Study on Yttrium-Enhanced Anti-Oxidation and Adhesion Properties of Al2O3 Oxide Scale on AFA Alloy Under Low Oxygen Partial Pressure
Abstract
1. Introduction
2. Experiments
2.1. Sample Preparation and Oxidation
2.2. Micro-Scratch Test
2.3. Sample Characterization and Phase Diagram Calculation
3. Results
3.1. Microstructure of the Annealed Alloys
3.2. Microstructure of the Alloys After Two-Step Pre-Oxidation Under Low Oxygen Partial Pressure
3.3. Microstructure of Pre-Oxidized Alloys After Cyclic Oxidation in Air
3.4. Scratch Evaluation of Adhesion of the Pre-Oxidized Oxide Scales
4. Discussion
4.1. Thermodynamic Analysis of Y on the Oxide Formation Under a Low Oxygen Partial Pressure
4.2. Effect of Y on Oxidation Resistance and Adhesion
5. Conclusions
Author Contributions
Funding
Institutional Review Board Statement
Informed Consent Statement
Data Availability Statement
Conflicts of Interest
References
- Taneike, M.; Abe, F.; Sawada, K. Creep-strengthening of steel at high temperatures using nano-sized carbonitride dispersions. Nature 2003, 424, 294–296. [Google Scholar] [CrossRef]
- Young, D.J.; Pint, B.A. Chromium volatilization rates from Cr2O3 scales into flowing gases containing water vapor. Oxid. Met. 2006, 66, 137–153. [Google Scholar] [CrossRef]
- Liu, T.; Zhang, D.; Wang, Z.; Xiang, L.; Zhao, Y.; Hu, S.; Huang, B.; Xie, Z. Enhanced structural stability and oxidation resistance of NiCoCrAlY bonding layer via Al addition. Vacuum 2023, 207, 111543. [Google Scholar] [CrossRef]
- Asteman, H.; Hartnagel, W.; Jakobi, D. The influence of Al content on the high temperature oxidation properties of state-of-the-art cast Ni-base alloys. Oxid. Met. 2013, 80, 3–12. [Google Scholar] [CrossRef]
- Yamamoto, Y.; Ren, Q.-Q.; Brady, M.P. Role of Cr content in microstructure, creep, and oxidation resistance of alumina-forming austenitic alloys at 850–900 °C. Metals 2022, 12, 717. [Google Scholar] [CrossRef]
- Shi, J.; Meng, F.; Huang, G.; Liu, F.; Zhai, L.; Chen, Y.; Zhang, F.; Lin, J.; Wang, L. Improving the oxidation resistance by forming continuous Al2O3 protective layer in alumina-forming austenitic stainless steel. Surf. Coat. Technol. 2024, 493, 131279. [Google Scholar] [CrossRef]
- Masari, F.; Hernández, R.; Serrano, M.; Torralba, J.; Campos, M. Design and characterisation of new low-alloyed alumina forming ferritic/martensitic steels. Mater. Sci. Eng. A 2025, 922, 147598. [Google Scholar] [CrossRef]
- Brady, M.P.; Yamamoto, Y.; Santella, M.L.; Maziasz, P.J.; Pint, B.A.; Liu, C.T.; Lu, Z.P.; Bei, H. The development of alumina-forming austenitic stainless steels for high-temperature structural use. JOM 2008, 60, 12–18. [Google Scholar] [CrossRef]
- Zhao, Y.; Chen, P.; Wen, W.; Deng, Y.; Peng, K.; Liu, Y. Effect of Mn content on the high-temperature oxidation behaviors of Mn-substituted-for-Ni alumina-forming austenitic stainless steel. J. Mater. Res. Technol. 2023, 26, 7816–7828. [Google Scholar] [CrossRef]
- Lu, Z.; Zhao, Y.; Deng, Y.; Chen, P.; Wen, W. Evolution of the oxide layers of an aluminum-forming austenitic heat-resistant steel with high-Mn substitution for Ni: Experiment and first-principle calculations. Mater. Charact. 2023, 205, 113334. [Google Scholar] [CrossRef]
- Brady, M.; Magee, J.; Yamamoto, Y.; Helmick, D.; Wang, L. Co-optimization of wrought alumina-forming austenitic stainless steel composition ranges for high-temperature creep and oxidation/corrosion resistance. Mater. Sci. Eng. A 2014, 590, 101–115. [Google Scholar] [CrossRef]
- Du, Y.; Zhang, C.; Ma, Q.; Zheng, Y.; Li, H.; Gao, Q. Precipitation behavior and strengthening mechanism of NbC phase in alumina-forming austenitic steel. Mater. Sci. Eng. A 2025, 936, 148421. [Google Scholar] [CrossRef]
- Wang, S.; Wu, Y.; Gesmundo, F.; Niu, Y. The effect of Si additions on the high-temperature oxidation of a ternary Ni–10Cr–4Al alloy in 1 atm O2 at 900–1000 °C. Oxid. Met. 2008, 69, 299–315. [Google Scholar] [CrossRef]
- Li, M.; Zhu, Y.; Zhou, C. Effect of yttrium on the coking behavior of Fe-based superalloy in heavy hydrocarbon. Corros. Sci. 2015, 98, 81–87. [Google Scholar] [CrossRef]
- Li, S.; Xu, M.; Zhang, C.; Niu, Y.; Bao, Z.; Zhu, S.; Wang, F. Co-doping effect of Hf and Y on improving cyclic oxidation behavior of (Ni,Pt)Al coating at 1150 °C. Corros. Sci. 2021, 178, 109093. [Google Scholar] [CrossRef]
- Liu, X.; Chen, Y.; Lu, J.; Li, L.; Huang, A.; Zhang, H.; Fan, X.; Zhang, X.; Zhao, X. A comparative study on the oxidation behavior of Y-, Hf- and YHf-doped NiCoCrAl alloys: Effect of reactive elements. Corros. Sci. 2023, 218, 111160. [Google Scholar] [CrossRef]
- Ren, H.; Chen, R.; Liu, T.; Gao, X.; Qin, G.; Wu, S.; Guo, J. Unraveling the oxidation mechanism of Y-doped AlCoCrFeNi high-entropy alloy at 1100 °C. Appl. Surf. Sci. 2024, 652, 159316. [Google Scholar] [CrossRef]
- Shi, H.; Fetzer, R.; Tang, C.; Szabó, D.V.; Schlabach, S.; Heinzel, A.; Weisenburger, A.; Jianu, A.; Müller, G. The influence of Y and Nb addition on the corrosion resistance of Fe-Cr-Al-Ni model alloys exposed to oxygen-containing molten Pb. Corros. Sci. 2021, 179, 109152. [Google Scholar] [CrossRef]
- Chen, L.; Yuan, M.; Liu, Y.; Chen, J.; Wu, C.; Su, X. The influence of Al and Nb on the low oxygen pressure pre-oxidation behavior of Fe-35Ni-20Cr-xAl-yNb alloys at 1000 °C. Materials 2024, 17, 2086. [Google Scholar] [CrossRef] [PubMed]
- Deng, X.; Liu, Y.; Guo, Z.; Wu, C.; Peng, H.; Tu, H.; Wang, J.; Su, X. Selective oxidation of FeNiCrAl-based alloys under low oxygen pressure and their coking resistance. Vacuum 2024, 224, 113174. [Google Scholar] [CrossRef]
- Bale, C.W.; Bélisle, E.; Chartrand, P.; Decterov, S.A.; Eriksson, G.; Gheribi, A.E.; Hack, K.; Jung, I.-H.; Kang, Y.-B.; Melançon, J.; et al. FactSage thermochemical software and databases, 2010–2016. Calphad 2016, 54, 35–53. [Google Scholar] [CrossRef]
- Fedorova, E.; Monceau, D.; Oquab, D. Quantification of growth kinetics and adherence of oxide scales formed on Ni-based superalloys at high temperature. Corros. Sci. 2010, 52, 3932–3942. [Google Scholar] [CrossRef]
- Bull, S.; Rickerby, D.; Matthews, A.; Leyland, A.; Pace, A.; Valli, J. The use of scratch adhesion testing for the determination of interfacial adhesion: The importance of frictional drag. Surf. Coat. Technol. 1988, 36, 503–517. [Google Scholar] [CrossRef]
- Morrell, R. Handbook of Properties of Technical and Engineering Ceramics; Her Majesty’s Stationery Office: London, UK, 1987. [Google Scholar]
- Burnett, P.; Rickerby, D. The scratch adhesion test: An elastic-plastic indentation analysis. Thin Solid Films 1988, 157, 233–254. [Google Scholar] [CrossRef]
- Attar, F.; Johannesson, T. Adhesion evaluation of thin ceramic coatings on tool steel using the scratch testing technique. Surf. Coat. Technol. 1996, 78, 87–102. [Google Scholar] [CrossRef]
- Tien, J.K.; Davidson, J.M. Oxide spallation mechanisms. In Stress Effects and the Oxidation of Metals; Cathcart, J.V., Ed.; The Metallurgical Society of AIME: New York, NY, USA, 1975; pp. 200–219. [Google Scholar]
- Bull, S. Failure mode maps in the thin film scratch adhesion test. Tribol. Int. 1997, 30, 491–498. [Google Scholar] [CrossRef]
- Monceau, D.; Pieraggi, B. Determination of parabolic rate constants from a local analysis of mass-gain curves. Oxid. Met. 1998, 50, 477–493. [Google Scholar] [CrossRef]
- Schumann, E.; Sarioglu, C.; Blachere, J.R.; Pettit, F.S.; Meier, G.H. High-temperature stress measurements during the oxidation of NiAl. Oxid. Met. 2000, 53, 259–272. [Google Scholar] [CrossRef]
- James, M.C.; Cattelan, M.; Fox, N.A.; Silva, R.F.; Silva, R.M.; May, P.W. Experimental studies of electron affinity and work function from aluminium on oxidized diamond (100) and (111) surfaces. Phys. Status Solidi B 2021, 258, 2100027. [Google Scholar] [CrossRef]
- Nunes, F.; de Almeida, L.; Dille, J.; Delplancke, J.-L.; Le May, I. Microstructural changes caused by yttrium addition to NbTi-modified centrifugally cast HP-type stainless steels. Mater. Charact. 2007, 58, 132–142. [Google Scholar] [CrossRef]
- Peterson, A.; Baker, I. Microstructural evolution of Fe–20Cr–30Ni–2Nb–5Al AFA steel during creep at 760 °C. Mater. Sci. Eng. A 2021, 806, 140602. [Google Scholar] [CrossRef]
- Shi, L.; Li, M.; Zhan, Z.; Yuan, Z.; Wang, X. Effect of yttrium on the formation, microstructure and high-temperature oxidation resistance of the oxide film on the surface of FeCr alloy. Surf. Coat. Technol. 2023, 475, 130177. [Google Scholar] [CrossRef]
- Allam, I.M.; Whittle, D.P.; Stringer, J. The oxidation behavior of CoCrAI systems containing active element additions. Oxid. Met. 1978, 12, 35–66. [Google Scholar] [CrossRef]
- Wang, T.; Liu, W.; Yang, S.; Li, J.; Zhao, P.; Xue, H. Effect of yttrium additions on the high-temperature oxidation behavior of GH4169 Ni-based superalloy. Materials 2024, 17, 2733. [Google Scholar] [CrossRef] [PubMed]
- Holmberg, K.; Laukkanen, A.; Ronkainen, H.; Wallin, K.; Varjus, S. A model for stresses, crack generation and fracture toughness calculation in scratched TiN-coated steel surfaces. Wear 2003, 254, 278–291. [Google Scholar] [CrossRef]
- Liu, H.; Guo, Y.; Zhao, P.; Li, D.; Sun, S. Anisotropy origins of coefficient of friction and scratch hardness in nano scratching monocrystalline copper. Tribol. Int. 2023, 188, 108808. [Google Scholar] [CrossRef]
- Ariharan, S.; Maurya, R. Assessment of plasma sprayed carbon nanotube reinforced Al2O3-based nanocomposite with micro-scratching. Surf. Coat. Technol. 2021, 418, 127216. [Google Scholar] [CrossRef]
- Bird, A.; Yang, L.; Wu, G.; Inkson, B. Failure mechanisms of diamond like carbon coatings characterised by in situ SEM scratch testing. Wear 2023, 530, 205034. [Google Scholar] [CrossRef]
- Wang, G.; Gleeson, B.; Douglass, D.L. An extension of Wagner’s analysis of competing scale formation. Oxid. Met. 1991, 35, 317–332. [Google Scholar] [CrossRef]
- Brady, M.P.; Yamamoto, Y.; Santella, M.L.; Walker, L.R. Composition, microstructure, and water vapor effects on internal/external oxidation of alumina-forming austenitic stainless steels. Oxid. Met. 2009, 72, 311–333. [Google Scholar] [CrossRef]
- Zhai, Y.; Chen, Y.; Zhao, Y.; Long, H.; Li, X.; Deng, Q.; Lu, H.; Yang, X.; Yang, G.; Li, W.; et al. Initial oxidation of Ni-based superalloy and its dynamic microscopic mechanisms: The interface junction initiated outwards oxidation. Acta Mater. 2021, 215, 116991. [Google Scholar] [CrossRef]
- Yang, D.; Liu, Y.; Han, T.; Zhou, F.; Qu, N.; Liao, M.; Lai, Z.; Zhu, J. High thermal stability and oxidation behavior of FeCrNiAl-based medium-entropy alloys prepared by powder metallurgy. J. Alloys Compd. 2022, 918, 165562. [Google Scholar] [CrossRef]
- Pilling, N.B.; Bedworth, R.E. The oxidation of metals at high temperatures. J. Inst. Met. 1923, 29, 529–582. [Google Scholar]
- Zhao, Z.; Wang, J.; Chen, M.; Zhang, J.; Wang, F.; Young, D.J. Comparative study on the initial oxidation behavior of conventional and nanocrystalline MCrAlY coatings—Effect of microstructure evolution and dynamic mechanisms. Acta Mater. 2022, 239, 118264. [Google Scholar] [CrossRef]
- Essuman, E.; Meier, G.H.; Żurek, J.; Hänsel, M.; Quadakkers, W.J. The effect of water vapor on selective oxidation of Fe–Cr alloys. Oxid. Met. 2008, 69, 143–162. [Google Scholar] [CrossRef]
- Ding, Z.; Cao, B.; Luan, J.; Jiao, Z. Synergistic effects of Al and Ti on the oxidation behaviour and mechanical properties of L12-strengthened FeCoCrNi high-entropy alloys. Corros. Sci. 2021, 184, 109365. [Google Scholar] [CrossRef]
- Begley, M.; Mumm, D.; Evans, A.; Hutchinson, J. Analysis of a wedge impression test for measuring the interface toughness between films/coatings and ductile substrates. Acta Mater. 2000, 48, 3211–3220. [Google Scholar] [CrossRef]
- Xu, K.; Ren, Z.; Li, C. Progress in application of rare metals in superalloys. Rare Met. 2014, 33, 111–126. [Google Scholar] [CrossRef]
- Li, W.; Han, K.; Niu, R.; Liang, T.; Lai, C.; Zhang, X. Effect of Si and Y2O3 additions on the oxidation behavior of Ni–xAl (x = 5 or 10 wt%) alloys at 1150 °C. Oxid. Met. 2018, 89, 731–753. [Google Scholar] [CrossRef]
- Sun, D.; Liang, C.; Shang, J.; Yin, J.; Song, Y.; Li, W.; Liang, T.; Zhang, X. Effect of Y2O3 contents on oxidation resistance at 1150 °C and mechanical properties at room temperature of ODS Ni-20Cr-5Al alloy. Appl. Surf. Sci. 2016, 385, 587–596. [Google Scholar] [CrossRef]
- Krbata, M.; Eckert, M.; Bartosova, L.; Barenyi, I.; Majerik, J.; Mikuš, P.; Rendkova, P. Dry sliding friction of tool steels and their comparison of wear in contact with ZrO2 and X46Cr13. Materials 2020, 13, 2359. [Google Scholar] [CrossRef]
- Naumenko, D.; Pint, B.A.; Quadakkers, W.J. Current thoughts on reactive element effects in alumina-forming systems: In memory of John Stringer. Oxid. Met. 2016, 86, 1–43. [Google Scholar] [CrossRef]
- Li, J.; Cao, G.; Wang, H.; Zhang, W.; Li, C.; Wang, G.; Liu, Z. Size effects of Y-enriched intermetallic precipitates in Fe-20Cr-5Al-0.25Y alloy on the spallation resistance of thermally grown α-Al2O3 scales. Corros. Sci. 2020, 174, 108796. [Google Scholar] [CrossRef]
















| Alloys | Fe | Ni | Cr | Al | Nb | Mn | Si | Y | C |
|---|---|---|---|---|---|---|---|---|---|
| Fe25Ni20Cr4Al1Nb1Mn1.5Si | Bal | 25.1 | 19.8 | 4.07 | 1.13 | 0.96 | 1.42 | - | 0.3 |
| Fe25Ni20Cr4Al1Nb1Mn1.5Si-0.1Y | Bal | 24.7 | 20.1 | 4.01 | 1.07 | 0.91 | 1.56 | 0.08 | 0.3 |
| Fe25Ni20Cr4Al1Nb1Mn1.5Si-0.2Y | Bal | 25.2 | 19.9 | 3.88 | 0.97 | 1.03 | 1.53 | 0.17 | 0.3 |
| Fe25Ni20Cr4Al1Nb1Mn1.5Si-0.3Y | Bal | 24.9 | 19.9 | 4.13 | 1.19 | 0.91 | 1.48 | 0.26 | 0.3 |
| Alloys | Phases | Al | Si | Cr | Mn | Fe | Ni | Y | Nb | |
|---|---|---|---|---|---|---|---|---|---|---|
| 0 Y | Gray | FCC | 4.8 | 3 | 21.2 | 0.7 | 48.7 | 21.5 | - | 0.1 |
| Black | B2-NiAl | 31.2 | 1.1 | 5.4 | 0.8 | 17.5 | 43.9 | - | 0.1 | |
| White | MC | 2 | 0.3 | 6.1 | 0.2 | 8 | 3.7 | - | 79.7 | |
| 0.1 Y | Gray | FCC | 5.3 | 4.6 | 21.8 | 0.1 | 47 | 21.1 | 0 | 0.1 |
| Black | B2-NiAl | 32.9 | 1.6 | 7.8 | 0.5 | 14.2 | 42.5 | 0.1 | 0.4 | |
| White | MC | 1.6 | 0.4 | 7.7 | 0.3 | 6.6 | 4.2 | 1.7 | 77.5 | |
| 0.2 Y | Gray | FCC | 5.2 | 2.9 | 21.6 | 0.8 | 48.7 | 20.6 | 0 | 0.2 |
| Black | B2-NiAl | 30.5 | 1.4 | 5.3 | 0.4 | 17.6 | 44.6 | 0.1 | 0.1 | |
| White | MC | 3 | 1.2 | 5.7 | 0.2 | 5.1 | 3.1 | 4.5 | 77.2 | |
| 0.3 Y | Gray | FCC | 4.7 | 3.8 | 21.1 | 0.5 | 48.2 | 21.3 | 0.2 | 0.2 |
| Black | B2-NiAl | 31.4 | 2.9 | 4.7 | 0.7 | 14.1 | 45.8 | 0.3 | 0.1 | |
| White | MC | 1.1 | 0.3 | 5.5 | 0.3 | 4.8 | 2.6 | 5.3 | 80.1 | |
| Alloys | Phase | O | Al | Si | Cr | Mn | Fe | Ni | Nb | Y |
|---|---|---|---|---|---|---|---|---|---|---|
| 0 Y | Al2O3 | 46.5 | 33.3 | 0.5 | 3.1 | 0.2 | 6.2 | 9.7 | 0.5 | - |
| 0.1 Y | Al2O3 | 53.8 | 34.7 | 0.3 | 3.1 | 0.1 | 2.4 | 5.2 | 0.4 | 0 |
| Y/Nb-oxide | 58.4 | 31.9 | 0.3 | 1.5 | 0 | 2.6 | 1.9 | 2.4 | 1.0 | |
| 0.2 Y | Al2O3 | 50.0 | 37.0 | 0.4 | 2.7 | 0 | 5.8 | 4.1 | 0 | 0 |
| Y/Nb-oxide | 65.3 | 22.2 | 0.1 | 1.0 | 0.1 | 1.0 | 2.3 | 7.7 | 0.3 | |
| 53.3 | 35.0 | 0.3 | 1.0 | 0 | 0.9 | 7.7 | 0.7 | 1.1 | ||
| 0.3 Y | Al2O3 | 39.5 | 33.0 | 1.0 | 6.0 | 0.2 | 12.8 | 7.3 | 0.2 | 0 |
| Y-oxide | 36.1 | 23.9 | 1.2 | 10.2 | 0.2 | 15.4 | 6.8 | 0.2 | 6.0 | |
| 33.9 | 31.0 | 1.1 | 6.3 | 0.4 | 14.0 | 12.2 | 0 | 1.1 | ||
| Nb-oxide | 53.6 | 33.3 | 0.1 | 0.7 | 0 | 0.9 | 9.5 | 1.9 | 0 |
| Alloys | Phase | O | Al | Si | Cr | Mn | Fe | Ni | Nb | Y |
|---|---|---|---|---|---|---|---|---|---|---|
| 0 Y | Al2O3 | 61.6 | 34.3 | 0.3 | 2.2 | 0.2 | 1.1 | 0.3 | 0 | - |
| Spinel | 60.8 | 2.8 | 0 | 20.1 | 1.5 | 13.2 | 0.7 | 0.9 | - | |
| 0.1 Y | M2O3 | 65.7 | 18.5 | 0 | 12.1 | 0.1 | 1.2 | 0.4 | 4.0 | 0 |
| Al2O3 | 61.4 | 35.5 | 0 | 2.2 | 0.1 | 0.5 | 0.1 | 0.2 | 0 | |
| 0.2 Y | Al2O3 | 61.3 | 34.7 | 0.1 | 2.8 | 0 | 0.7 | 0.3 | 0 | 0.1 |
| 0.3 Y | Al2O3 | 62.9 | 35.4 | 0 | 1.0 | 0.1 | 0.4 | 0.1 | 0 | 0.1 |
| Sample | L (mm) | Ft (N) | d (μm) | A1 (m2) | σ (GPa) | W (J m−2) | ||||
|---|---|---|---|---|---|---|---|---|---|---|
| Equation (4) | Equation (7) | Equation (6) ( ) | Equation (8) ( ) | |||||||
| 0 Y | 0.14 | 0.10 | 2.5 | 5.23 × 10−11 | 0.46 | 0.39 | 0.28 | 19.60 | 0.78 | 22.90 |
| 0.1 Y | 0.29 | 0.21 | 1.1 | 1.53 × 10−11 | 3.29 | 0.65 | 17.77 | 73.55 | 6.15 | 46.80 |
| 0.2 Y | 0.51 | 0.31 | 1.2 | 1.75 × 10−11 | 4.26 | 1.29 | 38.21 | 123.54 | 9.60 | 64.50 |
| 0.3 Y | 0.36 | 0.22 | 1.0 | 1.33 × 10−11 | 3.98 | 0.60 | 25.95 | 89.38 | 7.41 | 50.20 |
| Alloy | Oxide System | Energy Release Rate (J m−2) | Oxidation Conditions | Quantification Methods/Mode of Failure | Residual Stress Measurement Method | Ref. |
|---|---|---|---|---|---|---|
| AFA (0–0.3 wt.% Y) | Al2O3 | 19–125 (); 22–65 (); | 850 °C + 1100 °C 0.25% H2O | Scratch Test/ Interface delamination failure | Estimation of thermal expansion mismatch | Present work |
| AM1 Ni-7.5Cr-5.3Al | Al2O3 + NiAl2O4 | 39–113 (); 60–100 (); | 1000 °C Lab air | Scratch Test/buckling + wedge spallation | Estimation of thermal expansion mismatch | [22] |
| MCNG Ni-4Cr-6Al (0.1 wt.% Hf) | NiO + spinel + Al2O3 | 0.1–0.5 (); 33–306 (); | 1100 °C Lab air | Scratch Test/buckling + wedge spallation | Estimation of thermal expansion mismatch | [22] |
| MA956 superalloy | Al2O3 | 28 | 1150 °C + 1250 °C Lab air | Scratch Test/wedge spallation | XRD | [28] |
| Substrate | Al2O3 in TBC | 50–80 | - | wedge impression test | Residual Thermal Strain Model | [49] |
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.
Share and Cite
Ji, J.; Deng, X.; Wu, C.; Chen, J.; Zhu, X.; Liu, Y. Study on Yttrium-Enhanced Anti-Oxidation and Adhesion Properties of Al2O3 Oxide Scale on AFA Alloy Under Low Oxygen Partial Pressure. Coatings 2026, 16, 620. https://doi.org/10.3390/coatings16050620
Ji J, Deng X, Wu C, Chen J, Zhu X, Liu Y. Study on Yttrium-Enhanced Anti-Oxidation and Adhesion Properties of Al2O3 Oxide Scale on AFA Alloy Under Low Oxygen Partial Pressure. Coatings. 2026; 16(5):620. https://doi.org/10.3390/coatings16050620
Chicago/Turabian StyleJi, Jin, Xuxu Deng, Changjun Wu, Junxiu Chen, Xiangying Zhu, and Ya Liu. 2026. "Study on Yttrium-Enhanced Anti-Oxidation and Adhesion Properties of Al2O3 Oxide Scale on AFA Alloy Under Low Oxygen Partial Pressure" Coatings 16, no. 5: 620. https://doi.org/10.3390/coatings16050620
APA StyleJi, J., Deng, X., Wu, C., Chen, J., Zhu, X., & Liu, Y. (2026). Study on Yttrium-Enhanced Anti-Oxidation and Adhesion Properties of Al2O3 Oxide Scale on AFA Alloy Under Low Oxygen Partial Pressure. Coatings, 16(5), 620. https://doi.org/10.3390/coatings16050620