Next Article in Journal
Effect of Compaction Degree on the Carbonation Properties of Steel Slag
Next Article in Special Issue
Development of a Color-Changing Face Mask for Fever Detection Applications
Previous Article in Journal
Evaluation of Factors Affecting Fluoride Release from Compomer Restorative Materials: A Systematic Review
Previous Article in Special Issue
Evaluation of High-Temperature Sterilization Processes: Their Influence on the Mechanical Integrity of Additively Manufactured Polymeric Biomaterials
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Thermal and Optical Characterization of Polycarbonate Reflectors Doped with Titanium Dioxide Using Thermography

by
Isabella Luísa Vieira Aquino Cassimiro
1,*,
Juan Ignacio Tomsich
2,
Matheus Pereira Porto
1,
Rosemary do Bom Conselho Sales
3,
Izabella Helena Werneck Soares Rezende
1,
Nathan Funchal de Rezende
1 and
Maria Teresa Paulino Aguilar
1
1
Graduate Program in Mechanical Engineering, Federal University of Minas Gerais (UFMG), Belo Horizonte 31270-901, MG, Brazil
2
Graduate Program in Engineering, Universidad Tecnologica Nacional Facultad Regional Haedo, Haedo B1706, Argentina
3
Graduate Program in Design, State University of Minas Gerais (UEMG), Belo Horizonte 30160-042, MG, Brazil
*
Author to whom correspondence should be addressed.
Materials 2025, 18(7), 1628; https://doi.org/10.3390/ma18071628
Submission received: 20 February 2025 / Revised: 7 March 2025 / Accepted: 1 April 2025 / Published: 2 April 2025

Abstract

:
Automotive reflectors used in headlamps and rear lamps are typically made of polycarbonate. However, this polymer has low light reflectivity. To enhance its reflective properties, it undergoes a metallization process, which significantly increases production costs. Therefore, it is of interest to develop polymers that do not require metallization for the manufacturing of automotive reflectors. In this regard, the use of polycarbonate reinforced with titanium dioxide nanoparticles may be an alternative. Studies indicate that incorporating these nanoparticles can improve the degradation temperature and mechanical properties of the composites. In the case of automotive reflectors, in addition to degradation due to temperature, it is crucial to assess the thermal diffusivity and reflectivity of these composites, thus ensuring the lighting performance of the component. Studies on such characteristics in polycarbonates with titanium dioxide nanoparticles are mostly limited to investigations of hardness and optical properties using Raman and UV–Vis spectroscopy tests. This article investigates the thermal and lighting performance of polycarbonate (PC) samples with 10 wt% titanium dioxide (TiO2) nanoparticles and automotive reflectors with the same chemical composition. The thermal stability of PC and PC-10%TiO2 was analyzed by thermogravimetry (TGA), whereas the reflectors were evaluated using active infrared thermography. Spectral thermographic analysis in the mid- and long-wave infrared range provided thermal diffusivity data for the polycarbonates and offered important insights into their optical behavior under operational conditions (up to 70 °C). Furthermore, illumination tests were conducted on PC-10%TiO2, using metalized polymeric reflectors commonly employed in the automotive industry as a reference. The TGA results showed that incorporating 10 wt% TiO2 into PC increased the degradation temperature from 167 °C to 495 °C. The long-wave infrared emissivity of PC-10%TiO2 (averaging 0.96) was 3% lower than that of polycarbonate. PC-10%TiO2 exhibited a thermal diffusivity of 0.20 mm2/s, which was 28.6% lower than that of PC, indicating greater thermal inertia due to the presence of nanoparticles. The lighting performance of the PC-10%TiO2 reflector was on average 4% lower than that of a commercially available metallized polycarbonate reflector. However, for automotive reflectors, this value meets the sector’s regulatory criteria. These findings suggest that PC-10%TiO2 has potential for use in the production of internal vehicle lighting reflectors, without significantly compromising light reflectivity, while offering the advantages of thermal stability and reduced heating around the reflector.

1. Introduction

In the automotive sector, both internal and external lamps are essential components, as they contribute to vehicle signaling, safety, comfort, and esthetics [1]. Lamps comprise the lens, the reflector, and the light source. Reflectors play a key role in directing and reflecting light. The most used material for manufacturing reflectors is polycarbonate. Although polycarbonate (PC) possesses suitable thermal, mechanical, and impact resistance properties, it has low light reflectivity [2,3,4,5,6,7]. To overcome this drawback, a metallization process is applied to the reflectors. Metallization involves the deposition of a thin aluminum layer onto the polymer surface through evaporation [3,8,9]. This process is not only costly but also time-consuming, particularly when dealing with complex geometries [10,11,12]. A cost- and time-effective alternative to eliminate the metallization stage is the incorporation of titanium dioxide nanoparticles into PC, as this compound has been extensively studied for various applications due to its optical properties [13].
Literature studies using PC films with low TiO2 content (up to 6 wt%) indicate that increasing the TiO2 proportion enhances the composite’s mechanical and/or thermal properties, but the optical band gap values reduce with an increase in the TiO2 content of the nanocomposites [14,15,16,17,18,19,20,21,22,23,24]. Regarding thermal performance, most of these studies assess stability and degradation temperature as a function of TiO2 content. However, thermal conductivity and/or diffusivity, as well as heat reflection and lighting performance, have not been evaluated. Studies on PC with TiO2 concentrations above 6 wt%, whether related to thermal or optical performance, remain scarce. Jawad and Ahmed [25] investigated the effects of incorporating titanium dioxide nanoparticles in proportions ranging from 2% to 10% in PC/wood fiber composites. They assessed the material’s morphological, mechanical, thermal, electrical, and intrinsic properties. The results showed that adding TiO2 nanoparticles increased the thermal conductivity of the composites, with the highest values observed at around 3 wt% TiO2. Eskandari [26] conducted optical property studies using PC with 5% and 10% TiO2, employing Raman spectroscopy tests and UV–Vis spectroscopy, and showed that, by increasing the percentage of nanoparticles to PC, the band gap of the composites started to decrease, and the hardness values increased.
In addition to luminous performance, automotive light reflectors must also exhibit thermal stability to maintain their efficiency over time. They should have high reflectivity in both the visible and infrared spectra, along with low thermal diffusivity. High reflectivity in the long-wave infrared spectrum minimizes heat absorption, preventing performance degradation or damage to adjacent components. Low thermal diffusivity in the material hinders rapid heat propagation through the reflector, avoiding excessive heating of the components near the light source. Both properties are crucial to ensure optimal functionality of the lighting system. Despite the well-established knowledge of the thermal and optical properties of polycarbonate [27,28] and TiO2 [29,30,31], there is a lack of information regarding the thermal diffusivity and heat reflection of TiO2-modified PC composites. Moreover, no data have been found on the lighting performance of PC with 10 wt% TiO2 (PC-10%TiO2). Thus, a knowledge gap exists regarding the contribution of high TiO2 concentrations to the thermal stability, reflectivity, and thermal diffusivity of PC-10%TiO2. In this context, to further advance the field, this study investigates the optical and thermal performance of the raw material and reflectors made from PC with 10 wt% TiO2. Thermogravimetric analysis, active infrared thermography, and lighting performance testing were employed in this study.
Active infrared thermography, using a lamp and a climate chamber as the heat source, was chosen because it had been previously used to evaluate the thermal properties of components as a whole [32,33,34,35,36]. However, to achieve so, it is necessary to know the emissivity of the materials precisely. Emissivity is the capacity of a surface to emit thermal radiation when compared to that of a black body. This factor depends on the wavelength, the direction of observation in relation to the surface, and the temperature of the material [27]. The determination of emissivity by infrared thermography is commonly performed by the “tape method” [37]. However, this method can be improved by combining it with the two-color method to determine the emissivity of PC-10%TiO2, using two thermal cameras that operate in different regions of the infrared spectrum, thus adopting a spectral approach [23,38,39,40]. The combined use of the tape method with the two-color method as a technique for determining optical properties at temperatures close to room temperature represents, to the best of the authors’ knowledge, an unprecedented contribution to the field of materials. In this sense, it is believed that the methods discussed here can support the use of thermography in other studies.

2. Materials and Methods

2.1. Materials

Samples were analyzed, fabricated from PC plates with and without the incorporation of 10 wt% TiO2 nanoparticles (Figure 1). For thermal performance and luminosity tests, PC reflectors with the addition of 10 wt% titanium dioxide were specifically produced for the experiment (Figure 2). The reflectors were manufactured with dimensions of 136.7 mm in length, 70.7 mm in width, and 48.1 mm in height. Both the plates and the reflectors were custom-made for this study and processed under the supervision of the automotive manufacturer Stellantis, Betim, MG, Brazil.

2.2. Methods

The samples were prepared in the shapes and sizes corresponding to each type of test. TGAs were performed on the samples in powder form, while thermographic tests were conducted on the samples in the form of disks. Both sample types were taken from PC plates with and without the addition of 10% TiO2. PC-10%TiO2 reflectors were subjected to thermal performance and lighting tests.

2.2.1. Determination of the Thermal Stability of the Materials

The thermal stability of PC with and without the addition of 10%TiO2 was evaluated through thermogravimetry using 10 g of powder from each material. The TA Q600 model equipment (TA Instruments, New Castle, DE, USA) was used, within a temperature range of 40 °C to 800 °C, with a heating rate of 20 °C/min in an inert nitrogen dioxide (NO2) atmosphere.

2.2.2. Determination of the Emissivity of the Materials

Firstly, quantitative active infrared thermography was used to calculate the emissivity of the materials [32,33,34,35,36]. The emissivity of PC, with and without the addition of 10% TiO2, was determined using the “tape method”. The samples were cut from the plates in the form of disks with a diameter of 10 mm and a thickness of 3.5 mm [40]. The test involved using an adhesive tape (Scotch™ (St. Paul, MI, USA) by 3M) with a known emissivity [37] for comparative measurements. The tape was applied to half of the sample surfaces, as shown in Figure 3. The samples were then placed on a heated surface. After the necessary time for the system to reach thermal equilibrium, thermograms were recorded by the thermal camera. For measurements using the two-color method, two cameras operating in distinct spectra were employed [38]. Four measurement points were recorded with both thermal cameras: two on the tapes and two on the surface of the materials. The cameras used were the Flir T1020 (FLIR Systems, Wilsonville, OR, USA) (8 μm to 14 μm) and the Flir X6801sc (3 μm to 5 μm). The experimental setup is shown in Figure 3. Humidity and ambient temperature were kept under control, monitored by a thermohygrometer Testo 605i (Testo SE & Co. KGaA, Lenzkirch, Germany).
The emissivity of the tape was considered known, which allowed the use of Equation (1) to obtain the temperature of the disks. Considering thermal equilibrium between the regions of the sample with and without the tape, the temperature of the taped area could be assumed to be equal to that of the untaped area, leaving the emissivity as the one unknown in Equation (1) for the untaped region, as shown in Table 1. Since this was a gray surface, the emissivity measured in both spectra was expected to be similar.
L λ , a b s   = λ 0 L λ   T o b ε λ , o b 1 ε λ , a t m τ l e n s , λ R λ + L λ   T r e f l 1 ε λ , o b τ l e n s , λ R λ + L λ   T a t m ε a t m , λ τ l e n s , λ R λ d λ  
In Equation (1), λ represents the wavelength (µm), Lλ,abs is the radiance (W/m2) calculated for λ, Lλ is the radiance (W/m2) detected by the camera at λ, ελ,atm and ελ,ob are the emissivity of the atmosphere and the object (unknown), respectively, and Tob, Trefl, and Tatm are the temperatures of the object (K), the reflected surface, and the atmosphere, respectively. The transmissivity of the thermal lens τlensλ (dimensionless) and the spectral responsivity of the detector Rλ (dimensionless) were obtained from the manufacturer’s database.

2.2.3. Determination of the Thermal Diffusivity of the Material

Active infrared thermography was also used to measure and quantitatively determine the thermal diffusivity of the materials. The measurement was based on ASTM E1461-13—thermal diffusivity by the flash method—[41] which considers the use of a correction factor to calculate the average thermal diffusivity of the material. The method evaluates the thermal diffusivity of homogeneous solid materials that are opaque to the applied radiation [41]. Samples in the form of disks with a diameter of 10 mm and a thickness of 3.5 mm were used, having an area smaller than that of the energy beam. The Flir X6801sc (FLIR Systems, Wilsonville, OR, USA) thermographic camera with spectral sensitivity between 3 μm and 5 μm, a support to position the samples, a lamp (6 kJ linear) to generate the flash, temperature detectors, and equipment for data recording were used (Figure 4).
Thermal diffusivity was calculated from measurements at seven points on each sample and as a function of the time it took for the heat to propagate from the front surface of the samples to the back surface. The test sequence consisted of determining the temperature of the sample over time. Immediately after the application of the flash, the camera captured the radiation on the opposite side of the incidence for 30 s. Ten temperature measurements (T) were recorded every second. Using the data obtained over the 30 s, a T curve as a function of time (t) was plotted. In this way, the time to reach the temperature after 30 s could be calculated, considering the initial temperature of the sample. With this value, the thermal diffusivity (α) could be calculated using Equation (2). ASTM E1461-13 [41] recommends using three-time measurements, t0.25, t0.50, and t0.75, which represent the times to reach 25%, 50%, and 75% of the maximum temperature.
α =   k x   l 2   /   t x
where α is the thermal diffusivity (m2 s−1), l is the sample thickness (mm),   k x is a constant related to the speed to reach the temperature in time t x , and t x is the time to reach 25%, 50%, and 75% of the maximum temperature (s).
To calculate the representative thermal diffusivity of the material, it was necessary to use the   k r factor calculated by Equation (3). If the ratio of t0.75/t0.25 (s) was close to 2.272, as stipulated by ASTM E1461-13 [41], the corrected thermal diffusivity was recalculated (Equation (4)).
  k r = 0.3461467 + 0.361578   t 0.75 t 0.25
where t0.25 and t0.75 (s) correspond to the time to reach 25% and 75% of the maximum temperature.
α C = α 0.5   .   k r 13885
where α C is the corrected thermal diffusivity, and α 0.5 is the thermal diffusivity for the time corresponding to 50% of the time taken to reach the maximum temperature.

2.2.4. Determination of the Thermal Performance of the Reflector

For this study, a front roof lamp from one of Stellantis’ vehicles was used. The thermal performance was evaluated because, during operation, the reflector is positioned very close to the lamps within the lighting unit. The PC-10%TiO2 reflectors were manufactured by Olsa of Brazil, following the company’s compliance standards.
Active infrared thermography was used to estimate the temperatures during the heating of the reflector. A Flir ThermoCAM T420 thermal camera was employed, along with a Fuji N480D (Fujifilm Corporation, Tokyo, Japan) climate chamber, to maintain the reflector’s temperature, simulating vehicle operation. The tests followed a protocol specifically developed for this research. The thermal camera was placed one meter away from the reflector, which was positioned inside the climate chamber, regulated at a temperature of 60 °C. The lamps were connected to a 12 V electrical current and remained switched on for 60 min, the duration recommended by the manufacturer to operate the lamp without softening the material. After this period, both the lamps and the climate chamber were switched off, and temperature measurements were taken. The experimental procedure was conducted both qualitatively and quantitatively. The FLIR Research Studio software (2024.5.0) was used to extract temperature values from three regions of interest: two points at the sides of the lamps and one at the midpoint between them (Figure 5a). Additionally, two profile lines were drawn across each sample: one (L1) passing through a region where the heat from the lamps was not expected to have a direct influence and another (L2) crossing both lamps (Figure 5b).
The thermal camera was configured to obtain apparent temperature values, considering a reflected temperature of 20 °C, an atmospheric temperature of 20 °C, a relative humidity of 50%, and an emissivity of 0.95. Since it was a gray-diffuse surface, Equation (5) was used to estimate the actual temperature of the materials Tobj (K), where Tfull represented the apparent surface temperature, Trefl and Tatm corresponded to the reflected and atmospheric temperatures, respectively, both assumed to be 20 °C, and the transmissivity τatm = 1 (dimensionless). The measurement uncertainty provided by the manufacturer was ±2%.
T f u l l = ε τ a t m T o b j 4 + 1 ε   τ a t m T r e f l 4 + 1 τ a t m   T a t m 4 0.25

2.2.5. Determination of the Lighting Performance

The illuminance level was measured in lux, comparing the PC-10%TiO2 reflector with a metalized polycarbonate reflector used in Stellantis’ assembly line. The analysis considered the regions defined by the manufacturer’s internal lighting level standards. The reflectors were installed in the front roof section of a vehicle provided by the manufacturer. Nine points of interest were defined inside the vehicle for measurement: one point in the central console (Region 1), three points on the seat/backrest of the driver’s and passenger’s seats (Regions 2 to 8), and one point on the side of each front door (Regions 5 and 9). The reflection range used was the one required by Stellantis for lights installed in these regions of the vehicle, as shown in Table 2. The Konica Minolta CL-200 lux meter (Konica Minolta, Inc., Tokyo, Japan) was used, and a dark chamber was employed to eliminate any external light interference.

3. Results and Discussion

3.1. Thermal Stability of Materials

The thermogravimetric analysis curves for PC and PC-10%TiO2 are presented in Figure 6. For PC, an initial weight loss of 10.32% was observed at 167 °C due to the presence of residual solvent or monomer [42]. After this loss, the material remained stable up to 469 °C, when a continuous mass loss began in two stages, with losses of 65.48% and 23.59% at temperatures of 602 °C and 752 °C, respectively. No further weight loss was apparently observed beyond 698 °C, leaving a residue of 0.60%. The degradation mechanisms involved in each stage were complex, and there is no consensus in the literature regarding the chemical nature of the reactions involved [43]. Similar results are reported in the literature [44].
When analyzing the results for PC-10TiO2, it should be considered that TiO2 has thermal stability up to 1200 °C; therefore, within the temperature range considered for the experiments, no mass loss related to this compound was observed [26,29,30]. In PC-10%TiO2, the material was thermally stable up to 495 °C, with no initial loss around 167 °C, as seen in PC. This was likely due to TiO2 nanoparticles acting as a physical barrier, hindering the volatilization of residues and/or solvent. Two stages of continuous mass loss were also observed, with losses of 65.10% and 22.44% at temperatures of 609 °C and 748 °C, respectively, probably associated with the PC polymer. Mass stabilization for PC-10%TiO2 occurred around 749 °C, with a residue of 12.67%. Considering that the residue for pure PC was 0.6%, the data for PC-10%TiO2 indicated that effective incorporation of the oxide occurred [20,45]. Regarding the mass loss rate, the temperature at which the highest rate of weight loss occurred was either reduced or remained unchanged. The higher thermal stability, up to 495 °C, made the material more suitable for use in automotive reflectors, which can heat up to around 200 °C due to the lamp.

3.2. Emissivity of the Materials

In Figure 7a, the radiance thermograms for the Flir X6801sc and T1020 camera are shown, and Figure 7b shows the regions in the samples where the radiance values were measured for each camera. From the radiance values, it was possible to calculate the emissivity and the reflected surface temperature of each sample for each camera used, applying Equation (1).
The results obtained are presented in Table 3. The small difference between the emissivity results obtained from the different thermal cameras demonstrated that the emissivity could indeed be considered as a gray surface [23,39,40]. However, the comparison between the materials showed that the emissivity of the PC-10%TiO2 material was lower in both measurements. This indicated that this material had higher reflectivity and, consequently, minimized the transfer of heat by radiation [20,46]. Materials with low emissivity tend to degrade less over time because they absorb less heat, which could cause expansion and contraction, leading to wear. Therefore, the reflectors made with PC-10%TiO2 would have a more favorable thermal behavior over their lifespan.

3.3. Thermal Diffusivity of the Material

The thermograms of PC and PC-10%TiO2 (Figure 8) showed the seven points (seven different points inside the samples) where each frame of the measurement sequence was obtained. From these measurements, an average temperature value for the PC and PC-10%TiO2 was calculated, and this value was chosen as representative of the temperature of the entire surface at a given time. Using the average values obtained over 30 s, the temperature curve was plotted as a function of time. As a result, the temperature values for points (t0.25, t0.50, and t0.75) were determined, representing 25%, 50%, and 75% of the temperatures reached. A polynomial fitting curve was plotted to facilitate the visualization of the temporal evolution of the thermal response (Figure 9). It was observed that PC increased its temperature by 0.4 °C in 30 s. When using PC-10%TiO2, the temperature increased by only 0.25 °C over the same period, indicating the greater influence of the addition on the thermal behavior of the PC, which thus heated less, effectively maintaining the internal temperature of the environment in which it had been placed.
Table 4 presents the results obtained that allowed for the calculation of the corrected thermal diffusivity. The average corrected thermal diffusivity value for the PC sample was 0.28 mm2/s. For the PC-10%TiO2 sample, it was 0.20 mm2/s. The PC-10%TiO2 exhibited a lower thermal diffusivity coefficient, indicating greater thermal inertia. This was due to the increase in the TiO2 nanoparticle content, which promoted the formation of a more complex network which hindered heat dissipation [47,48]. Therefore, heat was not quickly dissipated into the environment, potentially causing overheating and degradation of the material. As a result, the material was more capable of maintaining a stable internal temperature. As an advantage, the reflector had less interference with the surrounding temperature.

3.4. Thermal Performance of the Reflector

The thermogram in Figure 10 shows the reflector PC-10%TiO2/light with the three points of interest and the profile lines, with L1 passing outside the region of the lamps and L2 passing through the concave part.
Figure 11 shows the apparent temperatures along the two lines (L1 and L2). The temperatures in L1 were close to the temperature of the climate chamber, around 65 °C, indicating that the PC-10%TiO2 was slightly affected by the heat from the lamps in that region. In line L2, the apparent temperature of the PC-10%TiO2/light reflector was 89.1 °C on the left and 96.5 °C on the right. In the central region, the apparent temperature was significantly lower, reaching 65.5 °C on the reflector body, very close to the temperatures of L1, meaning that it was only slightly affected by the heat from the lamps.
As it was a gray-diffuse surface, Equation (5) was used to estimate the temperature reached by the PC-10%TiO2 structure, as shown in Table 5 and Figure 11. The thermal radiation components from the lamps reflected over time on the concave surfaces, contributing to the considerable difference between the apparent and real temperatures. In this case, the lamp glass was considered opaque in the LWIR (long-wave infrared), leading to a reflected temperature (Trefl) of 113.7 °C on the left side and 112.7 °C on the right side. The emissivity of PC-10%TiO2 was expected to decrease with the emission angle [49], meaning that the temperature should have slightly decreased at the extremes of the concave surface, which can be observed upon closer inspection of the thermography analysis in Figure 11. The surface of PC-10%TiO2 reached less than 100 °C, staying below the material’s degradation temperature, as shown in Figure 6.

3.5. Lighting Performance

Table 6 presents the results obtained during the illumination level test of lamps manufactured with a PC-10%TiO2-based reflector and a metalized polycarbonate reflector (PC + Met). A variation of 7.1% to 0.9% was observed between the measured values at the nine points when using each type of lamp.
Overall, the reflective efficiency of PC-10%TiO2 was 4% lower than that of the metalized reflector. This was likely due to the glossy surface of PC + Met, which enhanced reflection. In contrast, the PC-10%TiO2 reflector exhibited lower light dispersion due to the presence of TiO2 nanoparticles, which reduced surface gloss [50,51].
Despite the slightly lower values, the illumination level of the PC-10%TiO2 reflector remained within the light reflection range required by Stellantis for lights installed in the upper front region of the vehicle.

4. Conclusions

A thermogravimetric analysis revealed that PC-10%TiO2 exhibited thermal stability up to 495 °C, significantly higher than PC, which showed an initial mass loss of 10.32% at around 167 °C. Notably, both materials displayed peak mass losses at similar temperatures, approximately 65% and 23%, respectively, values which aligned with the decomposition data of PC, as TiO2 remained stable up to 1200 °C. The residual mass data confirmed the effective incorporation of TiO2 nanoparticles into the PC matrix.
The emissivity measurements from thermal cameras indicated gray-surface behavior for both materials. PC-10%TiO2 demonstrated a lower emissivity than PC, suggesting enhanced reflectivity and reduced radiative heat transfer, which could contribute to improved long-term durability. These properties make it a promising candidate for reflector applications.
Furthermore, PC-10%TiO2 exhibited a lower thermal diffusivity coefficient compared to PC, suggesting that the nanoparticles impeded heat dissipation, potentially leading to increased material temperatures. When the PC-10%TiO2 reflector was integrated into the interior dome lamp and operated for 60 min, it reached a maximum temperature of approximately 91 °C, representing about 20% of its degradation temperature.
Regarding lighting performance, the PC-10%TiO2 reflector showed an average reflection variation of 4% compared to a metallized reflector, yet this value remained within the manufacturer’s acceptable range for vehicle roof interior lighting.
These results demonstrate that PC-10%TiO2 is a viable alternative for reflector production. It maintains acceptable light reflection while offering the benefit of reduced heat transfer to surrounding areas.
Future research should explore the broader applications of these findings, particularly within the context of the circular economy and other relevant industrial sectors.

Author Contributions

Methodology, R.d.B.C.S. and M.T.P.A.; Validation, N.F.d.R.; Formal analysis, M.P.P.; Investigation, J.I.T.; Data curation, I.H.W.S.R.; Writing—original draft, I.L.V.A.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

The authors would like to thank CAPES (Coordination for the Improvement of Higher Education Personnel), CNPq (National Council for Scientific and Technological Development), Fapemig (Minas Gerais State Research Support Foundation), CEMTEC (Multiuser Center for Scientific Thermography), and the Stellantis company for supporting this research.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Gupta, P.; Toksha, B.; Patel, B.; Rushiya, Y.; Das, P.; Rahaman, M. Recent Developments and Research Avenues for Polymers in Electric Vehicles. Chem. Rec. 2022, 22, e202200186. [Google Scholar] [CrossRef] [PubMed]
  2. Jaleh, B.; Shahbazi, N.; Jabbari, A. Optical and Thermal Properties of Polycarbonate–TiO2 Nanocomposite Film. Synth. React. Inorg. Met.-Org. Nano-Met. Chem. 2016, 46, 602–607. [Google Scholar] [CrossRef]
  3. Malnati, P. Enlightening Possibilities: Plastics Expand Role in Vehicle Lighting Applications. Plast. Eng. 2018, 74, 38–45. [Google Scholar] [CrossRef]
  4. Zhang, J.; Feng, J.; Jia, L.; Zhang, H.; Zhang, G.; Sun, S.; Zhou, T. Laser-Induced Selective Metallization on Polymer Substrates Using Organocopper for Portable Electronics. ACS Appl. Mater. Interfaces 2019, 11, 13714–13723. [Google Scholar] [CrossRef] [PubMed]
  5. Filonov, D.; Kolen, S.; Shmidt, A.; Shacham-Diamand, Y.; Boag, A.; Ginzburg, P. Volumetric 3D-Printed Antennas, Manufactured via Selective Polymer Metallization. Phys. Status Solidi (RRL)—Rapid Res. Lett. 2019, 13, 13. [Google Scholar] [CrossRef]
  6. Petrova, M.; Georgieva, M.; Lazarova, D.; Dobrev, D.; Pavlov, T. Electroless metallisation of ABS polymer samples produced by different technologies. Trans. IMF 2021, 99, 188–193. [Google Scholar] [CrossRef]
  7. Diniță, A.; Ripeanu, R.G.; Ilincă, C.N.; Cursaru, D.; Matei, D.; Naim, R.I.; Tănase, M.; Portoacă, A.I. Advancements in Fiber-Reinforced Polymer Composites: A Comprehensive Analysis. Polymers 2023, 16, 2. [Google Scholar] [CrossRef]
  8. Afshar, A.; Mihut, D. Enhancing durability of 3D printed polymer structures by metallization. J. Mater. Sci. Technol. 2020, 53, 185–191. [Google Scholar] [CrossRef]
  9. Lage-Rivera, S.; Ares-Pernas, A.; Abad, M. Last developments in polymers for wearable energy storage devices. Int. J. Energy Res. 2022, 46, 10475–10498. [Google Scholar] [CrossRef]
  10. Akhouri, D.; Banerjee, D.; Mishra, S.B. A review report on the plating process of fused deposition modelling (FDM) built parts. Mater. Today Proc. 2020, 26, 2140–2142. [Google Scholar] [CrossRef]
  11. Melentiev, R.; Yu, N.; Lubineau, G. Polymer metallization via cold spray additive manufacturing: A review of process control, coating qualities, and prospective applications. Addit. Manuf. 2021, 48, 102459. [Google Scholar] [CrossRef]
  12. Melentiev, R.; Yudhanto, A.; Tao, R.; Vuchkov, T.; Lubineau, G. Metallization of polymers and composites: State-of-the-art approaches. Mater. Des. 2022, 221, 110958. [Google Scholar] [CrossRef]
  13. Jaleh, B.; Shahidzadeh, E.S.; Azizian, S. Effects of UV irradiation treated polycarbonate substrates for nanocrystalline deposition of 10TiO2 thin films. J. Interfaces 2018, 2, 73–79. [Google Scholar]
  14. Vidakis, N.; Petousis, M.; Grammatikos, S.; Papadakis, V.; Korlos, A.; Mountakis, N. High Performance Polycarbonate Nanocomposites Mechanically Boosted with Titanium Carbide in Material Extrusion Additive Manufacturing. Nanomaterials 2022, 12, 1068. [Google Scholar] [CrossRef]
  15. Thatcher, J.E.; Crump, D.A.; Devivier, C.; Bailey, P.B.S.; Dulieu-Barton, J.M. Low cost infrared thermography for automated crack monitoring in fatigue testing. Opt. Lasers Eng. 2020, 126, 105914. [Google Scholar] [CrossRef]
  16. Zhu, C.; Hobbs, M.J.; Willmott, J.R. An accurate instrument for emissivity measurements by direct and indirect methods. Meas. Sci. Technol. 2020, 31, 044007. [Google Scholar] [CrossRef]
  17. Jahantigh, F.; Nazirzadeh, M. Synthesis and Characterization of TiO2 Nanoparticles with Polycarbonate and Investigation of Its Mechanical Properties. Int. J. Nanosci. 2017, 16, 1750012. [Google Scholar] [CrossRef]
  18. Saad, N.A.; Jwad, E.R. Investigation of Addition Titanium Dioxide on General Properties of Polycarbonate. OAlib 2018, 05, 1–11. [Google Scholar] [CrossRef]
  19. da Silva, D.J.; Escote, M.T.; Cruz, S.A.; Simião, D.F.; Zenatti, A.; Curvello, M.S. Polycarbonate/TiO2 nanofibers nanocomposite: Preparation and properties. Polym. Compos. 2018, 39, E780–E790. [Google Scholar] [CrossRef]
  20. Li, C.; Yu, H.; Song, Y.; Liang, H.; Yan, X. Preparation and characterization of PMMA/TiO2 hybrid shell microencapsulated PCMs for thermal energy storage. Energy 2019, 167, 1031–1039. [Google Scholar] [CrossRef]
  21. Pavličević, J.; Špírková, M.; Aroguz, A.; Jovičić, M.; Kojić, D.; Govedarica, D.; Ikonić, B. The effect of TiO2 particles on thermal properties of polycarbonate-based polyurethane nanocomposite films. J. Therm. Anal. Calorim. 2019, 138, 2043–2055. [Google Scholar] [CrossRef]
  22. Ghazaryan, L.; Handa, S.; Schmitt, P.; Beladiya, V.; Roddatis, V.; Tünnermann, A.; Szeghalmi, A. Structural, optical, and mechanical properties of TiO2 nanolaminates. Nanotechnology 2021, 32, 095709. [Google Scholar] [CrossRef] [PubMed]
  23. Ferreira, R.A.M.; Pottie, D.L.F.; Dias, L.H.C.; Filho, B.J.C.; Porto, M.P. A directional-spectral approach to estimate temperature of outdoor PV panels. Sol. Energy 2019, 183, 782–790. [Google Scholar] [CrossRef]
  24. Oliveira, A.H.P.; Moura, J.A.S.; Oliveira, H.P. Preparação e Caracterização de Microfibras de Poli(Álcool Vinílico)/Dióxido de Titânio. Polímeros 2013, 23, 196–200. [Google Scholar]
  25. Jawad, A.; Ahmed, S. Studying the influence of the addition of nano-titanium dioxide on the rheological, mechanical, thermal, and electrical properties of polycarbonate/wood flour. J. Thermoplast. Compos. Mater. 2023, 36, 4874–4904. [Google Scholar] [CrossRef]
  26. Eskandari, M.; Liavali, M.N.; Malekfar, R.; Taboada, P. Investigation of Optical Properties of Polycarbonate/TiO2/ZnO Nanocomposite: Experimental and DFT Calculations. J. Inorg. Organomet. Polym. Mater. 2020, 30, 5283–5292. [Google Scholar] [CrossRef]
  27. Bergman, T.L.; Lavine, A.S.; Incropera, F.P.; DeWitt, D.P. Fundamentals of Heat and Mass Transfer, 8th ed.; John Wiley & Sons: Hoboken, NJ, USA, 2020. [Google Scholar]
  28. Gohil, M.; Joshi, G. Perspective of polycarbonate composites and blends properties, applications, and future development: A review. In Green Sustainable Process for Chemical and Environmental Engineering and Science; Elsevier: Amsterdam, The Netherlands, 2022; pp. 393–424. [Google Scholar] [CrossRef]
  29. Parrino, F.; Palmisano, L. Titanium Dioxide (TiO₂) and Its Applications, 1st ed.; Elsevier: Amsterdam, The Netherlands, 2020. [Google Scholar]
  30. Haider, A.J.; Jameel, Z.N.; Al-Hussaini, I.H.M. Review on: Titanium Dioxide Applications. Energy Procedia 2019, 157, 17–29. [Google Scholar] [CrossRef]
  31. Pandey, A.K.; Tiwari, A.K.; Paliwal, H.K. Enhancement of mechanical, thermal and optical properties of TiO2 thin films using glancing angle deposition technique. Opt. Mater. 2022, 134, 113054. [Google Scholar] [CrossRef]
  32. Santoro, L.; Quercio, M.; Canova, A.; Sesana, R. Measuring thermal and electrical performances of additively manufactured magnetic shielding material: An active thermography approach. Nondestruct. Test. Eval. 2024, 39, 2692–2715. [Google Scholar] [CrossRef]
  33. Bison, P.; Cernuschi, F.; Muscio, A. Ermanno Grinzato: A survey on thermophysical properties assessment. Quant. Infrared Thermogr. J. 2024, 21, 438–450. [Google Scholar] [CrossRef]
  34. Bedoya, A.; Salazar, A.; Mendioroz, A.; Marín, E. Measuring the in-plane thermal diffusivity of anisotropic solids by lock-in infrared thermography: Laser-spot vs laser-line heating. J. Appl. Phys. 2024, 135, 135102. [Google Scholar] [CrossRef]
  35. Santos, T.; Amaral, J.S.; Amaral, V.S.; Costa, V.A.F. In-plane thermal anisotropy of natural cork and its variability. Measurement 2025, 242, 116062. [Google Scholar] [CrossRef]
  36. Zhang, Y.; Xu, R.; Zhang, T.; Yang, J.; Liu, Y.; Liu, Y.; Wang, J. Planar distribution measurement of cross-plane thermal diffusivity for microscale films using laser spot periodic heating technique. Int. J. Therm. Sci. 2025, 211, 109692. [Google Scholar] [CrossRef]
  37. Barreira, E.; Almeida, R.M.S.F.; Simões, M.L. Emissivity of Building Materials for Infrared Measurements. Sensors 2021, 21, 1961. [Google Scholar] [CrossRef]
  38. Savino, L.; De Cesare, M.; Musto, M.; Rotondo, G.; De Filippis, F.; Del Vecchio, A.; Russo, F. Free emissivity temperature investigations by dual color applied physics methodology in the mid- and long-infrared ranges. Int. J. Therm. Sci. 2017, 117, 328–341. [Google Scholar] [CrossRef]
  39. Moreira, M.D.O.; Abrão, A.M.; Ferreira, R.A.; Porto, M.P. Temperature monitoring of milling processes using a directional-spectral thermal radiation heat transfer formulation and thermography. Int. J. Heat Mass Transf. 2021, 171, 121051. [Google Scholar] [CrossRef]
  40. Ishikawa, M.; Emoto, A.; Suto, Y.; Nishino, H. Active Thermography Inspection of Surface-whitened Mortars—Measurement of Surface Spectral Absorptivity for Investigation of Efficient Heating Light Wavelengths. J. Nondestruct. Eval. 2024, 43, 7. [Google Scholar] [CrossRef]
  41. ASTM E1461-13; Standard Test Method for Thermal Diffusivity by the Flash Method. ASTM International: West Conshohocken, PA, USA, 2022.
  42. Bonjour, O.; Liblikas, I.; Pehk, T.; Khai-Nghi, T.; Rissanen, K.; Vares, L.; Jannasch, P. Rigid biobased polycarbonates with good processability based on a spirocyclic diol derived from citric acid. Green Chem. 2020, 22, 3940–3951. [Google Scholar] [CrossRef]
  43. Al-Hakami, Y.M.N.; Wahab, M.A.; Yildirir, E.; Ates, F. Thermal degradation kinetics, thermodynamics and pyrolysis behaviour of polycarbonate by TGA and Py-GC/MS. J. Energy Inst. 2024, 113, 101499. [Google Scholar] [CrossRef]
  44. Apaydin-Varol, E.; Polat, S.; Putun, A. Pyrolysis kinetics and thermal decomposition behavior of polycarbonate—A TGA-FTIR study. Therm. Sci. 2014, 18, 833–842. [Google Scholar] [CrossRef]
  45. Wu, X.; Wang, X.; Qin, Z.; Zhang, W. Polycarbonate composites with high light transmittance, haze, and flame retardancy based on a series of incomplete-cage oligomeric silsesquioxanes. J. Mater. Sci. 2021, 56, 428–441. [Google Scholar] [CrossRef]
  46. Li, C.; Yu, H.; Song, Y.; Wang, M.; Liu, Z. A n-octadecane/hierarchically porous TiO2 form-stable PCM for thermal energy storage. Renew. Energy 2020, 145, 1465–1473. [Google Scholar] [CrossRef]
  47. Gamarra, F.; Medina, J.; Lanchipa, W.; Tamayo, R.; Sacari, E. Structural, Optical, and Arsenic Removal Properties of Sol–Gel Synthesized Fe-Doped TiO2 Nanoparticles. Nanomaterials 2022, 12, 3402. [Google Scholar] [CrossRef]
  48. Svora, P.; Pawełkowicz, S.S.; Ecorchard, P.; Plocek, J.; Schieberová, A.; Prošek, Z.; Ptáček, P.; Pošta, J.; Targowski, P.; Kuklík, P.; et al. Study of Interactions Between Titanium Dioxide Coating and Wood Cell Wall Ultrastructure. Nanomaterials 2022, 12, 2678. [Google Scholar] [CrossRef]
  49. Howell, J.R.; Mengüc, M.P.; Daun, K.; Siegel, R. Thermal Radiation Heat Transfer, 7th ed.; CRC Press: Boca Raton, FL, USA, 2021; Volume 1. [Google Scholar]
  50. Kang, K.; Byeon, I.; Kim, Y.G.; Choi, J.; Kim, D. Nanostructures in Organic Light-Emitting Diodes: Principles and Recent Advances in the Light Extraction Strategy. Laser Photon Rev. 2024, 18, 2400547. [Google Scholar] [CrossRef]
  51. Chen, J.; Zhao, Q.; Yu, B.; Lemmer, U. A Review on Quantum Dot-Based Color Conversion Layers for Mini/Micro-LED Displays: Packaging, Light Management, and Pixelation. Adv. Opt. Mater. 2024, 12, 2300873. [Google Scholar] [CrossRef]
Figure 1. (a) Polycarbonate plates and (b) polycarbonate plates with 10% of TiO2.
Figure 1. (a) Polycarbonate plates and (b) polycarbonate plates with 10% of TiO2.
Materials 18 01628 g001
Figure 2. Polycarbonate reflector with the addition of 10% titanium dioxide (PC-10%TiO2).
Figure 2. Polycarbonate reflector with the addition of 10% titanium dioxide (PC-10%TiO2).
Materials 18 01628 g002
Figure 3. Experimental setup for emissivity measurement.
Figure 3. Experimental setup for emissivity measurement.
Materials 18 01628 g003
Figure 4. Experimental measurement setup of thermal diffusivity.
Figure 4. Experimental measurement setup of thermal diffusivity.
Materials 18 01628 g004
Figure 5. Points of interest for thermographic reading and profile lines on the reflector PC-10%TiO2: (a) points of interest and (b) profile lines.
Figure 5. Points of interest for thermographic reading and profile lines on the reflector PC-10%TiO2: (a) points of interest and (b) profile lines.
Materials 18 01628 g005
Figure 6. Thermogravimetric curve of PC-10%TiO2: (a) thermogram of PC and (b) thermogram of PC-10%TiO2.
Figure 6. Thermogravimetric curve of PC-10%TiO2: (a) thermogram of PC and (b) thermogram of PC-10%TiO2.
Materials 18 01628 g006
Figure 7. Radiance data obtained with the thermal cameras: (a) thermograms and (b) regions in the samples where the radiance values were measured.
Figure 7. Radiance data obtained with the thermal cameras: (a) thermograms and (b) regions in the samples where the radiance values were measured.
Materials 18 01628 g007
Figure 8. Thermograms for determining the thermal diffusivity as a function of time: (a) thermogram of PC and (b) thermogram of PC-10%TiO2.
Figure 8. Thermograms for determining the thermal diffusivity as a function of time: (a) thermogram of PC and (b) thermogram of PC-10%TiO2.
Materials 18 01628 g008
Figure 9. Thermal response of samples: (a) thermal response of PC and (b) thermal response of PC-10%TiO2.
Figure 9. Thermal response of samples: (a) thermal response of PC and (b) thermal response of PC-10%TiO2.
Materials 18 01628 g009
Figure 10. Thermogram of the three points of interest and profile lines of the reflector PC-10%TiO2.
Figure 10. Thermogram of the three points of interest and profile lines of the reflector PC-10%TiO2.
Materials 18 01628 g010
Figure 11. Values of apparent temperatures along lines L1 and L2 of the structure of the PC-10%TiO2.
Figure 11. Values of apparent temperatures along lines L1 and L2 of the structure of the PC-10%TiO2.
Materials 18 01628 g011
Table 1. Plots that make up the radiation signal in the thermographic measurement.
Table 1. Plots that make up the radiation signal in the thermographic measurement.
SampleTargetAtmosphereThermal Camera Image (Filters, Lenses, and Sensors)Full Simulation
Materials 18 01628 i001 L λ   T r e f 1 ε λ , o b 1 ε λ , a t m L λ   T r e f l 1 ε λ , o b 1 ε λ , a t m τ l e n s , λ R λ
L λ   T r e f 1 ε λ , o b Materials 18 01628 i002Materials 18 01628 i003 L λ , a b s  
Materials 18 01628 i004 L λ   T o b ε λ , o b 1 ε λ , a t m L λ   T o b ε λ , o b 1 ε λ , a t m τ l e n s , λ R λ Materials 18 01628 i005
Materials 18 01628 i006Materials 18 01628 i007
L λ   T o b ε λ , o b L λ   T a t m ε a t m , λ L λ   T a t m ε a t m , λ
Materials 18 01628 i008Materials 18 01628 i009Materials 18 01628 i010
Environmental Component Target Atmosphere
Source: Adapted from Flir System.
Table 2. Luminosity values in lux required.
Table 2. Luminosity values in lux required.
Location by RegionPoints Inside the VehicleMeasured PointsManufacturer’s Reflection Range (lux)
Materials 18 01628 i011Materials 18 01628 i0121˃4 ˂40
Materials 18 01628 i0132–3–4
6–7–8
˃15 ˂40
Materials 18 01628 i0145–9˃4 ˂40
Table 3. Values obtained for temperature and emissivity.
Table 3. Values obtained for temperature and emissivity.
SampleCalculated Temperature (°C)Emissivity
Camera X6801scCamera T1020Camera X6801scCamera T1020
PC62.3067.800.960.95
PC-10%TiO259.6065.200.930.92
Table 4. Results of the determination of thermal diffusivity.
Table 4. Results of the determination of thermal diffusivity.
MaterialCurve PointskxTemperature Thermal Diffusivity (mm2/s)krCorrected Mean Thermal Diffusivity (mm2/s)
PC25%0.0927224.200.280.140.28
50%0.1387924.240.29
75%0.2104924.270.29
PC-10%TiO225%0.0927223.960.180.150.20
50%0.1387924.060.26
75%0.2104924.160.23
Table 5. Apparent and actual temperature for the PC-10%TiO2 reflectors.
Table 5. Apparent and actual temperature for the PC-10%TiO2 reflectors.
SampleOutputTemperature (°C)
LeftCenterRight
PC-10%TiO2Apparent temperature89.165.596.5
Actual temperature78.1
(ε = 0.8, Τrefl = 113.7 °C)
67.2
(ε = 0.9, Τrefl = 30 °C)
90.9
(ε = 0.2, Τrefl = 112.7 °C)
Table 6. Reflector lighting performance.
Table 6. Reflector lighting performance.
Measured PointsManufacturer’s Lighting Limits Min/Max. (lux)Reflector PC + Met
(lux)
Reflector PC-10%TiO2 (lux)Variation (%)
1 >4 <40 21.1 19.6−7.1
2>15 <40 21.1 20.6 −2.4
3>15 <4021.0 19.9 −5.2
4>15 <40 17.6 16.7 −5.1
5>4 <40 19.2 18.5 −3.6
6>15 <40 17.2 16.7 −2.9
7>15 <40 21.0 19.6−6.7
8>15 <40 21.120.9 −0.9
9>4 <40 19.3 18.6−3.6
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Cassimiro, I.L.V.A.; Tomsich, J.I.; Porto, M.P.; Sales, R.d.B.C.; Rezende, I.H.W.S.; Rezende, N.F.d.; Paulino Aguilar, M.T. Thermal and Optical Characterization of Polycarbonate Reflectors Doped with Titanium Dioxide Using Thermography. Materials 2025, 18, 1628. https://doi.org/10.3390/ma18071628

AMA Style

Cassimiro ILVA, Tomsich JI, Porto MP, Sales RdBC, Rezende IHWS, Rezende NFd, Paulino Aguilar MT. Thermal and Optical Characterization of Polycarbonate Reflectors Doped with Titanium Dioxide Using Thermography. Materials. 2025; 18(7):1628. https://doi.org/10.3390/ma18071628

Chicago/Turabian Style

Cassimiro, Isabella Luísa Vieira Aquino, Juan Ignacio Tomsich, Matheus Pereira Porto, Rosemary do Bom Conselho Sales, Izabella Helena Werneck Soares Rezende, Nathan Funchal de Rezende, and Maria Teresa Paulino Aguilar. 2025. "Thermal and Optical Characterization of Polycarbonate Reflectors Doped with Titanium Dioxide Using Thermography" Materials 18, no. 7: 1628. https://doi.org/10.3390/ma18071628

APA Style

Cassimiro, I. L. V. A., Tomsich, J. I., Porto, M. P., Sales, R. d. B. C., Rezende, I. H. W. S., Rezende, N. F. d., & Paulino Aguilar, M. T. (2025). Thermal and Optical Characterization of Polycarbonate Reflectors Doped with Titanium Dioxide Using Thermography. Materials, 18(7), 1628. https://doi.org/10.3390/ma18071628

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop