Selective Corrosion of the α-Al Dendrite in a Hot-Dip Zn–14Al–0.5Mg Coating
Abstract
1. Introduction
2. Materials and Methods
3. Results
3.1. Surface Morphology of the Original Coated Steel
| Positions | Samples | Detected Composition (wt.%) | ||||
|---|---|---|---|---|---|---|
| O | Mg | Al | Fe | Zn | ||
| EDS A1 | Initial surface | 1.45 | 5.70 | 2.74 | 2.44 | 87.67 |
| EDS A2 | 0.85 | 0.79 | 18.63 | 2.41 | 77.32 | |
| EDS A3 | 1.70 | 0.24 | 1.25 | 2.41 | 94.41 | |
| EDS A4 | 11.18 | 0.80 | 24.94 | 2.28 | 60.80 | |
| EDS B1 | Coating surface, after 20 months of storage | 4.34 | 4.61 | 5.37 | 2.46 | 83.22 |
| EDS B2 | 1.48 | 0.26 | 20.85 | 2.92 | 74.50 | |
| EDS B3 | 3.19 | 0.20 | 1.96 | 2.30 | 92.35 | |
| EDS B4 | 30.73 | 0.29 | 38.41 | 1.46 | 29.11 | |
| EDS B5 | 1.76 | 0.77 | 0.67 | 3.02 | 93.77 | |
| EDS C6 | Cross-sectional area, after 20 months of storage | 1.13 | - | 18.58 | - | 80.29 |
| EDS C7 | 34.42 | - | 36.92 | - | 28.66 | |
| EDS C8 | 3.02 | - | 0.41 | - | 96.57 | |

3.2. Surface Morphology of the Coating After 20 Months of Storage in an Office Environment
3.3. Electrochemical Testing of the Coating After 20 Months of Storage in an Office Environment
3.4. Surface Morphology of the Coating After the Accelerated Corrosion Test
4. Discussion
4.1. The Reason for Selective Corrosion in the α-Al Dendrites
4.2. Corrosion Behavior of Selective Corroded α-Al Regions in the Zn–14Al–0.5Mg Coating During Salt Spraying
5. Conclusions
Author Contributions
Funding
Institutional Review Board Statement
Informed Consent Statement
Data Availability Statement
Conflicts of Interest
References
- Shibli, S.M.A.; Meena, B.N.; Remya, R. A review on recent approaches in the field of hot dip zinc galvanizing process. Surf. Coat. Technol. 2015, 262, 210–215. [Google Scholar] [CrossRef]
- Zhang, G.Q.; Song, R.B.; Liu, J.Y.; Zhao, S.; Cai, C.H. Effect of Mg content on structure and corrosion behavior of novel hot-dip Al-Zn-Si-Re-Mg coatings. Mater. Lett. 2022, 328, 133098. [Google Scholar] [CrossRef]
- Prosek, T.; Nazarov, A.; Goodwin, F.; Šerák, J.; Thierry, D. Improving corrosion stability of Zn–Al–Mg by alloying for protection of car bodies. Surf. Coat. Technol. 2016, 306, 439–447. [Google Scholar] [CrossRef]
- Xie, Y.X.; Jin, X.Y.; Wang, L. Development and application of hot-dip galvanized zinc-aluminum-magnesium coating. J. Iron Steel Res. 2017, 29, 167–174. [Google Scholar] [CrossRef]
- Yao, S.; Tian, G.; Ma, X.J.; Zhao, H.; Yan, L.; Zhao, A.M. Research status of hot-dip galvanized Zn–Al–Mg sheet. J. Iron Steel Res. 2023, 35, 1451–1462. [Google Scholar] [CrossRef]
- Truglas, T.; Duchoslav, J.; Riener, C.; Arndt, M.; Commenda, C.; Stifter, D.; Angeli, G.; Groiss, H. Correlative characterization of Zn–Al–Mg coatings by electron microscopy and FIB tomography. Mater. Charact. 2020, 166, 110407. [Google Scholar] [CrossRef]
- Cui, G.B.; Ju, X.H.; Yan, C.L.; Ma, Z.J. Microstructure characterization of hot-dip Zn–Al–Mg coating of low alloy high strength steel. Iron Steel 2023, 58, 153–160. [Google Scholar] [CrossRef]
- Salgueiro Azevedo, M.; Allély, C.; Ogle, K.; Volovitch, P. Corrosion mechanisms of Zn(Mg,Al) coated steel: 2. The effect of Mg and Al alloying on the formation and properties of corrosion products in different electrolytes. Corros. Sci. 2015, 90, 482–490. [Google Scholar] [CrossRef]
- Yao, C.Z.; Lv, H.B.; Zhu, T.P.; Zheng, W.G.; Yuan, X.D.; Gao, W. Effect of Mg content on microstructure and corrosion behavior of hot dipped Zn–Al–Mg coatings. J. Alloys Compd. 2016, 670, 239–248. [Google Scholar] [CrossRef]
- LeBozec, N.; Thierry, D.; Persson, D.; Riener, C.K.; Luckeneder, G. Influence of microstructure of zinc-aluminium-magnesium alloy coated steel on the corrosion behavior in outdoor marine atmosphere. Surf. Coat. Technol. 2019, 374, 897–909. [Google Scholar] [CrossRef]
- He, X.; Zhou, X.; Shang, T.; Liu, W.H.; Jiang, G.R.; Liu, C.; Chen, X.Q.; Zhang, X.; Li, X.G. Influence mechanism of different elements and alloy phases on the corrosion resistance of Zn–Al–Mg coated steel in the atmospheric environment: A review. Corros. Commun. 2024, 13, 49–59. [Google Scholar] [CrossRef]
- Zou, J.G.; Lu, L. Research progress on relationship between alloy phase and corrosion resistance in Zn–Al–Mg coating. Chin. J. Nonferr. Met. 2022, 32, 1934–1944. [Google Scholar] [CrossRef]
- Lee, S.-G.; Park, G.-D.; Kim, H.-J.; Kim, S.-J.; Lee, M.-H. Mechanisms of high corrosion resistance of Zn-12Al-5Mg alloy coatings prepared using Al/MgZn2 eutectic reaction. J. Alloys Compd. 2025, 1025, 180317. [Google Scholar] [CrossRef]
- Han, D.; Zheng, Z.Y.; Wang, J.L.; Du, A.; Ma, R.N.; Fan, Y.Z.; Zhao, X.; Cao, X.M. Study on the microstructure and corrosion resistance of Zn-3Al-xMg alloy. Surf. Coat. Technol. 2023, 473, 130011. [Google Scholar] [CrossRef]
- Schuerc, S.; Fleischanderl, M.; Luckeneder, G.H.; Preis, K.; Haunschmied, T.; Mori, G.; Kneissl, A.C. Corrosion behaviour of Zn–Al–Mg coated steel sheet in sodium chloride-containing environment. Corros. Sci. 2009, 51, 2355–2363. [Google Scholar] [CrossRef]
- Han, D.; Wu, H.Y.; Zheng, Z.Y.; Zhang, H.L.; Du, A.; Ma, R.N.; Fan, Y.Z.; Zhao, X.; Cao, X.M. Interfacial structure and corrosion resistance of Zn-3Al-3Mg coatings by hot-dip with a novel process. J. Alloys Compd. 2024, 1005, 176235. [Google Scholar] [CrossRef]
- Wang, S.X.; Zhou, W.L.; Chen, S.L.; Ma, R.N.; Du, A.; Zhao, X.; Fan, Y.Z.; Li, G.L. Study on corrosion behavior II of hot-dipped Zn-6Al-3Mg alloy coating: Surface oxide layer and ternary eutectic corrosion. J. Alloys Compd. 2024, 1008, 176534. [Google Scholar] [CrossRef]
- Wang, S.X.; Ma, X.H.; Bai, J.T.; Niu, J.; Ma, R.N.; Du, A.; Zhao, X.; Fan, Y.Z.; Li, G.L. Study on the structure and corrosion behavior of hot-dipped Zn-6Al-3Mg alloy coating in chlorine-containing environment. Corros. Sci. 2024, 231, 112001. [Google Scholar] [CrossRef]
- Du, X.; Zhang, M.C.; Duan, S.C.; Xu, R.X.; Zou, M.; Dong, S.W.; Guo, H.J.; Guo, J. Research status of high corrosion-resistant Zn–Al–Mg coating. Chin. J. Eng. 2019, 41, 847–856. [Google Scholar] [CrossRef]
- Chaouki, A.; Ben Ali, M.; El Maalam, K.; Aouadi, K.; Benabdallah, I.; El Fatimy, A.; Naamane, S. Optimizing corrosion protection: Performance comparison of Zn and Zn–Al–Mg alloys Hot-Dip galvanized coatings. J. Alloys Compd. 2024, 1007, 176371. [Google Scholar] [CrossRef]
- ISO 8353-2024; Steel Sheet, Zinc-Aluminium-Magnesium Alloy-Coated by the Continuous Hot-Dip Process, of Commercial, Drawing and Structural Qualities. The International Organization for Standardization: Geneva, Switzerland, 2024.
- ISO 9227-2022; Corrosion Tests in Artificial Atmospheres—Salt Spray Tests. The International Organization for Standardization: Geneva, Switzerland, 2022.
- Xu, M.; Han, D.; Zheng, Z.; Ma, R.; Du, A.; Fan, Y.; Zhao, X.; Cao, X. Effects of cooling rate on the microstructure and properties of hot-dipped Zn–Al–Mg coatings. Surf. Coat. Technol. 2022, 444, 128665. [Google Scholar] [CrossRef]
- Lee, J.-W.; Son, I.; Kim, S.J. Newly designed surface control using Si addition in trace quantity for Zn-2Al-3Mg alloy coated steel sheet with improved corrosion resistance. Appl. Surf. Sci. 2022, 598, 153868. [Google Scholar] [CrossRef]
- Chen, H.; Zhang, S.; Song, R.; Wang, X. Effect of bath temperature on the microstructure and electrochemical properties of (Si, Ti) micro-alloyed Zn-6Al-3Mg hot-dip coatings. Surf. Coat. Technol. 2025, 512, 132402. [Google Scholar] [CrossRef]
- Wang, S.X.; Ma, X.H.; Bai, J.T.; Du, T.T.; Ma, R.N.; Du, A.; Zhao, X.; Fan, Y.Z.; Li, G.L. Study of the corrosion behavior and mechanism of a hot-dipping Zn-6Al-3Mg alloy coating in 3.5 wt% neutral NaCl solution. Surf. Coat. Technol. 2023, 464, 129576. [Google Scholar] [CrossRef]
- Zhou, J.S.; Wang, Y.B.; Li, Y.K.; Xu, Z.B.; He, K.Z.; Wang, Z.D. Formation and Evolution of Corrosion Products on Eutectic Micro-structures: A Novel Study to Understand Corrosion Protection of Zn–Al–Mg Coatings. Mater. Corros. 2025, 76, 408–423. [Google Scholar] [CrossRef]
- Jorcin, J.-B.; Orazem, M.E.; Pébère, N.; Tribollet, B. CPE analysis by local electrochemical impedance spectroscopy. Electrochim. Acta. 2006, 51, 1473–1479. [Google Scholar] [CrossRef]
- Barranco, V.; Feliu, S., Jr.; Feliu, S. EIS study of the corrosion behaviour of zinc-based coatings on steel in quiescent 3% NaCl solution. Part 1: Directly exposed coatings. Corros. Sci. 2004, 46, 2203–2220. [Google Scholar] [CrossRef]
- Wang, S.; Guo, T.; Xu, G.; Ding, F. Corrosion behavior and mechanism of electric arc-sprayed Al-Mg coating and Zn–Al–Mg pseudo-alloy coatings. Surf. Coat. Technol. 2023, 475, 130126. [Google Scholar] [CrossRef]
- Singh, J.K.; Mandal, S.; Adnin, R.J.; Lee, H.-S.; Yang, H.-M. Role of coating processes on the corrosion kinetics and mechanism of zinc in artificial seawater. Materials 2021, 14, 7464. [Google Scholar] [CrossRef]
- Flitt, H.J.; Schweinsberg, D.P. Evaluation of corrosion rate from polarisation curves not exhibiting a Tafel region. Corros. Sci. 2005, 47, 3034–3052. [Google Scholar] [CrossRef]
- Honda, K.; Yamada, W.; Ushioda, K. Solidification structure of the coating layer on hot-dip Zn-11%Al-3%Mg-0.2%Si coated steel sheet. Mater. Trans. 2008, 49, 1395. [Google Scholar] [CrossRef]
- Mahdavi, M.; Bozorg, M. The impact of microstructural constituents on the corrosion performance of an Al-Zn-Mg-Cu aluminum alloy. J. Alloys Compd. 2025, 1042, 184019. [Google Scholar] [CrossRef]
- LeBozec, N.; Thierry, D.; Rohwerder, M.; Persson, D.; Luckeneder, G.; Luxem, L. Effect of carbon dioxide on the atmospheric corrosion of Zn-Mg-Al coated steel. Corros. Sci. 2013, 74, 379–386. [Google Scholar] [CrossRef]
- Katayama, H.; Kuroda, S. Long-term atmospheric corrosion properties of thermally sprayed Zn, Al and Zn-Al coatings exposed in a coastal area. Corros. Sci. 2013, 76, 35–41. [Google Scholar] [CrossRef]
- Laleh, M.; Jurak, T.; Gusieva, K.; Williams, J.; Renshaw, W.; Correnti, S.; Hodges, J.; Gazder, A.A. Corrosion morphology in Al-Zn-Mg-Si alloy coatings: Interdependence of microstructure heterogeneity and microstructure-induced local pH variations. Corros. Sci. 2026, 263, 113711. [Google Scholar] [CrossRef]
- Laleh, M.; Jurak, T.; Gusieva, K.; Williams, J.; Renshaw, W.; Correnti, S.; Hodges, J.; Gazder, A.A. New insights into corrosion initiation and propagation in a hot-dip Al-Zn-Mg-Si alloy coating via multiscale analytical microscopy. Corros. Sci. 2025, 245, 112695. [Google Scholar] [CrossRef]
- An, G.; Ma, Y.-Y.; Zhang, F.; Wen, C.; Zeng, R.-C. Intergranular corrosion of Zn–0.8 Mg alloy induced by anodic intermetallic compound Mg2Zn11 in 50-day immersion in Hanks’ solution with various glucose concentrations. Smart Mater. Manuf. 2026, 4, 100136. [Google Scholar] [CrossRef]
- Lamas, J.S.; Tacq, J.; Teerlinck, B. Assessing the potential of electrochemical techniques for monitoring pitting corrosion in carbon steel for offshore structures. Electrochim. Acta 2026, 563, 148721. [Google Scholar] [CrossRef]











| Elements | C | Si | Mn | P | S | Al | Fe |
|---|---|---|---|---|---|---|---|
| content | 0.04 | 0.021 | 0.23 | 0.010 | 0.008 | 0.022 | Bal. |
| Location | Rs (Ω·cm2) | CPE1 10−5 (Ω−1·cm−2·sn) | n1 | Rf (Ω·cm2) | CPE2 10−5 (Ω−1·cm−2·sn) | n2 | Rct (Ω·cm2) |
|---|---|---|---|---|---|---|---|
| Area 1 | 24.47 | 1.95 | 0.84 | 1117 | 213.4 | 0.61 | 2387 |
| Area 2 | 28.16 | 167.9 | 0.62 | 3075 | 2.25 | 0.82 | 1312 |
| Positions | Samples | Detected Composition (wt.%) | |||||
|---|---|---|---|---|---|---|---|
| O | Mg | Al | Cl | Fe | Zn | ||
| EDS D1 | Coating surface, after salt spray for 48 h | 28.68 | 0.24 | 1.86 | 9.67 | 2.46 | 57.09 |
| EDS D2 | 25.98 | 0.38 | 8.22 | 6.01 | 2.80 | 56.61 | |
| EDS D3 | 12.57 | 0.91 | 4.58 | 4.18 | 2.43 | 75.33 | |
| EDS D4 | 14.80 | 1.30 | 17.56 | 1.11 | 1.83 | 63.40 | |
| EDS D5 | 9.43 | 1.82 | 2.55 | 0.55 | 2.19 | 83.46 | |
| Positions | Samples | Detected Composition (wt.%) | |||||
|---|---|---|---|---|---|---|---|
| O | Mg | Al | Cl | Fe | Zn | ||
| EDS E1 | Coating surface, after salt spray for 130 h | 36.14 | 0.51 | 7.83 | 3.07 | 2.69 | 49.76 |
| EDS E2 | 25.52 | 0.40 | 6.81 | 2.90 | 3.51 | 60.86 | |
| EDS E3 | 28.77 | 0.96 | 6.49 | 2.35 | 1.96 | 59.47 | |
| EDS E4 | 22.38 | 0.47 | 4.86 | 1.36 | 2.25 | 68.69 | |
| Positions | Samples | Detected Composition (wt.%) | |||||
|---|---|---|---|---|---|---|---|
| O | Mg | Al | Cl | Fe | Zn | ||
| EDS F1 | cross-sectional, after salt spray | 16.15 | 0.56 | 27.50 | 0.77 | 1.57 | 53.45 |
| EDS F2 | 14.37 | 0.13 | 1.41 | 1.72 | 1.76 | 80.62 | |
| EDS F3 | 38.61 | 0.30 | 15.15 | 2.67 | 1.29 | 41.99 | |
| EDS F4 | 36.07 | 1.00 | 7.97 | 4.14 | 1.36 | 49.46 | |
| EDS F5 | 36.20 | 0.80 | 3.70 | 2.93 | 1.15 | 55.23 | |
| Positions | Samples | Detected Composition (wt.%) | |||||
|---|---|---|---|---|---|---|---|
| O | Mg | Al | Cl | Fe | Zn | ||
| EDS G1 | near surface | 22.62 | 0.61 | 7.18 | 0.18 | 2.99 | 66.43 |
| EDS G2 | half-thickness section | 25.24 | 0.51 | 14.98 | 4.34 | 3.11 | 51.82 |
| EDS G3 | near substrate | 43.55 | 0.51 | 36.55 | 1.43 | 1.95 | 16.01 |
| EDS G4 | near substrate | 29.61 | 0.54 | 15.52 | 3.44 | 4.12 | 46.77 |
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.
Share and Cite
Huang, Y.; Liu, Y.; Dong, B.; Zhu, X.; Wu, C. Selective Corrosion of the α-Al Dendrite in a Hot-Dip Zn–14Al–0.5Mg Coating. Coatings 2026, 16, 693. https://doi.org/10.3390/coatings16060693
Huang Y, Liu Y, Dong B, Zhu X, Wu C. Selective Corrosion of the α-Al Dendrite in a Hot-Dip Zn–14Al–0.5Mg Coating. Coatings. 2026; 16(6):693. https://doi.org/10.3390/coatings16060693
Chicago/Turabian StyleHuang, Yidong, Ya Liu, Bin Dong, Xiangying Zhu, and Changjun Wu. 2026. "Selective Corrosion of the α-Al Dendrite in a Hot-Dip Zn–14Al–0.5Mg Coating" Coatings 16, no. 6: 693. https://doi.org/10.3390/coatings16060693
APA StyleHuang, Y., Liu, Y., Dong, B., Zhu, X., & Wu, C. (2026). Selective Corrosion of the α-Al Dendrite in a Hot-Dip Zn–14Al–0.5Mg Coating. Coatings, 16(6), 693. https://doi.org/10.3390/coatings16060693