1. Introduction
The durability of building envelope materials is a critical factor in long-term building performance and service life [
1]. As mentioned in CSA S478 (2019), modern buildings are typically designed for service lives of 50–99 years, during which envelope materials are exposed to various environmental stressors such as temperature cycles, moisture gradients, and chemical aging [
2,
3]. Among envelope protection systems, polymer-based waterproofing membranes are widely used due to their flexibility and chemical and moisture resistance [
4]; however, their durability remains a concern, particularly under aggressive chemical and hygrothermal environments. Silicone-based materials have been extensively used in construction since their introduction in the 1950s [
5], initially as joint sealants [
6,
7] and later as surface coatings and waterproofing membranes [
8,
9,
10]. Silicone materials are valued for their elasticity, high UV resistance, and stability under thermal cycling [
11]. Fluid-applied silicone membranes extend these advantages to large-area envelope protection systems by forming seamless vapor-permeable barriers suitable for façades and roofing assemblies. Despite these favorable properties, silicone polymers are still susceptible to long-term chemical and physical aging under aggressive environmental conditions [
12].
The durability of silicone materials is governed primarily by the stability of the siloxane (Si–O–Si) backbone, which can undergo hydrolytic or chemically induced chain scission when exposed to moisture, temperature fluctuations, and ionic species. In particular, hydrolysis reactions can be accelerated in environments with extreme pH levels, leading to polymer chain degradation, surface hardening, and loss of mechanical flexibility. Previous studies and manufacturer guidelines indicate that silicone sealants and coatings may be particularly vulnerable to hydrolytic degradation when exposed to environments with extreme pH conditions [
13]. In strongly alkaline or acidic media, the siloxane network can be attacked by reactive chemical species, leading to depolymerization and reduced mechanical integrity [
14]. More recently, Masson et al. [
12] demonstrated that exposure of silicone membranes to a highly alkaline solution simulating concrete pore conditions led to progressive changes in surface and bulk morphology, chemical structure, and toughness, confirming the susceptibility of silicone membranes to strongly alkaline aqueous environments. The susceptibility of silicone polymers to chemical degradation depends on service conditions and the adjacent microenvironment, including temperature, moisture, exposure duration, and substrate chemistry. Consequently, understanding substrate–polymer interactions is essential for assessing compatibility and hence predicting the long-term durability of silicone-based waterproofing systems.
Hempcrete has emerged as a promising low-carbon building material for thermal insulation and envelope applications [
15,
16]. Hempcrete is a bio-composite produced by combining hemp shives with mineral binders, most commonly lime-based systems. The material is characterized by high porosity, low thermal conductivity, and strong hygroscopic moisture buffering capacity [
17]. From a sustainability perspective, hempcrete offers significant environmental advantages due to the carbon sequestration potential of hemp cultivation and the carbonation reactions associated with lime hardening [
16].
The performance of hempcrete is governed by the combined effects of binder chemistry and the composition of hemp shives. Binder type dictates the dominant reaction mechanisms, pore solution chemistry, and pH environment. Air lime (hydrated lime) hardens primarily through carbonation with atmospheric CO
2, resulting in high vapor permeability but relatively low early mechanical strength [
16]. In contrast, natural hydraulic lime (NHL) and Ordinary Portland cement (OPC) undergo hydraulic reactions in addition to carbonation, leading to higher early strength and improved mechanical performance [
18]. These differences in reaction pathways also influence the pore solution chemistry and moisture transport behavior of the composite.
In parallel, the chemical composition of hemp shives, including cellulose, hemicellulose, lignin, and other extractives, can further modify the microenvironment, particularly when influenced by pre-treatment or degradation processes [
19]. The interaction between binder and shives therefore defines the physicochemical environment of hempcrete, controlling pore structure, moisture dynamics, and interfacial characteristics. Consequently, these factors directly influence the conditions at the membrane–substrate interface, including local pH, ionic transport, and moisture state, which are critical to the long-term durability of polymeric waterproofing membranes, particularly silicone-based systems.
Despite increasing adoption of hempcrete in sustainable construction, limited understanding exists regarding the compatibility of polymer waterproofing membranes with lime-based bio-composites. Existing studies on silicone durability primarily focus on simplified alkaline environments or concrete systems, while the combined effects of moisture, ion-rich leachates, and bio-based substrates remain poorly understood. In particular, the role of interfacial moisture–ion interactions and fiber treatment in governing membrane degradation has not been systematically investigated. This knowledge gap is especially important because the high porosity, moisture transport capacity, and chemically active binder system of hempcrete may create interfacial conditions that affect the long-term durability of adjacent polymeric membranes. Therefore, membrane–hempcrete compatibility represents an important durability issue for bio-based envelope systems.
In this study, the long-term durability and chemical stability of a commercially available silicone-based fluid-applied membrane were investigated when applied to hempcrete substrates, with a specific focus on the effect of shiv pre-treatment. Hempcrete samples were produced in the lab using a hydrated lime binder and hemp shives, both non-treated and hydrothermally pre-treated, to assess the influence of shiv chemistry on interfacial conditions. Membrane specimens were subjected to accelerated hygrothermal aging under dry and wet conditions across a temperature range of 22 °C to 90 °C for up to 9 months, simulating realistic service scenarios, including moisture condensation, capillary water transport, and thermal cycling. Membrane degradation was characterized using thermal analysis, chemical spectroscopy, and microstructural imaging techniques. The work aims to elucidate the role of shiv modification in governing silicone membrane performance and to support the design of durable, bio-based building envelope systems.
3. Results and Discussion
3.1. pH Measurements
The evolution of pH in the aqueous suspensions in contact with hempcrete specimens stored under wet conditions at RT is presented in
Figure 2. The suspension was initially tap water; however, its pH changed over time due to the progressive release of leachates from the hempcrete. The results indicate that the pH of the surrounding environment increased rapidly to approximately 11 within the first two days due to leaching from the hempcrete and remained relatively stable thereafter, indicating a consistently strong alkaline system (pH 11–12). Due to rapid mold growth on the hempcrete specimens at RT, with visible fungal development within ~14 days, long-term exposure and subsequent characterization were discontinued due to safety concerns. Nevertheless, the high pH indicates that the alkalinity of the system is primarily controlled by the dissolution of hydroxide-bearing phases in the binder.
The average pH values of the suspensions at elevated temperatures for both non-treated (HWNT) and treated (HWT) hempcrete are shown in
Figure 3, while the corresponding weekly measurements are included in the
Supplementary Materials. For these conditions, aging was conducted over an extended period of up to 9 months, and the reported values represent the weekly average of pH measurements collected throughout this period. The results indicate that temperature and shiv treatment have a pronounced effect on leachate chemistry, which in turn influences pH. At 50 °C, the pH of HWNT samples was 10.4 ± 0.3, while HWT samples exhibited a higher pH of 11.8 ± 0.4. A similar trend, with treated samples showing higher alkalinity, was observed at 70 °C, where pH values were 10.6 ± 0.3 for HWNT and 11.2 ± 0.2 for HWT. However, increasing the temperature to 90 °C resulted in a substantial decrease in pH for both materials, reaching 8.9 ± 0.2 for HWNT and 9.0 ± 0.1 for HWT.
The chemistry of the suspension is influenced by two competing mechanisms: (i) continued leaching of alkaline species from the hydrated binder, and (ii) increased release of acidic organic compounds from hemp shives. These include hemicellulose- and lignin-derived compounds, which contribute to a reduction in pH. This was evidenced by the yellowish color of the suspension leached out of the hempcrete (
Figure 4). The combined effect of these opposing processes results in a moderate decrease in alkalinity for samples aged under 50 °C and 70 °C compared to RT conditions. Treated hempcrete samples consistently exhibited slightly higher pH values than non-treated samples across these temperatures. This behavior is attributed to the removal of a portion of acidic extractives during pre-treatment, thereby reducing their contribution to the leachate chemistry and allowing the alkaline binder phases to dominate.
At 90 °C, the influence of acidic extractives becomes dominant for both treated and non-treated samples, leading to a marked reduction in pH. This behavior may be attributed to accelerated thermal degradation of hemp shiv constituents, particularly hemicellulose, which can release organic acids such as acetic acid, as well as other low-molecular-weight and phenolic compounds [
22]. As a result, the leachate chemistry shifts from binder-dominated alkalinity toward a stronger contribution from thermally generated organic species, causing the pH to drop to mildly alkaline conditions (≈8–9). The similar pH range observed for treated and non-treated samples at 90 °C suggests that, at this temperature, newly generated degradation products may outweigh the initial reduction in soluble extractives achieved by hydrothermal treatment.
3.2. Thermogravimetric Analysis
TGA and derivative thermogravimetric (DTG) analyses of membranes exposed to hempcrete under dry conditions are presented for both non-treated and treated systems in
Figure 5 and
Figure 6, respectively. The control (non-aged) membrane shows two characteristic decomposition stages typical of silicone-based materials. The primary mass-loss event, with DTG peak at approximately 428 °C, is attributed to degradation of the PDMS network through Si–O bond cleavage and the evolution of volatile cyclic siloxane species [
23]. A secondary multi-step decomposition occurs at higher temperatures, with DTG peaks in a range of 625 to 702 °C, corresponding to the thermal dissociation of calcium carbonate (CaCO
3) fillers. The remaining residue at elevated temperatures is associated with thermally stable inorganic components, such as titanium dioxide (TiO
2), which do not undergo significant decomposition within the tested range. Membranes aged in contact with hempcrete under dry conditions (HDNT and HDT) exhibit negligible changes in their TGA/DTG profiles, even after prolonged exposure (up to 9 months). This indicates that thermal exposure alone, up to 90 °C, does not induce any significant chemical or structural alteration of the membrane when in contact with the hempcrete surface. This also suggests that degradation mechanisms such as depolymerization or chain scission are not activated under dry conditions. This behavior can be attributed to the high bond energy of the Si–O backbone in PDMS, which confers intrinsic thermal stability, and to the absence of moisture, which suppresses hydrolytic pathways and limits ionic mobility at the membrane–substrate interface [
24].
TGA/DTG analyses of membranes exposed to hempcrete under wet conditions (HWNT and HWT), presented in
Figure 7 and
Figure 8, reveal severe degradation compared to the control and dry-aged samples. Irrespective of aging temperature (50, 70, or 90 °C) or shives pre-treatment condition of the hempcrete, the characteristic DTG peak associated with the PDMS backbone (~430 °C) is significantly reduced or nearly absent. This observation indicates extensive degradation of the siloxane network, suggesting substantial disruption of the polymer structure during exposure to moisture-conditioned hempcrete. At the same time, the intensity of the high-temperature DTG peak attributed to carbonate decomposition (≈700–730 °C) increased markedly, accompanied by a higher residual mass at the end of the test, which suggests the deposition of thermally stable inorganic phases on the membrane surface.
These observations indicate that the degradation of the membrane is governed by chemically aggressive interactions with the hempcrete leachate under wet conditions. While the measured pH of the leachates ranged from moderately to highly alkaline (pH ≈ 9–11), the extent of degradation does not correlate directly with alkalinity alone. Significant degradation was observed even in samples exposed to lower pH conditions (≈9), suggesting that hydroxyl concentration is not the sole controlling factor. Instead, the results suggest that degradation is driven by a coupled moisture–ion mechanism, in which dissolved species such as Ca2+ and Mg2+, abundant in the hydrated binder, may contribute to interfacial reactions.
In aqueous environments, hydroxyl ions (OH
−) initiate nucleophilic attack on the siloxane (Si–O–Si) backbone, leading to bond cleavage and the formation of silanol groups (Si–OH) [
25]. This hydrolysis process is reported to be accelerated in the presence of divalent cations such as Ca
2+ and Mg
2+, although their specific contribution cannot be isolated in the present hempcrete-contact system. These cations act as Lewis acids, coordinating with oxygen atoms in the siloxane network and increasing the polarization of the Si–O bond, rendering the silicon center more susceptible to nucleophilic attack. This interaction lowers the activation energy required for bond cleavage and promotes depolymerization of the PDMS network into lower-molecular-weight species. Consequently, the combined effects of moisture, hydroxyl ions, and divalent cations result in rapid destabilization and breakdown of the polymer backbone, even under moderate alkaline conditions. This interpretation is consistent with previous studies, which have shown that PDMS degradation in alkaline environments is not governed solely by pH, but is strongly influenced by the nature of the cations present. In particular, Ca
2+ has been reported to promote significantly higher degradation rates compared to Na
+, even at similar pH levels, indicating a catalytic effect of divalent cations on siloxane bond cleavage and depolymerization processes [
25].
In addition to polymer degradation, the increased intensity of carbonate-related DTG peaks and higher residual mass indicate secondary mineral deposition on the membrane surface. In calcium-rich leachates, dissolved Ca2+ can react with carbonate species (e.g., CO32− formed via dissolution of atmospheric CO2) to precipitate calcium carbonate (CaCO3). These precipitates accumulate on the membrane surface, contributing to the increased residual mass observed in TGA and the enhanced peaks in the 700–730 °C range. Such mineral deposits may further influence degradation by modifying the local chemical environment and promoting localized reactions at the polymer–hempcrete interface.
Overall, the results demonstrate that membrane degradation under wet exposure conditions is controlled by coupled physicochemical processes, in which moisture-driven hydrolysis and ion-assisted chemical reactions act synergistically rather than by alkalinity alone. Water facilitates the transport and accessibility of reactive species. Dissolved ions, particularly divalent cations, may further modify the interfacial chemistry and contribute to siloxane bond cleavage. This interplay highlights the critical role of leachate composition in controlling reaction kinetics and pathways, particularly the presence of divalent cations, underscoring that the long-term stability of silicone-based membranes in contact with hempcrete is strongly dependent on the combined effects of moisture state and ionic environment. Further work involving controlled solution-based experiments at constant pH with systematically varied Ca2+ and Mg2+ concentrations is required to quantitatively isolate their individual effects on silicone degradation.
3.3. Fourier-Transform Infrared
Figure 9 shows the FTIR spectra of membranes aged in contact with both non-treated and treated hempcrete (HDNT and HDT) under dry conditions. The spectra for the control membrane exhibit characteristic PDMS absorption bands, including peaks at ~2960 cm
−1 (C–H stretching of CH
3 groups), 1260 cm
−1 (Si–CH
3 bending), and 800 cm
−1 (Si–CH
3 rocking). The strong bands in the 1000–1100 cm
−1 region correspond to Si–O–Si stretching vibrations, with contributions from Si–O–C linkages [
26]. In addition, the presence of the ~1440 cm
−1 band in the control sample confirms that calcium carbonate is an inherent filler in the membrane formulation.
Consistent with the TGA results, no significant structural changes are observed for membranes aged in contact with either non-treated or treated hempcrete (HDNT and HDT) under dry conditions, as evidenced by the strong overlap between the aged and control spectra. This indicates that, in the absence of moisture, prolonged contact with hempcrete does not induce degradation of the silicone membrane, and its structural integrity, and thus durability, is preserved.
In contrast,
Figure 10 shows clear chemical changes in membranes exposed to wet hempcrete.
Table 3 also summarizes the presence and intensity of the main FTIR bands, while
Table 4 provides their chemical assignments. The appearance of O–H (~3450 cm
−1) and H–O–H (~1640 cm
−1) bands confirms moisture uptake across all samples under wet exposure. This is accompanied by attenuation or partial disappearance of PDMS-related bands (1260, 1100–1000, and ~790 cm
−1), indicating degradation of the siloxane network. These changes generally become more pronounced with increasing exposure time and temperature, although some spectral variability is observed due to surface heterogeneity and mineral deposition. The persistent carbonate-related band at ~1440 cm
−1 further supports the presence of calcium carbonate filler and/or secondary carbonate deposition at the membrane surface. Compared with HWNT samples, HWT samples generally retain PDMS-related bands more consistently, suggesting that hydrothermal treatment slightly reduces leachate aggressiveness, likely through partial removal of soluble extractives. Overall, the FTIR results are consistent with the TGA results, where attenuation of siloxane-related bands corresponds to the reduction or disappearance of the characteristic PDMS decomposition peak (~430 °C). These findings confirm that wet exposure promotes degradation of the silicone membrane, while hemp shiv treatment mitigates but does not prevent this process.
3.4. Differential Scanning Calorimetry (DSC)
DSC results for membranes exposed under dry conditions are presented in
Figure 11. However, no measurable differences were observed relative to the control sample, indicating that thermal exposure alone does not alter the structure or thermal behavior of the silicone membrane. In contrast, membranes exposed to hempcrete under wet conditions exhibit clear and progressive changes in their thermal response, as shown in
Figure 12. The control sample displays a distinct melting transition (T
m) at approximately −41 °C and a crystallization transition (T
c) near −68 °C, characteristic of silicone elastomers [
27]. Upon wet exposure, these thermal transitions become progressively less defined with increasing aging duration, exhibiting noticeable reductions at 3 months and significant attenuation and broadening at 6 and 9 months. This effect is further pronounced at elevated temperatures (70–90 °C), indicating that temperature acts as an accelerating factor for degradation processes rather than the primary driving mechanism. The suppression and broadening of these thermal transitions reflect a reduction in polymer chain mobility and integrity. This behavior can be attributed to two concurrent mechanisms. First, chemical degradation of the siloxane backbone through hydrolysis and depolymerization in the presence of moisture and ion-rich leachates, leading to chain scission and molecular weight reduction. Secondly, physical restriction of chain mobility due to the formation and accumulation of inorganic deposits at or near the membrane surface, which impose additional constraints on segmental motion.
Overall, the progressive loss of the characteristic PDMS thermal signature with increasing exposure severity is consistent with FTIR evidence of siloxane bond cleavage and TGA results showing the disappearance of the PDMS decomposition peak. This agreement confirms that membrane deterioration is governed by coupled moisture–chemical interactions, with temperature primarily enhancing reaction kinetics rather than independently inducing degradation.
3.5. Optical Micrographs
Figure 13 presents the optical micrographs of the non-aged silicone membrane surfaces, showing a relatively uniform surface with minor irregularities such as wrinkles and small blister-like features arising from the coating application process. In comparison,
Figure 14 shows membranes aged under dry conditions (HDNT and HDT), which exhibit no significant morphological changes relative to the control, indicating that the surface remains largely unchanged after aging. Any observed color variations across the images are attributed to imaging conditions rather than actual material differences. Similar features are observed in the dry-aged samples, with no systematic changes in morphology or surface integrity. Any slight roughness detected appears random and unrelated to exposure conditions. Overall, the membrane maintains a smooth and continuous surface across all temperatures, indicating that dry contact with hempcrete does not induce detectable surface degradation. This observation is consistent with the absence of chemical and thermal changes identified by FTIR, TGA, and DSC analyses.
Optical micrographs of silicone membranes exposed to wet hempcrete, illustrated in
Figure 15, reveal clear surface modifications compared to the control and dry-aged samples. Wet-exposed specimens exhibit increased heterogeneity, including the formation of particulate deposits, irregular clusters, and localized surface disruptions. These features become more pronounced with increasing exposure time and temperature, with evidence of micro-scale roughening and the development of crystalline or granular structures distributed across the surface. The morphology suggests both occasional surface deposition and modifications of the underlying polymer structure.
These observations are consistent with the chemical and thermal changes identified by the complementary techniques presented in the previous sections. The presence of particulate and crystalline features aligns with FTIR results showing persistent or enhanced carbonate-related bands and TGA results indicating an increase in inorganic residue, supporting the occurrence of mineral deposition from ion-rich leachates. At the same time, the loss of surface uniformity and emergence of micro-scale defects are indicative of polymer degradation, consistent with the attenuation of PDMS-related FTIR peaks and the suppression of thermal transitions observed in DSC.
3.6. Scanning Electron Microscopy Images
Figure 16 shows the SEM-EDS analysis of the control membrane, exhibiting a generally uniform and homogeneous surface morphology without evidence of deposits or degradation features. The observed void is attributed to an application-induced artifact formed during the multi-layer coating process. The EDS spectrum confirms the expected composition of a PDMS-based system, with Si and O as the primary elements, while Ca and Ti indicate the presence of mineral fillers, consistent with FTIR and TGA observations.
As shown in
Figure 17, SEM observations reveal pronounced surface modification of the silicone membrane following wet exposure to hempcrete, evident even after 1 month of aging. The highest exposure temperature (90 °C) was selected to accentuate morphological changes and capture the most representative degradation features under HWNT-90-1-month and HWT-90-1-month conditions. Images at increasing magnification show the development of surface deposits and morphological changes, including dense crystalline coverage, heterogeneous surface features, and elongated prismatic crystals. Under these conditions, the membrane surface is partially to extensively covered by prismatic and angular crystalline deposits, accompanied by finer granular phases distributed across the surface. At higher magnifications, these features appear as well-defined faceted crystals with clear evidence of aggregation and localized clustering, indicating in situ nucleation and growth on the membrane surface. This behavior suggests that dissolved ionic species released from hempcrete, particularly Ca
2+ and carbonate species, supersaturate the interfacial suspension and precipitate as mineral phases, such as calcium carbonate, directly onto the membrane.
In addition to mineral deposition, regions exhibiting surface irregularities and localized disruption are observed, suggesting that physical deposition is accompanied by alteration of the underlying polymer matrix. The coexistence of crystalline deposits and disrupted regions suggests a coupled mechanism in which interfacial precipitation and moisture-driven chemical degradation occur simultaneously. Although calcium carbonate deposits are not expected to directly participate in siloxane bond cleavage, their accumulation on the membrane surface may indirectly influence the interfacial environment by altering moisture retention, ion accumulation, and local mass transport pathways. These deposits may therefore promote heterogeneous exposure conditions by retaining moisture and concentrating dissolved ionic species near the membrane surface, while the chemical destabilization of the silicone network is primarily attributed to moisture-enabled hydrolysis and ion-assisted reactions involving dissolved divalent cations. This interplay between mineral deposition and polymer degradation highlights the dynamic nature of the membrane–substrate interface under wet conditions, where both chemical reactions and physicochemical transport processes govern the observed morphology.
EDS analysis of the elongated prismatic crystalline features (
Figure 18), which were seen in both non-treated and treated samples, shows that these deposits are primarily composed of Ca, O, and C, consistent with calcium-based mineral phases, most likely calcium carbonate. The negligible contribution of Si in these regions confirms that the deposits are not part of the original silicone matrix but are externally formed phases. This interpretation is strongly supported by FTIR results, which show carbonate-related absorption bands, and by TGA data indicating an increase in inorganic residue following exposure. The formation of these deposits is attributed to the precipitation of dissolved calcium species from the hempcrete leachate, driven by supersaturation and carbonation reactions in a moisture-rich environment.
The combined SEM–EDS observations further support the degradation mechanisms inferred from FTIR and DSC analyses. The loss of surface uniformity and the presence of disrupted regions are consistent with chemical degradation of the siloxane network, as evidenced by the attenuation of PDMS-related FTIR bands and the disappearance of the PDMS decomposition peak in TGA. Overall, these results demonstrate that wet exposure induces a coupled degradation process involving both mineral deposition and polymer breakdown, governed by moisture-driven ion transport and chemically reactive leachate conditions at the membrane interface.