Next Article in Journal
Hazardous Elements in Asbestos Tremolite from the Basilicata Region, Southern Italy: A First Step
Next Article in Special Issue
Insight into the Effects of Solvent Treatment of Natural Fibers Prior to Structural Composite Casting: Chemical, Physical and Mechanical Evaluation
Previous Article in Journal
Seismic Performance of RC Beam–Column Joints Designed According to Older and Modern Codes: An Attempt to Reduce Conventional Reinforcement Using Steel Fiber Reinforced Concrete
Previous Article in Special Issue
Rammed Earth with Straw Fibers and Earth Mortar: Mix Design and Mechanical Characteristics Determination
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

ANN-Based Model for the Prediction of the Bond Strength between FRP and Concrete

by
Alessio Cascardi
1,* and
Francesco Micelli
2
1
ITC-CNR, Construction Technologies Institute, Italian National Research Council, 70124 Bari, Italy
2
Department of Innovation Engineering, University of Salento, Via per Monteroni, 73100 Lecce, Italy
*
Author to whom correspondence should be addressed.
Fibers 2021, 9(7), 46; https://doi.org/10.3390/fib9070046
Submission received: 25 March 2021 / Revised: 8 June 2021 / Accepted: 2 July 2021 / Published: 6 July 2021
(This article belongs to the Special Issue Fibres in Construction: Mechanical Modelling and Characterisation)

Abstract

:
In the last decades, the uses of fiber reinforced polymer (FRP) composites in the structural strengthening of reinforced concrete (RC) structures have become the state of the art, providing a valid alternative to the traditional use of steel plates. These relatively new materials present, in fact, great advantages, including high corrosion resistance in aggressive environments, low specific weight, high strength-to-mass-density ratio, magnetic and electric neutrality, low axial coefficient of thermal expansion and sustainable costs of installation. In flexural and shear strengthening of RC members, the effectiveness of the epoxy bonded FRP strongly depends on the adhesion forces exchanged with the concrete substrate. When the flexural moment is present, the FRP strengthening is activated through the stress transfer on the tension side, which is guaranteed by the contact beam region to which the adhesive is bonded to the beam itself. Hence, the determination of the maximum forces that cause debonding of the FRP-plate becomes crucial for a proper design. Over the years, many different analytical models have been provided in the scientific literature. Most of them are based on the calibration of the narrow experimental database. Now, hundreds of experimental results are available. The main goal of the current study is to present and discuss an alternative theoretical formulation for predicting the debonding force in an FRP-plate, epoxy-bonded to the concrete substrate by using an artificial neural networks (ANNs) approach. For this purpose, an extensive study of the state of the art, reporting the results of single lap shear tests, is also reported and discussed. The robustness of the proposed analytical model was validated by performing a parametric analysis and a comparison with other existing models and international design codes, as shown herein.

Graphical Abstract

1. Introduction

The existing reinforced concrete (RC) structures have been demonstrated to suffer extensive damage during seismic events [1,2,3]. In these cases, externally bonded reinforcements (EBR) in the forms of FRPs may represent a quick and suitable solution for the structural rehabilitation also because they can be applied in pre-stressed action. The knowledge on the bond behavior at the interface between the FRP and the concrete substrate is essential in order to provide a proper design of the FRP-strengthening. Bond performance between FRP and concrete has been widely studied either experimentally by using the pull-off tests, by calibrating theoretical models and by using finite element model (FEM), e.g., in [4,5,6,7,8,9,10,11,12,13,14,15,16,17,18,19]. The prediction of the ultimate tensile force that can be carried by an FRP plate in a simple pull-off test, before the debonding failure, has been the main target of these studies. Typically, concrete prisms are used, and a tensile force is applied (parallel to the longitudinal direction of the fibers) to the FRP to measure the ultimate load (Pu) which allows computation of the bond strength in terms of ultimate tangential stresses (τf).
The available research in the field (e.g., in [10,11,12,13,14,15,16,17,18,19]) has conclusively shown that the ultimate delamination load initially increases by increasing the bond length, but over a threshold value, any further increase in the bond length does not lead to a further increment of in the ultimate load. Therefore, it is well-known that only a part of the bond length is mobilized in resisting the ultimate load. The mentioned threshold value of the bond length is commonly referred to the active or effective bond length as reported in [18], which represents the length actively involved in the force transfer between the FRP strip and the concrete. The purpose of this research is to provide a new relationship for predicting the delamination load (Pu), calibrated by using an artificial neural networks (ANN) method, between an FRP plate and a concrete rigid substrate. It should be evidenced that the proposed formulation is based on an up-dated large database, analyzed by a modern and well recognized data-mining technique, such as the ANN. In this context a previous attempt was found in [20], where a database of fifty-nine experimental tests of FRP-strengthened specimens was used to study the debonding failure. Starting from that analysis, the present work aims to assess a new ANN predictive model, based on an updated database made up of more than 350 samples, tested in the single lap shear test configurations. In summary, the result consists in the calibration of relationships able to predict the ultimate delamination force Pu. The main goal is to perform a novel analytical expression which may answer to the requirement of improved simplicity and accuracy with respect to the available analytical models as demonstrated in the next sections.

2. A Background of the Bond Behavior between FRP and Concrete Substrate

It has been highlighted that the interfacial bond between FRP and concrete plays a crucial role in maintaining the mechanical performance and the durability of FRP-strengthened concrete structures. In the absence of specific standards, the recommendations reported in [21] are commonly recognized in relation to the bond test on an FRP strip/plate epoxy bonded to a rigid concrete block. The term rigid indicates that internal strains within the concrete block are neglected in the mechanical problem. Typically, the concrete support is fixed and an FRP strip/plate is externally bonded on it (see Figure 1) by using a manual procedure and an epoxy adhesive. A tensile force P is applied on the free side of the plate in the direction of the fibers. The force is increased until the delamination is reached, and the corresponding ultimate value of the load Pu is measured. The failure will occur along the weakest plane of the system: the FRP laminate, the adhesive or the substrate. In fact, three different failure modes have been commonly recognized (excluding the tensile breakage of the FRP itself): a concrete cover delamination, for which the concrete thickness is detached by remaining bonded to the FRP; an adhesive failure in which failure occurs within the resin (in this case the concrete substrate remains un-cracked) and a mixed fracture, namely both cohesive and adhesive. Referring to the Figure 1, the FRP strip/plate transmits the tensile force to the concrete through the tangential stresses τf; which arise at the interfaces. These stresses are not uniformly distributed since they are maximum at the loaded end, and decrease along the reinforcement, according to [13] and early in [22,23]. Based on non-linear fracture mechanics, the interfacial energy Gf is computed as the area below the bond stress–slip curve.
An extensive study on the analytical modeling of the FRP-concrete bond strength was conducted and the analyzed papers are listed in [22,23,24,25,26,27,28,29,30,31,32,33,34], while all the proposed formulations are resumed in Table 1. The models are chronologically arranged in order to show the evolution of the different approaches. The first effort in 1980 was made by Van Gemert [22]. The delamination load of an epoxy-bonded steel plate to a concrete substrate was expressed as the resultant of shear stresses, having a linear trend over the bond area. The maximum shear stress was related to the tensile strength of the concrete substrate. The analytical relationship was so-calibrated on the basis of the experimental results obtained by the authors and similar proposals can be found in [23] (Ph.D. thesis) and [28,29,30,31,32,33,34] (for FRP-plate). An energetic approach was primarily proposed in a scientific paper by Neidermeier in [28]; which considered the fracture energy, Gf, and the role of the effective bond length. This last work inspired more recent studies, such as those reported in [33,34,35,36,37]. Most of the proposed relationships to determine the bond strength consist in a piecewise defined function (see [28,29,30,34,35,36,38,39,40]) depending on the anchorage length of the FRP sheet. In 1997 Maeda et al. [26] developed an empirical model in which, for the first time, a value of the effective bond length is proposed as a function of the properties of the FRP. Khalifa et al. [27] modified Maeda et al. model by including the concrete compressive strength, when evaluating the maximum bond stress (τa). The reported formulations are applicable to both hand lay-up and prefabricated FRP-systems bonded to concrete substrates. It can be noticed that most of the models in Table 1 refers to an empirical calibration. Commonly, the experimental relationship between the bond shear stress and the distance from the applied force point was experienced non-linear (generally hyperbolic or trigonometric shape). In addition, the geometrical and the mechanical properties are generally considered by introducing them as dimensionless.

3. The Artificial Neural Networks (ANN)

Artificial neural networks (ANN) is a method for discovering useful patterns and trends in relatively large data-set. A network represents the joint probability models among given parameters (weight). Each variable is inputted in the system, and it is represented by a node in a graph (usually a tree scheme). The system is made up of an input layer, several hidden layers (chosen by the users) and an output layer.
The dependence between variables is indicated by direct links among the corresponding nodes and the conditional probabilities for each variable (hidden layer). The probability is conditioned (usually with an imposed bias) based on the possible combinations of values for the predecessors in the network. The information about the target is propagated through the network in a step-by-step updating of the probability distribution. The safe-scatter path is the ones which more accurately predict the desiderate output variable (i.e., target) by means of a transforming function. An analytical model is the result of this procedure adapted to extract information (namely “make knowledge”) from data for forecasting the outcomes. An example of the above-described network is schematized in Figure 2.
The ANN has been adopted and described exhaustively in the literature, e.g., in [40,41,42,43,44,45,46]. So, the fundamentals were only considered briefly in this paper. The most widely used ANN technique in civil engineering applications is the back-propagation networks (or B-ANN). The data flow from the input node to the output crossing a series of assumed hidden layer in which intermediate nodes are present in order to elaborate the inputs and make decisions related to the imposed bias. On the other hand, the error propagates in the opposite direction (from the computed output node to the inputs). In the propagation flow the weight and the bias are updated until the theoretical versus experimental scatter reaches a certain tolerance (small enough). The output node is then transformed by a non-linear function in the target, which is the outcome that the user is intended to predict. The relationships between the inputs and the outputs and the transforming function are typically written as reported in Equations (1) and (2), respectively.
y = b + i = 1 n w i · x i
T = 1 1 + e k y
where:
  • xi is the input data of the generic i-input-node;
  • wi is the weight of a generic node in the hidden layer;
  • b is the bias;
  • y is the value of the output node;
  • T is the target;
  • K is a shape factor.

4. Experimental Database for the Formulation of the Theoretical Model

The collection of a wide database related to the results of the single lap shear test on FRP plate/strips and concrete substrate has been analyzed for the definition of an ANN analytical model able to estimate the bond strength. The collected results are extracted from several experimental studies, i.e., [47,48,49,50,51,52,53,54,55,56,57,58,59,60,61,62,63,64], by considering a single layer of carbon or glass FRP bonded on concrete blocks. The experimental results used as references for the implementation of the ANN model are reported in the Appendix A (Table A1). The main parameters considered for the analysis are the following:
  • tf, the thickness of the FRP sheet (mm);
  • bf, the width of the FRP sheet (mm);
  • Ef, the Young’s modulus of the FRP sheet (GPa);
  • Lf, the bond length of the FRP sheet (mm);
  • fc, the compressive strength of the concrete (MPa);
  • bc, the width of the tested concrete element (mm).
In the case of FRP-sheets the term tf is referred to the thickness of the dry fiber unidirectional sheet, in the case of pultruded plates tf is the total thickness of the FRP plate. The ultimate force Pu (kN), namely the bond strength, was imposed as the target of the analysis.
In the database, different typologies of specimens are considered, such as sheet, plate, laminate and in situ cured FRP. The considered parameters have been normalized with respect to the corresponding maximum value and the relative frequency distribution has been computed and reported in the box-plot graphs of the Figure 3. In addition, the interquartile range—IQR (i.e., the difference between the third and the first quartile)—is illustrated in Table 2 for each studied property. It is clear that the most investigated parameters are the dimension of the FRP-plate, namely tf and bf (i.e., larger IQR); on the other hand, the dimension of the substrate, bc, is generally the same in the experimental programs (i.e., IQR = 0.12) as well as the length (Lf) of the FRP bonded on the concrete block (i.e., IQR = 0.21). Finally, the mechanical proprieties of the FRP (Ef) and the concrete (fc) results were explored; in fact, an IQR equal to 0.34 and 0.23 was reached for the compressive strength of the concrete and the elastic modulus of the FRP, respectively.

5. ANN Proposed Model

The most significant parameters that were meaningful in the physical problem were considered as the inputs and a dimensionless output factor was selected, α, in order to define a reliable relationship furnishing the bond strength in terms of maximum debonding load, Pu. Therefore, the outcome analytical model may assume a simple formulation according to Equation (3). Moreover, known parameters are introduced, namely bf, tf and fc; which are the width and the thickness of the FRP-plate and the concrete compressive strength, respectively. The main idea consists in computing the equivalent bond strength between the FRP and the concrete substrate by considering a reduction of the compressive strength of the concrete, i.e.,  fc × α1. Therefore, the ultimate bond force can be easily calculated by multiplying the bond strength with the net-area of the FRP (=bf × tf).
P u = b f · t f · f c · α 1
The ANN-procedure can perform a theoretical formulation for the determination of α based on the specimen mechanical and geometrical characteristics. Thus, three dimensionless parameters were introduced in the neural-networks in order to find out the relationship, which links them to the outcome α. The mentioned inputs are expressed in Equations (4)–(6) and the distribution of their frequency, represented by the number of specimens, is illustrated by the histograms reported in Figure 4. Specifically, β has been included in order to consider the effect of the stress distribution in the area around the FRP-plate, which is mostly affected by the ratio between the dimension of the FRP itself and that of the substrate (see [23,65,66,67]). Moreover, the γ factor considers the influence of the bonded length, that affects the bond strength in relation to the effective bond length [18]. Finally, the mechanical property of the FRP has been considered in Equation (6), according to [65].
β = b c b f
γ = L f t f
δ = E f f c
The database includes 368 specimens, with the highest frequency of β between 1.2 and 3.3 with a minimum value of 1.0 and a maximum of 20.0 (Figure 4a). The α factor presents the most populated range from 74.1 to 441.7 Figure 4b. The δ factor is the most regularly distributed in the database with the top frequency of 120 specimens in the 2.3–3.9 range (Figure 4c). In computing δ the Ef is considered in GPa while fc is expressed in MPa.
A non-linear input-output model was implemented with a polynomial active neuron type in a 3-hidden-layers network. The generated model is listed from Equations (7)–(13). As evident, α was computed by a sequence of polynomial simple equations in which x variables are processed from the characteristics of the specimen expressed through β, γ and δ.
x 1 = 25.20 10 5 β γ + 0.53
x 2 = 0.24 δ + 51.50 10 4 β γ + 1.34
x 3 = 0.81 ( x 1 + x 2 ) + 0.45 x 1 x 2 + 0.17 x 1 2
x 4 = 0.48 δ + 18.74 10 3 δ 2 + 2.07
x 5 = 42.07 10 5 γ 0.19 δ + 1.47
x 6 = 1.13 x 5 + 0.50 x 5 2 0.39 x 4 2
= 16.98 x 6 + 28.21 x 3 + 22.64 x 6 + 38.99

5.1. Model Evaluation

The theoretical value of the force Pu was then calculated by Equation (3). The frequency of the ratio between the experimental results and the predicted values is illustrated in Figure 5, where the normal distribution of the probability frequency (blue line) and the cumulative probability (red line) were both reported.
The domain of the Gaussian function can be divided into quartiles in order to obtain the box plot graph reported in Figure 6 and Table 3. Four quartiles are identified (Q0, Q1, Q2 and Q3) and the median (Me) is represented by a marked line. The range Q1–Q3 represents the box in which the 50% of the statistical population is contained while the range Q0–Q4 includes the whole domain. The mutual size of these two ranges provides information about the accuracy of the model; in fact, the smaller is the box respect to the domain the greater is the accuracy of the predictions of the proposed model. On the other hand, the position of the box gives a measure of the precision; in fact, if the box is located close to 1.0 it means that the theoretical values are close to the experimental ones and if the Me is centered in the box and close to 1.0 it means that most of the predictions tend to coincide with the target value (experimental).
The goodness of fit for the proposed model was performed firstly by verifying the linear correlation of the predicted results respect to the experimental ones in the quartile–quartile (Q–Q) range (Figure 7). Validation was run also by evaluating the prediction performance compared with the 368 tested specimens (Figure 8), found in literature. The robustness of the model was checked by analyzing the parametric influence of the considered input variables on the determination of the debonding ultimate force (Figure 9 and Figure 10). The correlation factor (R2) was calculated as equal to 0.95 in the box Q1–Q3 (see Figure 6 and Table 3) where more than 190 specimens are placed (Figure 7).
The grey area illustrated in Figure 8 is indicative of the validity of the model. A good match of the actual and predicted value of the Pu may be appreciated for the whole database. In particular, the specimens, with the worst forecast (i.e., larger scatter from the experimental relative result) are in the conservative side and represent the 15% of the whole population.

5.2. Robustness Analysis

In Figure 9 and Figure 10 the iso-parametric curves are reported, by varying two fundamental variables, such as the elastic modulus of the FRP and the width of the concrete substrate; in the first case the isoperimetric curves are plotted for different bond lengths, in the second diagram different concrete grades are assumed. As expected, for a fixed value of the elastic modulus of the FRP-plate, if the bond length increases also the debonding force increases (until the limit of the effective bond length). Considering a single iso-parametric curve, with a priori definition of the active bond length, the greater is the entity of the Young’s modulus of the FRP-plate the greater is the force necessary to detach it from the concrete block. In fact, high quality of the fibers means minor elongation of the FRP sheet or major force for inducing e unitary deformation according to [68]. Obviously, the theoretical model is assessed in order to catch the proportional relation between parameters, but the bond length must be limited by an upper bound equal to the effective bond length, experimentally determined (see [28,29,30,36,39]).
In Figure 10 the iso-parametric curves refer to constant values of the concrete compressive strength; the debonding load is plotted versus the width of the concrete block. The parametric study considers 20, 30, 40 and 50 MPa of the concrete compressive strength, which correspond to a value of the debonding force that increases up two times from 20 to 50 MPa of concrete resistance, at the same width. If the mechanical properties of the concrete increase, crack openings are delayed; therefore, the cohesive delamination within the concrete, that is the typical mode of failure occurs at higher load values. For example, concerning the 40 MPa compressive strength line, the increasing of the concrete width produces a small raise of the debonding force according to the experimental evidence (e.g., in [68]). Thus, the proposed model seems to be faithful to the trends that were found from the laboratory tests, as described in the literature database.
Since part of the concrete has been experienced to be pulled off in debonding tests, the tensile strength of the substrate plays a crucial role in the phenomena. For this reason, the sensitivity of the Pu prediction with respect to the fc and f’ct (compressive and tensile strength of the concrete respectively) input has been investigated according to Figure 11. A proportional pseudo linear correlation was found, with a gradient that slightly increases for high levels of concrete compressive strength (45–60 MPa) according to the tensile strength (2.5–3.0 MPa). Whereby, the analytical results are reliable with experimentations.
Further important consideration can be carried out from the calculation of the percentage increment of mean square error (%IncMSE). It refers to the mean increase of the accuracy of the theoretical model. The higher the %IncMSE is, the more important the parameter is that is involved in the global prediction of the target. It allows in finding the contribution a particular variable makes to the prediction of a criterion variable (target) in combination with other predictor variables according to Equation (14). The comparison of the %IncMSE for the imposed inputs is reported in Figure 12. It can be observed that δ is the input which more affect the accurate prediction of the outcome, while β and γ achieved comparable importance in the model performance. In other words, the bond strength is mostly affected by the mechanical properties of the FRP and the substrate. Contrarily, the substrate block dimensions less influenced the result, according to [68].
% IncMSE = S E A · n · 100
where:
  • SE is the square error between the experimental and theoretical values;
  • A is the SE higher response integer;
  • n total number of respondents.

6. Comparison with Existing Analytical Models

A comparison between the theoretical values of the bond strength at the interface between FRP and concrete, predicted by the existing models, is presented in this section. A statistical representation of the capacity of the models to catch accurately the experimental values is illustrated in Figure 13 and Table 4. In Figure 13 the results of the proposed model are highlighted in the grey area. The ability of the model depends on the accuracy and the precision in correlating through a linear relationship the experimental results with those theoretically computed. In this scenario, the box plot representation of Figure 13 seems the best tool to for the mentioned goal. Moreover, Table 4 provides numerical outcomes, further supporting the analysis of the comparison.
It should be remarked that Figure 13 and Table 4 are organized by reporting the increasing of the interquartile range (IQR), in order to obtain an immediate graphic evaluation of the models, as the smaller the IQR is, the more accurate the predictions are. The box-plot presents models with an increasing accuracy by starting from the left to the right in Figure 12 and from top to down in Table 5. Another key-issue is represented by the position of the box, which should be centered in when a precise prediction is found. For example, the models reported in [30,34] are characterized by the smallest dimension of the box, but distant from the unity, thus it can be considered an accurate, but not the precise proposal. Moreover, the position of the Me inside of the box indicates the type of predictions distribution in the Q–Q, namely symmetrical or not symmetrical. In fact, if Me is centered in the box, predictions are symmetrically disposed; it does not happen, for example, in the Chen and Teng model [30]. The kurtosis of the Gaussian curve is also calculated in Equation (15).
K = i = 1 n ( x i μ σ ) 4 n = 3.12
The following situations may occur by concerning about the kurtosis coefficient, K:
  • K > 0: the curve is defined leptokurtic, i.e., more “pointed” of a normal;
  • K < 0: the curve is defined platykurtic, that is “flatter” than a normal;
  • K = 0 the curve is defined normocurtica, i.e., “flat” as a normal.
Commonly, a value of the kurtosis of 3 is accepted as sufficient level for considering the frequency distribution as normal (see [69]). The precision of the frequency curve can be evaluated with the asymmetry of the mode (as1) and with the first and the second asymmetry Pearson’s coefficients (as2 and as3) expressed in Equations (16)–(18) respectively.
as 1 = μ M o σ
as 2 = 3 ( μ M o ) σ
as 3 = 3 ( μ M e ) σ
where:
  • Mo is the mode.
  • μ is the average value.
  • σ is the standard deviator.
Thus, the position of the box plot provides information about the accuracy of the model: if the entire box plot is far from 1 it implies that experimental values are non-linearly related to the theoretical outcomes. On the other hand, the position of the box with respect to the Me specifies if the model is precise or not as well as the Pearson’s coefficients (as1, as2 and as3); the Kurtosis (K) gives a measure of the accuracy, i.e., the lower are the Pearson’s coefficients and the more precise is the prediction and contemporary the higher is the kurtosis the more is the accuracy of the prediction (see [46]). In Table 5, the best value of IQR (min), K (max) and as1, as2 and as3 (min) are reported in bold. The proposed model exhibits the maximum value of K and the minimum of as1, as2 and as3. Based on the present study, the less accurate predictions were provided by very dated proposals (i.e., [24,25,26,27]) that do not evidence the importance enough of the mechanical parameter of the FRP, disagreeing with Figure 12.
A further consideration about the validity of the proposed model can be done based on statistical parameters such as the RRMSE (relative root mean square error), the MAE (mean absolute error) and the MAPE (mean absolute percentage error), expressed by Equations (19)–(21) respectively. Specifically, the RRMSD represents the standard deviation of the differences between the predicted values and the observed values (i.e., the calculation of the residuals) while the MAE and the MAPE are a measure of the average distance between two or more observations and the respective predictions in terms of dimension and dimensionless parameter, respectively. In other words, the MAE (or the MAPE) uses the same scale as the data being measured while the RRMSE reflects a kind of weight factor related to the square of the computed error. All the models were used with the same data base for calculation of the RRMSE, MAE, MAPE, and R2.
RRMSE = 1 n i = 1 n ( y i y ^ i y i ) 2 · 100
MAE = 1 n i = 1 n | y i y ^ i |
MAPE = 1 n i = 1 n | y i y ^ i y i | · 100
This section is not mandatory but may be added if there are patents resulting from the work reported in this manuscript.
where:
  • n is the number of samples in the input database,
  • i is the general sample,
  • yi is the experimental value,
y ^ i is the theoretical value.
The minimum values of the RRMSE, MAE and MAPE correspond to the minimum scatter and the best ability of the theoretical procedure to predict the experimental results. The analytical models cited in the background section are consequently compared in Figure 14 and Table 5 respectively from a graphical and numerical point of view. Moreover, a comparison also including the correlation coefficient R2 is reported in Figure 15. A deep evaluation and comparison of the literature analytical models and of the proposed one can be carried out. In fact, the predictive performance can be evaluated in terms of the best agreement of precision, accuracy and linear correlation between the experimental and theoretical values (see [46]). From this perspective, the precise model corresponds to the nearness of the average, the median and the mode (to each other) of the frequency of the ratio between the experimental and the theoretical outcomes. The accuracy is measured by the proximity of the average, the median and the mode to 1 and, at the same time, the lower value of the MAPE. The correlation is commonly computed by the R2 factor (the more R2 is close to 1 the higher is the correlation between variables). According to Figure 15, the models [24,25,26,27] give the worst predictions of the ultimate bond force; the reason could be related to the low weight attributed to the elastic modulus of the reinforcement, which resulted to affect mostly the accurate prediction of the target (see Figure 12). Controversially, the proposed model and the proposal reported in [35] have demonstrated to provide the best predictions of the failure of the FRP-to-concrete in pull-pull shear test.
Except for the proposed model, there are few other models demonstrating good predictive capacity, such as [28,31,53].
Nowadays, FRPs suffer the competition of FRCM (fabric reinforced cementitious matrix) due to the higher compatibility of the inorganic matrix with existing substrates ([70,71]). The proposed formulation is assumed to be not valid in case of FRCM because the properties of the matrix were neglected in the ANN-calibration [72,73,74].

7. Conclusions

A new empirical model for the prediction of the ultimate bond retention load between an FRP plate/strip and a concrete rigid substrate was presented and discussed within the paper. It is based on an artificial neural networks (ANN) approach that was applied to a large database including 368 available experimental results available from scientific literature. The proposed formulation was found to be effective both in terms of accuracy and precision, thus it can be considered competitive with the available existing analytical models reported in the present study. A parametric study was used to test the robustness of the proposed model. The results confirmed that the presented equation is consistent with the debonding phenomena observed for an FRP plate glued to a concrete block, when subjected to a single lap shear test. A good correlation of the actual and predicted values is shown as well as the outcome of the selected database of 368 specimens. The predictions were found acceptable for almost 65% of the population and conservative in the cases of inaccurate predictions. This result can be considered significant, due to the very brittle nature of the studied mechanical phenomena. The ANN method seems to be a powerful tool, which can be used in order to detect patterns in a large database, made by inhomogeneous data, and extract knowledge from it. The proposed model shows the advantages to be a simple formulation composed of a sequence of polynomial equations and a continuous function, which is formally different from the most available models, that considers varying functions to depend mainly on the active bond length.
Potential development of the proposed model is implementing factors in order to consider further variables affecting the bond strength, such as the type of the laminate, surface treatment, adhesive type, thickness, etc.

Author Contributions

Conceptualization, F.M.; methodology, A.C.; software, A.C.; validation, F.M; formal analysis, A.C.; data curation, A.C.; writing—original draft preparation, A.C.; writing—review and editing, F.M.; visualization, F.M.; supervision, F.M. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All data are available into the paper.

Conflicts of Interest

The authors declare no conflict of interest.

Appendix A

Table A1. Database of FRP-plate vs. concrete substrate bond test.
Table A1. Database of FRP-plate vs. concrete substrate bond test.
ReferencesSpecimen Labeltf (mm)bf (mm)Lf (mm)Ef (GPa)bc (mm)fc (MPa)Pu (kN)
[47]C11.01625.476.2108.478228.636.18.462
C21.01625.476.2108.478228.647.19.931
C31.01625.476.2108.478228.647.110.683
C41.01625.476.2108.478228.647.110.683
C51.01625.476.2108.478228.643.610.531
C71.01625.476.2108.478228.643.69.61
C81.01625.476.2108.478228.643.610.518
C91.01625.476.2108.478228.643.611.199
C101.01625.476.2108.478228.6249.869
C111.01625.476.2108.478228.628.99.343
C121.01625.476.2108.478228.643.711.204
C131.01625.476.2108.478228.636.48.094
C141.01625.476.2108.478228.636.412.811
C151.01625.476.2108.478228.636.411.917
C161.01625.476.2108.478228.636.411.57
[48]1_110.1674010023010028.888.75
1_120.1674010023010026.668.85
1_210.1674020023010028.889.3
1_220.1674020023010026.668.5
1_310.1674030023010028.889.3
1_320.1674030023010026.668.3
1_410.1674050023010028.888.05
1_420.1674050023010028.888.05
1_510.1674050023010026.478.45
1_520.1674050023010026.477.3
2_110.1674010023010024.998.75
2_120.1674010023010024.998.85
2_130.1674010023010026.177.75
2_140.1674010023010026.177.65
2_150.1674010023010024.49
2_210.1674010023010024.9912
2_220.1674010023010024.9910.8
2_310.1674010023010024.9912.65
2_320.1674010023010024.9914.35
2_410.1674010023010024.411.55
2_420.1674010023010024.411
2_510.1674010023010026.179.85
2_520.1674010023010026.179.5
2_610.1674010023010026.178.8
2_620.1674010023010026.179.25
2_710.1674010023010026.177.65
2_710.1674010023010026.176.8
2_810.1674010023010049.977.75
2_820.1674010023010049.978.05
2_910.1674010023010024.46.75
2_920.1674010023010024.46.8
2_1010.1674010023010024.997.7
2_1020.1674010023010026.176.95
[49]I-10.1652575256150234.75
I-20.1652585256150235.69
I-30.1652595256150235.76
I-40.1652595256150235.76
I-50.1652595256150236.17
I-60.16525115256150235.96
I-70.16525145256150235.95
I-80.16525190256150236.68
I-90.16525190256150236.35
I-100.1652595256150236.17
I-110.1652575256150235.72
I-120.1652585256150236
I-130.1652595256150236.14
I-140.16525115256150236.1
I-150.16525145256150236.27
I-160.16525190256150237.03
II-10.165259525615022.95.2
II-20.165259525615022.96.75
II-30.165259525615022.95.51
II-40.1652519025615022.97.02
II-50.1652519025615022.97.07
II-60.1652519025615022.96.98
III-10.1652510025615027.15.94
III-20.1655010025615027.111.66
III-30.1657510025615027.114.63
III-40.16510010025615027.119.07
III-71.272510022515027.14.78
IV-10.165259525615018.95.86
IV-20.165259525615018.95.9
IV-30.165259525615019.85.43
IV-40.165259525615019.85.76
IV-50.165259525615018.95
IV-60.165259525615019.87.08
IV-70.165259525615018.95.5
IV-80.165259525615019.85.93
IV-90.165259525615018.95.38
IV-100.165259525615019.86.6
IV-110.165259525615018.95.51
IV-120.165259525615019.85.67
IV-130.165259525615018.96.31
IV-140.165259525615019.86.19
V-10.165159525615021.13.81
V-20.165159525615021.14.41
V-30.165259525615021.16.26
V-40.165509525615021.112.22
V-50.165759525615021.114.29
V-60.1651009525615021.115.58
VI-10.165259525615021.96.01
VI-20.165259525615021.95.85
VI-30.1652514525615021.95.76
VI-40.1652514525615021.95.73
VI-50.1652519025615021.95.56
VI-60.1652519025615021.95.58
VI-70.1652524025615021.95.91
VI-80.1652524025615021.95.05
VII-10.165259525615024.96.8
VII-20.165259525615024.96.62
VII-30.1652514525615024.97.33
VII-40.1652514525615024.96.49
VII-50.1652519025615024.97.07
VII-60.1652519025615024.97.44
VII-70.1652524025615024.97.16
VII-80.1652524025615024.96.24
[50]I-30.825501001102001711.64
I-40.99501001102001712.86
II-10.4955010011020046.212.55
II-20.665010011020046.214.25
II-30.8255010011020046.217.72
II-40.995010011020046.218.86
III-10.4955010011020061.513.24
III-20.665010011020061.515.17
III-30.8255010011020061.518.86
III-40.995010011020061.519.03
[51]PG1-110.169501309710037.67.78
PG1-120.169501309710037.69.19
PG1-1W10.169751309710037.610.11
PG1-1W20.169751309710037.613.95
PG1-1L110.169501009710037.66.87
PG1-1L120.169501009710037.69.2
PG1-1L210.16950709710037.66.46
PG1-1L220.16950709710037.66.66
PG1-210.338501309710037.610.49
PG1-220.338501309710037.611.43
PC1-1C10.1115013023510037.69.97
PC1-1C20.1115013023510037.69.19
NJ20.08310010024015020.511
NJ30.08310015024015020.511.25
NJ40.08310010024015036.712.5
NJ50.08310015024015036.712.25
NJ60.08310015024015036.712.75
[52,53]DLUT5-2G0.5072015083.0315028.75.81
DLUT5-5G0.5075015083.0315028.710.6
DLUT5-7G0.5078015083.0315028.718.23
DLUT30-1G0.5072010083.0315045.34.63
DLUT30-2G0.5072015083.0315045.35.77
DLUT30-3G0.507506083.0315045.39.42
DLUT30-4G0.5075010083.0315045.311.03
DLUT30-6G0.5075015083.0315045.311.8
DLUT30-7G0.5078010083.0315045.314.65
DLUT30-8G0.5078015083.0315045.316.44
DLUT50-1G0.5072010083.0315055.55.99
DLUT50-2G0.5072015083.0315055.55.9
DLUT50-4G0.5075010083.0315055.59.84
DLUT50-5G0.5075015083.0315055.512.28
DLUT50-6G0.5078010083.0315055.514.02
DLUT50-7G0.5078015083.0315055.516.71
DLUT15-2C0.332015020715028.75.48
DLUT15-5C0.335015020715028.710.02
DLUT15-7C0.338015020715028.719.27
DLUT30-1C0.332010020715045.35.54
DLUT30-2C0.332015020715045.34.61
DLUT30-4C0.335010020715045.311.08
DLUT30-5C0.335010020715045.316.1
DLUT30-6C0.335015020715045.321.71
DLUT30-7C0.338010020715045.322.64
DLUT50-1C0.332010020715055.55.78
DLUT50-4C0.335010020715055.512.95
DLUT50-5C0.335015020715055.516.72
DLUT50-6C0.338010020715055.516.24
DLUT50-7C0.338015020715055.522.8
[54]Ueda_A10.11507523010029.746.25
Ueda_A20.115015023010052.319.2
Ueda_A30.115030023010052.3111.95
Ueda_A40.22507523010055.5110
Ueda_A50.115015023010054.367.3
Ueda_A60.165506537210054.369.55
Ueda_A70.225015023010054.7516.25
Ueda_A80.115070023010054.7511
Ueda_A90.115015023010051.0310
Ueda_A100.111015023010030.512.4
Ueda_A110.112015023010030.515.35
Ueda_A120.332015023010030.519.25
Ueda_A130.552015023010031.6711.75
Ueda_B10.1110020023050031.6720.6
Ueda_B20.3310020023050052.4438
Ueda_B30.3310020023050058.8534
[55]D-CFS-150-30 a0.08310030023010058.8512.2
D-CFS-150-30 b0.08310030023010073.8511.8
D-CFS-150-30 c0.08310030023010073.8512.25
D-CFS-300-30 a0.16710030023010073.8518.9
D-CFS-300-30 b0.16710030023010073.8516.95
D-CFS-300-30 c0.16710030023010073.8516.65
D-CFS-600-30 a0.33310030023010073.8525.65
D-CFS-600-30 b0.33310030023010073.8525.35
D-CFS-600-30 c0.33310030023010073.8527.25
D-CFM-300-30 a0.16710030039010073.8519.5
D-CFM-300-30 b0.16710030039010073.8519.5
S-CFS-400-25 a0.2224025023010073.8515.4
S-CFS-400-25 b0.2224025023010073.8513.9
S-CFS-400-25 c0.2224025023010073.8513
S-CFM-300-25 a0.1674025039010073.8512
S-CFM-300-25 b0.1674025039010073.8511.9
S-CFM-900-25 a0.54025039010073.8525.9
S-CFM-900-25 b0.54025039010073.8523.4
S-CFM-900-25 c0.54025039010073.8523.7
[56]C165-1001.25010016510029.718.25
C165-1301.25013016510029.724.5
C165-1501.25015016510029.728.44
C165-1751.25017516510029.732
C165-2001.25020016510029.734.22
C165-2501.25025016510029.733.14
C165-3001.25030016510029.734.24
CFRP-C2101.25015021010035.830.4
C210-1801.25018021010035.834
C210-1901.25019021010035.836
C210-2001.25020021010035.836.02
C210-2301.25023021010035.837.02
C210-2551.25025521010035.836.8
CFRP-C3001.25016030010029.738.02
C300-1801.25018030010029.741.15
C300-2001.25020030010029.746.35
C300-2501.25025030010029.745.5
C300-3001.25030030010029.745.95
[57]-1.41050152.2200305.15
-1.410100152.2200307.55
-1.410150152.2200307.7
-1.410200152.2200307.9
-1.410250152.2200306.25
-1.410300152.2200307.58
-1.41050152.2200405.1
-1.410100152.2200406.85
-1.410150152.2200406.35
-1.410200152.2200406.95
-1.410250152.2200406.8
-1.410300152.2200406.4
-1.41050152.2200504.55
-1.410100152.2200507.1
-1.410150152.2200507.78
-1.410200152.2200507.65
-1.410250152.2200506.8
-1.410300152.2200507.25
-1.43050152.2200309.3
-1.430100152.22003016.25
-1.430150152.22003016.2
-1.430200152.22003022.1
-1.430250152.22003015.6
-1.430300152.22003015.85
-1.43050152.2200409.15
-1.430100152.22004014.9
-1.430150152.22004016.05
-1.430200152.22004016.15
-1.430250152.22004016.11
-1.430300152.22004016.9
-1.430100152.22005017.8
-1.430150152.22005015.22
-1.430200152.22005018.5
-1.430250152.22005019
-1.430300152.22005017.71
-1.45050152.22003013.3
-1.450100152.22003026
-1.450150152.22003027.8
-1.450200152.22003027.2
-1.450250152.22003024.84
-1.450300152.22003023
-1.450100152.22004024.5
-1.450150152.22004027.75
-1.450200152.22004019.3
-1.450250152.22004021.9
-1.450300152.22004027.3
-1.450100152.22005016
-1.450150152.22005021.25
-1.450200152.22005025
-1.450250152.22005024.9
-1.450300152.22005034
[58]T1a0.3521006020914055.620
T1b0.3521006020914055.618.8
T2a0.3521008020914055.625.8
T2b0.3521008020914055.625.2
T3a0.35210010020914055.625.8
T3b0.35210010020914055.627.3
T4a0.35210014020914055.626.7
T4b0.35210014020914055.625.9
T5a0.35210018020914055.627.8
T5b0.35210018020914055.631.7
T6a0.35210022020914055.631.7
T6b0.35210022020914055.628.6
T7a0.35210010020914055.633
T7b0.35210010020914055.626.9
T8a0.35210010020914055.628.5
T8b0.35210010020914055.629.8
T9a1.05610010020914055.628.4
T9b1.05610010020914055.629.8
T10a1.05610014020914055.637.4
T10b1.05610014020914055.633.3
T11a1.05610018020914055.642.8
T11b1.05610018020914055.639
T12a0.3527010020914055.621.1
T12b0.3527010020914055.624.2
C150_10.1651001502301503518.97
C150_20.1651001502301503516.51
C150_30.1651001502301503514.26
C100_10.1651001002301503513.63
C100_20.1651001002301503513.36
C100a_10.33501502301503515.24
C100a_20.33501502301503518.19
C100a_30.33501502301503520.53
C100a_40.1651001502301503519.5
[59]C-60-11.3603001751601919.5
C-6021.3603001751601919.5
C-60-31.3603001751601919.5
C-100-11.61003001091601919.5
C-100-21.61003001091601919.5
C-100-31.61003001091601919.5
C-100-41.21003001661601919.5
[60,61]C-1.3 × 60-11.3603001751601933.18
C-1.3 × 60-21.3603001751601929.86
C-1.3 × 60-31.3603001751601931.88
C-1.6 × 100-11.61003001091601941.41
C-1.6 × 100-21.61003001091601939.87
C-1.6 × 100-31.61003001091601947.72
C-1.2 × 100-11.21003001661601949.85
C-1.2 × 100-21.21003001661601948.08
C-1.2 × 100-31.21003001661601952.6
C-1.25 × 100-11.251003001711601941.25
C-1.25 × 100-21.251003001711601938.14
C-1.25 × 100-31.251003001711601932.68
C-1.7 × 100-11.71003002211601954.79
C-1.7 × 100-21.71003002211601951.41
C-1.7 × 100-31.71003002211601954.57
5 (25)1.45025014015037.5539.78
11 (25)1.45025014015035.731
17 (25)1.45020014015032.7835.65
[62]-1.0225203108.38228.636.411.57
-1.25040016515052.623
-1.28040016515052.636.75
-1.25020016515052.619.8
-1.28020016515052.633
-1.280355195.715052.634.5
-1.280355195.715052.633.5
-1.280355197.6315052.637.6
-1.280355197.6315052.639.1
-1.280355195.4615052.641
-1.280355195.4615052.638
-0.1380355283.65315052.616.5
-0.1380355283.65315052.617.4
-0.1380355291.02415052.614.4
-0.1380355291.02415052.614.6
V12A1.2804001801502640
V9A1.2804001801502637
V13A1.2804001801502637.5
V16A0.1661004002411502625.1
V14A0.1661004002411502624.27
V17A0.1661004002411502625.19
V14B0.1661001002411502627
V16B0.1661001002411502621
V15B0.1661001002411502621.5
V11A1.2804001801502632.77
V7A1.2804001801502635.01
V8A1.2804001801502629.15
V24A0.1661004002411502625.39
V26A0.1661004002411502621.71
V25A0.1661004002411502629.09
V24B0.1661001002411502620.45
V25B0.1661001002411502621.22
V26B0.1661001002411502621.45
V21b0.1661004002411502620.82
V22b0.1661004002411502618.97
V23b0.1661004002411502620.14
V21a0.1661001002411502616.85
V23a0.1661001002411502619.4

References

  1. Hasan, K.; Salih, Y.; Binici, H.; Erhan, Y.; Nihat, C. May 1, 2003 Turkey-Bingöl earthquake: Damage in reinforced concrete structures. Eng. Fail. Anal. 2004, 11, 279–291. [Google Scholar]
  2. Funari, M.F.; Verre, S. The Effectiveness of the DIC as a Measurement System in SRG Shear Strengthened Reinforced Concrete Beams. Crystals 2021, 11, 265. [Google Scholar] [CrossRef]
  3. Funari, M.F.; Spadea, S.; Fabbrocino, F.; Luciano, R. A moving interface finite element formulation to predict dynamic edge debonding in FRP-strengthened concrete beams in service conditions. Fibers 2020, 8, 42. [Google Scholar] [CrossRef]
  4. Aiello, M.A.; Leone, M. Interface analysis between FRP EBR system and concrete. Compos. Part B Eng. 2008, 39, 618–626. [Google Scholar] [CrossRef]
  5. Leone, M.; Sciolti, M.S.; Aiello, M.A. Analysis of the Interface Performance of Concrete Elements Reinforced with Synthetic, Natural and Steel FRP Materials. In Proceedings of the 4th International Symposium on Bond in Concrete 2012: Bond Anchorage, Detailing, Volume 2: Bond in Concrete 2012: Bond in New Materials and under Severe Conditions, Brescia, Italy, 17–20 June 2012; ISBN 978-88-907078-3-4. [Google Scholar]
  6. Teng, J.G.; Smith, S.T.; Yao, J.; Chen, J.F. Intermediate crack-induced debonding in RC beams and slabs. Constr. Build. Mater. 2003, 17, 447–462. [Google Scholar] [CrossRef]
  7. Savoia, M.; Ferracuti, B.; Mazzotti, C. Non-linear bond slip law for FRP-concrete interface. In Proceedings of the FRPRCS-6, Singapore, 8–10 July 2003. [Google Scholar]
  8. Ulaga, T.; Vogel, T. Bilinear stress-slip bond model: Theoretical background and significance. In Proceedings of the FRPRCS-6, Singapore, 8–10 July 2003. [Google Scholar]
  9. Dai, J.G.; Ueda, T. Local bond stress slip relations for FRP sheets-concrete interfaces. In Proceedings of the FRPRCS-6, Singapore, 8–10 July 2003. [Google Scholar]
  10. Chen, J.F.; Teng, J.G. Anchorage strength models for FRP and steel plates bonded to concrete. J. Struct. Eng. ASCE 2001, 127, 784–791. [Google Scholar] [CrossRef]
  11. Wu, Z.S.; Yuan, H.; Niu, H.D. Stress transfer and fracture propagation in different kinds of adhesive joints. J. Eng. Mech. ASCE 2002, 128, 562–573. [Google Scholar] [CrossRef]
  12. Yuan, H.; Teng, J.G.; Seracino, R.; Wu, Z.S.; Yao, J. Full-range behaviour of FRP-to-concrete bonded joints. Eng. Struct. 2004, 26, 553–565. [Google Scholar] [CrossRef]
  13. Yao, J.; Teng, J.G.; Chen, J.F. Experimental study on FRP-to-concrete bonded joints. Compos. Part B Eng. 2005, 36, 99–113. [Google Scholar] [CrossRef]
  14. Czaderski, C. Strengthening of reinforced concrete members by pre-stressed, externally bonded reinforcement with gradient anchorage. Ph.D. Thesis, ETH, Zurich, Switzerland, 2012. Available online: http://dx.doi.org/10.3929/ethz-a-007569614 (accessed on 5 June 2021).
  15. Ceroni, F.; Barros, J.; Pecce, M.; Ianniciello, M. Assessment of nonlinear laws for near-surface-mounted system in concrete elements. Compos. Part B Eng. 2013, 45, 666–681. [Google Scholar] [CrossRef] [Green Version]
  16. Lua, X.Z.; Ye, L.P.; Teng, J.G.; Jianga, J.J. Meso-scale finite element model for FRP sheets/plates bonded to concrete. Eng. Struct. 2005, 27, 564–575. [Google Scholar] [CrossRef]
  17. Lu, X.Z.; Jiang, J.J.; Teng, J.G.; Ye, L.P. Finite element simulation of debonding in FRP-to-concrete bonded joints. Constr. Build. Mater. 2006, 20, 412–424. [Google Scholar] [CrossRef]
  18. Sümer, Y.; Aktaş, M. Bond length effect of fiber reinforced polymers bonded reinforced concrete beams. Int. J. Phys. Sci. 2011, 6, 5795–5803. [Google Scholar]
  19. Atheer, F.; Al-Saoudi; Kalfat, R.; Al-Mahaidi, R. Finite Element Assessment on Bond Behavior of FRP-to-Concrete Joints under Cyclic Loading. Int. J. Civ. Environ. Struct. Constr. Archit. Eng. 2015; 9, 1610–1615. [Google Scholar]
  20. Smith, S.T.; Teng, J.G.; Lu, M. Neural Network prediction of plate end debonding in FRP-plated RC beams. In Proceedings of the FRPRCS-6, Singapore, 8–10 July 2003. [Google Scholar]
  21. Ghen, J.F.; Yang, Z.J.; Holt, G.D. FRP or steel plate-to-concrete bonded joints: Effect of test methods on experimental bond strength. Steel Compos. Struct. 2001, 1, 231–244. [Google Scholar]
  22. Van Gemert, D. Force transfer in epoxy bonded steel/concrete joints. Int. J. Adhes. Adhes. 1980, 1, 67–72. [Google Scholar] [CrossRef]
  23. Holzenkämpfer, P. Ingenieur Modelle des Verbundes Geklebter Bewehrung für Betonbauteile. Ph.D. Thesis, TU Braunschweig, Brunswick, Germany, 1994. (In German). [Google Scholar]
  24. Tanaka, T. Shear Resisting Mechanism of Reinforced Concrete Beams with CFS as Shear Reinforcement. Master’s Thesis, Hokkaido University, Hokkaido, Japan, 1996. [Google Scholar]
  25. Hiroyuki, Y.; Wu, Z.S. Analysis of debonding fracture properties of CFS strengthened member subject to tension. In Proceedings of the 3rd International Symposium on Non-Metallic (FRP) Reinforcement for Concrete Structures, Sapporo, Japan, 14–16 October 1997; Japan Concrete Institute: Tokyo, Japan, 1997; Volume 1, pp. 287–294. [Google Scholar]
  26. Maeda, T.; Asano, Y.; Sato, Y.; Ueda, T.; Kakuta, Y. A study on bond by mechanism of carbon fiber sheet. In Proceedings of the 3rd International Symposium on Non-metallic (FRP) Reinforcement for Concrete Structures, Sapporo, Japan, 14–16 October 1997; Japan Concrete Institute: Tokyo, Japan, 1997; Volume 1, pp. 279–286. [Google Scholar]
  27. Khalifa, A.; Gold, W.J.; Nanni, A.; Abdel Aziz, M. Contribution of externally bonded FRP to shear capacity of flexural members. J. Compos. Constr. 1998, 2, 195–203. [Google Scholar] [CrossRef] [Green Version]
  28. Niedermeier, R. Envelope line of tensile forces while using externally bonded reinforcement. Ph.D. Thesis, TU München, Munich, Germany, 2000. (In German). [Google Scholar]
  29. Singh, A.; del Rey Castillo, E.; Ingham, J. FRP-to-FRP bond characterization and force-based bond length model. Compos. Struct. 2019, 210, 724–734. [Google Scholar] [CrossRef]
  30. fib. Externally Bonded FRP Reinforcement for RC Structures. Design and Use of Externally Bonded Fiber Reinforced Polymer Reinforcement (FRP EBR) for Reinforced Concrete Structures; fib Bulletin 14. Task Group 9.3; FRP Reinforcement for Concrete Structures; fib: Lausanne, Switzerland, 2001. [Google Scholar]
  31. Yang, Y.X.; Yue, Q.R.; Hu, Y.C. Experimental study on bond performance between carbon fiber sheets and concrete. J. Build. Struct. 2001, 22, 36–42. [Google Scholar]
  32. Japan Concrete Institute (JCI). Technical report of technical committee on retrofit technology. In Proceedings of the International Symposium on Latest Achievement of Technology and Research on Retrofitting Concrete Structures, Kyoto, Japan, 14–15 July 2003; Japan Concrete Institute (JCI): Tokyo, Japan, 2003. [Google Scholar]
  33. SIA 166. Kelebebewehrungen (Externally Bonded Reinforcement); Schweizerichenr Ingegneur-und Architektenveirein SIA: Zurich, Switzerland, 2004. [Google Scholar]
  34. Dai, J.; Ueda, T.; Sato, Y. Development of the nonlinear bond stress–slip model of fiber reinforced plastics sheet–concrete interfaces with a simple method. J. Compos. Constr. 2005, 9, 52–62. [Google Scholar] [CrossRef] [Green Version]
  35. Lu, X.Z.; Teng, J.G.; Ye, L.P.; Jiang, J.J. Bond-slip models for FRP sheets/plates bonded to concrete. J. Eng. Struct. 2005, 27, 920–937. [Google Scholar] [CrossRef]
  36. Wu, Z.S.; Islam, S.M.; Said, H. A three-parameter bond strength model for FRP–concrete interface. J. Reinf. Plast. Compos. 2009, 28, 2309–2323. [Google Scholar] [CrossRef]
  37. Wu, Y.; Zhou, Z.; Yang, Q.; Chen, W. On shear bond strength of FRP-concrete structures. J. Eng. Struct. 2010, 32, 897–905. [Google Scholar] [CrossRef]
  38. TR 55 Design Guidance for Strengthening Concrete Structures Using Fibre Composite Materials, 3rd ed.; Concrete Society: Camberley, UK, 2012.
  39. CNR-DT 200 R1/2013. Istruzioni per la Progettazione, l’Esecuzione ed il Controllo di Interventi di Consolidamento Statico mediante l’utilizzo di Compositi Fibrorinforzati; Concilio Nazionale delle Ricerche: Roma, Italy, 2013. (In Italian) [Google Scholar]
  40. Alqedra, M.A.; Ashour, A.F. Prediction of shear capacity of single anchors located near a concrete edge using neural networks. Comput. Struct. 2005, 83, 2495–2502. [Google Scholar] [CrossRef]
  41. Dahou, Z.; Sbartai, Z.M.; Caste, A.; Ghomari, F. Artificial neural network for steel-concrete bond prediction. Eng. Struct. 2009, 31, 1724–1733. [Google Scholar] [CrossRef]
  42. Tinoco, J.; Correia, A.G.; Cortez, P. Application of data mining techniques in the estimation of the uniaxial compressive strength of jet grouting columns over time. Constr. Build. Mater. 2011, 25, 1257–1262. [Google Scholar] [CrossRef] [Green Version]
  43. Amani, J.; Moeini, R. Prediction of shear strength of reinforced concrete beams using adaptive neuro-fuzzy inference system and artificial neural network. Sci. Iran. A 2012, 19, 242–248. [Google Scholar] [CrossRef] [Green Version]
  44. Yousif, S.T. New model of CRFP-confined circular concrete columns: ANN approach. Int. J. Civ. Eng. Technol. 2013, 4, 98–110. [Google Scholar]
  45. Cascardi, A.; Micelli, F.; Aiello, M.A. Analytical model based on artificial neural network for masonry shear walls strengthened with FRM systems. Compos. Part B Eng. 2016, 95, 252–263. [Google Scholar] [CrossRef]
  46. Cascardi, A.; Micelli, F.; Aiello, M.A. An Artificial Neural Networks model for the prediction of the compressive strength of FRP-confined concrete circular columns. Eng. Struct. 2017, 140, 199–208. [Google Scholar] [CrossRef]
  47. Chajes, M.J.; Finch, W.W.; Januszka, T.F.; Thonson, T.A. Bond and force transfer of composite material plates bonded to concrete. ACI Struct. J. 1996, 93, 209–217. [Google Scholar]
  48. Takeo, K.; Matstushiba, H.; Makizumi, T.; Nagashima, G. Bond characteristics of CFRP sheets in the CFRP bonding technique. Proc. Japan Concr. Inst. 1997, 19, 1599–1604. [Google Scholar]
  49. Yao, J. Debonding Failures in Reinforced Concrete Structures Strengthened with Externally Bonded FRP Sheets/Plates. Ph.D. Thesis, Hong Kong Polytechnic University, Hong Kong, 2004. [Google Scholar]
  50. Toutanji, H.; Saxena, P.; Zhao, L.Y.; Ooi, T. Prediction of interfacial bond failure of FRP-concrete surface. J. Compos. Constr. 2007, 11, 427–436. [Google Scholar] [CrossRef]
  51. Tan, Z. Experimental Research for RC Beam Strengthened with GFRP. Master’s Thesis, Tsinghua University, Beijing, China, 2002. [Google Scholar]
  52. Zhao, H.D.; Zhang, Y.; Zhao, M. Research on the bond performance between CFRP plate and concrete. In Proceedings of the 1st Conference on FRP-Concrete Structures of China; 2000; pp. 247–253. [Google Scholar]
  53. Ren, H.T. Study on Basic Theories and Long-Time Behavior of Concrete Structures Strengthened by Fiber Reinforced Polymers. Master’s Thesis, Dalian University of Technology, Dalian, China, 2003. (In Chinese). [Google Scholar]
  54. Ueda, T.; Sato, Y.; Asano, Y. Experimental study on bond strength of continuous carbon fiber sheet. Spec. Publ. 1999, 188, 407–416. [Google Scholar]
  55. Wu, Z.S.; Yuan, H.; Hiroyuki, Y.; Toshiyuki, K. Experimental/analytical study on interfacial fracture energy and fracture propagation along FRP-concrete interface. Spec. Publ. 2001, 201, 133–152. [Google Scholar]
  56. Sharma, S.K.; Mohamed, M.S.; Goldar, D.; Sikdar, P.K. Plate–concrete interfacial bond strength of FRP and metallic plated concrete specimens. J. Compos. Part B Eng. 2006, 37, 54–63. [Google Scholar] [CrossRef]
  57. Woo, S.K.; Lee, Y. Experimental study on interfacial behavior of CFRP-bonded concrete. J. Civil. Eng. 2010, 14, 385–393. [Google Scholar] [CrossRef]
  58. Pham, H.B.; Al-Mahaidi, R. Modelling of CFRP-concrete shear-lap test. Constr. Build. Mater. 2005, 21, 727–735. [Google Scholar] [CrossRef]
  59. Ceroni, F.; Pecce, M. Bond performance in concrete elements strengthened with CFRP sheets. In Proceedings of the FRP RCS8, Patras, Greece, 16–18 July 2007. [Google Scholar]
  60. Mazzotti, C.; Ferracuti, B.; Bilotta, A.; Ceroni, F.; Nigro, E.; Pecce, M. Sensitivity of FRP-concrete bond behavior to modification of the experimental set-up. In Proceedings of the International Conference on FRP Composites in Civil Engineering-CICE 2012, Rome, Italy, 13–15 June 2012. [Google Scholar]
  61. Bilotta, A.; Ceroni, F.; Di Ludovico, M.; Nigro, E.; Pecce, M.; Manfredi, G. Bond efficiency of EBR and NSM FRP systems for strengthening of concrete members. J. Compos. Constr. 2011. [Google Scholar] [CrossRef]
  62. Faella, C.; Nigro, E.; Martinelli, E.; Sabatino, M.; Salerno, N.; Mantegazza, G. Aderenza tra calcestruzzo e Lamine di FRP utilizzate come placcaggio di elementi inflessi. Parte I: Risultati sperimentali. In Proceedings of the XIV Congresso, C.T.E., Mantova, Italy, 7–8 November 2002. (In Italian). [Google Scholar]
  63. Ferracuti, B. Strengthening of RC Structures by FRP: Experimental Analyses and Numerical Modelling. Ph.D. Thesis, University of Bologna, Bologna, Italy, 2006. [Google Scholar]
  64. Savoia, M.; Bilotta, A.; Ceroni, F.; Di Ludovico, M.; Fava, G.; Ferracuti, B. Experimental round robin test on FRP-concrete bonding. In Proceedings of the 9th International Symposium on Fiber Reinforced Polymer Reinforcement for Concrete Structures, Sydney, Australia, 13–15 July 2009. [Google Scholar]
  65. Czaderski, C.; Soudki, K.; Motavalli, M. Front and side view image correlation measurements on FRP to concrete pull-off bond tests. J. Compos. Constr. 2010, 14, 451–463. [Google Scholar] [CrossRef]
  66. Haddad, R.H.; Al-Rousan, R.; Almasry, A. Bond-slip behavior between carbon fiber reinforced polymer sheets and heat-damaged concrete. Compos. Part B Eng. 2013, 45, 1049–1060. [Google Scholar] [CrossRef]
  67. Zhu, H.; Wu, G.; Shi, J.; Liu, C.; He, X. Digital image correlation measurement of the bond–slip relationship between fiber-reinforced polymer sheets and concrete substrate. J. Reinf. Plast. Compos. 2014, 33, 1590–1603. [Google Scholar] [CrossRef]
  68. McSweeney, B.M.; Lopez, M.M. FRP-concrete bond behavior: A parametric study through pull-off testing. Spec. Publ. 2005, 230, 441–460. [Google Scholar]
  69. Joanes, D.N.; Gill, C.A. Comparing measures of sample skewness and kurtosis. J. R. Stat. Soc. (Ser. D) Stat. 1998, 47, 183–189. [Google Scholar] [CrossRef]
  70. Iorfida, A.; Verre, S.; Candamano, S.; Ombres, L. Tensile and direct shear responses of basalt-fibre reinforced mortar-based materials. Int. Conf. Strain Hardening Cem. Based Compos. 2018. [Google Scholar] [CrossRef]
  71. Ombres, L.; Mancuso, N.; Mazzuca, S.; Verre, S. Bond between carbon fabric-reinforced cementitious matrix and masonry substrate. J. Mater. Civ. Eng. 2019, 31. [Google Scholar] [CrossRef]
  72. Longo, F.; Cascardi, A.; Lassandro, P.; Aiello, M.A. A new Fabric Reinforced Geopolymer Mortar (FRGM) with mechanical and energy benefits. Fibers 2020, 8, 49. [Google Scholar] [CrossRef]
  73. Cascardi, A.; Longo, F.; Micelli, F.; Aiello, M.A. Compressive strength of confined column with Fiber Reinforced Mortar (FRM): New design-oriented-models. Constr. Build. Mater. 2017, 156, 387–401. [Google Scholar] [CrossRef]
  74. Cascardi, A.; Micelli, F.; Aiello, M.A. FRCM-confined masonry columns: Experimental investigation on the effect of the inorganic matrix properties. Constr. Build. Mater. 2018, 186, 811–825. [Google Scholar] [CrossRef]
Figure 1. Sketch of the pull-pull shear test setup.
Figure 1. Sketch of the pull-pull shear test setup.
Fibers 09 00046 g001
Figure 2. Artificial neural networks scheme example.
Figure 2. Artificial neural networks scheme example.
Fibers 09 00046 g002
Figure 3. Variability ranges of the input-parameters by means the box plot representation.
Figure 3. Variability ranges of the input-parameters by means the box plot representation.
Fibers 09 00046 g003
Figure 4. Distribution of data in terms of input parameters: (a) β, (b) γ and (c) δ.
Figure 4. Distribution of data in terms of input parameters: (a) β, (b) γ and (c) δ.
Fibers 09 00046 g004aFibers 09 00046 g004b
Figure 5. Distribution of the frequency of the experimental/predicted values of Pu.
Figure 5. Distribution of the frequency of the experimental/predicted values of Pu.
Fibers 09 00046 g005
Figure 6. Box-plot of the frequency of the experimental/predicted values of Pu.
Figure 6. Box-plot of the frequency of the experimental/predicted values of Pu.
Fibers 09 00046 g006
Figure 7. Experimental vs. theoretical correlation in the quartile–quartile range.
Figure 7. Experimental vs. theoretical correlation in the quartile–quartile range.
Fibers 09 00046 g007
Figure 8. Area graph of the actual/predicted Pu.
Figure 8. Area graph of the actual/predicted Pu.
Fibers 09 00046 g008
Figure 9. Influence of the Young’s modulus of the FRP and the active bond length on the debonding force.
Figure 9. Influence of the Young’s modulus of the FRP and the active bond length on the debonding force.
Fibers 09 00046 g009
Figure 10. Influence of the width and the compressive strength of the concrete on the debonding force.
Figure 10. Influence of the width and the compressive strength of the concrete on the debonding force.
Fibers 09 00046 g010
Figure 11. Influence of the concrete compressive (left) and tensile (right) strength on the debonding force.
Figure 11. Influence of the concrete compressive (left) and tensile (right) strength on the debonding force.
Fibers 09 00046 g011
Figure 12. Variable of importance: the %IncMSE.
Figure 12. Variable of importance: the %IncMSE.
Fibers 09 00046 g012
Figure 13. Variable of importance: the %IncMSE.
Figure 13. Variable of importance: the %IncMSE.
Fibers 09 00046 g013
Figure 14. Statistical coefficients: RRMSE (top), MAE (middle) and MAPE (bottom).
Figure 14. Statistical coefficients: RRMSE (top), MAE (middle) and MAPE (bottom).
Fibers 09 00046 g014
Figure 15. Comparison of the performance of the analytical models with respect the proposed one.
Figure 15. Comparison of the performance of the analytical models with respect the proposed one.
Fibers 09 00046 g015
Table 1. Analytical models for the prediction of the bond strength between FRP and concrete.
Table 1. Analytical models for the prediction of the bond strength between FRP and concrete.
ReferenceYearModelDescription
[22]1980 P u = 0.5 b f L f c t m Based on an assumed triangular bond-stress distribution.
[23]1994 P u = b f E f t f G f
where:
G f = c f f c t m with cf = 0.204 mm
Introduction of the fracture energy in a Ph.D thesis.
[24]1996 P u = τ a b f L
where:
τ a = 6.13 l n L
Analytical linear interpretation of the bond-stress based on experimental data.
[25]1997 P u = τ a b f L
where:
τ a = 5.88 L 0.669
Analysis of debonding in RC members strengthened with FRP.
[26]1997 P u = τ a b f L e
where:
L e = e [ 6.13 0.58 l n ( E f t f ) ]
τ a = 110.2 × 10 6 E f t f
First definition of the effective bond length calibrated with non-linear regression analysis based on experimental data. A linear bond-stress distribution is assumed.
[27]1998 P u = τ a b f L e
where:
L e = e [ 6.13 0.58 l n ( E f t f ) ]
τ a = 110.2 × 10 6 E f t f ( f c 42 ) 2 / 3
Effective bond length calibration with non-linear regression analysis based on experimental data. Non-linear bond-stress distribution is assumed
[28]2000 P u = { 0.78 b f E f t f G f                                   s e   L L e 0.78 b f E f t f G f   L L e ( 2 L L e )             s e   L < L e
where:
L e = E f t f 4 f c t m
G f = c f f c t m β w 2
β w = 1.125 ( 2 b f / b c 1 + b f / 400 )
Introduction of the geometrical factor related to the width of the bonded plate and the width of the concrete member.
[29]2001 P u = { 0.427 β w b f L e f c                                 s e   L L e 0.427 β w b f L e f c   sin ( π L 2 L e   ) s e   L < L e
where:
L e = E f t f f c
β w = 2 b f / b c 1 + b f / b c
A modified version of the model reported in [23], validated for both CFRP and steel plates. The shear-slip relationship is represented by a triangular shape.
[30]2001 P u = { 0.64 α β w b f k c E f t f f c t m                         s e   L L e 0.64 α β w b f k c E f t f f c t m   L L e ( 2 L L e )   s e   L < L e
where:
β w = 1.06 2 b f / b c 1 + b f / 400
L e = E f t f 2 f c t m
with α = 1 and kc = 1.
International code based on the proposals from [27,28].
[31]2001 P u = ( 0.5 + 0.08 E f t f 100 f c t m ) τ a b f L e
where:
τ a = 0.5 f c t m
Le = 100 mm
The effective bond length has been considered not affected by the compressive strength of the substrate and fixed to 100 mm based on authors experimentations. An empirical model has been calibrated.
[32]2003 P u = τ a b f L e
where:
L e = 0.125 ( E f t f ) 0.57
τ a = 0.93 f c 0.44
Simplified empirical model based on literature database. A non-linear bond-stress distribution, along the FRP-length, has been assumed.
[33]2004 P u = b f 2 E f t f G f = b f 2 f c t m 8 E f t f = 0.5 b f E f t f f c t m
where:
G f = f c t m 8
Further empirical model based on literature database.
[34]2005 P u = { b f 2 E f t f G f                           s e   b f < 100   mm ( b f + 2 Δ b f ) 2 E f t f G f           s e   b f 100   mm
where:
G f = 0.514 f c 0.236
Δ b f = 3.7   mm
Analytical model for defining the nonlinear bond stress–slip law by means of non-linear regression analysis (authors data consisting in 26 tests).
[35]2005 P u = β l b f 2 E f t f G f
where:
β l = { 1                               s e   L L e L L e ( 2 L L e )               s e   L < L e
L e = a + 1 2 λ 1 l n [ λ 1 + λ 2 t g ( λ 2 a ) λ 1 λ 2 t g ( λ 2 a ) ]
G f = 0.308 β w 2 f c t m
λ 1 = λ m a x s o E f t f
λ 2 = λ m a x ( s f s o ) E f t f
λ m a x = 1.5 β w f c t m
s o = 0.0195 β w f c t m
s f = 2 G f λ m a x
β w = 2.25 b f / b c 1.25 + b f / b c
A linear best-fit line between finite element predictions, data collected from the existing literature (253 tests) and theoretical outcomes has been proposed by regression analysis.
[36]2009 P u = { 0.585 b f β w f c 0.1 ( E f t f ) 0.54                   s e   L L e 0.585 b f β w f c 0.1 ( E f t f ) 0.54 ( L L e ) 1.2       s e   L < L e
where:
β w = 2.25 b f / b c 1.25 + b f / b c
L e = 0.395 ( E f t f ) 0.54 f c 0.09
A bond strength model has been calibrated in order to reach an empirical formulation from the analysis of about 311 experimental data.
[37]2010 P u = β w b f 2 ( 1 + λ Σ ) E f t f G c f
where:
β w = 2 b f / b c 1 + b f / b c
λ = t d t f with td = 3.5 mm
Σ = E f E c
Gcf = 0.17 N/mm
A finite element analysis has been performed to determine the fracture energy.
[38]2012 P u = 0.5 b f β w E f t f f c t m
where:
β w = 1.06 2 b f / b c 1 + b f / 400
Simplified model calibrated by existing literature. It indicates that limiting the longitudinal shear stress (at the ultimate limit state) to a value not greater than 0.8 MPa, premature peeling failure can be avoided. It is further recommended that a minimum anchorage length of 500 mm should be provided.
[39]2013 P u = { b f γ F d 2 E f t f K G β w f c f c t m                       s e   L L e b f γ F d 2 E f t f K G β w f c f c t m L L e ( 2 L L e )     s e   L < L e
where:
L e = m a x { 1 γ R d f b d π 2 E f t f K G β w f c f c t m 2   ;   200   mm }
β w = 2 b f / b c 1 + b f / b c . se bf/bc < 0.25
γRd = 1.25
f b d = 2 Γ F d s u with su = 0.25 mm
Γ F d = K G β w f c f c t m
with γFd = 1.25
Empirical model derived from available data and based on the evaluation of the specific fracture energy— Γ F d .
Table 2. Interquartile ranges of the input parameters.
Table 2. Interquartile ranges of the input parameters.
Parametertf (mm)bf (mm)Lf (mm)Ef (GPa)bc (mm)fc (MPa)
Interquartile range (IQR)0.610.550.210.230.120.34
Max1.4010070039050074
Min0.08310508310017
Table 3. Quartiles border values.
Table 3. Quartiles border values.
QuartileValue
Q00.15
Q10.79
Q31.20
Q42.53
Me1.01
Table 4. Comparison of the precision and the accuracy of the analyzed models.
Table 4. Comparison of the precision and the accuracy of the analyzed models.
ReferencesYearIQRKas1as2as3
[34]20050.232.880.000.00−0.11
[35]20050.233.750.000.000.25
[30]20010.243.280.000.000.09
[29]20010.254.490.501.500.50
[38]20120.273.240.501.500.08
[39]20130.303.090.000.000.34
[36]20090.352.45−0.50−1.50−0.25
[28]20000.383.170.501.500.11
Proposed Model [[–]-0.414.860.000.000.00
[32]20030.424.69−0.50−1.500.11
[33]20040.442.640.000.000.01
[37]20100.454.020.000.000.72
[31]20010.452.700.501.500.24
[23]19940.492.640.000.000.01
[22]19801.147.760.501.500.52
[24]19961.857.430.501.501.02
[25]19976.293.550.501.500.90
[26]199715.923.160.000.000.36
[27]199833.462.17−0.50−1.500.09
Max33.467.760.501.501.02
Min0.232.170.000.000.00
Table 5. Statistical coefficients determination for the considered models.
Table 5. Statistical coefficients determination for the considered models.
ReferencesRRMSE (%)MAE (kN)MAPE (%)R2
[34]2.00%3.3420.00%0.98
[35]0.00%0.460.60%0.99
[30]1.00%2.8717.00%0.97
[29]0.00%0.461.10%0.99
[38]0.00%0.610.40%0.98
[39]1.00%2.7115.00%0.96
[36]3.00%6.3537.00%0.90
[28]1.00%2.2615.00%0.98
Proposed Model [–]0.00%0.840.30%0.95
[32]1.00%1.091.80%0.95
[33]1.00%1.6710.00%0.97
[37]0.00%0.951.10%0.94
[31]1.00%0.964.90%0.95
[23]1.00%2.2914.00%0.97
[22]1.00%2.2712.00%0.86
[24]2.00%4.0524.70%0.80
[25]3.00%7.6944.70%0.93
[26]4.00%8.4349.10%0.98
[27]4.00%7.5648.90%0.90
Max4.00%8.4349.100.99
Min0.000.460.30%0.80
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Cascardi, A.; Micelli, F. ANN-Based Model for the Prediction of the Bond Strength between FRP and Concrete. Fibers 2021, 9, 46. https://doi.org/10.3390/fib9070046

AMA Style

Cascardi A, Micelli F. ANN-Based Model for the Prediction of the Bond Strength between FRP and Concrete. Fibers. 2021; 9(7):46. https://doi.org/10.3390/fib9070046

Chicago/Turabian Style

Cascardi, Alessio, and Francesco Micelli. 2021. "ANN-Based Model for the Prediction of the Bond Strength between FRP and Concrete" Fibers 9, no. 7: 46. https://doi.org/10.3390/fib9070046

APA Style

Cascardi, A., & Micelli, F. (2021). ANN-Based Model for the Prediction of the Bond Strength between FRP and Concrete. Fibers, 9(7), 46. https://doi.org/10.3390/fib9070046

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop