Unveiling the Degradation Mechanism of Impermeability and Pore Structure in Concrete Under Long-Term Water Exposure
Abstract
1. Introduction
2. Material Proportions and Test Methods
2.1. Material Proportions
2.2. Analysis of Relative Permeability Coefficient Testing
2.3. Analysis of MIP Microporous Structure
2.4. Pore Parameter Testing
2.5. X-Ray Diffraction Phase Analysis
2.6. Microstructural Testing
3. Test Results and Analysis
3.1. Relative Permeability Test
3.2. Pore Structure Analysis
3.2.1. Analysis of Mercury Injection Test Results
3.2.2. Pore Parameter Analysis
3.3. Component and Phase Analysis
3.3.1. X-Ray Analysis
3.3.2. Microstructural Analysis
4. Conclusions
Author Contributions
Funding
Data Availability Statement
Conflicts of Interest
References
- Lei, B.; Li, W.; Li, Z.; Wang, G.; Sun, Z. Effect of cyclic loading deterioration on concrete durability: Water absorption, freeze-thaw, and carbonation. J. Mater. Civ. Eng. 2018, 30, 04018220. [Google Scholar] [CrossRef]
- Peng, Y.; Li, X.; Wang, W.; Ke, L.; Chuan, L. A simulation-based research on carbon emission mitigation strategies for green container terminals. Ocean Eng. 2018, 163, 288–298. [Google Scholar] [CrossRef]
- Kaloop, M.R.; Samui, P.; Iqbal, M.; Hu, J.W. Soft computing approaches towards tensile strength estimation of GFRP rebars subjected to alkaline-concrete environment. Case Stud. Constr. Mater. 2022, 16, e00955. [Google Scholar] [CrossRef]
- Yu, H.F.; Da, B.; Ma, H.Y.; Dou, X.M.; Wu, Z.Y. Service life prediction of coral aggregate concrete structure under island reef environment. Constr. Build. Mater. 2020, 246, 118390. [Google Scholar] [CrossRef]
- Zhang, K.; Zhou, J.; Yin, Z.G. Experimental Study on Mechanical Properties and Pore Structure Deterioration of Concrete Under Freeze-Thaw Cycles. Materials 2021, 14, 6568. [Google Scholar] [CrossRef] [PubMed]
- Kuosa, H.; Ferreira, R.M.; Holt, E.; Leivo, M.; Vesikari, E. Effect of coupled deterioration by freeze–thaw, carbonation and chlorides on concrete service life. Cem. Concr. Compos. 2014, 47, 32–40. [Google Scholar] [CrossRef]
- Shuang, N.; Chen, B.; Lu, X.; Tian, B.; Xiong, B.; Zhang, J. A chemo-transport-damage mesoscopic model quantifying the influence of ITZ for concrete under sulfate attack. Constr. Build. Mater. 2025, 494, 143335. [Google Scholar] [CrossRef]
- Zhang, G.-Y.; Tian, Y.; Tian, Z.S.; Zhao, R.-Y.; Huang, B.-T.; Li, Y.-J.; Li, B.; Chen, Z.-X. Role of ITZ and aggregates in concrete carbonation: Multiscale-coupled modeling and experimental validation. J. Build. Eng. 2025, 112, 113900. [Google Scholar] [CrossRef]
- Saetta, A.V.; Vitaliani, R.V. Experimental investigation and numerical modeling of carbonation process in reinforced concrete structures: Part I: Theoretical formulation. Cem. Concr. Res. 2005, 35, 958–967. [Google Scholar]
- Shi, X.; Zhang, C.; Wang, L.; Yao, Y. Numerical investigations on the influence of ITZ and its width on the carbonation depth of concrete with stress damage. Cem. Concr. Compos. 2022, 132, 104630. [Google Scholar] [CrossRef]
- Li, X.Y.; Li, Y.L.; Chen, J.H. Mechanical properties and pore structure evolution of hydraulic concrete under sustained low-temperature freezing. J. Build. Eng. 2025, 111, 113602. [Google Scholar] [CrossRef]
- Li, X.Y.; Liu, Y.F.; Guo, H.Y.; Li, Y. Investigation of the freeze-thaw deterioration behavior of hydraulic concrete under various curing temperatures. J. Build. Eng. 2024, 95, 110247. [Google Scholar] [CrossRef]
- Huang, Y.; Wu, X.; Fang, C.; Wang, X.; Liu, C.; Su, H. Study on water permeability of hydraulic concrete under freeze-thaw deterioration based on microscopic pore structure evolution. Constr. Build. Mater. 2025, 504, 144502. [Google Scholar] [CrossRef]
- Gu, L.; Zhao, J.; Yang, F.; Liu, S. Structure and properties of underwater non-dispersible concrete in seawater environment. J. Dalian Jiaotong Univ. 2018, 39, 104–108. [Google Scholar] [CrossRef]
- Wang, Y.; Song, Y.; Sun, X. Research Progress on Chloride Ion Transport Characteristics in Concrete under Marine Environments. J. Waterw. Harb. 2025, 46, 657–672. [Google Scholar]
- Hussain, Z.; Ansari, W.S.; Akbar, M.; Azam, A.; Lin, Z.; Yosri, A.M.; Shaaban, W.M. Microstructural and mechanical assessment of sulfate-resisting cement concrete over portland cement incorporating sea water and sea sand. Case Stud. Constr. Mater. 2024, 21, e03689. [Google Scholar] [CrossRef]
- Andrade, C. Steel corrosion rates in concrete in contact to sea water. Cem. Concr. Res. 2023, 165, 107085. [Google Scholar] [CrossRef]
- Patil, A.; Dwivedi, A.K. Mechanical strength and durability performance of sea water concrete incorporating supplementary cementitious materials in different curing conditions. Mater. Today Proc. 2022, 65, 969–974. [Google Scholar] [CrossRef]
- Benny, B.; Bazli, M.; Rajabipour, A.; Arashpour, M. Durability of tubular sea water sea sand concrete and fibre-reinforced polymer hybrid structures: Mechanisms and effective parameters: Critical overview and discussion. Constr. Build. Mater. 2023, 366, 130206. [Google Scholar] [CrossRef]
- Qi, X.; Huang, Y.; Li, X.; Hu, Z.; Ying, J.; Li, D. Mechanical Properties of Sea Water Sea Sand Coral Concrete Modified with Different Cement and Fiber Types. J. Renew. Mater. 2020, 8, 915–937. [Google Scholar] [CrossRef]
- Gan, L.; Zou, Z.Y.; Zhang, Z.L.; Zhang, H.; Gu, H.; Jin, H. Investigation on the evolution of concrete pore structure under freeze-thaw and fatigue loads. J. Build. Eng. 2024, 97, 110914. [Google Scholar] [CrossRef]
- Li, F.; Luo, D.M.; Niu, D.T. Durability evaluation of concrete structure under freeze-thaw environment based on pore evolution derived from deep learning. Constr. Build. Mater. 2025, 467, 140422. [Google Scholar] [CrossRef]
- SL/T 352-2020; Test Code for Hydraulic Concrete China. Water & Power Press: Beijing, China, 2020.
- ASTM C457/C457M-16; Standard Test Method for Microscopical Determination of Parameters of the Air-Void System in Hardened Concrete. ASTM International: West Conshohocken, PA, USA, 2016.
- JGJ 63-2006; Standard of Water for Concrete. China Architecture & Building Press: Beijing, China, 2006.
- SL 775-2018; Specification for Durability Assessment of Hydraulic Concrete Structures. China Water & Power Press: Beijing, China, 2018.

















| Gradation | Cement | Fly ash | Water | Sand | Aggregate (5–20 mm) | Aggregate (20–40 mm) |
|---|---|---|---|---|---|---|
| Two-stage gradation | 260 | 70 | 140 | 700 | 600 | 600 |
| Three-stage gradation | 240 | 60 | 145 | 600 | 800 | 800 |
| Engineering Section | Dept (mm) | Permeation Condition | Permeation Test Duration (h) | Permeation Height (mm) | Permeability Coefficient (cm/s) |
|---|---|---|---|---|---|
| UMD | 0~50 | No | 24 | 0.6 | <1.0 × 10−13 |
| 50~100 | No | 24 | 0.4 | <1.0 × 10−13 | |
| 100~150 | No | 24 | 0.3 | <1.0 × 10−13 | |
| DMD | 0~50 | Yes | 0.5 | 30.0 | 9.19 × 10−9 |
| 50~100 | Yes | 3.5 | 30.0 | 1.31 × 10−9 | |
| 100~150 | Yes | 24 | 0.5 | <1.0 × 10−13 | |
| UAD | 0~50 | No | 24 | 0.3 | <1.0 × 10−13 |
| 50~100 | No | 24 | 0.2 | <1.0 × 10−13 | |
| 100~150 | No | 24 | 0.1 | <1.0 × 10−13 | |
| UW | 0~50 | No | 24 | 14.6 | 4.54 × 10−11 |
| 50~100 | No | 24 | 0.6 | <1.0 × 10−13 | |
| 100~150 | No | 24 | 0.1 | <1.0 × 10−13 |
| Engineering Location | Test Sample Depth (mm) | Air Content (%) | Average Chord Length (mm) | Most Probable Chord Length (mm) | Bond-Air Ratio | Specific Surface Area (mm2 /mm3) | Porosity (mm−1) | Bubble Spacing Factor (mm) |
|---|---|---|---|---|---|---|---|---|
| UMD | 0~50 | 4.88 | 0.070 | 0.0129 | 4.10 | 56.87 | 0.694 | 0.0721 |
| 50~100 | 2.26 | 0.047 | 0.0118 | 8.85 | 85.27 | 0.481 | 0.0704 | |
| 100~150 | 2.86 | 0.084 | 0.0121 | 6.99 | 47.74 | 0.342 | 0.1131 | |
| DMD | 0~50 | 35.64 | 0.090 | 0.0129 | 0.56 | 44.45 | 3.961 | 0.0126 |
| 50~100 | 44.48 | 0.118 | 0.0138 | 0.45 | 34.03 | 3.784 | 0.0132 | |
| 100~150 | 16.45 | 0.094 | 0.0151 | 1.22 | 42.53 | 1.749 | 0.0286 | |
| UAD | 0~50 | 2.24 | 0.048 | 0.0119 | 8.93 | 82.99 | 0.465 | 0.0726 |
| 50~100 | 7.63 | 0.057 | 0.0125 | 2.62 | 69.80 | 1.331 | 0.0376 | |
| 100~150 | 15.68 | 0.072 | 0.0125 | 1.28 | 55.80 | 2.188 | 0.0229 | |
| UW | 0~50 | 7.03 | 0.096 | 0.0150 | 2.84 | 41.46 | 0.729 | 0.0686 |
| 50~100 | 13.87 | 0.087 | 0.0133 | 1.44 | 45.90 | 1.591 | 0.0314 | |
| 100~150 | 5.29 | 0.074 | 0.0150 | 3.78 | 54.18 | 0.716 | 0.0698 |
| Water Sample | Sampling Location | pH | Sulfate Ion (mg/L) | Chloride Ion (mg/L) |
|---|---|---|---|---|
| 1 | Reservoir Area | 6.79 | 15.78 | 14.36 |
| 2 | Corridor | 6.73 | 9.04 | 13.39 |
| Soil Sample | Sampling Location | Sulfate Ion (mg/kg) | Chloride Ion (mg/L) |
|---|---|---|---|
| 1 | Reservoir inlet | 104.55 | 241.87 |
| 2 | Reservoir mid-section | 205.19 | 170.11 |
| 3 | Dam perimeter | 90.03 | 195.19 |
| 4 | Downstream face (near the dam body) | 44.16 | 145.63 |
| 5 | Downstream face (far from dam body) | 237.75 | 145.28 |
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.
Share and Cite
Wei, H.; Sun, Y.; Li, C.; He, Y.; Lu, H.; Tang, L. Unveiling the Degradation Mechanism of Impermeability and Pore Structure in Concrete Under Long-Term Water Exposure. Materials 2026, 19, 496. https://doi.org/10.3390/ma19030496
Wei H, Sun Y, Li C, He Y, Lu H, Tang L. Unveiling the Degradation Mechanism of Impermeability and Pore Structure in Concrete Under Long-Term Water Exposure. Materials. 2026; 19(3):496. https://doi.org/10.3390/ma19030496
Chicago/Turabian StyleWei, Hua, Yi Sun, Chunhe Li, Yang He, Hao Lu, and Lan Tang. 2026. "Unveiling the Degradation Mechanism of Impermeability and Pore Structure in Concrete Under Long-Term Water Exposure" Materials 19, no. 3: 496. https://doi.org/10.3390/ma19030496
APA StyleWei, H., Sun, Y., Li, C., He, Y., Lu, H., & Tang, L. (2026). Unveiling the Degradation Mechanism of Impermeability and Pore Structure in Concrete Under Long-Term Water Exposure. Materials, 19(3), 496. https://doi.org/10.3390/ma19030496