Next Article in Journal
Mathematical and Statistical Evaluation of Reverse Osmosis in the Removal of Manganese as a Way to Achieve Sustainable Operating Parameters
Next Article in Special Issue
Polymeric Inclusion Membranes Based on Ionic Liquids for Selective Separation of Metal Ions
Previous Article in Journal
Electrostatic Potentials Caused by the Release of Protons from Photoactivated Compound Sodium 2-Methoxy-5-nitrophenyl Sulfate at the Surface of Bilayer Lipid Membrane
Previous Article in Special Issue
Modeling and Optimal Operating Conditions of Hollow Fiber Membrane for CO2/CH4 Separation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Iron Control in Liquid Effluents: Pseudo-Emulsion Based Hollow Fiber Membrane with Strip Dispersion Technology with Pseudo-Protic Ionic Liquid (RNH3+HSO4) as Mobile Carrier

by
Francisco Jose Alguacil
* and
Jose Ignacio Robla
Centro Nacional de Investigaciones Metalurgicas (CSIC), Avda. Gregorio del Amo 8, 28040 Madrid, Spain
*
Author to whom correspondence should be addressed.
Membranes 2023, 13(8), 723; https://doi.org/10.3390/membranes13080723
Submission received: 26 June 2023 / Revised: 26 July 2023 / Accepted: 5 August 2023 / Published: 8 August 2023

Abstract

:
The transport of iron(III) from aqueous solutions through pseudo-emulsion-based hollow fiber with strip dispersion (PEHFSD) was investigated using a microporous hydrophobic hollow fiber membrane module. The pseudo-protic ionic liquid RNH3HSO4 dissolved in Solvesso 100 was used as the carrier phase. This pseudo-protic ionic liquid was generated by the reaction of the primary amine Primene JMT (RNH2) with sulphuric acid. The aqueous feed phase (3000 cm3) containing iron(III) was passed through the tube side of the fiber, and the pseudo-emulsion phase of the carrier phase (400 cm3) and sulphuric acid (400 cm3) were circulated through the shell side in counter-current operational mode, using a single hollow fiber module for non-dispersive extraction and stripping. In the operation, the stripping solution (sulphuric acid) was dispersed into the organic membrane phase in a tank with a mixing arrangement (a four-blade impeller stirrer) designed to provide strip dispersion. This dispersed phase was continuously circulated from the tank to the membrane module in order to provide a constant supply of the organic solution to the fiber pores. Different hydrodynamic and chemical parameters, such as feed (75–400 cm3/min) and pseudo-emulsion phases (50–100 cm3/min) flows, sulphuric acid concentration in the feed and stripping phases (0.01–0.5 M and 0.5–3 M, respectively), metal concentration (0.01–1 g/L) in the feed phase, and PPILL concentration (0.027–0.81 M) in the carrier phase, were investigated. From the experimental data, different diffusional parameters were estimated, concluding that the resistance due to the feed phase was not the rate-controlling step of the overall iron(III) transport process. It was possible to concentrate iron(III) in the strip phase using this smart PEHFSD technology.

1. Introduction

Iron(III) is an element in close relationship with Mankind, both for natural and anthropogenic causes. This element widely exists in the environment and is considered essential for humans and generally for life however, low or high iron levels in the human organism can be the cause of different diseases. Low iron levels in the body promote anemia, whereas high iron concentrations lead to organ damage, arthritis, liver disease, etc.; thus, high iron(III) concentrations in water are the cause of environmental problems. The presence of iron(III) in waters is accompanied by some characteristics such as odour, taste, and colour (Figure 1); its presence also causes corrosion and staining effects [1,2,3,4].
Also, iron(III) is an often-found constituent in many raw materials; thus, in the production, via Pyrometallurgical or Hydrometallurgical technologies, of other most valuable metals, a step devoted to the removal of this non-profitable iron(III) is very often considered.
In conclusion, extraction or removal of iron(III) from high to trace concentrations plays an important role in many fields, i.e., waste stream treatment, determination of iron in minerals, separation and purification of radionuclide solutions, water treatment, organic synthesis, etc.
It is of the utmost necessity to develop effective strategies for the detection and removal of iron(III) in water environments. These strategies included the use of different separation technologies from precipitation to adsorption, with recent publications considering liquid-liquid extraction using (acidic, solvation, and ionic liquid-based extractants) [5,6,7,8,9], ion-exchange resins (Lewatit TP-208) [2], adsorption (carbon derivatives, zeolites, and microgels) [10,11,12,13], and membrane [4,14] procedures.
In the case of membrane technologies, supported liquid membranes both in flat-sheet or hollow fiber modules are gaining special consideration in the recovery of metals [15,16,17,18]. In the case of hollow fiber membrane processing, one of the more advanced developments is the so-called pseudo-emulsion-based hollow fiber strip dispersion (PEHFSD), which is characterised by its ability to afford high mass transfer rates of solutes and is accompanied by high selectivity by the use of specific carriers or extractants.
Among these extractants, ionic liquids are considered one of the smartest types of reagents to be used in the recovery of metals from different sources. These ionic liquids have gained widespread use due to their properties [19,20]: low volatility and flammability [21,22], high refractive index and thermal stability [23,24], strong conductivity and selectivity [25], and solvation power of both organic and inorganic compounds [26,27]. Mostly due to these properties, this type of reagent is considered a green solvents, though their environmental greenness status is also under debate [28,29].
Moreover, ionic liquids can also be divided into some subfamilies [30]: (i) aprotic ionic liquids and task-specific ionic liquids, both types being considered fully ionic; (ii) protic ionic liquids, generated by the reaction of an acid and a base; and (iii) pseudo-protic ionic liquids (PPILs), which are also generated by the reaction of an acid and a base but are sometimes considered not fully ionic. A special case of these (iii) types of compounds is the PPILS formed from tertiary amines [31,32], and probably for extension and reactive similarities by primary and secondary amines [33].
The present work presented an investigation about the facilitated transport of iron(III) using a pseudo-protic ionic liquid (RNH3+HSO4), derived from the reaction of the primary amine Primene JMT and sulphuric acid, as a mobile carrier and pseudo-emulsion-based hollow fiber strip dispersion membrane operation. The influence of different variables, such as hydrodynamic conditions and chemical parameters, is considered in order to yield efficient membrane technology.

2. Materials and Methods

2.1. Materials

Amine Primene JMT (Dow Chem., Midland, MI, USA) and sulphuric acid are the precursors of the pseudo-protic ionic liquid (PPIL) used in this work. Primene JMT is a primary amine having highly branched alkyl chains (C16–22), in which the nitrogen atom of the amine group is linked to a tertiary carbon atom. The amine has an average molecular weight of 315 and a density (25 °C) of 0.840 g/cm3 [34].
Solvesso 100 is an aromatic (99%) diluent (Exxon Chem Iberia, Madrid, Spain). All other reagents used in the work are of AR grade.
The hollow fiber module device used in the investigation was manufactured by Hoechst Celanese: Liqui-Cel 8 × 28 cm 5PCG-259 contactor and 5PC5-1002 Liqui-Cel laboratory LLE, whose specifications are summarised in Table 1.

2.2. Methods

2.2.1. Liquid-Liquid Extraction Experiments (Generation of the PPIL)

To establish conditions for the generation of the pseudo-protic ionic liquid (RNH3+HSO4) used as a carrier in this work, several liquid-liquid extraction experiments were carried out under the following conditions: equal volumes of 25 cm3 each containing 1 M sulphuric acid and the amine dissolved in Solvesso 100 were put in thermostatically controlled (25 °C) glass vessels and mechanically shaken via four bladed glass impellers. Equilibrium was reached within a few minutes (less than 5 min). After phase disengagement, the acidic content in the organic phase was analysed by titration in ethalonic medium with standard NaOH solutions, using bromothimol blue as an indicator, whereas the acid content in the corresponding equilibrated aqueous phases was analysed in the same manner. The distribution coefficient of sulphuric acid, defined as the ratio of concentrations of the acid in the organic phase (org) and in the aqueous phase (aq), at equilibrium, was calculated as:
D H 2 S O 4 = H 2 S O 4 o r g H 2 S O 4 a q

2.2.2. Membrane Operation

The hollow fiber strip dispersion operation comprised a single membrane contactor, one stirred tank containing the pseudo-emulsion phase formed by the PPIL solution (carrier phase) and sulphuric acid solution (stripping phase), and one stirred tank containing the iron(III)-bearing feed phase. The set-up also contained two gear pumps to provide variable flows for both phases and flow meters.
In the operation, the organic solution wet the porous wall of the fiber due to its hydrophobic nature, whereas the interface was maintained at the pore by the application of a higher pressure to the feed phase than to the pseudo-emulsion phase. This differential pressure was set below the breakthrough pressure; in the present investigation, the pressure applied to the feed phase was 0.2 bar higher than the corresponding pressure applied to the pseudo-emulsion phase.
A view of the membrane operation using one contactor and in the recirculation mode is shown in Figure 2.
The membrane operation was carried out by passing the iron(III)-bearing feed phase across the tube side of the fibers and the pseudo-emulsion phase through the shell side in counter-current mode. The tank containing the feed phase was stirred in order to homogenise the solution, whereas the stirring of the tank containing the pseudo-emulsion phase was needed in order to maintain the pseudo-emulsion and homogenise it. In addition, the characteristics of the pseudo-emulsion must be such that it must have clear and fast organic and strip-phase disengagement when mixing is stopped; thus, the pseudo-emulsion reservoir tank acts as a mixer-settler.
In the operation, the volume of the pseudo-emulsion phase was 800 cm3 (400 cm3 each of the organic and stripping solutions), whereas the volume of the feed phase was 3000 cm3. At elapsed times, aliquots of the feed and pseudo-emulsion tanks were taken and analysed for iron concentration in the aqueous solutions by conventional atomic absorption spectrometry (Perkin Elmer 1100B spectrophotometer). The permeation coefficient (P) was calculated by the next equation:
ln F e f , t F e f , 0 = A · P V t
where A was the membrane area (1.4 m2), V was the volume (3000 cm3) of the feed phase, and t was the elapsed time. In the above equation, [Fe]f,t and [Fe]f,0 were the iron(III) concentrations in the feed phase at an elapsed time and time zero, respectively.

3. Results and Discussion

3.1. Generation of the Pseudo-Protic Ionic Liquid (PPIL)

Upon reaction of the amine (RNH2) with sulphuric acid, the pseudo-protic ionic liquid was generated according to the next reactions:
R N H 2 o r g + H 2 S O 4 a q R N H 3 + 2 S O 4 o r g 2
R N H 3 + 2 S O 4 o r g 2 + H 2 S O 4 a q 2 R N H 3 + · H S O 4 o r g
Thus, firstly, the amine sulphate (RNH3+)2SO42− was formed (Equation (3)), and in excess of acid, the amine bisulfate RNH3+HSO4 was generated (Equation (4)). The overall reaction being:
R N H 2 o r g + H 2 S O 4 a q R N H 3 + · H S O 4 o r g
To estimate the extraction equilibrium for Equation (5), experiments were carried out mixing organic phases of the amine (0.068–0.54 M) in Solvesso 100 and 1 M sulphuric acid solutions. The results of the acid extraction by the amine were summarised in Table 2, in which the acid extraction into the organic phase was calculated as the acid distribution coefficient (Equation (1)).
In Equation (5), the acid extraction constant (Kext) was defined as:
K e x t = R N H 3 + · H S O 4 o r g R N H 2 o r g H 2 S O 4 a q
and taking into consideration Equation (1), taking log, and rearranging, the next expression was obtained:
log D H 2 S O 4 = log K e x t + log R N H 2 o r g
Thus, a plot of log DH2SO4 versus log [RNH2]org allowed us to estimate the stoichiometric coefficient (slope) and the value of log Kext (ordinate). Figure 3 showed such a plot, and it can be seen that the slope was close to 1 (as expected from Equation (5), with log Kext 2.22).
The results of Table 2 were numerically treated by a computer programme that minimised the U function, defined as:
U = Σ log D exp log D c a l 2
where Dexp was the experimental sulphuric acid distribution coefficient and Dcal was the corresponding one calculated by the programme. The results from these calculations confirmed the formation of the pseudo-protic ionic liquid (RNH3+·HSO4) and the stoichiometry proposed in Equation (5). The value of lo Kext (U = 0.0006) calculated by the programme was 2.25 ± 0.26, which was close to the graphical value obtained from Figure 3.

3.2. Hollow Fiber Membrane Experiments

The iron(III) flux (J) through the hollow fiber module was given by the next relationship:
J = P F e f D F e , s t D F e , f F e s t
where P was the permeation coefficient, [Fe]f and [Fe]st were the iron concentrations in the feed and in the strip solutions, DFe,f was the iron distribution coefficient between the membrane and the feed phases, at the reaction equilibrium, at the feed phase-side interface, and DFe,st was the iron distribution coefficient between the membrane and the strip phases, at the reaction equilibrium, at the strip-side interface. In practise, DFe,f values were much greater than DFe,st values, and the second term between the squares in Equation (9) can be neglected in comparison with [Fe]f. Thus, the mass balance in the feed solution can be expressed as:
V d F e f d t = A · P · F e f
where V was the feed phase volume, A represented the membrane area, and t was the elapsed time. Integration of the above resulted in Equation (2).
The operation of the hollow fiber module for the removal and concentration of iron(III) using the overall permeation coefficient was based on three mass transfer resistances: (i) one occurring in the solution flowing through the tube side of the fiber; (ii) a second, corresponding to the diffusion of the iron-PPIL complex across the immobilised liquid membrane located in the fiber pores; and (iii) the resistance due to the aqueous interface created on the outside of the hollow fiber.
Thus,
1 P = 1 k a + r i r ln 1 P m + r i r o 1 k o
where ka and ko were the mass transfer coefficients corresponding to the inner and outer aqueous boundary layers, and rln was the hollow fiber log mean radius. The membrane permeability (Pm) was related to the distribution coefficient by the next equation:
P m = D F e , f k m
where km represents the membrane mass transfer coefficient. Inserting Equation (12) into Equation (11) resulted in:
1 P = 1 k a + r i r ln 1 D F e , f k m + r i r o 1 k o
When the reaction was instantaneous on the stripping side, the contribution of the outer aqueous phase can be removed from Equation (13), and the overall permeability coefficient is expressed as:
1 P = 1 k a + r i r ln 1 D F e , f k m

3.2.1. Influence of the Feed Phase Flow on Iron(III) Permeation

The influence of this variable on iron(III) permeation was first investigated by using a feed phase containing 0.01 g/L Fe(III) and 0.1 M sulphuric acid medium and a pseudo-emulsion phase containing 0.27 M PPIL in Solvesso 100 as organic solution and 3 M sulphuric acid as stripping solution.
The results of this set of experiments are shown in Table 3. It can be seen that the permeation coefficient increased with the increase in feed phase flow up to 300 cm3/min and decreased at a higher feed phase flow. In a transport process across a liquid membrane, two types of diffusional resistances can be considered: (i) the resistance due to the feed phase boundary layer and (ii) the resistance associated with the membrane support. It is often found that the magnitude of the first competes with the value of the support resistance [35]. The experimental results shown in Table 4 indicated that at 300 cm3/min, the feed boundary layer was at a minimum and the feed phase resistance to mass transfer was minimised, thus, the diffusion contribution of the aqueous species to the mass transfer phenomena can be considered constant [36].
The decrease of the permeation coefficient value at flows exceeding 300 cm3/min can be explained in terms of (i) the increase of the turbulence in the feed phase, which forced organic solution out of the membrane pores; (ii) the lower residence time of the feed phase in the module as a consequence of increasing the flow; and (iii) the formation of an emulsion along the lumen side also due to the increase of the flow [37].

3.2.2. Influence of the Pseudo-Emulsion Phase Flow on Iron(III) Permeation

Using the same feed and pseudo-emulsion phases as in the previous subsection and a feed phase flow of 300 cm3/min, a series of experiments were conducted to investigate the influence of the pseudo-emulsion phase flow on iron(III) permeation. These experiments showed that in the 50–100 cm3/min flow range, the variation of these flows had a negligible influence on the removal of iron(III) from the feed phase.

3.2.3. Influence of the Strip Solution Composition on Iron(III) Permeation

The permeation of iron(III) under different strip solutions was also investigated. In these experiments, the feed phase contained 1 g/L Fe(III) in 0.1 M sulphuric acid medium, whereas the pseudo-emulsion phase was contained and an organic solution of 0.14 M PPIL in Solvesso 100 and 0.5–3 M sulphuric acid solution were used as strippants.
The values of the iron(III) permeation coefficients derived from the experimentation are shown in Table 4. These values showed that the removal of iron(III) from the feed phase increased (higher permeation coefficient) with the increase in sulphuric acid concentration in the stripping solution. In addition, metal recovery in these stripping solutions increased with the increase of in acid concentration; this result was especially noted in the case of using 0.5 M acid versus 1.5 or 3 M sulphuric acid solutions in the strip solution.

3.2.4. Influence of the Sulphuric Acid Concentration in the Feed Phase on Iron(III) Permeation

The variation of the sulphuric acid concentration in the feed phase on iron(III) permeation was also investigated by using feed phases of 0.01 g/L Fe(III) and varying acid concentrations and pseudo-emulsion phases containing 0.14 M PPIL in Solvesso 100 and 3 M sulphuric acid.
These results were presented in Figure 4, plotting ln ([Fe]f,t/[Fe]f,0) versus time at the various acid concentrations in the feed phase. It was concluded that the variation of the acid concentration in the feed phase had a key influence on the removal of iron(III) from this phase since the permeation coefficient value decreased from 1.8·10−2 cm/min using feed phases containing 10−2 M acid to 3.0·10−3 cm/min when the feed phase contained 0.5 M sulphuric acid.

3.2.5. Influence of the Initial Iron(III) Concentration in the Feed Phase on Metal Extraction

Using a pseudo-emulsion phase of 0.14 M PPIL in Solvesso 100 and 3 M sulphuric acid as a stripping solution, the variation of the initial metal concentration in the feed phase on the iron(III) permeation coefficient was investigated. In these experiments, the feed phase contained 0.01–1 g/L Fe(III) in 0.1 M sulphuric acid medium, and flows of 300 cm3/min and 100 cm3/min were used in the feed and pseudo-emulsion phases, respectively.
The results of these experiments (Figure 5) indicated that the increase of the metal concentration in the feed phase decreased iron(III) permeation. These results can be explained in terms of the fact that as the iron(III) concentration in the feed phase increased, the organic phase immobilised in the fiber pores became saturated with the iron-PPIL complex. Further, this complex diffused at a slow rate into the bulk of the organic solution, which resulted in a decrease in the mass transfer in the organic solution. However, this slow transfer can be remedied either by increasing the membrane surface or running the transport operation for longer periods of time.
The initial metal flux (J) can be defined by the relationship:
J = P · F e f , 0
Table 5 shows the flux values corresponding to the various initial iron(III) concentrations used in this work.
These results showed that, as somewhat expected from Equation (15), the iron flux increased with the increase in the initial metal concentration in the feed phase [38].

3.2.6. Influence of the Carrier Concentration on Iron(III) Permeation

It was obvious that the presence of the carrier in the pseudo-emulsion phase was another key factor in achieving good metal permeation across the hollow fiber membrane and, thus, a convenient removal of this undesirable solute in a given feed phase. To investigate the effect of varying the pseudo-protic ionic liquid (carrier) concentration in the organic phase on iron(III) permeation, experiments were conducted using feed phases of 0.01 g/L Fe(III) in 0.1 M sulphuric acid medium and pseudo-emulsion phases of various carrier concentrations in Solvesso 100 and 3 M sulphuric acid concentrations.
The results derived from these series of experiments were shown in Figure 6, which showed that the removal of iron(III) from the feed phase increased with the increase of the carrier concentration from 0.027 M to 0.27 M; these results indicated that in this range of concentrations, iron(III) transport was governed by membrane diffusion, though in the maximum transport or permeability region, diffusion in the membrane fibers was negligible and the transport rate was therefore limited by diffusion through the boundary film of the aqueous solution on the feed side of the fibers. However, at carrier concentrations higher than 0.27 M, iron(III) permeation decreased, probably as a consequence of an increase in the organic phase viscosity due to the increase in the carrier concentration in the organic solution, which resulted in a decrease in iron(III) transport across the fiber pores [39].
Table 6 showed the permeation coefficient values at these various PPIL concentrations. This table also showed the percentage of iron(III) recovered in the stripping solution. It can be seen that the percentage of iron(III) recovered in the strip solution was in excess of 80%.

3.2.7. Estimation of Diffusional Parameters

It can be assumed that the PPIL concentration in the membrane module was constant; under this assumption, the apparent diffusion coefficient for iron(III) can be calculated by the next expression [40]:
D 0 a = J · d o r g P P I L o r g
being J the metal flux (Table 4), dorg the fiber thickness (Table 1), and using a PPIL concentration of 0.27 M (concentration at which maximum iron(III) permeation was obtained), the value of this apparent diffusion coefficient was calculated as 1.9·10−8 cm2/min.
An estimation of the membrane mass transfer coefficient (km) can be performed using the next relationship [41]:
k m = D o r g · ε τ d o d i 2
In the above expression, Dorg was the diffusion coefficient of the metal-carrier species in the fibers, with an average value of 6·10−5 cm2/min [42], ε was the fiber porosity, τ was the fiber tortuosity, and do and di were the values of the outer and inner fiber diameters, respectively (values of ε, τ, do, and di were given in Table 1). In the present investigation, the value of km was estimated at 3.3·10−5 cm/min.
The membrane mass transfer coefficient did not depend on the hydrodynamic conditions applied to a system; it was only related to the fiber properties and the diffusion coefficients of the extracted complex in the organic solution filling the fiber pores.
The effective diffusion coefficient (Deff) of iron(III)-PPIL complex across the organic membrane phase was also determined. This diffusion coefficient for the solute in the immobilised organic liquid membrane was calculated as [43,44]:
D e f f = k m · d o r g · τ
where dorg is the hollow fiber thickness (Table 1). Thus, the value of Deff for the present system was calculated to be near 2.0·10−3 cm2/min.
It was previously mentioned (Section 3.2.) that the distribution coefficient in the feed phase (DFe,f) was normally much greater than the distribution coefficient in the stripping solution (DFe,st), and it was also often considered that the stripping reaction was instantaneous; thus, the mass transfer resistance for the strip solution was negligible if compared with the overall mass transfer resistance. The individual feed mass transfer coefficient (ka) was dependent on the mean flow velocity of the feed phase (ua) [45]:
k a = 1.5 D a q d i d i 2 · u a D a q · L 1 3
where Daq was the diffusion coefficient or iron species in the feed phase (averaging 6·10−4 cm2/min [46]), di the inner diameter of the fibers, and L was the fiber length (Table 1). Thus, at 300 cm3/min, the value of ka can be calculated as 6.1·10−2 cm/min.
Equations (13) and (14) showed that the overall resistance was the sum of the values of the individual resistances, and the results shown in Table 6 indicated the overall resistance values were in the 55–155 min/cm range, whereas the value of the resistance due to the feed phase (Ra = 1/ka) was 16 min/cm. The fractional resistance due to the feed phase (Ra0) to the overall process (R) can be calculated as:
R a 0 = R a R · 100
Under the present experimental conditions, the value of Ra0 was 17%, this value clearly indicated that this step was not rate-controlling the overall iron(III) transport process.

4. Conclusions

Hollow fiber membrane, in the strip dispersion operational form, investigations were carried out in a single membrane module for simultaneous extraction and stripping in counter-current mode. From the results derived from this investigation, it can be concluded that the experimental conditions: (i) using a pseudo-emulsion phase consisting of a mixture of 0.27 M RNH3+HSO4 (pseudo-protic ionic liquid derived from the reaction of the primary amine Primene JMT and sulphuric acid) in Solvesso 100 and 3 M sulphuric acid, and maintaining flows of 300 cm3/min and 100 cm3/min for feed and pseudo-emulsion phases, respectively, were suitable for the efficient removal and concentration of iron(III) under optimum conditions.
From the experimental data, several diffusional parameters were calculated, and it was shown that iron(III) transport rate was mostly controlled by membrane diffusion. Under proper operation, the stability of PEHFSD was found to be good. This type of membrane operation presented a promising alternative to conventional separation methodologies and should increase its interest for the potential removal of iron(III) (and other undesirable solutes) as well as the recovery of valuable metals from liquid effluents, especially when the concentrations of these solutes are low.

Author Contributions

Conceptualization, F.J.A.; methodology, F.J.A.; investigation, F.J.A. and J.I.R.; resources, J.I.R.; data curation, F.J.A. and J.I.R.; writing-original draft preparation, F.J.A.; writing—review and editing, F.J.A. and J.I.R.; visualisation, F.J.A. and J.I.R.; supervision, F.J.A. and J.I.R. All authors have read and agreed to the published version of the manuscript.

Funding

This investigation is performed under CSIC-Project 202250E019.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors would like to thank CSIC (Spain) for support. In addition, the authors thank Martin Ian Maher for checking the English language.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Atchudan, R.; Edison, T.N.J.I.; Perumal, S.; Vinodh, R.; Sundramoorthy, A.K.; Babu, R.S.; Lee, Y.R. Leftover kiwi fruit peel-derived carbon dots as a highly selective fluorescent sensor for detection of ferric ion. Chemosensors 2021, 9, 166. [Google Scholar] [CrossRef]
  2. Alguacil, F.J. The removal of toxic metals from liquid effluents by ion exchange resins. Part XVI: Iron(III)/H+/Lewatit TP208. Rev. Metal. 2021, 57, e203. [Google Scholar] [CrossRef]
  3. Li, C.; Marin, L.; Chen, X. Chitosan based macromolecular probes for the selective detection and removal of Fe3+ ion. Int. J. Biol. Macromol. 2021, 186, 303–313. [Google Scholar] [CrossRef] [PubMed]
  4. Samavati, Z.; Samavati, A.; Goh, P.S.; Fauzi Ismail, A.; Sohaimi Abdullah, M. A comprehensive review of recent advances in nanofiltration membranes for heavy metal removal from wastewater. Chem. Eng. Res. Des. 2023, 189, 530–571. [Google Scholar] [CrossRef]
  5. Kasikov, A.; Sokolov, A.; Shchelokova, E. Extraction of iron(III) from nickel chloride solutions by mixtures of aliphatic alcohols and ketones. Solvent Extr. Ion Exch. 2022, 40, 251–268. [Google Scholar] [CrossRef]
  6. Chukreev, C.G.; Dorozhko, V.A.; Afonin, M.A. Mathematical model of FeCl3 and HCl extraction in the FeCl3–HCl–H2O–undecan-1-ol system. Russian J. Gen. Chem. 2022, 92, 108–116. [Google Scholar] [CrossRef]
  7. Pavón, S.; Haneklaus, N.; Meerbach, K.; Bertau, M. Iron(III) removal and rare earth element recovery from a synthetic wet phosphoric acid solution using solvent extraction. Min. Eng. 2022, 182, 107569. [Google Scholar] [CrossRef]
  8. Wen, J.; Lee, M.S. Options to recover high-purity MnO2 from leach liquors of manganese dust containing Mn3O4 and iron and zinc oxide as minor impurities. Hydrometallurgy 2023, 218, 106056. [Google Scholar] [CrossRef]
  9. Cubova, K.; Semelova, M.; Nemec, M.; Benes, V. Liquid-liquid extraction of ferric ions into the ionic liquids. Minerals 2022, 12, 11. [Google Scholar] [CrossRef]
  10. Wang, H.; Huang, C.; Ma, S.; Guo, S.; Gong, B.; Ou, J. Fabrication of bifunctional macroporous adsorption resin via grafting carbon dot and application in the detection and adsorption of iron (III) ion. Mater. Today Comm. 2023, 34, 105220. [Google Scholar] [CrossRef]
  11. Arif, M. Extraction of iron (III) ions by core-shell microgel for in situ formation of iron nanoparticles to reduce harmful pollutants from water. J. Environ. Chem. Eng. 2023, 11, 109270. [Google Scholar] [CrossRef]
  12. Aljabarin, N. Chemical adsorption of iron ions from drinking water using Jordanian zeolitic tuff. Desalin. Water Treat. 2023, 281, 196–203. [Google Scholar] [CrossRef]
  13. Brishti, R.S.; Kundu, R.; Habib, M.A.; Ara, M.H. Adsorption of iron(III) from aqueous solution onto activated carbon of a natural source: Bombax ceiba fruit shell. Res. Chem. 2023, 5, 100727. [Google Scholar] [CrossRef]
  14. Zhao, Y.; Lai, G.S.; Li, C.; Wang, R. Acid-resistant polyamine hollow fiber nanofiltration membrane for selective separation of heavy metals and phosphorus. Chem. Eng. J. 2023, 453, 139825. [Google Scholar] [CrossRef]
  15. Cheng, Z.; Zhang, Y.; Chen, K.; Xiao, K.; Yin, Y. Preparation and properties of phosphinic acid–functionalized polyacrylonitrile hollow fiber membrane for heavy metal adsorption. Environ. Sci. Poll. Res. 2023, 30, 31408–31420. [Google Scholar] [CrossRef]
  16. Arguillarena, A.; Margallo, M.; Arruti-Fernández, A.; Pinedo, J.; Gómez, P.; Ortiz, I.; Urtiaga, A. Circular economy in hot-dip galvanizing with zinc and iron recovery from spent pickling acids. RSC Adv. 2023, 13, 6481–6489. [Google Scholar] [CrossRef] [PubMed]
  17. Suren, S.; Punyain, W.; Maneeintr, K.; Nootong, K.; Pancharoen, U. The simultaneous elimination of arsenic and mercury ions via hollow fiber supported liquid membrane and their reaction mechanisms: Experimental and modeling based on DFT and generating function. Arabian J. Chem. 2023, 16, 104501. [Google Scholar] [CrossRef]
  18. Traiwongsa, N.; Suren, S.; Pancharoen, U.; Nootong, K.; Maneeintr, K.; Punyain, W.; Lothongkum, A.W. Mechanisms of mercury ions separation by non-toxic organic liquid membrane via DFT, thermodynamics, kinetics and mass transfer model. J. Ind. Eng. Chem. 2023, 117, 522–537. [Google Scholar] [CrossRef]
  19. Gu, J.; Zang, H.; Yao, S.; Wang, X.; Zhu, M.; Song, H. Study on degradation of benzothiazolium-based ionic liquids by UV-H2O2. Appl. Sci. 2020, 10, 894. [Google Scholar] [CrossRef] [Green Version]
  20. Singh, S.K.; Savoy, A.W. Ionic liquids synthesis and applications: An overview. J. Mol. Liq. 2020, 297, 112038. [Google Scholar] [CrossRef]
  21. Ahrenberg, M.; Beck, M.; Neise, C.; Keßler, O.; Kragl, U.; Verevkin, S.P.; Schick, C. Vapor pressure of ionic liquids at low temperatures from AC-chip-calorimetry. Phys. Chem. Chem. Phys. 2016, 18, 21381–21390. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  22. Wu, H.B.; Zhang, B.; Liu, S.-H.; Chen, C.-C. Flammability estimation of 1-hexyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide. J. Loss Prev. Process Ind. 2020, 66, 104196. [Google Scholar] [CrossRef]
  23. Chiappe, C.; Margari, P.; Mezzetta, A.; Pomelli, C.S.; Koutsoumpos, S.; Papamichael, M.; Giannios, P.; Moutzouris, K. Temperature effects on the viscosity and the wavelength-dependent refractive index of imidazolium-based ionic liquids with a phosphorus containing anion. Phys. Chem. Chem. Phys. 2017, 19, 8201–8209. [Google Scholar] [CrossRef] [PubMed]
  24. Mezzetta, A.; Perillo, V.; Guazzelli, L.; Chiappe, C. Thermal behavior analysis as a valuable tool for comparing ionic liquids of different classes. J. Therm. Anal. Calor. 2019, 38, 3335–3345. [Google Scholar] [CrossRef]
  25. Zhang, Q.; Cai, S.; Zhang, W.; Lan, Y.; Zhang, X. Density, viscosity, conductivity, refractive index and interaction study of binary mixtures of the ionic liquid 1–ethyl–3–methylimidazolium acetate with methyldiethanolamine. J. Mol. Liq. 2017, 233, 471–478. [Google Scholar] [CrossRef]
  26. Becherini, S.; Mezzetta, A.; Chiappe, C.; Guazzelli, L. Levulinate amidinium protic ionic liquids (PILs) as suitable media for the dissolution and levulination of cellulose. New J. Chem. 2019, 43, 4554–4561. [Google Scholar] [CrossRef]
  27. Karmakar, A.; Mukundan, R.; Yang, P.; Batista, E.R. Solubility model of metal complex in ionic liquids from first principle calculation. RSC Adv. 2019, 9, 18506–18526. [Google Scholar] [CrossRef]
  28. Bystrzanowska, M.; Pena-Pereira, F.; Marcinkowski, L.; Tobiszewski, L. How green are ionic liquids?—A multicriteria decision analysis approach. Ecotox. Environ. Safety 2019, 174, 455–458. [Google Scholar] [CrossRef]
  29. Marcionilio, S.M.L.O.; Araújo, D.M.; Nascimento, T.V.; Martínez-Huitle, C.A.; Linares, J.L. Evaluation of the toxicity reduction of an ionic liquid solution electrochemically treated using BDD films with different sp3/sp2 ratios. Electrochem. Comm. 2020, 118, 106792. [Google Scholar] [CrossRef]
  30. Castillo-Ramírez, C.; Janssen, C.H.C. Pseudo-protic ionic liquids for the extraction of metals relevant for urban mining. Ind. Eng. Chem. Res. 2023, 62, 627–636. [Google Scholar] [CrossRef]
  31. Kobrak, M.N.; Yager, K.G. X-Ray scattering and physicochemical studies of trialkylamine/carboxylic acid mixtures: Nanoscale structure in pseudoprotic ionic liquids and related solutions. Phys. Chem. Chem. Phys. 2018, 20, 18639–18646. [Google Scholar] [CrossRef] [PubMed]
  32. Patsos, N.; Lewis, K.; Picchioni, F.; Kobrak, M.N. Extraction of acids and bases from aqueous phase to a pseudoprotic ionic liquid. Molecules 2019, 24, 894. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  33. Alguacil, F.J.; Robla, J.I. On the use of pseudo-protic ionic liquids to extract gold(III) from HCl solutions. Int. J. Mol. Sci. 2023, 24, 6305. [Google Scholar] [CrossRef] [PubMed]
  34. Wing, Q.; Shi, Y.; Yang, D.; Ning, P. Extraction of phenol from water with primary amine Primene JMT. Emerg. Contam. 2022, 8, 90–96. [Google Scholar] [CrossRef]
  35. Bohrer, M.P. Diffusional boundary layer resistance for membrane transport. Ind. Eng. Chem. Fundam. 1983, 22, 72–78. [Google Scholar] [CrossRef]
  36. Alguacil, F.J.; Martinez, S. Permeation of iron(III) by an immobilised liquid membrane using Cyanex 923 as mobile carrier. J. Membr. Sci. 2000, 176, 249–255. [Google Scholar] [CrossRef]
  37. Neplenbroek, A.M.; Bargeman, D.; Smolders, C.A. Mechanism of supported liquid membrane degradation: Emulsion formation. J. Membr. Sci. 1992, 67, 133–148. [Google Scholar] [CrossRef] [Green Version]
  38. Shukla, J.P.; Misra, S.K. Carrier-mediated transport of uranyl ions across tributyl phosphate—Dodecane liquid membranes. J. Membr. Sci. 1991, 64, 93–102. [Google Scholar] [CrossRef]
  39. Gupta, S.K.; Rathore, N.S.; Sonawane, J.V.; Pabby, A.K.; Janardan, P.; Changrani, R.D.; Dey, P.K. Dispersion-free solvent extraction of U(VI) in macro amount from nitric acid solutions using hollow fiber contactor. J. Membr. Sci. 2007, 300, 131–136. [Google Scholar] [CrossRef]
  40. El Aamrani, F.Z.; Kumar, A.; Sastre, A.M. Kinetic modelling of the active transport of copper(II) across a liquid membrane using thiourea derivatives immobilized on microporous hydrophobic supports. New J. Chem. 1999, 23, 517–523. [Google Scholar] [CrossRef]
  41. Prasad, R.; Kiani, A.; Bhave, R.R.; Sirhar, K.K. Further studies on solvent extraction with immobilized interfaces in a microporous hydrophobic membrane. J. Membr. Sci. 1986, 26, 79–97. [Google Scholar] [CrossRef]
  42. Kumar, A.; Haddad, R.; Alguacil, F.J.; Sastre, A.M. Comparative performance of non-dispersive solvent extraction using a single module and the integrated membrane process with two hollow fiber contactors. J. Membr. Sci. 2005, 248, 1–14. [Google Scholar] [CrossRef]
  43. Urtiaga, A.M.; Ortiz, M.I.; Salazar, E.; Irabien, J.A. Supported liquid membrane for the separation-concentration of phenol. I. Viablility and mass-transfer evaluation. Ind. Eng. Che. Res. 1992, 31, 877–886. [Google Scholar] [CrossRef]
  44. Kumar, A.; Haddad, R.; Benzal, G.; Sastre, A.M. Use of modified membrane carrier system for recovery of gold cyanide from alkaline cyanide media using hollow fiber supported liquid membranes: Feasibility studies and mass transfer modelling. J. Membr. Sci. 2000, 174, 17–30. [Google Scholar] [CrossRef]
  45. Kumar Pabby, A.; Haddad, R.; Alguacil, F.J.; Sastre, A.M. Improved kinetics-based gold cyanide extraction with mixture of LIX 79 + TOPO utilizing hollow fiber membrane contactors. Chem. Eng. J. 2004, 100, 11–22. [Google Scholar] [CrossRef]
  46. Alguacil, F.J.; Alonso, M.; Lopez, F.; Lopez-Delgado, A. Uphill permeation of Cr(VI) using Hostarex A327 as ionophore by membrane-solvent extraction processing. Chemosphere 2008, 72, 684–689. [Google Scholar] [CrossRef]
Figure 1. Presence of iron(III) in tap water due to degradation of pipelines (picture Alguacil and Robla).
Figure 1. Presence of iron(III) in tap water due to degradation of pipelines (picture Alguacil and Robla).
Membranes 13 00723 g001
Figure 2. View of the hollow fiber module operating in the recycling mode of the phases. (1) Hollow fiber membrane contactor, (2) feed phase tank, and (3) pseudo-emulsion phase tank. Red colour: feed phase flow. Green colour: pseudo-emulsion phase flow.
Figure 2. View of the hollow fiber module operating in the recycling mode of the phases. (1) Hollow fiber membrane contactor, (2) feed phase tank, and (3) pseudo-emulsion phase tank. Red colour: feed phase flow. Green colour: pseudo-emulsion phase flow.
Membranes 13 00723 g002
Figure 3. Plot of log DH2SO4 versus log [PJMT]org. The dotted line shows the 95% confidence interval of the regression line. Experimental conditions as in the text and Table 2.
Figure 3. Plot of log DH2SO4 versus log [PJMT]org. The dotted line shows the 95% confidence interval of the regression line. Experimental conditions as in the text and Table 2.
Membranes 13 00723 g003
Figure 4. Plot of ln([Fe]f,t/[Fe]f,0) versus time at various initial sulphuric acid concentrations in the feed phase. Feed phase flow: 300 cm3/min. Pseudo-emulsion flow: 100 cm3/min. Temperature: 20 °C.
Figure 4. Plot of ln([Fe]f,t/[Fe]f,0) versus time at various initial sulphuric acid concentrations in the feed phase. Feed phase flow: 300 cm3/min. Pseudo-emulsion flow: 100 cm3/min. Temperature: 20 °C.
Membranes 13 00723 g004
Figure 5. Iron(III) transport at various initial metal concentrations in the feed phase. Temperature: 20 °C.
Figure 5. Iron(III) transport at various initial metal concentrations in the feed phase. Temperature: 20 °C.
Membranes 13 00723 g005
Figure 6. Variation with time of ln([Fe]f,t/[Fe]f,0) at various PPIL concentrations. Feed phase flow: 300 cm3/min. Pseudo-emulsion flow: 100 cm3/min. Temperature: 20 °C.
Figure 6. Variation with time of ln([Fe]f,t/[Fe]f,0) at various PPIL concentrations. Feed phase flow: 300 cm3/min. Pseudo-emulsion flow: 100 cm3/min. Temperature: 20 °C.
Membranes 13 00723 g006
Table 1. Specifications of the hollow fiber module.
Table 1. Specifications of the hollow fiber module.
Contactor length28 cm
Contactor diameter8 cm
Active area (A)1.4 m2
Number of fibers (n)10,000
Fiber internal diameter (di)24·10−3 cm
Fiber outer diameter (do)30·10−3 cm
Fiber wall thickness (dorg)3.0·10−2 cm
Fiber length (L)15 cm
Porosity (ε)30%
Tortuosity (τ)3
Pore size3.0·10−6 cm
Polymeric material3.0·10−6 cm
Table 2. Generation of the pseudo-protic ionic liquid (Equation (5)).
Table 2. Generation of the pseudo-protic ionic liquid (Equation (5)).
[Amine], MDH2SO4
0.0680.072
0.140.16
0.270.36
0.541.1
Temperature: 20 °C. Equilibration time: 10 min. O/A ratio: 1.
Table 3. Overall permeation coefficients at various feed phase flows.
Table 3. Overall permeation coefficients at various feed phase flows.
Feed Flow, cm3/minP, cm/min
752.1·10–3
1504.1·10−3
3006.9·10−3
4004.7·10−3
Pseudo-emulsion phase flow: 100 cm3/min. Temperature: 20 °C.
Table 4. Influence of the sulphuric acid concentration in the strip solution on iron(III) permeation.
Table 4. Influence of the sulphuric acid concentration in the strip solution on iron(III) permeation.
[H2SO4], MP, cm/min[Fe]st, g/La % Rst
0.59.9·10−41.450
1.51.5·10−32.972
32.8·10−34.275
Feed phase flow: 300 cm3/min. Pseudo-emulsion phase flow: 100 cm3/min. Temperature: 20 °C. a After 105 min.
Table 5. Variation of iron(III) permeation coefficient and initial flux at various initial metal concentrations in the feed phase.
Table 5. Variation of iron(III) permeation coefficient and initial flux at various initial metal concentrations in the feed phase.
[Fe]f,0, g/LP, cm/minJ, mol/cm2·min[Fe]st, g/La % Rst
0.019.6·10−31.7·10−90.0684
0.17.5·10−31.3·10−80.4580
12.8·10−35.0·10−84.275
Experimental conditions as in Figure 5. a After 105 min.
Table 6. Iron(III) permeation coefficients at various carrier concentrations in the organic solution.
Table 6. Iron(III) permeation coefficients at various carrier concentrations in the organic solution.
[PPIL], MP, cm/mina % Rst
0.0276.6·10−380
0.0688.1·10−382
0.149.6·10−384
0.271.8·10−284
0.541.3·10−285
0.811.1·10−283
Experimental conditions as in Figure 6. Temperature: 20 °C. a After 105 min.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Alguacil, F.J.; Robla, J.I. Iron Control in Liquid Effluents: Pseudo-Emulsion Based Hollow Fiber Membrane with Strip Dispersion Technology with Pseudo-Protic Ionic Liquid (RNH3+HSO4) as Mobile Carrier. Membranes 2023, 13, 723. https://doi.org/10.3390/membranes13080723

AMA Style

Alguacil FJ, Robla JI. Iron Control in Liquid Effluents: Pseudo-Emulsion Based Hollow Fiber Membrane with Strip Dispersion Technology with Pseudo-Protic Ionic Liquid (RNH3+HSO4) as Mobile Carrier. Membranes. 2023; 13(8):723. https://doi.org/10.3390/membranes13080723

Chicago/Turabian Style

Alguacil, Francisco Jose, and Jose Ignacio Robla. 2023. "Iron Control in Liquid Effluents: Pseudo-Emulsion Based Hollow Fiber Membrane with Strip Dispersion Technology with Pseudo-Protic Ionic Liquid (RNH3+HSO4) as Mobile Carrier" Membranes 13, no. 8: 723. https://doi.org/10.3390/membranes13080723

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop