Next Article in Journal
Design, Characterization, and Incorporation of the Alkaline Aluminosilicate Binder in Temperature-Insulating Composites
Next Article in Special Issue
Powder Bed Fusion 3D Printing in Precision Manufacturing for Biomedical Applications: A Comprehensive Review
Previous Article in Journal
Effects of Polybutylene Succinate Content on the Rheological Properties of Polylactic Acid/Polybutylene Succinate Blends and the Characteristics of Their Fibers
Previous Article in Special Issue
Microhardness and Microstructure Analysis of the LPBF Additively Manufactured 18Ni300
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Innovative Approaches to 3D Printing of PA12 Forearm Orthoses: A Comprehensive Analysis of Mechanical Properties and Production Efficiency

1
Department of Manufacturing Systems, Faculty of Mechanical Engineering and Robotics, AGH University of Science and Technology in Cracow, 30-059 Cracow, Poland
2
Mediprintic sp. z o.o., 39-300 Mielec, Poland
3
Department of Manufacturing Techniques and Automation, Faculty of Mechanical Engineering and Aeronautics, Rzeszow University of Technology, 35-959 Rzeszow, Poland
*
Author to whom correspondence should be addressed.
Materials 2024, 17(3), 663; https://doi.org/10.3390/ma17030663
Submission received: 15 December 2023 / Revised: 19 January 2024 / Accepted: 24 January 2024 / Published: 29 January 2024

Abstract

:
This research paper aims to explore the mechanical characteristics of polyamide PA12 (PA12) as a 3D material printed utilizing Selective Laser Sintering (SLS) and HP MultiJet Fusion (HP MJF) technologies in order to design and manufacture forearm orthoses. The study assessed the flowability of the materials used and compared the mechanical performance of PA12 with each other using tensile, flexure, and impact tests in five different fabrication orientations: X, Y, Z, tilted 45° XZ, and tilted 45° YZ. The results of the study provide, firstly—the data for testing the quality of the applied polyamide powder blend and, secondly—the data for the design of the orthosis geometry from the aspect of its strength parameters and the safety of construction. The mechanical parameters of SLS specimens had less variation than MJF specimens in a given orientation. The difference in tensile strength between the 3D printing technologies tested was 1.8%, and flexural strength was 4.7%. A process analysis of the forearm orthoses revealed that the HP MJF 5200 system had a higher weekly production capacity than the EOS P396 in a production variance based on obtaining maximum strength parameters and a variance based on maximizing economic efficiency. The results suggest that medical device manufacturers can use additive manufacturing technologies to produce prototypes and small-batch parts for medical applications. This paper pioneers using 3D printing technology with Powder Bed Fusion (PBF) methods in designing and manufacturing forearm orthoses as a low- to medium-volume product. The applied solution addresses the problem of medical device manufacturers with regard to the analysis of production costs and mechanical properties when using 3D printing for certified medical devices.

1. Introduction

Additive Manufacturing (AM) techniques are among the fastest-growing technologies to make even the most geometrically complex models [1,2]. Nowadays, many publications report concern models made by additive manufacturing techniques from polymeric materials used in medicine [3]. The most common applications of polymeric materials are the manufacture of surgical templates or instruments [4,5,6], implants [7,8], and scaffolds [9,10]. Concerning the fact that not only prototypes but often functional models are produced using additive manufacturing technologies, quality requirements are imposed on them related to the assessment of, among other things, mechanical properties [11,12,13], dimensional and geometry accuracy [14,15], and surface roughness [16,17,18]. These properties are closely related to the applied printing parameters, e.g., the applied print layer thickness, the model’s orientation in the 3D printer space, or the model fill density [11,12]. The parameters also affect the manufacturing costs of the model, which is also an important research topic [19,20].
As a result of continuous improvements in the mechanical and performance properties of polymeric materials, their use in the 3D printing process of orthoses, among others, is currently being expanded [21,22,23,24]. For orthoses, it is essential to use the correct type of material to stabilize the joint and maintain a constant temperature around it [24,25,26,27,28,29,30,31,32,33]. Additionally, it is crucial to ensure that the orthosis provides airflow and moisture wicking. For the additive manufacturing of orthoses, the most common materials used are Acrylonitrile Butadiene Styrene (ABS) [29], Polyethylene Terephthalate Glycol (PETG) [34], Polylactic Acid (PLA) [35] or composites [30]. However, these materials are now replaced by polyamide PA12 [29,31]. This is due to this material’s high mechanical, thermal, and fatigue strength [27,30]. In addition, this material is resistant to less aggressive chemicals. This material is also highly hygroscopic, quickly absorbing water from the environment [33,36]. A significant feature of this material is its biocompatibility according to ISO 10993-1, and it is also approved for food contact according to EU Directive 2002/72/EC (excluding alcoholic products) [37,38]. An essential feature that orthosis should fulfill also concerns the aesthetics of its manufacture. The PA12 material offers many possibilities for finishing parts, such as polishing, dyeing, lacquering, powder coating, or gluing the products.
Most commonly, models made from PA12 material are produced using Multi Jet Fusion (MJF) [39,40] and Selective Laser Sintering (SLS) [41,42,43,44,45] technologies. A vital aspect of the mechanical properties obtained may also relate to how successive print layers are fused. In the case of the MJF method, the powder bed in the machine is heated uniformly using a thermal head. Then, the precision print head applies two types of agents to support the printing process. The first agent is dispensed in the model areas, and its properties multiply the absorption of thermal radiation. The second is applied at the outer contours of the parts to facilitate the separation of the unmelted powder [46]. In the case of SLS technology, a laser is used to scan and sinter each layer [39]. Due to the differences in bonding of the print layers, an important aspect is to carry out strength tests. The literature has mainly presented tensile tests on samples made of PA12 material [47,48,49,50] and only in specific orientations [51,52].
Taking into account the literature review concerning the production of forearm orthoses [53,54], research was mainly conducted on models made using the Material Extrusion (MEX) methods with the materials ABS [35,55], PLA [35], PA12 [35], high-impact polystyrene (HIPS) [35] and PLA-CaCO3 [30]. Some authors have also extended their research by analyzing the Finite Element Method (FEM) and designed models of orthoses [35,53]. Research is also being introduced into making personalized designs for forearm orthoses using SLS technology. They are designed according to the Design for Additive Manufacturing (DFAM) methodology, considering lattice structure and topology optimization solutions on desktop machines, such as Sinterit LISA 1.5 (Sinterit sp. z o.o., Cracow, Poland) and EOS P395 (EOS GmbH, Krailling, Germany) industrial systems [56,57]. However, there needs to be more research on the broader field of manufacturing forearm orthoses made of nylon by SLS and MJF. A separate issue concerns the evaluation of the manufacturability of the MJF and SLS methods in the context of producing models of forearm orthoses from PA12 material. To date, research on this aspect has not been addressed extensively. Particular attention needs to be paid to, among other things, the maximum number of components to be placed in the working chamber. In addition, as the process of layer-by-layer curing is different in MJF and SLS technology, it is necessary to assess fabrication and cooling times. It is also necessary to pay attention to the start-up time of the 3D printer and material acquisition costs.
Currently, in the healthcare market, some solutions are using 3D printing using Powder Bed Fusion (PBF) methods for the production of orthopedic products, including ankle foot orthoses [58], prosthetic sockets [59], and foot orthotics [60]. On the other hand, for this moment, clinical research is being conducted into personalized orthoses made by 3D printing technologies like the Fused Filament Fabrication (FFF) method with ABS and polypropylene (PP) material and the SLS method with PA2200 material. The presented research is based on a solution according to a concept consisting of four stages: firstly, make a 3D scan of the forearm; secondly, generate a 3D orthosis model; thirdly, order and manufacture the designed 3D printed orthosis; finally, wear the ordered orthosis [61,62,63]. As a result, each is designed and manufactured to meet individual needs. Concern for the possibilities of 3D printing at low- to medium-volume production is necessary.
Thanks to the research presented in this paper, it is possible to expand the information on the mechanical properties of the PA12 material to manufacture forearm orthoses using SLS and MJF technology. Samples fabricated from PA12 material using SLS and HP MJF underwent comprehensive tensile, flexural, and impact strength assessments. Strength tests considered printing the samples in five different orientations. Thanks to the knowledge of the material’s strength and deformation capacity, it is possible to design a lightweight, openwork structure for the orthosis, which reduces its weight and production and operating costs. In addition, impact testing is essential in safety assessment, as it allows us to determine how the material behaves in impact situations, which is essential when a patient falls with an orthosis on the forearm. Before printing, the PA12 material was tested using the volumetric melt flow (MVR) method for both SLS and MJF methodologies to test the feedstock’s quality before starting the 3D printing process.
In addition, SLS and MJF technologies were reviewed for producing forearm orthoses, investigating the impact of mechanical properties on production time and cost. Furthermore, the potential of PBF methods as a production tool for developing medium-sized orthopedic supplies as an alternative to plaster casts in hospital emergency departments by orthopaedists as a solution available on-site without waiting several days for a personalized product to be made was highlighted.

2. Materials and Methods

2.1. Methods of Making Test Samples

The selection of material and manufacturing technology is a crucial factor in the design of a new solution. The material choice affects wall thickness, strength, flexibility, minimum feature size, build quality, and ease of certification of the new product. Consequently, this impacts the final geometry of the orthosis, which is the subject of this study [64,65,66,67,68]. The material commonly used in PBF technology is PA12 polyamide, which is used in SLS and HP MJF technologies. In the present study, two types of polyamide 12 powder were used—PA2200 (EOS GmBH, Krailling, Germany; EOS trade name of white PA12) [69] for SLS and PA12 (HP Inc., Barcelona, Spain) [70] for HP MJF certified for biocompatibility by ISO 10993 [71]. PA2200 polyamide powder is white due to the titanium oxide additives in the polyamide 12 (PA12) material. Using titanium oxide additives in PA12 improves the mechanical properties of sintered parts, making them more suitable for a wide range of applications [69]. In SLS technology, fabrication parameters such as scan vector length, incident laser power, and energy density play a key role in the mechanical and morphological properties of the parts produced [72,73]. The color of the powder in HP MJF technology is usually grey. This is due to the use of a polymer powder, such as polyamide-12, which is heated and exposed to infrared lamps during the MJF process. The grey color of the powder is a result of the specific composition of the raw material and the manufacturing process, which distinguishes MJF from other PBF techniques, such as SLS. The use of fusing and detoxifying agents, together with a planar infrared (IR) source, contributes to the unique grey powder color used in HP MJF technology [74,75].
This study aims to characterize products manufactured by 3D printing for use in producing parts for the medtech sector. Therefore, the powder data sheet information was adopted for this purpose. In order to optimize the 3D printing process with SLS and HP MJF methods, different PA12 polyamide powders with different color shades were used due to the different sources of energy supplied (laser for SLS, heat lamp with agent factor for HP MJF). Therefore, for each PBF technology, a set of manufacturing process parameters was selected for the powder used. These data are presented in Table 1.
Samples of PA2200 powder were made in an EOS P396 machine (EOS GmBH, Krailling, Germany) [78], while PA12 powder was made in an HP MJF 5200 machine (HP Inc., Barcelona, Spain) [79]. After manufacturing, they were subjected to a finishing process of cleaning unmelted powder from them. In the case of SLS technology, the printed parts are contained in a container together with the unmelted polymer material. Unpacking them requires the container with the parts to cool down beforehand, which can take up to 12 h. Once unloaded at the unloading station, a cleaning process follows, usually carried out using compressed air or another cleaning agent. After this, the components are ready for use. In the case of HP MJF technology, the printed parts are contained in a container along with the unmelted polymer material in the build unit. The build unit is then transferred from the 3D printer to the processing station to cool down. At the processing station, a cleaning process occurs, usually carried out via compressed air or another cleaning agent analogous to the cleaning procedure in SLS technology. When the process is complete, the parts are ready for use. The parameters of the machines are shown in Table 2.

2.2. MVR Powder Test

To measure the thermoplastic’s melt volume flow rate (MVR), 100 g of each powder blend was prepared for testing. They were certified according to ISO 10993 [71] and were classified as intermediate products from which biocompatible components are made, as shown in Table 3.
The thermoplastics’ melt volume flow rate (MVR) was determined according to ISO 1133:2002 [80]. These parameters allow the assessment of the rheological properties of thermoplastics, which is crucial for designing and manufacturing products from these materials. MVR allows an understanding of how a material behaves during processing, including its flow ability, plasticity, and viscosity. These tests make it possible to compare different thermoplastics and select those that best meet the requirements of a given application. The MVR measurement was carried out on a capillary plastometer DYNISCO 4781 Kayeness Inc., Honey Brook, PA, USA (Figure 1), PA12 and PA2200 under the following conditions (before testing, the plastics were dried in a vacuum dryer for 4 h at 130 °C) shown in Table 4.
For this purpose, samples (mixtures of new and recycled powder for PA2200 and PA12) weighing approximately 5 g were introduced into the properly heated apparatus. A preload of 1.16 kg was applied using a balance for 30 s. After this time, the load was changed to the correct 5 kg, and measurements were taken when the length of the strand exceeded 2 cm to measure the volume after the extrusion of the polymer.
The results of MVR tests for PA2200 and PA12, produced using SLS and HP MJF technologies, can be interpreted as follows: MVR represents the volume of the molten material. A higher MVR value indicates a larger volume, while a lower MVR value indicates a smaller volume. MVR is determined by multiplying the MFR and the density of the molten sample. For PA 12, a higher MVR value indicates a greater volume of molten material, which can be important for various applications, such as injection molding or 3D printing [81,82,83,84].
The reason for conducting that test is to ensure the quality and properties of the produced plastic material and evaluate the powder’s flowability in the molten state. This is particularly important for applications in SLS and HP MJF technologies, which rely on the proper flow and adhesion of the material during the printing process [81,82,83,84].

2.3. Preparation and Manufacture of Specimens for Strength Tests

In order to obtain the characteristics of the PA12 polyamide material group, test samples oriented in 5 different directions were examined and compared: flat (X), edge (Y) and vertical (Z), tilted by 45° in the XZ axis, and tilted by 45° in the YZ axis in to assess the anisotropy of 3D printed materials:
  • Based on ISO 527 [85], tensile test specimens were designed on an Instron 5985 universal quasi-static testing machine (Instron Corp, Norwood, MA, USA) with a maximum load of 250 kN;
  • Based on ISO 178 [86], flexural test specimens were designed on an Instron 5985 universal quasi-static testing machine with a full load of 250 kN;
  • Based on ISO 179 [87], impact test specimens were made on an Instron CEAST 9050 machine (Instron Corp, Norwood, MA, USA) with a hammer energy range of 0.5–50 J.
Table 5 and Figure 2, Figure 3, Figure 4 and Figure 5 show the designed test samples.

2.4. ANOVA Analysis for Mechanical Tests

In the statistical analyses, the confidence interval for the mean was calculated for a confidence level of 95%. In the analyses of variance carried out, the level of significance was assumed to be ∝ = 0.01. This was due to the performance of multiple statistical tests, which increased the probability of a type I error. The post hoc tests conducted after the analysis of variance were Tukey–Kramer HSD tests. All statistical analyses were performed in JMP 12 (SAS Institute Inc.: Cary, NC, USA) software [88].

2.5. Preparation of the Analysis of the Manufacturing Process—Analysis in a CAM Environment—Case Study of Forearm Orthoses

In order to analyze the manufacturing process using PBF technology, components were selected for SLS and HP MJF technology. The forearm orthosis manufactured using 3D printing technology consists of 3 separate components—the upper component of the orthosis frame—designated number 001; the lower component of the orthosis frame—designated number 002; and the thumb grip—designated number 003. All the above 3 components make up an integrated forearm orthosis assembly. These are shown in Table 6 and Table 7. The forearm orthoses were designed in SolidWorks 2022 [89]. After designing them using the writing to STL function, the software prepared and read files to prepare the 3D printing process for PBF technology. To analyze the manufacturing process in a computer-aided manufacturing (CAM) environment in Materialise Magics 25 [90] and Autodesk Netfabb 2023 [91] software, performance analyses were carried out for medical devices from Mediprintic sp. z o.o (Mielec, Poland).
Because of the stacking of 3D models in the virtual chamber of the 3D printer, it uses the following methods [92]:
  • Manual component placement carried out by an experienced technologist.
  • 3D packing scanline—during the packing process, the parts rotate as necessary and according to user-defined settings to find the best orientation for denser packing. Once packing begins, the calculations continue until they are completed.
  • 3D packing Monte Carlo (the Monte Carlo method is a technique used for the mathematical modeling of processes that are too complex, such as the calculation of integrals or chains of statistical processes. It involves the use of random sampling of quantities that characterize a process according to a known distribution [93])—during the packing process, if the settings allow, the parts are rotated at the beginning but not afterward. The process is similar to random shuffling, where parts move into gaps as they find them. Monte Carlo method packing aims to move the parts as low as possible in the compilation space to minimize platform height.
  • 3D packing gravity—allows parts to self-settle in the production room under simulated gravity.
  • 3D packing size sorting—is a combination of Monte Carlo and Scanline, focusing on the requirement first to pack large parts and stack them towards the center of the platform. Then, in that order, medium and small parts fill gaps and achieve a high overall packing density in the process.
Using the available tools in the CAM environment, the authors arranged the maximum number of orthoses that could be accommodated in the working chambers of the EOS and HP machines. Parameters such as packing density and the total volume occupied by the components in the working chamber, which are key parameters affecting the manufacturing process, were measured using the analysis tools available in the software. Then, using the dedicated software, analyses were carried out on the duration of the manufacturing process.
An analysis of the production possibilities for the best alignment of the 3D models in a 45° tilt in terms of the mechanical properties obtained and for the highest packing in light of the density of the filling of the working chamber was presented to compare the production possibilities. The analysis was based on data on forearm injuries in the Hospital Emergency Department of the Independent Public Clinical Hospital No. 1 of the Pomeranian Medical University in Szczecin. There were 263 forearm injuries in July and 214 in December, indicating a demand for 477 forearm orthoses using 3D printing technology during these two months [94].
The authors conducted a study comparing the production performance of the EOS P396 and HP MJF 5200 machines. They considered the following parameters in the analysis:
  • Maximum number of parts to be stacked in the working chamber;
  • Density of the chamber;
  • Total volume of elements in the working chamber;
  • Manufacturing time, cooling time, process start-up time;
  • Price per material used.
However, there is a specific disclaimer: SLS and MJF systems have different performance levels in powder use. The HP MJF 3D printer requires parts to be widely spaced apart to reduce the potential for heat build-up. The recommended packing density is limited to around 8–10%, meaning that as much material goes into the printed parts, it will need to be discarded. This means that HP MJF systems produce a lot of non-recyclable powder, which increases ongoing printing costs. With SLS technology, the recommended packing density is limited to 15%. For both of these large systems, the energy required to run 3D prints means that starting with just a few small parts is inefficient, highlighting that only manufacturers with predictable, high-volume 3D printing needs [95].
It is worth noting that the components shown in the benchmark were designed per the Design for Additive Manufacturing methodology, which focuses on consolidating multiple components into a single functional object and using lattice structures [96].

3. Results and Discussion

3.1. MVR Results

During the measurement, the time taken for the appropriate section of plastic to flow out of the capillary was determined. Based on the results obtained, the MVR was calculated according to the following formula, and the results obtained are summarised in Table 8.
M V R T , m = A 600 l t
  • T—test temperature [°C]
  • m—load [kg]
  • A—arithmetic mean of the cross-sectional areas of the cylinder and piston head [cm2]
  • T—measurement time [s]
  • l—piston displacement distance [cm]
Table 8. Test results for the volumetric melt flow rate MVR [cm3/10 min].
Table 8. Test results for the volumetric melt flow rate MVR [cm3/10 min].
Material185 °C190 °C
PA12-7.521 ± 0.553
PA22003.543 ± 0.94611.385 ± 0.883
Based on the material data, MVR measurements were carried out in the upper melting temperature range of the plastics, i.e., 185 °C for PA2200 and 190 °C for PA12. However, in the case of PA2200, inhomogeneous plasticization of the plastic was observed, which resulted in a considerable variation in results. Therefore, for PA2200, MVR measurements were also carried out at 190 °C, resulting in better plastic flow and the possibility of accurately determining the tested parameter. The MVR values obtained in the MVR test presented in Table 8 are in accordance with the accepted values in ISO 1133-1:2011 and other tests in the range of 0–50 cm3/10 min [97,98]. Therefore, obtained values are measurable parameters to refer to as appropriate parameters for characterizing the polyamide powder blend for SLS and HP MJF technologies in forearm orthosis application.
It is essential to consider the specific requirements of the application and the desired material properties when interpreting the results of MVR tests for PA2200 and PA12 produced using SLS or HP MJF technologies. In conclusion, the MVR results indicate that powdered plastic blends according to the proportions for variants 1 and 2 can produce biocompatible components using 3D printing technology.

3.2. Tensile Test

The results of an ANOVA for repeated measures investigating the effect of the manufacturing method on the values of a given tensile test parameter are shown in Table 9. The same table also shows the results of analyses of variance investigating the effect of model orientation—carried out separately for SLS and MJF specimens—on the tensile parameters. Assuming a significance level of ∝ = 0.01, the ultimate tensile strength and tensile modulus of the SLS and MJF fabricated samples are statistically equal. However, the fabrication method has a statistically significant effect on the tensile elongation at break εt. This is mainly due to the significantly higher εt values of the SLS specimens in X and Y orientations.
The model’s orientation in printer space statistically affects all tested strength parameters—for both SLS and MJF samples. As for tensile strength, the Tukey test showed that the strength of SLS samples printed in XZ orientation is higher than in X, Y, and YZ. The difference in ultimate tensile strength between XZ (with the highest σt) and YZ samples (with the lowest value of σt) was 4.1 MPa. In the case of MJF samples, the statistically significant effect of orientation on ultimate tensile strength was due to the lower strength of samples printed in the Y direction relative to all other samples.
The results of the strength parameters of the specimens obtained from the tensile tests are shown in Table 10 and Figure 6 and Figure 7. The results shown in Figure 6 clarify that the ultimate tensile strength and tensile modulus values in the same orientation as the values obtained for the SLS and MJF specimens are not significantly different. The average σt value of all SLS specimens was 43.05 ± 0.71 MPa, and that of the MJF specimens was 42.31 ± 1.52 MPa. Therefore, the average values differ by about 1.8%. The smallest value of σt = 41.32 ± 0.34 of the SLS samples was recorded for the YZ orientation, and the MJF σt = 36.76 ± 3.52 at the Y orientation.
Similar tensile strength tests of SLS samples, but printed only in three orientations (X, Y, Z) on EOS devices, were carried out by the authors of publications [47,99,100,101], among others. The tensile strength values we obtained of 41–45 MPa are similar to those presented by [47,100,101]. Lammens [99] obtained slightly higher σt values (45.0–49.4 MPa), while Calignano [51] obtained significantly lower σt values (34.8–38.3 MPa). Analogous strength tests in three orientations for the MJF method are presented in the literature [47,100,102]. Tensile strength values of 36.5–44.5 MPa, similar to those obtained by us, were obtained by Mehdipour [47]. Calignano [51] received noticeably lower σt values (34–38 MPa), while in [101] and Morales [49] received the highest σt values above 47 MPa. Due to the layered structure of printed models, the topic of anisotropy is raised when analyzing tensile strength. In the case of tensile strength, it is expected that models for which the direction of force is consistent with the direction of model building are less intense [103]. However, the anisotropy of the properties depends mainly on the bonding energy. The bonds between successive layers are smaller at low bonding energy, and the model has more significant anisotropy. Increasing the bonding energy makes the model properties more isotropic [76]. In our study, as in the publications [47,100,103], the lowest strength was not associated with samples printed in Z orientation, i.e., in the direction of tensile force.
Depending on the orientation, the tensile modulus value Et of the SLS samples varied in the range of 1.54–1.67 GPa and that of the MJF samples in the range of 1.51–1.73 GPa. The smallest value of Et for SLS was recorded in the YZ orientation and for MJF samples in the Y orientation. Similar Et values of SLS and MJF samples were reported by the authors of [47,48], among others. The Et values reported by Calignano [51] are similar for SLS samples but slightly lower (1.2–1.4 MPa) for MJF samples.
The orientation of the model had the most significant effect on tensile elongation. The largest εt values were obtained for the X and Y orientations. SLS specimens exhibited more excellent elongation in these orientations in the order of 20%. The anisotropy of the strength properties of the models resulting from the layered structure is, therefore, mainly manifested in the tensile elongation. This is also confirmed by other test results [47,99,100,101,102].
Compared to the MJF specimens in a given orientation, the SLS specimens showed less variation in the parameters obtained from the tensile test. This indicates that the properties of the SLS samples are more repeatable (assuming 3D printing in the same orientation). The coefficients of variation of ultimate tensile strength and tensile elongation calculated for all samples in the case of SLS are also smaller. This means that the SLS samples had an overall greater homogeneity of the parameters, as mentioned earlier. The more significant coefficient of variation of the SLS specimens in the case of tensile elongation is due to the significantly higher elongation of the specimens 3D printed in X and Y orientation.

3.3. Flexural Test

The results of the strength parameters of the specimens obtained in the flexural tests are presented in Table 11 and Figure 8 and Figure 9. Table 12 shows the results of the ANOVA analysis of variance for repeated measures investigating the effect of the manufacturing method on the values of a given parameter from the bending test. The same table also shows the results of variance analyses investigating the effect of model orientation—carried out separately for SLS and MJF specimens—on the strength parameters. Assuming a significance level of ∝ = 0.01, the chosen manufacturing method had a statistically significant effect on flexural strength and flexural modulus.
For SLS specimens, model orientation had a statistically significant effect on flexural strength. The statistical significance is due to the differences between the values obtained for the YZ, XZ, and Z orientations. These differences are relatively small (approximately 3%), as seen in Figure 9. For MJF specimens, the model’s orientation had a statistically significant effect on flexural modulus.
The specimens made by the MJF method showed higher flexural strength by 4.7%. The average σf value of all SLS specimens was 61.25 ± 0.53 MPa, and that of MJF specimens was 65.73 ± 1.45 MPa. The smallest value of σy = 60.30 ± 2.01 of the SLS specimens was recorded for the Z orientation, and for the MJF specimens, σy = 62.77 ± 8.15 at the X orientation. The observed orientation effect on σy is consistent with the results presented in [101]. In [102], MJF Z specimens had the highest flexural strength. This was due to the lowest porosity of these samples. The values of σy reported in [101] are smaller than in this study and vary in the 46.3–57.7 MPa range. On the other hand, the values reported in [102] have more significant variation (50–70 MPa).
A higher flexural modulus also characterized the MJF specimens. Depending on the orientation, the tensile modulus value E f of the SLS specimens varied in the range of 1.43–1.54 GPa, and that of the MJF specimens in the range of 1.52–1.69 GPa. The smallest value of E f for SLS was recorded in the Z orientation and for MJF samples, in the X orientation. The mean values of flexural elongation depending on the orientation for the SLS samples varied in the range of 7.3–8.0%, and for the MJF samples in in the range of 7.0–8.0%. The observed values for the MJF samples are similar to those presented in the publication [102]. The authors of [101] reported lower Ef values in the range of 0.87–1.07 GPa.
Compared to the MJF specimens in a given orientation, the SLS specimens showed less variation in the parameters obtained from the flexural test. This shows that the properties of the SLS samples are more repeatable (assuming printing in the same orientation). The coefficients of variation calculated for all samples in the case of SLS are also smaller. This means the SLS samples had an overall greater homogeneity of the analyzed parameters related to the flexural test.

3.4. Impact Test

The impact test results are shown in Table 13 and Figure 10. The analysis of variance showed that the printing method has a statistically significant effect on impact strength (p-value = 0.003). The orientation of the print had a statistically significant effect on the Re value only for SLS samples. For SLS samples printed in the X and Y orientation, impact strengths of approximately 6 and 7 kJ/m2 were determined, respectively. These values are approximately 1.5–3 times higher than the others. As noted earlier, the SLS samples in the X and Y orientation also had significantly higher tensile elongation, which is related to the anisotropy of the SLS samples. The smallest value of Re = 2.21 ± 0.07 kJ/m2 of the SLS samples was recorded for the YZ orientation and for the MJF Re = 2.63 ± 0.65 kJ/m2 at the X orientation. A minor mean variation in impact strength (calculated as the average of the CVs from the different orientations) was observed for the SLS samples. This means that SLS samples exhibit more excellent uniformity in the Re parameter when printed in the same orientation. The higher coefficient of variation of all SLS samples is due to the significantly higher impact strength of samples printed in the X and Y orientations. Publication [104] also studies the impact strength of SLS and MJF samples from PA12 in X and Z orientation. Most samples had similar impact strengths of 2.1–2.7 kJ/m2. The exception was the X-oriented MJF sample, for which Re was about 5 kJ/m2.

3.5. Result of Capacity Analysis in 3D Printers—A Case Study of Forearm Orthoses

In order to optimize the positioning of parts in the working chambers of the EOS P396 and HP MJF 5200 machines, 3D packing size and manual sorting methods were used to position the medical components—forearm orthoses—best. The component stacking process was carried out in Autodesk Netfabb 2023 and Materialise Magics 25, which is integrated by default with the 3D printers offered by EOS and HP. When the Autodesk Netfabb 2023 and Materialise Magics 25 [95,105] software launches, a list of available 3D printers opens, with process parameters and configured build platforms. Accordingly, the user focuses on arranging the parts in the working chamber using packaging tools like 3D packing Monte Carlo.
Two cases were investigated in the analysis, the first for the best mechanical parameters obtained from the tensile test (XZ tilted 45 degrees)—optimized for mechanical properties; the second for the maximum filling of the working chamber with forearm orthoses—optimized for economic efficiency. The SLS technology on the EOS P396 machine produced 9 sets of M-size orthoses sets (three components) for the first option and 15 sets for the second option. In comparison, the HP MultiJet Fusion technology on the HP MJF 5200 produced 7 sets of S-size orthoses for the first option and 11 sets for the second option. The difference between the volumes of the models between sizes M and S was 7.9%. The results of the production capacity for each machine are shown in Table 14 and Figure 11 and Figure 12.
In the case of the HP MJF technology, the cooling down process is carried out in a separate machine, so the total time associated with the 3D printing process in the HP MJF 5200 is 12.35 h, and the remaining 11 h of the process associated with cooling down and unpacking the working chamber is 11 h. In the case of SLS technology, the entire process, from 3D printing to the cooling down process, takes place in one machine, which ultimately takes 34.88 h. Significantly, the production time depends on the height of the parts in the working chamber. For the EOS, the height of the arranged elements was 570 mm; for the HP, it was 380 mm, so the production times are the same for both variants (1 and 2).
Considering the weekly production capacity for SLS, it is possible to run three production processes, equivalent to producing 27/45 sets (variant 1/variant 2) of orthoses. At the same time, for HP MJF, it is possible to start five production processes, which make 35/55 (variant 1/variant 2) sets of orthoses. Operating assumptions have been made for single-shift operation and a working week of Monday to Friday (therefore, the JOB 3 chamber will be unpacked on Monday of the following week), as shown in Table 15 and Table 16.
A capacity analysis was carried out on the machine capacity side for variant (option) 1 and variant (option) 2 is shown in Table 17.
From the comparison of production capacities made, the following conclusions can be reached:
  • More parts can be made in one production cycle on the EOS P396 machine than on the HP MJF 5200;
  • Total production costs are lower for HP MJF technology than SLS;
  • The HP MJF 5200 system has a higher weekly production capacity than the EOS P396 by 30% for option 1 and 18.2% for option 2;
  • Manufacturing components with high mechanical properties is 13% more expensive for SLS and 4% more expensive for HP MJF than the variant associated with economic efficiency;
  • The filling density of the parts in the working chambers is lower than the recommended packing density of the parts, as it is below 10% of the parts will not warp due to their packing density in the working chamber;
  • From the side of the delivery time of the finished orthosis, the most efficient is the HP MJF 5200 system in the economical variant;
  • For the case study presented, total production costs are 32.6% lower for option 1 and 26.6% lower for option 2 between HP MJF and SLS;
  • From the point of view of the powder used and its cost, it is more cost-effective to produce on the HP MJF 5200 system.
Within the context of investigating the manufacturability of a 3D-printed forearm orthosis, similar studies have been conducted using FFF technology for ABS, PLA, HIPS, and nylon materials in which criteria related to manufacturing accuracy with regard to manufacturing time and cost were investigated. The results of the obtained studies indicated a significant influence of mechanical parameters on the geometry of the orthosis depending on the positioning of the 3D model in the working chamber of the 3D printer. However, it is essential to consider the high anisotropy of the mechanical properties of 3D printing with FFF technology [35,55,107].

3.6. Result of Defects Analysis in 3D Printing—Case Study of Forearm Orthoses

Based on the manufacturing processes performed with SLS and HP MJF technology, potential problems for the production of forearm orthoses were investigated, such as [108]:
  • Surface defects. Unfavorable surface properties of the printed parts can result from the sedimentation process of the material or imperfections in the 3D printing technology itself. This problem can be solved by optimizing the positioning of the workpiece in the 3D printer’s work chamber space. In order to obtain the best surface quality for SLS technology, the relevant surfaces of the orthosis should be inverted with the Z-axis manufacturing direction. As well as for HP MJF technology, the relevant surfaces of the orthosis should be oriented towards the Z-axis manufacturing direction.
  • Geometric distortion. Geometric distortion may occur as a result of internal stresses. In the present case, the filling density of the working chamber is below the critical values for optimal filling of the chamber, so there is no reason for this phenomenon to occur.
  • Cracks. These can occur as a result of material inhomogeneity, inadequate cooling, or excessive stress. For this purpose, it is essential to check the machine settings and its calibration—especially the laser source in the SLS and the heating lamps in the HP MJF—before starting the 3D printing process.
  • Material quality problems. Material defects, such as impurities or inhomogeneities, can lead to defects in the prints. To avoid this, quality control of the powder mixture should be carried out before production starts.
Furthermore, these defects can occur for various reasons, including printing parameters, material quality, equipment maintenance, or even the 3D model design. Therefore, the HP MJF 5200 (orthoses examples showed in Figure 13) and EOS P396 (orthoses examples showed in Figure 14) must take care of the equipment’s annual servicing and calibration and carry out quality control for the powder mixes. An essential factor is to control the quality of the STL file from which the actual product is created and to control the nesting density of the working chamber so that its maximum density does not exceed 10%. The element packing analysis performed indicates a direction in establishing a manufacturing criterion for forearm orthoses. In the case of an analysis based on maximizing the critical mechanical property parameters, a low packing density was obtained, similar to the case of maximizing the elements in the working chamber of the 3D printer. Therefore, in the case of the production variants presented in the form of option 1 and option 2 from the point of view of the appearance of potential production defects is not significant due to the low working chamber density in the range of 1.8% to 3.7%. Therefore, an essential factor affecting capacity is the delivery of a certain number of orthoses that satisfy the end customer’s demand.

4. Conclusions

The purpose of this research work was to investigate the mechanical properties of polyamide PA12 as a 3D printed material using Selective Laser Sintering (SLS) and HP MultiJet Fusion (HP MJF) technologies to design and manufacture forearm orthoses. The study evaluated the flowability of the materials used and compared the mechanical properties of PA12 with each other using tensile, flexural, and impact tests in five different manufacturing orientations. In addition, analyses were conducted on the manufacturing process—a case study of forearm orthoses.
The MVR analysis carried out allows the quality of the PA12 and PA2200 polyamide blend used to determine the properties of the HP MJF and SLS technologies. Moreover, the measurement results obtained from the MVR test can be used to assess the repeatability of production for an ordered batch of orthoses in order to determine the quality of the powder mixtures for each manufacturing process in the 3D printer. The results obtained from the ISO 527 tensile test could be used to compare the mechanical properties of the orthoses between different manufacturing processes on the same 3D printer. In practice, two ISO 527 tensile specimens, for example, can be added to each working chamber, and then a tensile test can be carried out to compare the mechanical properties with the results obtained in the tests to evaluate the mechanical performance of the manufactured forearm orthoses.
The ISO 527 tensile test, ISO 179 bending test, and ISO 178 impact test provided important information on the mechanical properties of the polyamide powder blends used for the selected technologies. The data collected are important from the perspective of the design of a 3D-printed forearm orthosis from the point of view of its strength properties and evaluation of the safety of the final product. From the point of view of the 3D-printed forearm orthosis user, what is important is orthosis stiffness, susceptibility to flexure, and resistance to collisions such as a fall or accidental impact by another person.
Regarding the tests carried out and the analysis of the results, the following conclusions are presented:
  • The PA2200 and PA12 powder blends used are suitable for producing biocompatible components, which is confirmed by certificates from the manufacturers EOS and HP MJF. The values obtained in the MVR test for PA12 and PA2200 powders were about 7.5 and 11.4 cm3/10 min, respectively.
  • SLS samples had an average 1.8% higher tensile strength than MJF samples. MJF samples, on the other hand, had a 4.7% higher flexural strength. Therefore, from the point of view of the forearm orthosis manufacturer, it is appropriate to analyze the production costs to the expected mechanical properties of the final product.
  • SLS specimens in a given orientation have less variability in mechanical properties than HP MJF specimens. Therefore, more repeatable mechanical parameters can be predicted by producing in the specified orientation components using SLS technology relative to HP MJF technology. On the other hand, MJF samples were more isotropic—their mechanical properties were less dependent on orientation.
  • For the presented case study, it is possible to select tensile samples from the Y orientation for each 3D printing technology in which the smallest mechanical values were obtained as a reference for assessing the reproducibility of orthoses made by several manufacturing processes.
  • This is important information from the point of view of selecting the wall thickness of the orthosis in relation to its strength, which ultimately translates into the weight of the plaster. In the case in question, the total weight of the orthosis is about 180 g for size M. At the same time, the classic white cast weighs about 1 kg, so we have a 5× reduction in weight while maintaining the rigidity that stabilizes the forearm in the correct position.
  • The orientation of the 3D model alignment in the working chamber of the 3D printer significantly affects strength parameters such as tensile strength, flexural strength, and impact strength. In order to verify the necessary mechanical parameters of the orthosis, strength analysis should be carried out based on the data obtained [109,110], e.g., in Ansys 2023 R2 software, in order to investigate the occurring stresses in relation to the biomechanics of the forearm. The best solution is to tilt the 3D models in the working chamber of the machine. The process’s economics should also be considered when analyzing the total cost of manufacturing forearm orthoses.
  • The results obtained from the capacity analysis indicate to the 3D-printed forearm orthosis manufacturer the direction in which it is important to focus on the development of the product from the point of view of its mechanical properties and production capabilities.
  • Total production costs for HP MJF technology are 11.5% lower than for SLS technology. Manufacturing components with high mechanical properties is 13% more expensive for SLS and 4% more expensive for HP MJF than the variant associated with economic efficiency. From the side of the delivery time of the finished orthosis, the most efficient is the HP MJF 5200 system in the economical variant.
  • The EOS P396 system allows more orthoses to be made simultaneously in a single process than the HP MJF 5200. However, during the course of one manufacturing cycle on the EOS machine, it is possible to perform two manufacturing cycles on the HP machine, resulting in a more significant number of forearm orthoses produced. To sum up, the HP MJF 5200 system has a higher weekly production capacity than the EOS P396 by 30% for the optimized mechanical properties variant as well as 18.2% for the optimized economical efficiency variant.
  • The application of 3D printing technology for small batch, prototyped production is applicable for medical devices as a solution for their immediate production. The proposed PBF technologies can replace conventional methods such as injection molding or milling and produce a series of up to several dozen sets in a weekly cycle.
  • Adopting a production-based solution using PBF technology reduces production start-up costs due to the lack of need to design and manufacture industrial molds needed for injection molding, among other things. Based on the presented case study, it is possible to schedule in advance the production of orthoses that will meet the volume requirements for a hospital placing an order for a medium-sized batch of forearm orthoses.
  • The choice of the manufacturing method for forearm orthoses focuses primarily on optimum mechanical properties, production capacity, and manufacturing costs, as the materials used, PA12 and PA2200, have similar mechanical properties.
  • It is possible to interchangeably use both the EOS P396 and the HP MJF 5200 in order to meet market needs and to be able to choose the shade of the orthosis in white or grey due to customer’s needs of ordered orthosis sets.
  • Potential additive manufacturing defects such as surface defects, geometric distortion, cracks, and material quality problems that a medical device manufacturer using 3D printing technology should pay attention to are diagnosed. One solution is to control the filling density of the working chamber to a maximum of 10%.
  • The results of the studies obtained allowed for the implementation of the presented SLS and HP MJF technologies as certified methods of production of forearm orthoses and for registration as a medical device at the Office for Registration of Medicinal Products, Medical Devices, and Biocidal Products and EUDAMED.
  • The applied materials, PA12 and PA2200, are used in producing forearm orthoses at Mediprintic sp. z o.o. due to their mechanical properties and production capability.
The research and development work was integrated into existing trends based on zero waste production and Industry 4.0 to achieve sustainable development goals. The strength test results were applied to the ORT Light forearm orthosis design manufactured by Mediprintic sp. z o.o.
The strength tests carried out for five different orientations can be used to develop a material model for static strength analyses [109,110]. Further development directions may be directed at studying the impact of the mechanical properties of 3D-printed forearm orthoses subjected to finishing treatments such as dyeing, mechanical polishing, and chemical smoothing. Similarly, research and development efforts are needed to optimize the design of forearm orthoses to correct production capacity and performance.

Author Contributions

Conceptualization, A.Z., P.T., A.B. and J.C.; Investigation, A.Z., A.B. and P.T.; Methodology, A.Z.; MVR test, A.Z., Mechanical tests A.B.; Production test, A.Z.; writing—original draft preparation, A.Z., P.T. and A.B.; writing—review and editing, J.C.; supervision, J.C. All authors have read and agreed to the published version of the manuscript.

Funding

The study was financially supported by European Regional Development Fund grant number POPW.01.01.02-18-0084/20 by The Polish Agency for Enterprise Development. The APC has no external funding.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are contained within the article.

Acknowledgments

We would like to thank Mediprintic sp. z o.o. for their support and the opportunity to present a case study on 3D-printed forearm orthoses.

Conflicts of Interest

Author Andrzej Zakręcki was employed by Mediprintic sp. z o.o. The remaining authors declare that the research was conducted without any commercial or financial relationships that could be construed as a potential conflict of interest. The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
SLSSelective Laser Sintering
HP MJFHP MultiJet Fusion
PBFPowder Bed Fusion
FFFFused Filament Fabrication
AMAdditive Manufacturing
DFAMDesign for Additive Manufacturing
MVRVolumetric Melt Flow
CAMComputer Aided Manufacturing
PA12, PA2200Polyamide 12
FEMFinite Element Method
StdStandard Deviation
CVCoefficient of Variation
σ t ultimate tensile strength
E t tensile modulus
ε t tensile elongation at break
σ f flexural strength (at maximum load)
E f flexural modulus
ε f flexural elongation (at maximum load)
R e impact strength

References

  1. Gardan, J. Additive manufacturing technologies. In Additive Manufacturing Handbook; CRC Press: Boca Raton, FL, USA, 2017; pp. 149–168. [Google Scholar] [CrossRef]
  2. Thompson, M.K.; Moroni, G.; Vaneker, T.; Fadel, G.; Campbell, R.I.; Gibson, I.; Bernard, A.; Schulz, J.; Graf, P.; Ahuja, B.; et al. Design for Additive Manufacturing: Trends, opportunities, considerations, and constraints. CIRP Ann. 2016, 65, 737–760. [Google Scholar] [CrossRef]
  3. Salmi, M. Additive Manufacturing Processes in Medical Applications. Materials 2021, 14, 191. [Google Scholar] [CrossRef] [PubMed]
  4. Tack, P.; Victor, J.; Gemmel, P.; Annemans, L. 3D-printing techniques in a medical setting: A systematic literature review. Biomed. Eng. Online 2016, 15, 115. [Google Scholar] [CrossRef] [PubMed]
  5. Dawood, A.; Marti, B.M.; Sauret-Jackson, V.; Darwood, A. 3D printing in dentistry. Br. Dent. J. 2015, 219, 521–529. [Google Scholar] [CrossRef] [PubMed]
  6. Turek, P.; Filip, D.; Przeszłowski, Ł.; Łazorko, A.; Budzik, G.; Snela, S.; Oleksy, M.; Jabłoński, J.; Sęp, J.; Bulanda, K.; et al. Manufacturing Polymer Model of Anatomical Structures with Increased Accuracy Using CAx and AM Systems for Planning Orthopedic Procedures. Polymers 2022, 14, 2236. [Google Scholar] [CrossRef] [PubMed]
  7. Mishra, S.; Chowdhary, R. PEEK materials as an alternative to titanium in dental implants: A systematic review. Clin. Implant. Dent. Relat. Res. 2019, 21, 208–222. [Google Scholar] [CrossRef]
  8. AlOtaibi, N.M.; Naudi, K.B.; Conway, D.I.; Ayoub, A.F. The current state of peek implant osseointergration and future perspectives: A systematic review. Eur. Cells Mater. 2020, 40, 1–20. [Google Scholar] [CrossRef]
  9. Chen, C.Y.; Ke, C.J.; Yen, K.C.; Hsieh, H.C.; Sun, J.S.; Lin, F.H. 3D Porous Calcium-Alginate Scaffolds Cell Culture System Improved Human Osteoblast Cell Clusters for Cell Therapy. Theranostics 2015, 5, 643–655. [Google Scholar] [CrossRef]
  10. Melchels, F.P.; Feijen, J.; Grijpma, D.W. A review on stereolithography and its applications in biomedical engineering. Biomaterials 2010, 31, 6121–6130. [Google Scholar] [CrossRef]
  11. Agarwal, K.; Kuchipudi, S.K.; Girard, B.; Houser, M. Mechanical properties of fiber reinforced polymer composites: A comparative study of conventional and additive manufacturing methods. J. Compos. Mater. 2018, 52, 3173–3181. [Google Scholar] [CrossRef]
  12. Dana, H.R.; Barbe, F.; Delbreilh, L.; Azzouna, M.B.; Guillet, A.; Breteau, T. Polymer additive manufacturing of ABS structure: Influence of printing direction on mechanical properties. J. Manuf. Process. 2019, 44, 288–298. [Google Scholar] [CrossRef]
  13. Goh, G.D.; Yap, Y.L.; Tan, H.K.J.; Sing, S.L.; Goh, G.L.; Yeong, W.Y. Process–structure–properties in polymer additive manufacturing via material extrusion: A review. Crit. Rev. Solid State Mater. Sci. 2020, 45, 113–133. [Google Scholar] [CrossRef]
  14. Budzik, G.; Turek, P.; Dziubek, T.; Gdula, M. Elaboration of the measuring procedure facilitating precision assessement of the geometry of mandible anatomical model manufactured using additive methods. Meas. Control 2020, 53, 181–191. [Google Scholar] [CrossRef]
  15. Bazan, A.; Turek, P.; Przeszłowski, Ł. Assessment of InfiniteFocus system measurement errors in testing the accuracy of crown and tooth body model. J. Mech. Sci. Technol. 2021, 35, 1167–1176. [Google Scholar] [CrossRef]
  16. Bazan, A.; Turek, P.; Przeszłowski, Ł. Comparison of the contact and focus variation measurement methods in the process of surface topography evaluation of additively manufactured models with different geometry complexity. Surf. Topogr. Metrol. Prop. 2022, 10, 035021. [Google Scholar] [CrossRef]
  17. Townsend, A.; Senin, N.; Blunt, L.; Leach, R.; Taylor, J. Surface texture metrology for metal additive manufacturing: A review. Precis. Eng. 2016, 46, 34–47. [Google Scholar] [CrossRef]
  18. Triantaphyllou, A.; Giusca, C.L.; Macaulay, G.D.; Roerig, F.; Hoebel, M.; Leach, R.K.; Tomita, B.; Milne, K.A. Surface texture measurement for additive manufacturing. Surf. Topogr. Metrol. Prop. 2015, 3, 024002. [Google Scholar] [CrossRef]
  19. DePalma, K.; Walluk, M.R.; Murtaugh, A.; Hilton, J.; McConky, S.; Hilton, B. Assessment of 3D printing using fused deposition modeling and selective laser sintering for a circular economy. J. Clean. Prod. 2020, 264, 121567. [Google Scholar] [CrossRef]
  20. Kumar, A.; Chhabra, D. Adopting additive manufacturing as a cleaner fabrication framework for topologically optimized orthotic devices: Implications over sustainable rehabilitation. Clean. Eng. Technol. 2022, 10, 100559. [Google Scholar] [CrossRef]
  21. Patel, P.; Gohil, P. Custom orthotics development process based on additive manufacturing. Mater. Today Proc. 2022, 59, A52–A63. [Google Scholar] [CrossRef]
  22. Górski, F.; Kuczko, W.; Weiss, W.; Wichniarek, R.; Zukowska, M. Prototyping of an Individualized Multi-Material Wrist Orthosis using Fused Deposition Modelling. Adv. Sci. Technol. Res. J. 2019, 13, 39–47. [Google Scholar] [CrossRef]
  23. Palousek, D.; Rosicky, J.; Koutny, D.; Stoklásek, P.; Navrat, T. Pilot study of the wrist orthosis design process. Rapid Prototyp. J. 2014, 20, 27–32. [Google Scholar] [CrossRef]
  24. Barrios-Muriel, J.; Romero-Sánchez, F.; Alonso-Sánchez, F.J.; Salgado, D.R. Advances in Orthotic and Prosthetic Manufacturing: A Technology Review. Materials 2020, 13, 295. [Google Scholar] [CrossRef] [PubMed]
  25. Raj, R.; Dixit, A.R.; Łukaszewski, K.; Wichniarek, R.; Rybarczyk, J.; Kuczko, W.; Górski, F. Numerical and Experimental Mechanical Analysis of Additively Manufactured Ankle–Foot Orthoses. Materials 2022, 15, 6130. [Google Scholar] [CrossRef] [PubMed]
  26. Totah, D.; Kovalenko, I.; Saez, M.; Barton, K. Manufacturing Choices for Ankle-Foot Orthoses: A Multi-objective Optimization. Procedia CIRP 2017, 65, 145–150. [Google Scholar] [CrossRef]
  27. Maso, A.D.; Cosmi, F. 3D-printed ankle-foot orthosis: A design method. Mater. Today Proc. 2019, 12, 252–261. [Google Scholar] [CrossRef]
  28. Shahar, F.S.; Sultan, M.T.H.; Lee, S.H.; Jawaid, M.; Shah, A.U.M.; Safri, S.N.A.; Sivasankaran, P.N. A review on the orthotics and prosthetics and the potential of kenaf composites as alternative materials for ankle-foot orthosis. J. Mech. Behav. Biomed. Mater. 2019, 99, 169–185. [Google Scholar] [CrossRef] [PubMed]
  29. Paterson, A.M.; Donnison, E.; Bibb, R.J.; Campbell, I. Computer-aided design to support fabrication of wrist splints using 3D printing: A feasibility study. Hand Ther. 2014, 19, 102–113. [Google Scholar] [CrossRef]
  30. Varga, P.; Lorinczy, D.; Toth, L.; Pentek, A.; Nyitrai, M.; Maroti, P. Novel PLA-CaCO3 composites in additive manufacturing of upper limb casts and orthotics—A feasibility study. Mater. Res. Express 2019, 6, 045317. [Google Scholar] [CrossRef]
  31. Shakiba, M.; Ghomi, E.R.; Khosravi, F.; Jouybar, S.; Bigham, A.; Zare, M.; Abdouss, M.; Moaref, R.; Ramakrishna, S. Nylon—A material introduction and overview for biomedical applications. Polym. Adv. Technol. 2021, 32, 3368–3383. [Google Scholar] [CrossRef]
  32. Jafferson, J.; Chatterjee, D. A review on polymeric materials in additive manufacturing. Mater. Today Proc. 2021, 46, 1349–1365. [Google Scholar] [CrossRef]
  33. Miguel, M.; Leite, M.; Ribeiro, A.; Deus, A.; Reis, L.; Vaz, M. Failure of polymer coated nylon parts produced by additive manufacturing. Eng. Fail. Anal. 2019, 101, 485–492. [Google Scholar] [CrossRef]
  34. Schmitz, C.; Mori, Y.T.; Gamba, H.R.; Nohama, P.; de Souza, M.A. Development and Evaluation of a Customized Wrist-Hand Orthosis Using 3D Technology for a Child with Cerebral Palsy—A Case Study. In Proceedings of the 2019 41st Annual International Conference of the IEEE Engineering in Medicine and Biology Society (EMBC), Berlin, Germany, 23–27 July 2019; pp. 1476–1479. [Google Scholar] [CrossRef]
  35. Górski, F.; Wichniarek, R.; Kuczko, W.; Żukowska, M.; Lulkiewicz, M.; Zawadzki, P. Experimental studies on 3D printing of automatically designed customized wrist-hand orthoses. Materials 2020, 13, 4091. [Google Scholar] [CrossRef] [PubMed]
  36. Dickson, A.N.; Ross, K.A.; Dowling, D.P. Additive manufacturing of woven carbon fibre polymer composites. Compos. Struct. 2018, 206, 637–643. [Google Scholar] [CrossRef]
  37. Campobasso, A.; Battista, G.; Colombo, S.; Paglia, M.; Gianolio, A.; Beretta, M. New 3D printed polymers in orthodontics: A scoping review. Eur. J. Paediatr. Dent. 2023, 24, 224–228. [Google Scholar] [CrossRef] [PubMed]
  38. Priyadarshini, B.M.; Kok, W.K.; Dikshit, V.; Feng, S.; Li, K.H.H.; Zhang, Y. 3D printing biocompatible materials with Multi Jet Fusion for bioreactor applications. Int. J. Bioprinting 2023, 9, 14–35. [Google Scholar] [CrossRef]
  39. Bazan, A.; Turek, P.; Sułkowicz, P.; Przeszłowski, Ł.; Zakręcki, A. Influence of the Size of Measurement Area Determined by Smooth-Rough Crossover Scale and Mean Profile Element Spacing on Topography Parameters of Samples Produced with Additive Methods. Machines 2023, 11, 615. [Google Scholar] [CrossRef]
  40. Wudy, K.; Sapishchuk, S.; Hofmann, J.; Schmidt, J.; Konwitschny, F.; Töpper, H.C.; Daub, R. Polymer-based separator for all-solid-state batteries produced by additive manufacturing. J. Appl. Polym. Sci. 2023, 140, e53690. [Google Scholar] [CrossRef]
  41. Obst, P.; Launhardt, M.; Drummer, D.; Osswald, P.V.; Osswald, T.A. Failure criterion for PA12 SLS additive manufactured parts. Addit. Manuf. 2018, 21, 619–627. [Google Scholar] [CrossRef]
  42. Razaviye, M.K.; Tafti, R.A.; Khajehmohammadi, M. An investigation on mechanical properties of PA12 parts produced by a SLS 3D printer: An experimental approach. CIRP J. Manuf. Sci. Technol. 2022, 38, 760–768. [Google Scholar] [CrossRef]
  43. Kudelski, R.; Cieślik, J.; Kulpa, M.; Dudek, P.; Zagórski, K.; Rumin, R. Comparison of cost, material and time usage in FDM and SLS 3D printing methods. In Proceedings of the 2017 XIIIth International Conference on Perspective Technologies and Methods in MEMS Design (MEMSTECH), Lviv, Ukraine, 20–23 April 2017. [Google Scholar] [CrossRef]
  44. Nieciąg, H.; Kudelski, R.; Dudek, P.; Cieślik, J. An Exploratory Study on the Accuracy of Parts Printed in FDM Processes from Novel Materials. Acta Mech. Autom. 2020, 14, 59–68. [Google Scholar] [CrossRef]
  45. Pawlik, J.; Dzindziora, A.; Cieślik, J. Design of a hand orthosis manufactured by 3D printing. In International Conference Cybernetic Modelling of Biological Systems MCSB 2021. Bio-Algorithms Med-Syst. 2021, 17, eA1–eA45. [Google Scholar] [CrossRef]
  46. Turek, P.; Bazan, A.; Zakrecki, A. Influence of post-processing treatment on the surface roughness of polyamide PA12 samples manufactured using additive methods in the context of the production of orthoses. Proc. Inst. Mech. Eng. B J. Eng. Manuf. 2023, 09544054231202423. [Google Scholar] [CrossRef]
  47. Mehdipour, F.; Gebhardt, U.; Kästner, M. Anisotropic and rate-dependent mechanical properties of 3D printed polyamide 12-A comparison between selective laser sintering and multi jet fusion. Results Mater. 2021, 11, 100213. [Google Scholar] [CrossRef]
  48. Rosso, S.; Meneghello, R.; Biasetto, L.; Grigolato, G.; Concheri, G.S. In-depth comparison of polyamide 12 parts manufactured by Multi Jet Fusion and Selective Laser Sintering. Addit. Manuf. 2020, 36, 101713. [Google Scholar] [CrossRef]
  49. Morales-Planas, S.; Minguella-Canela, J.; Lluma-Fuentes, J.; Travieso-Rodriguez, J.A.; García-Granada, A.A. Multi Jet Fusion PA12 manufacturing parameters for watertightness, strength and tolerances. Materials 2018, 11, 1472. [Google Scholar] [CrossRef] [PubMed]
  50. Puttonen, T.; Salmi, M.; Partanen, J. Mechanical properties and fracture characterization of additive manufacturing polyamide 12 after accelerated weathering. Polym. Test. 2021, 104, 107376. [Google Scholar] [CrossRef]
  51. Calignano, F.; Giuffrida, F.; Galati, M. Effect of the build orientation on the mechanical performance of polymeric parts produced by multi jet fusion and selective laser sintering. J. Manuf. Process. 2021, 65, 271–282. [Google Scholar] [CrossRef]
  52. Chen, K.; Koh, Z.H.; Le, K.Q.; Teo, H.W.B.; Zheng, H.; Zeng, J.; Du, H. Effects of build positions on the thermal history, crystallization, and mechanical properties of polyamide 12 parts printed by Multi Jet Fusion. Virtual Phys. Prototyp. 2022, 17, 631–648. [Google Scholar] [CrossRef]
  53. Buonamici, F.; Furferi, R.; Governi, L.; Lazzeri, S.; McGreevy, K.S.; Servi, M.; Volpe, Y. A CAD-based procedure for designing 3D printable arm-wrist-hand cast. Comput. Aided Des. Appl. 2019, 16, 25–34. [Google Scholar] [CrossRef]
  54. Blaya, F.; Pedro, P.S.; Silva, J.L.; D’Amato, R.; Heras, E.S.; Juanes, J.A. Design of an orthopedic product by using additive manufacturing technology: The arm splint. J. Med. Syst. 2018, 42, 54. [Google Scholar] [CrossRef] [PubMed]
  55. Sala, F.; Carminati, M.; D’Urso, G.; Giardini, C. A feasibility analysis of a 3D customized upper limb orthosis. Procedia CIRP 2022, 110, 207–212. [Google Scholar] [CrossRef]
  56. Raschke, R.; Vehse, M. Polyamide based wrist orthosis generated by selective laser sintering. Trans. Addit. Manuf. Meets Med. 2019, 1, S04T07. [Google Scholar] [CrossRef]
  57. Modi, Y.K.; Khare, N. Patient-specific polyamide wrist splint using reverse engineering and selective laser sintering. Adv. Perform. Mater. 2022, 37, 71–78. [Google Scholar] [CrossRef]
  58. Available online: https://www.eos.info/en/innovations/all-3d-printing-applications/medical/orthoses-prostheses (accessed on 12 December 2023).
  59. Available online: https://augosocket.com/ (accessed on 12 December 2023).
  60. Available online: https://www.iorthotics.com/products (accessed on 12 December 2023).
  61. Chen, Y.J.; Lin, H.; Zhang, X.; Huang, W.; Shi, L.; Wang, D. Application of 3D–printed and patientspecific cast for the treatment of distal radius fractures: Initial experience. 3D Print. Med. 2017, 3, 11. [Google Scholar] [CrossRef] [PubMed]
  62. Guida, P.; Casaburi, A.; Busiello, T.; Lamberti, D.; Sorrentino, A.; Iuppariello, L.; D’Albore, M.; Colella, F.; Clemente, F. An alternative to plaster cast treatment in a pediatric trauma center using the CAD/CAM technology to manufacture customized three-dimensional-printed orthoses in a totally hospital context: A feasibility study. J. Pediatr. Orthop. B 2019, 28, 248–255. [Google Scholar] [CrossRef]
  63. Tobler-Ammann, B.; Schnuind, F.; Voillat, L.; Vogelin, E. Acceptability and Safety of 3D Printed Wrist-Based Splints Compared to Plaster Casts for the Treatment of Non-Surgical Distal Radius- and Scaphoid Fractures: Feasibility Study. Swibraces’s Cast Experience with Inselspital. Universitatsspital Bern Hopital Uviversitaire de Berne. Available online: https://swibrace.com/scientific-data-2/ (accessed on 15 January 2024).
  64. What Is MJF (HP’s Multi Jet Fusion) 3D Printing? Available online: https://www.hubs.com/knowledge-base/what-is-multi-jet-fusion/ (accessed on 15 January 2024).
  65. What Is SLS 3D Printing? Available online: https://www.hubs.com/knowledge-base/what-is-sls-3d-printing/ (accessed on 15 January 2024).
  66. What Is the Difference between Selective Laser Sintering (SLS) and Multi Jet Fusion (MJF) 3D Printing? Available online: https://www.hubs.com/knowledge-base/hp-mjf-vs-sls-3d-printing-technology-comparison/ (accessed on 15 January 2024).
  67. How Do You Design Parts for MJF (Multi Jet Fusion) 3D Printing? Available online: https://www.hubs.com/knowledge-base/how-to-design-parts-for-mjf/ (accessed on 15 January 2024).
  68. How to Design Parts for SLS 3D Printing. Available online: https://www.hubs.com/knowledge-base/how-design-parts-sls-3d-printing/ (accessed on 15 January 2024).
  69. EOS PA2200 Material Properties. Available online: https://drukarki3d.pl/oferta/eos-pa-12-poliamid-12/#PA2200 (accessed on 27 October 2023).
  70. HP MJF PA12 Material Properties. Available online: https://www.drukarki3dhp.pl/materialy/hp-3d-high-reusability-pa-12/ (accessed on 27 October 2023).
  71. ISO 10993; Biological Evaluation of Medical Devices—Part 1: Evaluation and Testing in the Risk Management Process. ISO: Geneva, Switzerland, 2018.
  72. Gadelmoula, A.M.; Aldahash, S. Effects of Fabrication Parameters on the Properties of Parts Manufactured with Selective Laser Sintering: Application on Cement-Filled PA12. Adv. Mater. Sci. Eng. 2019, 2019, 8404857. [Google Scholar] [CrossRef]
  73. Stoia, D.I.; Marsavina, L.; Linul, E. Correlations between Process Parameters and Outcome Properties of Laser-Sintered Pol-yamide. Polymers 2019, 11, 1850. [Google Scholar] [CrossRef]
  74. Lee, K.P.M.; Kajtaz, M. Experimental Characterisation and Finite Element Modelling of Polyamide-12 Fabricated via Multi Jet Fusion. Polymers 2022, 14, 5258. [Google Scholar] [CrossRef]
  75. Mele, M.; Campana, G.; Monti, G. A finned-riser design to avoid the capillarity effect in multi-jet fusion technology. Rapid Prototyp. J. 2021, 27, 1–12. [Google Scholar] [CrossRef]
  76. Hofland, E.C.; Baran, I.; Wismeijer, D.A. Correlation of Process Parameters with Mechanical Properties of Laser Sintered PA12 Parts. Adv. Mater. Sci. Eng. 2017, 2017, 4953173. [Google Scholar] [CrossRef]
  77. PA12 MJF Materials Properties. Available online: https://www.sicam.com/Materials/MJF-Materials (accessed on 7 November 2023).
  78. EOS P396 3D Printer. Available online: https://drukarki3d.pl/oferta/eos-p396/ (accessed on 27 October 2023).
  79. HP MJF 5200 3D Printer. Available online: https://www.drukarki3dhp.pl/modele/hp-jet-fusion-3d-5200/ (accessed on 27 October 2023).
  80. ISO 1133-1:2011; Plastics—Determination of Melt Mass Flow Rate (MFR) and Melt Volume Flow Rate (MVR) of Thermoplastics—Part 1: Standard Method. ISO: Geneva, Switzerland, 2011.
  81. Nowak, A.J.; Lis, A. Oznaczenia współczynnika szybkości płynięcia (MFI) Zawartość ołowiu w owocach. Lab. Apa-Ratura Badania 2020, 4, 26–29. [Google Scholar]
  82. Krzyżak, A.; Bondyra, R.; Dulebova, L.; Moravsky, V. Wskaźnik Szybkości Płynięcia kompozytów na osnowie polipropyle-nowej z dodatkiem ciętego włókna szklanego oraz talku. Postępy Nauk. Tech. 2012, 13, 78–85. [Google Scholar]
  83. Zimniak, P. Recyrkulacja tworzyw stosowanych w technice przyrostowej SLS. Inżynieria I Apar. Chem. 2010, 49, 148–149. [Google Scholar]
  84. Available online: https://tenslab.pl/szybkosc-plyniecia-mfr (accessed on 12 December 2023).
  85. ISO 527; Plastics—Determination of Mechanical Properties in Static Tension—Part 1: General Principles. ISO: Geneva, Switzerland, 2012.
  86. ISO 178:2019-06; Plastics—Determination of Bending Properties. ISO: Geneva, Switzerland, 2019.
  87. ISO 179-2:2020; Plastics—Determination of Charpy Impact Strength—Part 2: Instrumental Impact Testing. ISO: Geneva, Switzerland, 2020.
  88. Available online: https://www.jmp.com/en_us/software/data-analysis-software.html (accessed on 12 December 2023).
  89. Available online: https://www.solidworks.com/product/solidworks-3d-cad (accessed on 12 December 2023).
  90. Available online: https://www.materialise.com/en/industrial/software/magics-data-build-preparation (accessed on 12 December 2023).
  91. Available online: https://www.autodesk.com/products/netfabb/overview?us_oa=dotcom-us&us_si=6d4dbadb-6f7a-459e-9df4-bb145a0c88e3&us_st=Netfabb&us_pt=NETF&term=1-YEAR&tab=subscription&plc=F360NFP (accessed on 12 December 2023).
  92. About Packing. Available online: https://help.autodesk.com/view/NETF/2023/ENU/?guid=GUID-52326727-C6CE-44DA-ACC3-7BBBFF7694DC (accessed on 7 November 2023).
  93. Johansen, A.M. Monte Carlo Methods. In International Encyclopedia of Education, 3rd ed.; Elsevier: Amsterdam, The Netherlands, 2010; pp. 296–303. [Google Scholar] [CrossRef]
  94. Starczewska, M.E.; Kordalska, M.; Augustyniuk, K.; Stanisławska, M.; Rybicka, A. Analysis of injuries treated in the emergency department. Pielęgniarstwo Chir. Angiol. 2018, 4, 159–165. [Google Scholar]
  95. MJF vs. SLS: Plastic Powder Bed Fusion 3D Printers Comparison. Available online: https://formlabs.com/eu/blog/mjf-vs-sls-plastic-powder-bed-fusion-3d-printer-comparison/ (accessed on 7 November 2023).
  96. Egan, P.F. Design for Additive Manufacturing: Recent Innovations and Future Directions. Designs 2023, 7, 83. [Google Scholar] [CrossRef]
  97. Riedelbauch, J. Analysis of material aging and the influence on the mechanical properties of polyamide 12 in the Multi Jet Fusion process. Addit. Manuf. 2019, 27, 259–266. [Google Scholar] [CrossRef]
  98. Mielicki, C.; Wegner, A.; Gronhoff, B.; Wortberg, J.; Witt, G. Prediction of PA12 melt viscosity in Laser Sintering by a Time and Temperature dependent rheological model. RTejournal 2012, 32, 1–32. [Google Scholar]
  99. Lammens, N.; Kersemans, M.; De Baere, I.; Van Paepegem, W. On the visco-elasto-plastic response of additively manufactured polyamide-12 (PA-12) through selective laser sintering. Polym. Test. 2017, 57, 149–155. [Google Scholar] [CrossRef]
  100. Rodríguez, A.G.; Mora, E.E.; Velasco, M.A.; Tovar, C.A.N. Mechanical properties of polyamide 12 manufactured by means of SLS: Influence of wall thickness and build direction. Mater. Res. Express 2023, 10, 105304. [Google Scholar] [CrossRef]
  101. Cai, C.; Tey, W.S.; Chen, J.; Zhu, W.; Liu, X.; Liu, T.; Zhao, L.; Zhou, K. Comparative study on 3D printing of polyamide 12 by selective laser sintering and multi jet fusion. J. Mater. Process. Technol. 2021, 288, 116882. [Google Scholar] [CrossRef]
  102. O’Connor, H.J.; Dickson, A.N.; Dowling, D.P. Evaluation of the mechanical performance of polymer parts fabricated using a production scale multi jet fusion printing process. Addit. Manuf. 2018, 22, 381–387. [Google Scholar] [CrossRef]
  103. Ajoku, U.; Saleh, N.; Hopkinson, N.; Hague, R.; Erasenthiran, P. Investigating mechanical anisotropy and end-of-vector effect in laser-sintered nylon parts. Proc. Inst. Mech. Eng. B J. Eng. Manuf. 2006, 220, 1077–1086. [Google Scholar] [CrossRef]
  104. Sillani, F.; Kleijnen, R.G.; Vetterli, M.; Schmid, M.; Wegener, K. Selective laser sintering and multi jet fusion: Process-induced modification of the raw materials and analyses of parts performance. Addit. Manuf. 2019, 27, 32–41. [Google Scholar] [CrossRef]
  105. Available online: https://h20195.www2.hp.com/v2/GetDocument.aspx?docname=4AA7-4998ENA (accessed on 12 January 2024).
  106. Overview of Materials for Nylon 6, Nylon 12, MatWeb Material Property Data. Available online: http://www.matweb.com/search/DataSheet.aspx?MatGUID=0e37a459c4eb452faa9d92659f9a0ccc (accessed on 27 October 2023).
  107. Kim, H.; Jeong, S. Case study: Hybrid model for the customized wrist orthosis using 3D printing. J. Mech. Sci. Technol. 2015, 29, 5151–5156. [Google Scholar] [CrossRef]
  108. Sun, S.; Brandt, M.; Easton, M. Powder bed fusion processes: An overview. In Laser Additive Manufacturing; Woodhead Publishing Series in Electronic and Optical Materials; Woodhead Publishing: Sawston, UK, 2017; pp. 55–77. [Google Scholar] [CrossRef]
  109. Cazon, A.; Kelly, S.; Peterson, A.M.; Bibb, R.J.; Campbell, R.I. Analysis and comparison of wrist splint designs using the finite element method: Multi-material three-dimensional printing compared to typical existing practice with thermoplastics. Proc. Inst. Mech. Eng. H J. Eng. Med. 2017, 231, 881–897. [Google Scholar] [CrossRef] [PubMed]
  110. Tsiokou, V.; Papatheodorou, A.; Ntenekou, D.; Zouboulis, P.; Karatza, A. An Integrative Computational Design Workflow and Validation Methodology for 3D-Printed Personalized Orthopedic Devices: Case Study of a Wrist–Hand Orthosis (WHO). Processes 2023, 11, 2204. [Google Scholar] [CrossRef]
Figure 1. Capillary plastometer DYNISCO 4781 Kayeness.
Figure 1. Capillary plastometer DYNISCO 4781 Kayeness.
Materials 17 00663 g001
Figure 2. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 527 tensile specimens in the working chamber of the machine (a). Tensile test specimen dimensions in accordance with ISO 527 (b).
Figure 2. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 527 tensile specimens in the working chamber of the machine (a). Tensile test specimen dimensions in accordance with ISO 527 (b).
Materials 17 00663 g002
Figure 3. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 178 flexure specimens in the working chamber of the machine (a). Flexural test specimen dimensions in accordance with ISO 178 (b).
Figure 3. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 178 flexure specimens in the working chamber of the machine (a). Flexural test specimen dimensions in accordance with ISO 178 (b).
Materials 17 00663 g003
Figure 4. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 179 impact specimens in the working chamber of the machine (a). Impact test specimen dimensions in accordance with ISO 179 (b).
Figure 4. Preparation of specimens to be made from polyamide PA12 material on EOS P396 and HP MJF 5200 machines. Arrangement of ISO 179 impact specimens in the working chamber of the machine (a). Impact test specimen dimensions in accordance with ISO 179 (b).
Materials 17 00663 g004
Figure 5. ISO 527 tensile test specimens (a); ISO 178 flexural test specimens (b); ISO 179 impact test specimens (c); white color—SLS technology specimens; grey color—HP MJF technology specimens.
Figure 5. ISO 527 tensile test specimens (a); ISO 178 flexural test specimens (b); ISO 179 impact test specimens (c); white color—SLS technology specimens; grey color—HP MJF technology specimens.
Materials 17 00663 g005
Figure 6. Ultimate tensile strength σ t (a) and tensile modulus E t (b) depending on fabrication method and specimen orientation.
Figure 6. Ultimate tensile strength σ t (a) and tensile modulus E t (b) depending on fabrication method and specimen orientation.
Materials 17 00663 g006
Figure 7. Tensile elongation ε t depending on fabrication method and specimen orientation.
Figure 7. Tensile elongation ε t depending on fabrication method and specimen orientation.
Materials 17 00663 g007
Figure 8. Flexural strength σ f (a) and flexural modulus E f (b) depending on fabrication method and specimen orientation.
Figure 8. Flexural strength σ f (a) and flexural modulus E f (b) depending on fabrication method and specimen orientation.
Materials 17 00663 g008
Figure 9. Flexural elongation ε f depending on fabrication method and specimen orientation.
Figure 9. Flexural elongation ε f depending on fabrication method and specimen orientation.
Materials 17 00663 g009
Figure 10. Impact strength Re depending on fabrication method and specimen orientation.
Figure 10. Impact strength Re depending on fabrication method and specimen orientation.
Materials 17 00663 g010
Figure 11. Case study of component alignment based on the best strength properties in the working chamber of a 3D printer for forearm orthoses; medical component alignment in HP MJF 5200 (a); alignment in EOS P396 (b).
Figure 11. Case study of component alignment based on the best strength properties in the working chamber of a 3D printer for forearm orthoses; medical component alignment in HP MJF 5200 (a); alignment in EOS P396 (b).
Materials 17 00663 g011
Figure 12. Case study of component alignment based on the maximum elements in the working chamber of a 3D printer for forearm orthoses; medical component alignment in HP MJF 5200 (a); alignment in EOS P396 (b).
Figure 12. Case study of component alignment based on the maximum elements in the working chamber of a 3D printer for forearm orthoses; medical component alignment in HP MJF 5200 (a); alignment in EOS P396 (b).
Materials 17 00663 g012
Figure 13. Forearm orthoses production example made in HP MJF technology.
Figure 13. Forearm orthoses production example made in HP MJF technology.
Materials 17 00663 g013
Figure 14. Forearm orthoses production example made in SLS technology.
Figure 14. Forearm orthoses production example made in SLS technology.
Materials 17 00663 g014
Table 1. Parameters of the powders used to produce the samples [76,77].
Table 1. Parameters of the powders used to produce the samples [76,77].
Powder’s NamePA2200PA 12
Average grain-particle size56 µm60 µm
Bulk density0.45 g/cm30.425 g/cm3
Powder melting point176 °C187 °C
Density of parts0.93 g/cm31.01 g/cm3
Table 2. Parameters of the equipment on which the samples were made [78,79].
Table 2. Parameters of the equipment on which the samples were made [78,79].
Manufacturing MethodHP MultiJet FusionSelective Laser Sintering
3D PrinterHP MJF 5200EOS P396
Building volume380 mm × 284 mm × 380 mm340 mm × 340 mm × 600 mm
Building speedUp to 0.014 m/sUp to 6 m/s
Layer thickness0.08 mm0.12 mm
Sintering energy sourceheating lampslaser
Average power consumption12 kW2.4 kW
Power supply380–415 V, 50 A max400 V/32 A
Table 3. Powder mixture used as a mixture of new powder and recycled powder [73,74].
Table 3. Powder mixture used as a mixture of new powder and recycled powder [73,74].
MaterialPA12PA2200
Fresh powder20%50%
Recycled powder80%50%
Table 4. MVR measurement parameters.
Table 4. MVR measurement parameters.
ParameterPA12PA2200
Preload [kg]1.161.16
Basic load [kg]55
Plasticisation time [s]300300
Plasticisation temperature [°C]190185, 190
Table 5. Summary of completed strength test specimens: tensile test, flexural test, impact test.
Table 5. Summary of completed strength test specimens: tensile test, flexural test, impact test.
TechnologyMaterialType of Sample
and Their Orientation
Number of Samples
SLSPA2200tensile test, flexure test, impact test samples in X, Y, Z, tilted 45° XZ (XZ), tilted 45° YZ (YZ)6 samples in each orientation for ISO 527 tensile test, ISO 178 flexure test, ISO 179 impact test
HP MJFPA12tensile test, flexure test, impact test samples in X, Y, Z, tilted 45° XZ (XZ), tilted 45° YZ (YZ)6 samples in each orientation for ISO 527 tensile test, ISO 178 flexure test, ISO 179 impact test
Table 6. Part benchmark for SLS technology and PA2200 material.
Table 6. Part benchmark for SLS technology and PA2200 material.
Part NameM_RIGHT_001M_RIGHT_002M_RIGHT_003
Part pictureMaterials 17 00663 i001Materials 17 00663 i002Materials 17 00663 i003
Volume83.14 cm357.68 cm310.07 cm3
Weight~77.3 g~53.6 g~9.4 g
Table 7. Part benchmark for HP MJF technology and PA12 material.
Table 7. Part benchmark for HP MJF technology and PA12 material.
Part NameS_RIGHT_001S_RIGHT_002S_RIGHT_003
Part pictureMaterials 17 00663 i004Materials 17 00663 i005Materials 17 00663 i006
Volume76.60 cm349.17 cm38.04 cm3
Weight~77.4 g~46.7 g~8.1 g
Table 9. Results (p-value) of ANOVA for repeated measures investigating the effect of manufacturing method and model orientation on the parameter values obtained in the tensile test.
Table 9. Results (p-value) of ANOVA for repeated measures investigating the effect of manufacturing method and model orientation on the parameter values obtained in the tensile test.
Effect σ t E t ε t
Method0.2950.6060.009
Orientation—SLS<0.001<0.001<0.001
Orientation—MJF0.001<0.001<0.001
Table 10. Descriptive statistic of ultimate tensile strength σ t , tensile modulus E t , and tensile elongation ε t of SLS and MJF specimens.
Table 10. Descriptive statistic of ultimate tensile strength σ t , tensile modulus E t , and tensile elongation ε t of SLS and MJF specimens.
MethodOrientation σ t , MPa E t , GPa ε t , %
MeanStdCVMeanStdCVMeanStdCV
SLSX42.40.290.691.60.031.7620.491.276.21
Y42.082.175.151.550.16.6619.991.15.52
Z43.731.63.671.670.021.458.791.7519.87
XZ45.420.250.551.670.010.839.980.424.19
YZ41.320.280.671.540.021.5212.390.987.95
All43.051.864.331.610.074.4914.45.2436.43
MJFX42.810.872.041.590.031.9313.071.914.57
Y36.763.389.191.510.042.8717.233.4920.28
Z43.424.8811.241.730.042.48.84.6853.12
XZ44.391.954.391.60.074.3911.271.2210.82
YZ44.222.776.271.650.085.0411.961.129.41
All42.324.069.61.610.095.6912.463.8630.93
Table 11. Descriptive statistic of flexural strength σ f , flexural modulus E f , and flexural elongation ε f of SLS and MJF specimens.
Table 11. Descriptive statistic of flexural strength σ f , flexural modulus E f , and flexural elongation ε f of SLS and MJF specimens.
MethodOrientation σ f , MPa E f , GPa ε f , %
MeanStdCVMeanStdCVMeanStdCV
SLSX61.880.851.381.470.032.057.890.253.17
Y60.961.352.211.470.064.397.280.8712.01
Z60.31.923.181.540.085.527.920.425.35
XZ60.520.420.691.430.010.537.770.263.36
YZ62.630.570.911.460.021.48.030.324
All61.261.42.281.470.064.037.780.526.72
MJFX62.776.5610.461.650.127.267.120.9913.91
Y68.011.652.431.690.042.227.430.395.19
Z67.651.852.741.630.052.877.870.354.49
XZ65.312.363.621.620.042.57.040.7911.26
YZ64.173.014.681.520.053.337.990.33.81
All65.733.745.691.620.0857.480.699.2
Table 12. Results (p-value) of an ANOVA for repeated measures investigating the effect of manufacturing method and model orientation on the parameter values obtained in the flexural test.
Table 12. Results (p-value) of an ANOVA for repeated measures investigating the effect of manufacturing method and model orientation on the parameter values obtained in the flexural test.
Effect σ f E f ε f
Method<0.001<0.0010.058
Orientation—SLS0.0090.0150.103
Orientation—MJF0.0820.0040.062
Table 13. Descriptive statistic of impact strength R e of SLS and MJF specimens.
Table 13. Descriptive statistic of impact strength R e of SLS and MJF specimens.
MethodOrientation R e , kJ/m2
MeanStdCV
SLSX5.960.6210.33
Y6.961.3719.64
Z2.40.5824.36
XZ2.350.094.02
YZ2.210.073.04
All3.982.1955.15
MJFX2.630.6424.26
Y2.680.6223.15
Z3.440.349.79
XZ2.730.5620.46
YZ2.730.5620.46
All2.840.621.04
Table 14. Production capacity comparison of the EOS P396 with the HP MJF 5200 [106].
Table 14. Production capacity comparison of the EOS P396 with the HP MJF 5200 [106].
Optimized for Mechanical PropertiesOptimized for Economic Efficiency
ParameterEOS P396HP MJF 5200EOS P396HP MJF 5200
Powder cost63 €/kg35 €/kg63 €/kg35 €/kg
Number of parts in working chamber27214533
Number of orthosis sets971511
Nesting density1.96%1.82%3.7%3.37%
Refresh rate50%80%50%80%
Bulk density of powder0.45 g/cm30.425 g/cm30.45 g/cm30.425 g/cm3
Density of parts0.93 g/cm31.01 g/cm30.93 g/cm31.01 g/cm3
Total part volume1357.95 cm3745.7 cm32263.4 g/cm31471.9 g/cm3
Mass of powder used8790 g8046 g16,600 g14,898 g
Weight of sintered components1262.9 g753.1 g2104.9 g1486.6 g
Total powder costEUR 581.4EUR 349.5EUR 1098EUR 647.1
Total powder cost per jobEUR 1154.7EUR 1000.9EUR 1671.3EUR 1498.5
Preparation2 h0.75 h2 h0.75 h
Build time/job20.38 h11.6 h20.38 h11.6 h
Cool down time/job10 h10 h10 h10 h
Setup time and unpacking time2.5 h1 h2.5 h1 h
Total manufacturing time34.88 h23.35 h34.88 h23.35 h
Table 15. Production scenario for EOS P396.
Table 15. Production scenario for EOS P396.
Production Scenario for EOS P396 for 9/15 Orthosis Sets
Monday 9:00Tuesday 9:00Wednesday 9:00Thursday 9:00Friday 9:00 Saturday 9:00
JOB 1
JOB 2
JOB 3
Table 16. Production scenario for HP MJF 5200.
Table 16. Production scenario for HP MJF 5200.
Production Scenario for HP MJF 5200 for 7/11 Orthosis Sets
Monday 9:00Tuesday 9:00Wednesday 9:00Thursday 9:00Friday 9:00
JOB 1
JOB 2
JOB 3
JOB 4
JOB 5
Table 17. Production capacity comparison of the EOS P396 with the HP MJF 5200 based on hospital case study (263 forearm injuries in July; 214 injuries in December—summary 477 forearm injuries).
Table 17. Production capacity comparison of the EOS P396 with the HP MJF 5200 based on hospital case study (263 forearm injuries in July; 214 injuries in December—summary 477 forearm injuries).
Optimized for Mechanical PropertiesOptimized for Economic Efficiency
ParameterEOS P396HP MJF 5200EOS P396HP MJF 5200
Number of parts in working chamber27214533
Number of orthosis sets971511
Number of work chambers required to complete the need for orthosis in July30381824
Number of work chambers required to complete the need for orthosis in December24311520
Total number of possible technological operations to be performed during one week3535
Total number of weeks to complete the job for July and December1814119
Total cost per jobEUR 1154.7EUR 1000.9EUR 1671.3EUR 1498.5
Total production costEUR 20,784.8EUR 14,012.6EUR 18,384.3EUR 13,486.8
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Zakręcki, A.; Cieślik, J.; Bazan, A.; Turek, P. Innovative Approaches to 3D Printing of PA12 Forearm Orthoses: A Comprehensive Analysis of Mechanical Properties and Production Efficiency. Materials 2024, 17, 663. https://doi.org/10.3390/ma17030663

AMA Style

Zakręcki A, Cieślik J, Bazan A, Turek P. Innovative Approaches to 3D Printing of PA12 Forearm Orthoses: A Comprehensive Analysis of Mechanical Properties and Production Efficiency. Materials. 2024; 17(3):663. https://doi.org/10.3390/ma17030663

Chicago/Turabian Style

Zakręcki, Andrzej, Jacek Cieślik, Anna Bazan, and Paweł Turek. 2024. "Innovative Approaches to 3D Printing of PA12 Forearm Orthoses: A Comprehensive Analysis of Mechanical Properties and Production Efficiency" Materials 17, no. 3: 663. https://doi.org/10.3390/ma17030663

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop