [CrossRef]
  29. Park, C.; Na, S.; Park, H.G.; Park, K. Synergistic effect of calcination and sintering on the reduction of grain boundary resistance of LATP solid electrolyte. ACS Appl. Mater. Interfaces 2023, 15, 26985–26992. [Google Scholar] [CrossRef]
  30. Davaasuren, B.; Tietz, F. Impact of sintering temperature on phase formation, microstructure, crystallinity and ionic conductivity of Li1.5Al0.5Ti1.5(PO4)3. Solid State Ion. 2019, 338, 144–152. [Google Scholar] [CrossRef]
Figure 1. (a) The schematic illustration of the AC-EPD setup used for depositing LFP/CB/PVDF onto an SS foil, along with an optical micrograph of the LFP composite film on the SS foil. (b) The XRD pattern of the LFP cathode film fabricated via AC-EPD, confirming its crystalline structure.
Figure 1. (a) The schematic illustration of the AC-EPD setup used for depositing LFP/CB/PVDF onto an SS foil, along with an optical micrograph of the LFP composite film on the SS foil. (b) The XRD pattern of the LFP cathode film fabricated via AC-EPD, confirming its crystalline structure.
Applsci 15 07120 g001
Figure 2. (a) Rate performance of AC-EPD LFP electrodes in three cell configurations: Sample 1 (Li/LATP (900 °C)/LFP), Sample 2 (Li/LATP (1000 °C)/LFP), and Sample 3 (Li/LiPF6/LFP), cycled at 1C, 2C, 5C, and returned to 1C. (bd) Corresponding charge–discharge voltage profiles at various C-rates for (b) Sample 1, (c) Sample 2, and (d) Sample 3.
Figure 2. (a) Rate performance of AC-EPD LFP electrodes in three cell configurations: Sample 1 (Li/LATP (900 °C)/LFP), Sample 2 (Li/LATP (1000 °C)/LFP), and Sample 3 (Li/LiPF6/LFP), cycled at 1C, 2C, 5C, and returned to 1C. (bd) Corresponding charge–discharge voltage profiles at various C-rates for (b) Sample 1, (c) Sample 2, and (d) Sample 3.
Applsci 15 07120 g002
Figure 3. Cyclic voltammetry (CV) analysis and b-value determination for AC-EPD LFP electrodes in three different battery configurations. (a,c,e) CV curves recorded at scan rates ranging from 0.1 to 1.0 mV/s for (a) Sample 1 (Li/LATP 900 °C/LFP), (c) Sample 2 (Li/LATP 1000 °C/LFP), and (e) Sample 3 (Li/LiPF6/LFP). (b,d,f) Corresponding log(i) vs. log(scan rate) plots at anodic and cathodic peak currents for the three samples, used to extract b-values.
Figure 3. Cyclic voltammetry (CV) analysis and b-value determination for AC-EPD LFP electrodes in three different battery configurations. (a,c,e) CV curves recorded at scan rates ranging from 0.1 to 1.0 mV/s for (a) Sample 1 (Li/LATP 900 °C/LFP), (c) Sample 2 (Li/LATP 1000 °C/LFP), and (e) Sample 3 (Li/LiPF6/LFP). (b,d,f) Corresponding log(i) vs. log(scan rate) plots at anodic and cathodic peak currents for the three samples, used to extract b-values.
Applsci 15 07120 g003
Figure 4. The determination of Li-ion diffusivity in AC-EPD LFP electrodes for three battery configurations. (ac) The plots of peak current versus the square root of the scan rate (ν1/2) for anodic and cathodic processes in (a) Sample 1 (Li/LATP 900 °C/LFP), (b) Sample 2 (Li/LATP 1000 °C/LFP), and (c) Sample 3 (Li/LiPF6/LFP), based on the Randles–Ševčík equation. Linear fits confirm diffusion-controlled behavior. (d) Extracted diffusivity values for anodic (red circles) and cathodic (blue squares) processes.
Figure 4. The determination of Li-ion diffusivity in AC-EPD LFP electrodes for three battery configurations. (ac) The plots of peak current versus the square root of the scan rate (ν1/2) for anodic and cathodic processes in (a) Sample 1 (Li/LATP 900 °C/LFP), (b) Sample 2 (Li/LATP 1000 °C/LFP), and (c) Sample 3 (Li/LiPF6/LFP), based on the Randles–Ševčík equation. Linear fits confirm diffusion-controlled behavior. (d) Extracted diffusivity values for anodic (red circles) and cathodic (blue squares) processes.
Applsci 15 07120 g004
Figure 5. SEM images showing morphological evolution of AC-EPD LFP electrodes under different cycling and interfacial conditions. (a) As-deposited LFP electrode before cycling. (b) LFP after cycling in contact with liquid electrolyte (1 M LiPF6 in EC/DEC). (c) LFP after cycling with LATP solid electrolyte sintered at 900 °C. (d) LFP after cycling with LATP sintered at 1000 °C.
Figure 5. SEM images showing morphological evolution of AC-EPD LFP electrodes under different cycling and interfacial conditions. (a) As-deposited LFP electrode before cycling. (b) LFP after cycling in contact with liquid electrolyte (1 M LiPF6 in EC/DEC). (c) LFP after cycling with LATP solid electrolyte sintered at 900 °C. (d) LFP after cycling with LATP sintered at 1000 °C.
Applsci 15 07120 g005
Table 1. The summary table comparing the electrochemical characteristics of the three battery samples based on b-value analysis and Li-ion diffusivity.
Table 1. The summary table comparing the electrochemical characteristics of the three battery samples based on b-value analysis and Li-ion diffusivity.
Sampleb-Value (Avg.)Dominant MechanismDiffusivityInterpretation
1~0.52–0.53Diffusion-controlledHigh (~10−9 cm2/s)Fast ion transport aligns with diffusion-limited kinetics
2~0.54Mostly diffusion, minor capacitiveLow (~10−10 cm2/s)Low diffusivity causes sluggish kinetics, limited surface contribution
3~0.58Mixed with capacitive dominanceModerate (~10−9 cm2/s)Capacitive contribution increases due to fast surface reaction in liquid system
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Lee, S.J.; Park, B. Probing Solid-State Interface Kinetics via Alternating Current Electrophoretic Deposition: LiFePO4 Li-Metal Batteries. Appl. Sci. 2025, 15, 7120. https://doi.org/10.3390/app15137120

AMA Style

Lee SJ, Park B. Probing Solid-State Interface Kinetics via Alternating Current Electrophoretic Deposition: LiFePO4 Li-Metal Batteries. Applied Sciences. 2025; 15(13):7120. https://doi.org/10.3390/app15137120

Chicago/Turabian Style

Lee, Su Jeong, and Byoungnam Park. 2025. "Probing Solid-State Interface Kinetics via Alternating Current Electrophoretic Deposition: LiFePO4 Li-Metal Batteries" Applied Sciences 15, no. 13: 7120. https://doi.org/10.3390/app15137120

APA Style

Lee, S. J., & Park, B. (2025). Probing Solid-State Interface Kinetics via Alternating Current Electrophoretic Deposition: LiFePO4 Li-Metal Batteries. Applied Sciences, 15(13), 7120. https://doi.org/10.3390/app15137120

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop