Article

Microstructure Evolution and Properties of ZrC–NbC System Titanium Matrix Composites Based on Experiments and ANSYS Simulations

1
School of Intelligent Manufacturing and Elevator, Huzhou Vocational & Technical College, Huzhou 313000, China
2
School of Materials and Chemical Engineering, Xi’an Technological University, Xi’an 710021, China
*
Author to whom correspondence should be addressed.
Coatings 2025, 15(6), 626; https://doi.org/10.3390/coatings15060626
Submission received: 24 April 2025 / Revised: 15 May 2025 / Accepted: 20 May 2025 / Published: 23 May 2025

Abstract

:
The extreme environment of aerospace requires severe material properties, and in situ autogenous ZrC–NbC dual-phase reinforced titanium matrix composites have attracted much attention. In this study, TiC/Ti composites (TMC1–TMC4) with different NbC contents (0–9 wt%) were prepared and investigated in depth by various means and ANSYS simulations. The results show that the variation in NbC content significantly changes the TiC morphology from fine needles at 0 wt% to needles with a small amount of ellipsoidal grains at 3 wt%, to an ideal uniform distribution (mostly granular or nearly spherical) at 6 wt%, and to a large number of aggregates (dendritic or coarse rod-like) at 9 wt%. In terms of mechanical properties, the compressive strength and elongation firstly increased and then decreased, and reached the optimum at 6 wt% NbC, with the ultimate compressive strength as high as 1379.50 MPa, the compressive yield strength at 817.3 MPa, the compressive strain up to 38.73%, and typical ductile fracture characteristics; at 9 wt%, it transformed into a mixed fracture mode, with a decrease in performance. ZrC and NbC synergistically stabilize the microstructure, with the best synergistic effect at 6 wt% NbC, which effectively improves the overall performance and meets the requirements of aerospace applications. The simulation is highly compatible with the experiment and verifies the experiment; this helps to reveal the mechanism, provides guidance for the design of high-performance materials, and promotes the development of materials technology in the aerospace field.

1. Introductions

In today′s era of rapid global technological development, high-performance materials, as the cornerstone of modern industry and cutting-edge technology, are playing a key role as never before [1,2]. High-performance materials have become a core driver for technological innovation, performance breakthroughs, and meeting the demands of extreme operating conditions in many industries such as aerospace, automotive manufacturing, biomedicine, and energy [3,4,5,6]. Titanium matrix composites, with their unique low-density properties, stand out in the modern engineering field that strives for lightweight design, offering the possibility to improve structural efficiency and energy efficiency [7]. High specific strength and high specific modulus endow the material with the ability to maintain structural stability even when subjected to high-intensity loads [8], which has made titanium matrix composites popular in the manufacture of critical components for aerospace vehicles [7,9]. The material’s excellent corrosion resistance ensures long-term service reliability in harsh environments. Whether in the seawater erosion environment in offshore engineering or in corrosive media in the chemical industry, titanium matrix composites have shown excellent durability [10,11]. Excellent high-temperature performance makes this material an ideal candidate for aerospace engine hot-end components and high-speed aircraft surface structures, able to maintain good performance under extreme conditions of high temperature, high pressure, and high stress [12,13].
In the aerospace industry, the continuous advancement of vehicle performance places extremely demanding and diverse requirements on material properties [2,14,15]. Under high-speed flight conditions, the vehicle not only has to face the challenge of high temperature generated by air friction, but also has to withstand the high-pressure load brought by aerodynamic pressure, and also has to cope with the dynamic stress generated by the complex and variable flight attitude [16,17], which means that the material must have extraordinary mechanical properties, including high strength, high toughness, and good fatigue properties, to ensure structural integrity and safety under extreme loads. Stable thermal properties are essential to maintain the performance consistency of the vehicle under different temperature environments, and to prevent the fluctuation in material properties due to temperature changes from affecting the flight performance [3,18,19]. Good antioxidant properties are crucial to ensure the long service life of materials in high-temperature oxidative environments to avoid the degradation of material properties due to oxidative reactions [18], thus prolonging the service life of critical components of the vehicle [14,20,21].
Although conventional titanium alloys are able to meet some of the performance specifications to a certain extent [22], their performance limitations are gradually revealed in the face of increasingly demanding flight requirements. Especially in the synergistic enhancement of room-temperature plasticity and high-temperature strength, it is difficult for conventional titanium alloys to maintain good room-temperature plasticity and increase their high-temperature strength at the same time, which limits the scope of their application in high-performance aerospace components.
The emergence of in situ autogenous two-phase strengthened titanium matrix composites has brought a new light to solve these challenges. Among them, ZrC–NbC system composites have theoretically demonstrated a number of attractive properties, such as high hardness, high melting point, good thermal stability, and oxidation resistance [23,24], which make them be expected to stand out in harsh aerospace environments [25], and to provide a powerful material solution for the performance enhancement of the critical components of the aircraft. However, the current research on composites in this family is still in its infancy and faces many technical challenges despite its promising future. Among them, the mechanism of the NbC and ZrC in composites is still unclear, which makes it difficult to precisely regulate the material properties. Traditional research methods have limitations in analyzing the relationship between microstructure and properties, and it is difficult to reveal the influence of microstructural features on macroscopic properties, which in turn limits the optimal regulation of material properties.
The aim of this study is to fill this research gap and to carry out a systematic and in-depth study of ZrC–NbC system composites by using an innovative research method that combines experiments and ANSYS simulations. As an advanced numerical simulation technology, ANSYS simulation, with its powerful multi-physics field coupling analysis capability [26,27], can break through the limitations of the traditional experimental methods, and can accurately predict and provide in-depth analysis of the evolution of the material microstructure and the rule of change in the mechanical properties [28]. This study is dedicated to revealing the mechanism of the autogenous co-strengthening effect of NbC and ZrC in situ, exploring the influence of different contents of NbC and ZrC on the microstructure and mechanical properties of composites, and then providing a solid scientific basis and efficient technical support for the design and application of composites in this series [29,30]. This study has significant innovative points, which are expected to promote the rapid development of the field of in situ autogenous dual-phase reinforced titanium matrix composites, open up new paths for the research and development of high-performance aerospace materials, and help aerospace and other high-end fields to achieve the precise regulation of material properties and the optimization of applications.

2. Preparation and Characterization of In Situ TMCs

2.1. Experimental Materials

In the present research endeavor, pure titanium (Shandong Xingke New Materials Co., Ltd., Zibo, China) was judiciously chosen as the matrix material, predicated upon its remarkable biocompatibility and mechanical attributes. Zirconium carbide (ZrC) (Shandong Xingke New Materials Co., Ltd., Zibo, China) and niobium carbide (NbC) (Shandong Xingke New Materials Co., Ltd., Zibo, China) powders were employed as carbon sources for the synthesis of TiC/Ti composites. During the fabrication process, in situ reactions transpired between titanium (Ti) and ZrC/NbC, culminating in the formation of a TiC reinforcing phase, thereby effectuating the reinforcement of the composites. The specific reactions are delineated in Equations (1) and (2). It is noteworthy that a fraction of the zirconium (Zr) elements was incorporated into the composite matrix in the form of α-Ti, while a certain proportion of niobium (Nb) elements existed as β-Ti. Moreover, a portion of the zirconium and niobium elements was integrated within the TiC phase.
Ti + NbC → TiC + Nb (β − Ti)
Ti + ZrC → TiC + Zr (α − Ti)
The raw materials consisted of primary sponge titanium and high-purity ZrC and NbC powders. The purity and particle size particulars of the ZrC and NbC powders are tabulated in Table 1, and their morphological characteristics are depicted in Figure 1 and Figure 2.
The experimental preparation process encompasses pretreatment steps. The ultrasonic cleaning technique was employed to place the primary sponge titanium, ZrC powder, and NbC powder into the cleaning machine, with ethanol or acetone serving as the medium, to eliminate impurities such as oil stains and dust. After cleaning, the samples were placed in a drying oven and dried under vacuum or inert gas protection to ensure a dry surface. Subsequently, sieving was carried out, and the materials were weighed again to meet the proportion requirements of the ingredients. The ingredients were proportioned according to the scheme of 5ZrC + xNbC/Ti (where x takes values of 0, 3, 6, and 9 wt%), weighed using a high-precision electronic balance, and the mixed raw materials were then placed into a copper crucible after weighing. The melting equipment was a QK20-006 vacuum arc melting furnace. Under a vacuum degree of 5 × 10−4 Pa, vacuum pumping and argon gas introduction were performed to prevent the oxidation of the raw materials. During the melting process, at a current of 50 A, a 5–30 A adjustable electromagnetic stirring system was utilized to promote the uniform mixing of elements. Moreover, circulating cooling water was employed for rapid solidification into an ingot. To enhance the compositional uniformity, the solidified ingot was flipped and remelted four times, and samples were taken for analysis after each melting.

2.2. The Microstructure and Mechanical Properties

The microstructural and mechanical property characterizations were carried out as follows. Phase identification was performed using a D8-ADVANCE X-ray (Bruker, Billerica, MA, USA) diffractometer with a scanning range of 2θ from 30° to 90°, ensuring comprehensive coverage of the material′s phase structure and accurate determination of phase compositions. The TMC1–TMC4 billets were ground, polished, and then etched with a 4% nitric acid–ethanol solution. Their microstructures were observed under a US-made QUANTA FEG250 SEM (FEI, Hillsboro, OR, USA) equipped with an EDS (FEI, Hillsboro, OR, USA) for elemental analysis.
For TEM observation, thin foil samples were mechanically polished to a thickness of 45 μm under strictly controlled pressure and time to prevent deformation and damage. The microstructural features were examined using a Tecnai G2 F30 TEM (FEI, Hillsboro, OR, USA) with an HRTEM system.
Compression tests were conducted on cylindrical samples (6 mm in diameter and 9 mm in length) via an AG-IC100KN (Shimadzu, Kyoto, Japan) universal testing machine at an initial strain rate of 1 mm/min. The samples were carefully placed between the platens to ensure good contact, preloaded with 100 N and held for 15 s. Subsequently, compression loading was applied at the set strain rate until sample failure while recording the stress–strain curves to evaluate the compressive properties. To ensure the accuracy of the test results, each specimen was tested five times, and the average value was calculated as the final result for evaluating the compressive properties.
The hardness tests were conducted on the specimens using an HM-211 Vickers (Mitutoyo South Asia Pvt. Ltd., New Delhi, India) microhardness tester. Cube specimens with dimensions of 8 × 8 × 8 mm3 were cut by a wire electrical discharge machine, followed by successive grinding and polishing to ensure smooth and bright surfaces. The test parameters were set as a load of 150 g and a dwell time of 15 s. Ten measurement points were tested for each sample, and the average value was taken as the final hardness value of the specimen to ensure accuracy and reliability.

2.3. ANSYS Finite Element Analysis

For model building, the titanium matrix, TiC reinforcing phase, and interfacial regions in the composite were precisely partitioned. A combination of tetrahedral and hexahedral elements was used for meshing. In the titanium matrix′s uniform regions, hexahedral elements with 0.5–1 mm edge length ensured efficiency and accuracy. For complex TiC and interface areas, 0.1–0.3 mm tetrahedral elements captured details. Mesh refinement verified convergence.
Material properties were defined by experimental data. The titanium matrix had a Young′s modulus of ~110 GPa and Poisson′s ratio of 0.34. The TiC had a Young′s modulus of ~450 GPa and Poisson’s ratio of 0.19. The interface was modeled as a cohesive zone, with an initial stiffness of 5 GPa/mm and a critical energy release rate of 10 J/m2.
A Johnson–Cook constitutive model was chosen, calibrated with experimental stress–strain curves. For loading and boundary conditions, the bottom platen was set to fixed constraints (all degrees of freedom locked), while the top platen applied a displacement-controlled load along the axial direction (Z-axis) at a rate of 1 mm/min, consistent with the experimental conditions. After model construction, simulated compression tests on 6 mm diameter and 9 mm height samples, matching the experiments, were performed at 1 mm/min loading rate. Predicted curves had <5% error in the elastic modulus and ~8% in the ultimate compressive strength compared to the experiments. Discrepancies were optimized by adjusting the mesh and model parameters.

3. Results and Discussion

3.1. XRD Results

X-ray diffraction analysis was performed on the TiC/Ti composites with varying NbC additions (Figure 3). The results demonstrated that the addition of NbC and ZrC successfully led to the formation of TiC, validating the feasibility of the preparation method. The phases of this composite consist of α/α′-Ti, β-Ti, and TiC. As the amount of the NbC addition increases, the in situ reaction generates a greater quantity of niobium elements. In accordance with the relationship between elements and phase structures in titanium alloys, niobium, being a strong β-stabilizing element, has the following effect: its increasing content promotes the transformation of α-Ti to β-Ti. Consequently, the diffraction peak intensity of α-Ti decreases, visually presenting the trend of phase structure variation with the NbC content. This provides crucial phase information for investigating the connection between the material properties and the microstructure.

3.2. Analysis of Microstructures

Figure 4 presents the microstructural morphologies of the composites with different niobium carbide (NbC) additions. It can be observed that the TiC phase exhibits diverse morphological characteristics in the composites and undergoes significant changes with the variation in the NbC addition. In TMC1 (0 wt% NbC), it exists in the form of eutectic titanium carbide, manifesting as fine particles or short rods, which are dispersedly distributed along the grain boundaries and between lamellae, with a relatively sparse quantity. This is attributed to the limited content of C atoms in the system and the lack of NbC to facilitate its formation.
When the NbC addition is increased to 3 wt% (TMC2), needle-like microstructures and a small amount of ellipsoidal granular TiC emerge, with enhanced regularity and an increased quantity due to the additional C elements brought by the NbC introduction. In TMC3 (6 wt% NbC), the TiC is mostly granular or approximately spherical, uniformly distributed and arranged in an orderly way at the grain boundaries, and its quantity is further increased, optimizing the distribution state. However, in TMC4 (9 wt% NbC), the TiC aggregates massively, appearing as dendrites or coarse rods with obvious agglomeration. Although the quantity increases, the excessive aggregation leads to a deteriorated uniformity of distribution.
Simultaneously, in conjunction with Figure 5, it is observed that the α-Ti phase in the composites is mainly in the form of lamellar particles (α′ phase), and its characteristics change with the amount of the NbC addition. In TMC1, the α′ phase is in the form of white-contrast lamellae with prominent bundling characteristics. The lamellar width is 5.7 ± 0.3 μm, and the bundle size reaches 23.5 μm. The lamellae within the same bundle are parallel, and this structure dominates in the matrix.
When the NbC addition increases to 3 wt% (TMC2), the width of the lamellar α′ phase narrows, the bundle size decreases, and the angle between the different bundles of the α′ phase changes to 60° or 120°, while the lamellae within the same bundle remain parallel. The quantity of the α-Ti phase decreases because NbC promotes the transformation of the α-Ti phase to the β-Ti phase.
In TMC3, the α-Ti phase is affected by the TiC phase and exhibits a specific distribution around and at the grain boundaries. Its lamellar characteristics are locally deformed, and the quantity continues to decrease due to the further stabilization and increase in the β-Ti phase.
When the NbC content reaches 9 wt% (TMC4), the lamellar structure of the α-Ti phase is damaged, and the distribution becomes disordered. It coexists with a large amount of the aggregated TiC phase and an increased β-Ti phase. The quantity of the α-Ti phase decreases significantly, and most of it is transformed into the β-Ti phase. The diffraction pattern calibration of the light gray area in the TEM determines it as the α-Ti phase, which helps to clarify its properties in different states.
Studies have shown that the morphology, distribution, and quantity of the β-Ti phase in the composites change significantly with the NbC addition amount, which has a profound impact on the material properties. In TMC1, the β-Ti phase is distributed along the lamellae, presenting a black contrast and a linear arrangement. It is mainly located between the bundles of the α′ phase, with a relatively small quantity, laying the foundation for the initial microstructure of the material.
When the NbC addition amount increases to 3 wt% (TMC2), the β-Ti phase is distributed between the lamellae and constitutes the matrix together with the lamellae and the needle-like α′ phase. The quantity increases due to the solid solution stabilization effect of NbC, optimizing the matrix structure.
In TMC3, the β-Ti phase is uniformly distributed and intertwined with the α-Ti phase and TiC phase. The quantity increases stably, and it cooperates with other phases to optimize the material properties, forming a stable matrix structure.
When the NbC content reaches 9 wt% (TMC4), the β-Ti phase exists in a large amount, but there is a tendency of segregation around the TiC particles. Although the quantity increases significantly, the overall performance of the material is weakened due to the non-uniformity of the microstructure. The β-Ti phase is determined by the dark gray area in the TEM characterization, providing microscopic evidence for its existence.
Upon examining Figure 6, the microstructural highlights of the in situ autogenous composites emerge. This precise and efficient process prevents unwanted intermediate phases. High-resolution microscopy shows a clean interface with only the titanium matrix and titanium carbide, free of impurities.
Such an interface benefits composites. It enables smooth stress transfer, avoiding concentration, and allows uniform stress distribution under loads, enhancing mechanical strength. Also, the simple two-phase interface stabilizes the microstructure, preventing disorder and ensuring integrity, supporting excellent performance in harsh conditions.

3.3. Microhardness

Figure 7 shows the average microhardness of TMC1 to TMC4. It can be seen that the average microhardness of the TMCs increase with the increase in NbC content. At 6 wt% NbC content, the microhardness of TMC3 reaches the highest value of 286.082 HV.
When the NbC addition in TMC3 is 6 wt%, the microhardness reaches the maximum value of 286.082 HV, which is closely related to the microstructure and internal factors. Microscopically, at this time, the distribution of the NbC particles is ideal. As a reinforcing phase, it effectively hinders dislocation movement. When dislocations migrate, they are blocked by the uniformly distributed NbC particles, increasing the slip resistance and enhancing the material’s ability to resist deformation. Moreover, it avoids agglomeration and forms a “skeleton”-like structure that bears and disperses stress, exhibiting high hardness characteristics.
When the NbC content increases to 9 wt%, the hardness value decreases. This is because excessive NbC destroys the uniformity of the microstructure, leading to agglomeration and stress concentration. Originally, when the NbC content was 6%, the matrix and the reinforcing phase cooperatively resisted deformation. However, at 9% NbC content, due to agglomeration and non-uniformity, the synergy fails, the ability to resist deformation weakens, and the hardness decreases. The variation law of hardness with the NbC content reflects the internal relationship between the microstructure and properties, providing a basis and reference for understanding the performance evolution and material optimization.

3.4. Compressive Property Characterization

The compressive stress–strain curves of the TMC1–4 composites with different NbC additions shown in Figure 8 are the key basis for in-depth analysis of the compressive characteristics of the materials. They can clearly reveal the variation law of stress with strain during the compression process and accurately explore the internal relationship between the compressive strength and the microstructure of the composites, providing core clues for understanding the evolution mechanism of material properties.
In general, as the NbC addition amount gradually increases from 0 wt%, the compressive strength of the composites shows a trend of first increasing and then decreasing, reaching the maximum value at TMC3 (with 6 wt% NbC addition). This variation trend is closely related to the evolution of the material’s microstructure and is the result of the synergistic effect of multiple factors. The following is a detailed analysis of each composite.
For TMC1, its compressive strength is relatively low. In TMC1, the TiC phase is sparse and dispersedly distributed. From the perspective of microstructure, this distribution state makes the ability of the TiC phase to impede dislocation movement limited during the compression process. According to the dislocation theory, when dislocations slip in the matrix, the TiC phase makes it difficult to effectively prevent their movement because dislocations can relatively easily bypass or pass through the sparse TiC phase particles, making the material prone to deformation and having an insignificant effect on enhancing the compressive strength. At the same time, the α-Ti phase dominates, but its lamellar structure has poor deformation coordination during compression, making it difficult to effectively relieve local stress concentration. The β-Ti phase has a low content and is poorly distributed, unable to fully play the role of bearing load. The synergistic effect of the two phases on enhancing the compressive strength is not significant, resulting in a relatively low overall compressive strength of the material.
The compressive strength of TMC2 is higher than that of TMC1. At this time, the TiC phase becomes finer, denser, and more uniformly distributed, which to some extent hinders dislocation movement. When dislocations move and encounter the finer and uniformly distributed TiC phase, they need to consume more energy to bypass or pass through the particles, thus enhancing the material’s resistance to deformation and having a positive impact on the compressive strength. However, the homogeneity of the microstructure is still affected to a certain extent, limiting the full reinforcing effect of the TiC phase. The relative content of the α-Ti lamellar phase increases slightly, and its combined effect with the refined TiC phase increases the compressive strength. However, the distribution of the α-Ti phase and the β-Ti phase is not ideal, resulting in a relatively small increase in strength.
TMC3 exhibits a relatively high compressive strength, which is attributed to the synergistic optimization of multiple factors. In TMC3, the TiC phase exhibits an ideal state of further refinement, uniform distribution, and close combination with the matrix, forming an effective strengthening network. During the compression process, the dislocation movement is strongly hindered by the TiC phase. According to the dislocation theory, when dislocations encounter TiC phase particles, they need to consume additional energy to bypass or pass through them. Let the dislocation movement resistance be τ and the increased resistance caused by the TiC phase particles be τ , and then the actual dislocation movement resistance becomes τ + τ , significantly increasing the resistance to dislocation slip and thus improving the yield strength and compressive strength.
At the same time, the proportion and distribution of the α-Ti and β-Ti phases reach an almost optimal synergistic state. The plastic deformation ability of the α-Ti phase is fully utilized. When a local stress concentration occurs, it absorbs and disperses the stress through its own plastic deformation, preventing the stress concentration area from expanding rapidly. The β-Ti phase also gives full play to its load-bearing capacity and bears the external compressive load together with α-Ti phase. This synergistic effect enables the material to maintain a good stress balance when stressed, and the stress transfer between the phases is more uniform and efficient, further improving the overall compressive strength of the material.
In addition, the solid solution strengthening effect of the Zr and Nb elements on the matrix is significantly enhanced. These elements dissolve in the matrix, causing lattice distortion. According to the solid solution strengthening theory, lattice distortion increases the resistance to dislocation movement. Let the increased resistance to dislocation movement caused by lattice distortion be τ , and then when dislocations move in the matrix containing Zr and Nb elements, the total resistance becomes τ + τ + τ . This solid solution strengthening effect further improves the strength and stability of the matrix, providing additional support for the material during the compression process and contributing to the improvement in compressive strength. In summary, the ideal distribution of the TiC phase, the synergistic optimization of the α-Ti and β-Ti phases, and the solid solution strengthening effect of the Zr and Nb elements in TMC3 jointly contribute to the maximum compressive strength, achieving a good balance between the strength and the plasticity of the material and providing an important reference basis for the design and application of high-performance composites.
The compressive strength of TMC4 is significantly lower than that of TMC3. In TMC4, the TiC phase severely agglomerates, forming local stress concentration regions. During compression, these agglomerated regions become the source of crack initiation and propagation, leading to the premature failure of the material and a significant reduction in compressive strength. The distribution of matrix elements is uneven, and the distribution of the α-Ti phase and the β-Ti phase is disturbed, losing their good synergistic effect and making them unable to effectively transfer and disperse stress. Although the solid solution strengthening of the Zr and Nb elements may be enhanced, the deterioration of the microstructure weakens its positive impact on the compressive strength, resulting in a decline in the overall compressive performance.

3.5. Fracture Morphology Analysis of TMCs

Figure 9 shows the compression fracture morphology of the composites with different amounts of NbC. The compression fracture of TMC1 (Figure 9a,a1) is very flat, with no macro features of plastic deformation, showing typical brittle fracture. Microscopically, the TiC phase is sparse and coarse, the α-Ti phase is dominant and has a simple structure, and the β-Ti phase is sparse, which results in the low compression strength of the material and makes it brittle and easy to fracture.
When NbC reaches 3 wt% (Figure 9b,b1), the fracture is now slightly undulating and uneven, with a few signs of plastic deformation, small tear ribs, and similar tough nest features, but the brittle fracture is still dominant. This indicates that the plastic deformation ability of the material is beginning to improve but is still weak. Microscopically, the Zr element contributes to a finer and more uniform distribution of the TiC phase, an adjustment of the ratio of the α-Ti and β-Ti phases, a slight increase in the content of the β-Ti phase, and a clearer phase interface. This leads to the increase in dislocation motion resistance and the initial synergy between the α-Ti and β-Ti phases; the plastic deformation is limited, but the compressive strength is improved compared with TMC1, and the fracture characteristics are in line with the trend of strength change.
The compression fracture of TMC3 (Figure 9c,c1) shows significant toughness fracture characteristics, and the toughness nest characteristics indicate that the full plastic deformation absorbs energy to improve toughness. Microscopically, the TiC phase is utilized, the α-Ti and β-Ti phases are synergistic, and the Zr and Nb elements are solid solution strengthened and structurally stable. The advantages of each phase are brought into play, the dislocations are hindered, the plastic deformation is strong, the strength and plasticity are balanced, and the ultimate compressive strength reaches 1379.50 mPa, which provides a basis for the design of high-performance composites.
The macroscopic fracture of TMC4 (Figure 9d,d1) shows a mixed fracture mode, with both brittle and plastic characteristics, and the plastic deformation ability is weaker than that of TMC3. At the microscopic level, the TiC phase is severely agglomerated, the distribution of matrix elements is uneven, and the structural stability of the α-Ti and β-Ti phases is damaged, which leads to cracks caused by the stress concentration and the reduction in strength.
Overall, when the NbC content increases from 0 wt% to 6 wt%, the fracture of TMC1–TMC3 changes from brittle to ductile, which is related to the utilization of the microstructure and the increase in the strength, and when the NbC increases to 9 wt%, the plastic deformation ability of TMC4 decreases due to the deterioration of the microstructure, and the compression property decreases significantly, which highlights the key influence of microstructure on the properties of composites, and provides an important basis for the design of high-performance composite materials.

3.6. Analysis Based on Crystal Growth Kinetics and Thermodynamics: Effect of NbC Addition on TiC Morphology and Compression Properties of Composites

(1)
Basic theory of kinetics and thermodynamics of crystal growth
In the field of materials science, crystal growth is driven by both kinetics and thermodynamics. From the thermodynamic point of view, the driving force of crystal growth originates from the reduction in free energy of the system; in order for the Ti–C system to form the TiC phase, according to the Gibbs free energy change formula G = H T S ( H for enthalpy change, T for temperature, S for entropy change), the growth is thermodynamically favorable when G < 0. Kinetically, the crystal growth rate v is related to a number of factors and is commonly expressed as v = k G n (k is the rate constant; n depends on the growth mechanism).
(2)
Effect of NbC addition on the morphology of titanium carbide
At 0 wt% NbC, the TiC phase is dispersed in the form of fine particles or short rods at the grain boundaries and in the interlayers, and its quantity is scarce. Thermodynamically, the C-atoms in the system are limited, which restricts the generation of the TiC phases. Kinetically, the C-atom supply rate γ c is low, which is similar to the TiC growth and consumption rate γ T i C at equilibrium, but the low γ c makes the growth driving force G small; the growth is slow, and the formation of small-sized TiC phases makes it difficult to impede the dislocation motion, and the enhancement of the compressive strength is not obvious.
At 3 wt% NbC, acicular and a small amount of ellipsoidal granular TiC appear with increased regularity and quantity. The introduction of more C elements into NbC thermodynamically shifts the reaction Ti + C ⇌ TiC to the right, increasing the amount of TiC produced. Kinetically, there is a relative increase in the C-atom supply rate ( γ c ), and an increase in the growth drive, G . Assuming a multiplicative increase in the C element concentration of x, for the new growth rate v n e w = k   ( x G ) n, the growth rate is accelerated. During the crystal growth process, due to anisotropy, the TiC phase grows faster in certain directions, resulting in the formation of needle-like structures, while a small amount of ellipsoidal granular TiC is formed in some regions. This morphological change allows the TiC phase to hinder dislocation motion to a certain extent, which enhances the deformation resistance of the material and thus positively affects the compressive strength, but the microstructural homogeneity is still affected to a certain extent, so the TiC phase enhances the compressive strength. However, due to the uniformity of the microstructure, the enhancement effect of the TiC phase is not fully utilized and the strength enhancement is relatively small.
At 6 wt% NbC, the TiC is mostly granular or nearly spherical, uniformly distributed and ordered at the grain boundaries, further increasing in number and distribution. The thermodynamic equilibrium leads to a balanced growth trend of the TiC phase, which is characterized by the low surface energy of the morphology according to the principle of minimum surface energy. Kinetically, the appropriate supply of C atoms and the growth driving force lead to uniform growth, and the interfacial energy γ T i C m a t r i x is in the right range for stable growth. This TiC phase effectively hinders the dislocation motion during compression, and works well with the matrix to achieve a balance between strength and plasticity and the best compression performance.
With 9 wt% NbC, the TiC phase aggregates in large quantities, showing dendrites or thick rods and obvious agglomerations, increasing in quantity but with poor distribution uniformity. Thermodynamically, the excessive NbC makes the C concentration too high, and the local chemical potential is high to promote TiC overgrowth and agglomeration. Kinetically, the high C concentration makes the growth drive force too large and the growth rate too fast. According to the diffusion-controlled growth model, the fast diffusion of C atoms leads to the rapid growth of the TiC phase into a specific shape. The agglomerated TiC phase becomes a source of cracks during compression, leading to the premature failure of the material. Despite solid solution strengthening, microstructural deterioration diminishes the positive effect on compressive strength, resulting in a reduction in overall properties.
(3)
Effect of NbC incorporation on compression properties of composites
The morphology of the TiC phase is closely related to the dislocation motion. For example, at 0 wt% NbC, the finely dispersed TiC phase makes it difficult to hinder dislocations, and the dislocations are easy to bypass or pass through, and the material is easily deformed; at 6 wt% NbC, the uniformly distributed granular TiC phase can effectively hinder the dislocations, and improve the yield and compression strength.
TiC phase morphology also affects stress transfer. Ideally (at 6 wt% NbC), the TiC phase disperses stress uniformly and is tightly bonded to the matrix, with the phases working together to bear the load; at 9 wt% NbC, the agglomerated TiC phase leads to stress concentration, and the matrix and reinforcing phases work together to fail, which reduces the compressive properties.

3.7. ANSYS Finite Element Analysis Results and Discussion

Combined with the above results, when the addition of zirconium carbide is 6 wt%, the microstructure distribution of the composites is more uniform and the compression performance is optimal. Further, the compressive properties of TMC1–4 were simulated and calculated by ANSYS simulation software, and the results are shown in Figure 10.
Figure 10 shows the total deformation simulation results (mapped to equivalent plastic strain, EPS) of TMC1–TMC4. For TMC1 (0 wt% NbC), the internal deformation is uneven, with a large strain range (1.048 × 10⁵ Max–8.1429 × 10¹⁰ Min), coefficient of variation (CV) = 0.35, and 35% of the area exhibiting high strain (>1.5× the mean). This correlates with its inhomogeneous microstructure (sparse TiC, Figure 4a) and low compressive strength (Figure 8).
For TMC2 (3 wt% NbC), the deformation homogeneity improves, with a reduced strain range (1.0369 × 10⁵ Max–1.3005 × 10⁹ Min), CV = 0.22, and 22% high-strain area. This aligns with its moderate microstructure refinement (needle-like TiC, Figure 4b) and intermediate compressive performance.
For TMC3 (6 wt% NbC), the simulation shows a uniform color distribution dominated by blue-green tones (EPS values concentrated in the lower range), with a strain range of 1.0202 × 10⁻⁵–1.2321 × 10⁻⁹, CV = 0.12, and only 12% high-strain area. This indicates homogeneous deformation during loading, directly reflecting the optimized microstructure (uniform granular TiC, Figure 1) and efficient stress dispersion, consistent with its peak compressive strength (1379.50 MPa, Figure 8).
For TMC4 (9 wt% NbC), severe strain localization occurs, with a strain range of 1.0021 × 10⁵–1.4371 × 10⁹, CV = 0.28, and 28% high-strain area, attributed to the TiC agglomeration (Figure 4d) and compromised stress transfer, leading to degraded mechanical properties. Overall, the ANSYS simulation results correlate closely with the experimental observations, particularly the uniform deformation in TMC3, which validates the microstructural optimization and provides a theoretical basis for high-performance titanium matrix composite design.
Equivalent stress maps with total deformation simulations (Figure 11, Figure 12 and Figure 13) were performed for TMC1 (0 wt% NbC). Stress distribution simulations (Figure 11a and Figure 13a) show extreme inhomogeneity, with discrete stress values and obvious stress concentration areas at the macroscopic level. Microscopically, the TiC phase is small and diffuse (Figure 3), and the stress component σ i j I (i, j = 1, 2, 3) varies drastically. According to the stress concentration factor equation Kt = σ m a x σ n o m (where σ m a x is the maximum stress and σ n o m is the nominal stress), the value K t is larger in the stress concentration region. This is because the TiC phase makes it difficult to disperse the stress. From the crystallographic point of view, the dispersion of the TiC phase leads to relatively weak interfacial bonding with the matrix, and when subjected to external loads, the stress cannot be effectively transferred between the matrix and the reinforcing phases through the interface, which results in the concentration of stress in the local area.
Analyzed from dislocation theory, dislocations move relatively easily under this stress distribution. According to the dislocation motion resistance formula τ = τ 0   + α G b ρ (where τ is the shear stress required for dislocation motion, τ 0 is the lattice friction, α is a constant, G is the shear modulus, b is the Berthold vector, and ρ is the density of dislocations), in the region of stress concentration, dislocations are easy to gather and slip in the region of lower stress due to the unevenness of the stresses, resulting in the material being easily deformed, with an enhancement of the compressive strength The effect is not obvious.
The simulation of the deformation characteristics of TMC1 (Figure 12a) shows that the total deformation is inhomogeneous, with a maximum deformation of 1.0786 e−5 Max (assuming that the minimum value is close to 0). In terms of the relationship between microstructure and deformation, the dislocations can slip relatively easily in the matrix during compression due to the diffuse TiC phase, which is small in size and unevenly distributed according to the crystal growth kinetics analyzed earlier. Let the dislocation slip distance be x. According to the equation of deformation caused by dislocation slip, ε = b x L (where ε is the strain and L is the crystal length), the dislocations can easily slip, which makes the material easily deformed under a small stress. At the same time, the α-Ti phase-dominated lamellar structure cannot coordinate the deformation effectively during the deformation process, which further exacerbates the inhomogeneity of the local deformation, leading to the material being unable to disperse the energy effectively through uniform deformation when subjected to compressive load, thus reducing the compressive property of the material.
For TMC2, the simulation results of stress distribution are analyzed as shown in Figure 11b and Figure 13b. It can be seen that the stress distribution of TMC2 is improved compared with that of TMC1, but it is still not uniform, and the change in color gradient in the stress cloud shows that the stress value varies at different locations. The addition of NbC optimizes the TiC phase, but the uniformity of the microstructure is not good. From the stress transfer theory, the stress transfer efficiency at the interface of the matrix-reinforced phase is η = σ T i C σ m a t r i x (where σ T i C is the stress in the TiC phase and σ m a t r i x is the stress in the matrix), and the value of η in the stress concentration area is not ideal because the distribution of the α-Ti and β-Ti phases is not ideal, and the interaction of the three is not optimized, which makes the local deformation easy to be enlarged when subjected to external load, and this affects the overall performance.
Moreover, combined with the simulation results of the deformation characteristics of TMC2 (Figure 12b), it can be seen that the maximum deformation of TMC2 is 1.0766 e−5 Max, and the deformation homogeneity is improved but still uneven. The TiC phase increases the dislocation motion resistance, and according to the equation of the dislocation motion resistance, τ = τ 0   + α G b ρ , where τ is the shear stress required for dislocation motion, τ 0   is the lattice friction, α is a constant, G is the shear modulus, b is the Bergner vector, and ρ is the dislocation density, at which time the resistance to dislocation motion increases. However, the distribution of the α-Ti and β-Ti phases is not ideal, which leads to uneven dislocation motion resistance. Setting the dislocation motion resistance in different regions as τ 1   and τ 2 ( τ 1   τ 2 ), the different dislocation slip rates make the deformation degree of different parts of the material different, and the coordination of the overall deformation should be improved, which restricts the enhancement of the compression performance.
When the addition of NbC is 6 wt% (TMC3), the simulation results of stress distribution (Figure 11c and Figure 13c) show that the stress distribution of TMC3 is highly uniform, and the color of the stress cloud is uniform without any sudden change. This is due to the fact that the TiC phase is refined, uniformly distributed, and tightly bonded with the matrix (Figure 3), and the interfacial bonding energy formula E i n t e r f a c e = i n t e r f a c e γ T i C m a t r i x   d A ( γ T i C m a t r i x is the interface; A is the interfacial area) shows that a good interfacial bonding ensures that the stresses are effectively transferred and dispersed. Meanwhile, the ratio and distribution of the α-Ti and β-Ti phases are nearly optimal, the plastic deformation of α-Ti relieves the stress concentration, the load-bearing capacity of β-Ti is utilized, and the solid solution strengthening of Zr and Nb strengthens the substrate, which balances the stresses and achieves a uniform distribution of the stresses when the material is subjected to stresses.
Meanwhile, the simulation results of TMC3 show that the maximum deformation of TMC3 is 1.0737 e−5 Max, which is uniformly distributed, and the deformation is consistent in all regions during loading (Figure 12c). According to the theory of dislocation motion, the uniform TiC phase makes the average free range of dislocations smaller, which strongly prevents dislocation slip. The α-Ti and β-Ti phases are well coordinated with each other, so the coordination of plastic deformation is excellent. From the energy absorption point of view, according to the plastic deformation energy formula W p = V σ ϵ p dV ( ϵ p is plastic strain), the material absorbs energy uniformly and achieves a perfect balance between strength and plasticity, which demonstrates excellent compression performance.
Further analysis of the stress distribution simulation results (Figure 11d and Figure 13d) shows that the stress distribution of TMC4 is seriously uneven, with significant local stress concentration areas and large color differences in the stress maps. Microscopically, the TiC phase is seriously agglomerated and poorly bonded with the matrix (Figure 3). According to the stress concentration theory, the agglomeration results in a large stress gradient, which makes it difficult for the stress to be transmitted uniformly by destroying the interfacial bonding. The uneven distribution of matrix elements aggravates the disorder, and the structural stability of the α-Ti and β-Ti phases is impaired, which interferes with their stress-transferring and dispersing roles. Although Zr, Nb has solid solution strengthening, the microstructure deterioration weakened its role, and the stress concentration is prone to cracking, so that the mechanical properties decreases significantly.
At the same time, from the simulation results of the deformation characteristics of TMC4 (Figure 12d), the following can be seen: the maximum deformation of TMC4 is nearly 1.0737 e−5 Max, the distribution is very uneven, and the local deformation is concentrated, which is related to the uneven distribution of stress. The deformation in the stress concentration area is far more than in other areas. The TiC agglomeration and matrix destruction make the dislocation motion resistance extremely uneven; the dislocation motion resistance around the agglomerate is set, and the dislocation motion resistance away from the agglomerate is set to be τ 4 ( τ 3   > >   τ 4 ), and the dislocations easily pile up around the agglomerate and lead to the concentration of stress to cause the local deformation to be too large. The α-Ti and β-Ti phases have disordered distribution and cannot work together to resist deformation, exacerbating the inhomogeneity, and the material is subjected to small loads, and thus the material has a high deformation rate. The disordered distribution of the α-Ti and β-Ti phases cannot resist deformation in a synergistic way, which increases the inhomogeneity, and the material may fail locally under a small load, and the overall compressive property decreases drastically, which makes it not able to meet the actual demand.
Comparing the ANSYS simulation and the experimental data (Figure 8 and Figure 9), the two are in high agreement, e.g., the simulated and the experimental stress, strain, and fracture characteristics of TMC3 at 6 wt% NbC are consistent. This verifies the accuracy of the simulation method, shows that the model and parameters can reflect the mechanical behavior, confirms the correctness of the analysis of the influence mechanism of NbC content, and provides a theoretical basis for the optimization of material design. The simulation results reveal the influence mechanism, and the agreement with the experiment verifies its reliability, which helps aerospace and other fields to precisely regulate the material properties and promote the development of high-performance titanium matrix composites.

4. Conclusions

  • Microstructural Evolution Law: The content of NbC significantly regulates the morphology of the TiC phase and the composition of the matrix phases. As the NbC content increases from 0 wt% to 9 wt%, the TiC phase gradually transforms from fine acicular shapes to uniform granular shapes (optimal at 6 wt%), and then forms coarse dendrites due to agglomeration. Meanwhile, the proportion of the β-Ti phase increases with the NbC content, and the lamellar structure of the α-Ti phase evolves from regular arrangement to disordered distribution. An ideal microstructure of “uniform TiC particles + optimized α/β-Ti phase synergy” is formed at 6 wt% NbC.
  • Mechanism of Mechanical Property Optimization: The compressive strength and plasticity of the composites exhibit a non-monotonic variation, reaching the peak at 6 wt% NbC (compressive strength: 1379.50 MPa, strain: 38.73%), which is attributed to the synergistic effects of multiple factors: uniformly distributed TiC particles enhance strength by hindering dislocation motion (Orowan mechanism); the optimized α/β-Ti phase ratio (plastic coordination of α phase + load-bearing capacity of β phase) balances plasticity; and the Zr/Nb elements strengthen the matrix lattice through solid solution. When the NbC content increases to 9 wt%, the agglomeration of TiC leads to stress concentration, significantly deteriorating the properties, and the fracture mode transforms from ductile fracture to mixed brittle–ductile fracture.
  • Simulation Validation and Engineering Application Potential: ANSYS simulation results are highly consistent with the experimental data, confirming the decisive role of microstructural uniformity in mechanical properties: at 6 wt% NbC, the stress distribution within the material is uniform (equivalent stress deviation < 5%), and deformation coordination is optimal. The established “composition–structure-property” correlation model provides an experimental–simulation collaborative optimization path for the design of titanium matrix composites. The developed 6 wt% NbC composite meets the requirements of aerospace extreme environments for high-strength and high-toughness materials, and its in situ autogenous preparation process has the potential for industrial scale-up.

Author Contributions

Conceptualization, J.W. and Z.Y.; methodology, J.W.; software, J.W. and D.Z.; validation, J.W. and H.Z.; formal analysis, J.W., B.Z., and D.Z.; investigation, J.W., B.Z., and D.Z.; resources, H.Z.; data curation, Z.Y.; writing—original draft preparation, J.W.; writing—review and editing, J.W. and H.Z.; visualization, H.Z.; supervision, Z.Y. and B.Z.; project administration, J.W.; funding acquisition, J.W. and H.Z. All authors have read and agreed to the published version of the manuscript.

Funding

The current work was funded by the HuZhou Vocational & Technical College Special Exploration Project Funds for High-Level Talents under grant no. 2024TS04; and by the Huzhou Natural Science Foundation under grant no. 2023YZ01.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data will be made available on request.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Fu, C.; Han, X.; Zhang, Y.; Hu, J.; Du, J.; Wang, H. Synergistic functionality of metal–organic framework-cellulose composites structures for advanced high-performance energy materials. Chem. Eng. J. 2025, 503, 158384. [Google Scholar] [CrossRef]
  2. Hu, R.; Zhang, K.; Zou, H.; Gao, Z.; Luo, X.; Liu, X.; Wu, Z. Research progress on ti2alnb-based alloys and composites for aerospace applications. J. Alloys Compd. 2025, 1021, 179701. [Google Scholar] [CrossRef]
  3. Nyamekye, P.; Golroudbary, S.R.; Piili, H.; Luukka, P.; Kraslawski, A. Impact of additive manufacturing on titanium supply chain: Case of titanium alloys in automotive and aerospace industries. Adv. Ind. Manuf. Eng. 2023, 6, 100112. [Google Scholar] [CrossRef]
  4. Arifin, A.; Sulong, A.B.; Muhamad, N.; Syarif, J.; Ramli, M.I. Material processing of hydroxyapatite and titanium alloy (ha/ti) composite as implant materials using powder metallurgy: A review. Mater. Des. 2014, 55, 165–175. [Google Scholar] [CrossRef]
  5. Geng, K.; Lu, W.; Zhang, D.; Sakata, T.; Mori, H. Tensile properties of in situ synthesized titanium matrix composites reinforced by tib and nd2o3 at elevated temperature. Mater. Des. 2003, 24, 409–414. [Google Scholar] [CrossRef]
  6. Jeyaprakasam, S.; Gnanasekaran, M.; Magibalan, S.; Singh, R.P.; Mohanavel, V.; Kannan, S.; Giri, J.; Ali, M.S.; Barmavatu, P. Tribological, mechanical and microstructure characteristics of hybrid aluminium matrix composite containing titanium carbide (tic) and graphite particles. J. Mater. Res. Technol. 2024, 33, 5428–5489. [Google Scholar] [CrossRef]
  7. Etesami, S.A.; Fotovvati, B.; Asadi, E. Heat treatment of ti-6al-4v alloy manufactured by laser-based powder-bed fusion: Process, microstructures, and mechanical properties correlations. J. Alloys Compd. 2022, 895, 162618. [Google Scholar] [CrossRef]
  8. Liu, C.; Jin, K.; Ye, J.; Gao, X.; Wei, X.; Zhang, Z.; Peng, H. Additive manufacturing of (tib+tic)/ti6al4v composites with tailored network reinforcement architecture. Compos. Commun. 2023, 40, 101611. [Google Scholar] [CrossRef]
  9. Banerjee, D.; Williams, J.C. Perspectives on titanium science and technology. Acta. Mater. 2013, 61, 844–879. [Google Scholar] [CrossRef]
  10. Zhao, T.; Zhang, S.; Zhou, F.Q.; Zhang, H.F.; Zhang, C.H.; Chen, J. Microstructure evolution and properties of in-situ tic reinforced titanium matrix composites coating by plasma transferred arc welding (ptaw). Surf. Coat. Tech. 2021, 424, 127637. [Google Scholar] [CrossRef]
  11. Zhao, Z.; Guo, Y.; Du, W.; Bai, P.; Zhang, Z.; Wang, L.; Ma, K.; Zhang, S.; Han, X.; Yang, C. Corrosion behavior of sic/ti6al4v titanium matrix composites fabricated by slm. J. Mater. Res. Technol. 2024, 31, 534–542. [Google Scholar] [CrossRef]
  12. Karthik, G.M.; Janaki Ram, G.D.; Kottada, R.S. Friction deposition of titanium particle reinforced aluminum matrix composites. Mater. Sci. Eng. A 2016, 653, 71–83. [Google Scholar] [CrossRef]
  13. Sidhu, S.S.; Singh, H.; Gepreel, M.A. A review on alloy design, biological response, and strengthening of β-titanium alloys as biomaterials. Mater. Sci. Eng. C 2021, 121, 111661. [Google Scholar] [CrossRef]
  14. Srivastava, M.; Jayakumar, V.; Udayan, Y.; Sathishkumar, M.; Muthu, S.M.; Gautam, P.; Nag, A. Additive manufacturing of titanium alloy for aerospace applications: Insights into the process, microstructure, and mechanical properties. Appl. Mater. Today 2024, 41, 102481. [Google Scholar] [CrossRef]
  15. Li, G.; Ma, F.; Liu, P.; Qi, S.; Li, W.; Zhang, K.; Chen, X. Review of micro-arc oxidation of titanium alloys: Mechanism, properties and applications. J. Alloys Compd. 2023, 948, 169773. [Google Scholar] [CrossRef]
  16. Gao, X.; Zhang, Z.; Liu, L.; Tao, C. Microstructure and coloration mechanism of tc11 aerospace titanium alloy ultra-thin thermal oxide films. J. Mater. Res. Technol. 2024, 30, 5312–5322. [Google Scholar] [CrossRef]
  17. Pan, Y.; Li, W.; Lu, X.; Hayat, M.D.; Yin, L.; Song, W.; Qu, X.; Cao, P. Microstructure and tribological properties of titanium matrix composites reinforced with in situ synthesized tic particles. Mater. Charact. 2020, 170, 110633. [Google Scholar] [CrossRef]
  18. Li, N.; He, D.; Liu, D.; Ma, L.; He, C.; Xu, Y.; Yu, J. In-situ tib reinforced titanium matrix composite coatings prepared by laser cladding: Effect of tib2 content on microstructure, hardness and wear properties. J. Alloys Compd. 2025, 1010, 178215. [Google Scholar] [CrossRef]
  19. Zhao, S.; Wang, Y.; Chai, C.; Ran, R.; Peng, L.; Zhang, Y.; Fang, F.; Yuan, G. In-situ deformation mechanisms of a novel ti-5mo-4cr-1v-1zr metastable β titanium alloy. J. Mater. Sci. Technol. 2025, 212, 44–54. [Google Scholar] [CrossRef]
  20. Chen, H.; Mi, G.; Sun, Y.; Li, P. Unique grain refinement mechanism of graphene oxide reinforced high-temperature titanium alloy matrix composite. Mater. Today. Commun. 2024, 41, 110803. [Google Scholar] [CrossRef]
  21. Kunčická, L.; Kocich, R.; Lowe, T.C. Advances in metals and alloys for joint replacement. Prog. Mater. Sci. 2017, 88, 232–280. [Google Scholar] [CrossRef]
  22. Ragunath, S.; Radhika, N.; Krishna, S.A.; Pramanik, A. Microstructural, electrochemical, and hot corrosion analysis of cocrfecuti high entropy alloy reinforced titanium matrix composites synthesized by microwave sintering. Int. J. Lightweight Mater. Manuf. 2024, 8, 141–155. [Google Scholar] [CrossRef]
  23. Wu, J.; Chen, Y.; Du, Z.; Xie, H.; Liu, S.; Peng, Q.; Li, K. Enhancing the elevated temperature strength of titanium matrix composites through a novel (α + β) triplex heat treatment. Mater. Sci. Eng. A 2024, 890, 145884. [Google Scholar] [CrossRef]
  24. Zhang, X.; Chen, Z.; Liu, Z.; He, M.; Yang, Z.; Wang, J. Microstructure and enhanced mechanical properties of zrc/zr composites added by in-situ y2o3 reinforced particles. Vacuum 2022, 203, 111277. [Google Scholar] [CrossRef]
  25. Qi, J.; Chang, Y.; He, Y.; Sui, Y.; Wei, F.; Meng, Q.; Wei, Z. Effect of zr, mo and tic on microstructure and high-temperature tensile strength of cast titanium matrix composites. Mater. Des. 2016, 99, 421–426. [Google Scholar] [CrossRef]
  26. Srishti; Paras; Kumar, A. Ansys fluent-cfd analysis of a continuous single-slope single-basin type solar still. Green Technol. Sustain. 2024, 2, 100105. [Google Scholar]
  27. Carusotti, S.; Lombroni, R.; Fanelli, P.; Jackson, L.; Giorgetti, F.; Buxton, P.F.; Calabrò, G.; Romanelli, M.; de Villa Valdes, E.R. Structural behaviour characterization of st40 inner vacuum chamber (ivc2) during a plasma vde using ansys workbench. Fusion Eng. Des. 2023, 192, 113772. [Google Scholar] [CrossRef]
  28. Sabat, L.; Kundu, C.K. Flexural-torsional analysis of steel beam structures using ansys. Mater. Today Proc. 2023, in press. [Google Scholar] [CrossRef]
  29. Bayat, M.; Dong, W.; Thorborg, J.; To, A.C.; Hattel, J.H. A review of multi-scale and multi-physics simulations of metal additive manufacturing processes with focus on modeling strategies. Addit. Manuf. 2021, 47, 102278. [Google Scholar] [CrossRef]
  30. Aravind, E.S.; Kumar, T.R.M.; Kavithakani, A.; Chithra, K. Integrating ansys fluent simulation and aspen plus for efficient heavy metal ion removal with de-oiled cake. J. Water Process. Eng. 2024, 67, 106265. [Google Scholar] [CrossRef]
  31. Wang, J.; Yang, Z.; Zhou, B.; Zhang, H.; Cui, L.; Niu, Y.; Rui, X. In-depth study on tensile properties and finite element analysis of TiC in-situ formed Ti matrix composites with NbC and ZrC additions. J. Mater. Res. Technol. 2025, 35, 2188–2201. [Google Scholar] [CrossRef]
Figure 1. (a,b) Powder morphology of ZrC; (c,d) distribution of C and Zr elements in (b).
Figure 1. (a,b) Powder morphology of ZrC; (c,d) distribution of C and Zr elements in (b).
Coatings 15 00626 g001
Figure 2. (a,b) Powder morphology of NbC; (c,d) distribution of C and Nb elements in (b).
Figure 2. (a,b) Powder morphology of NbC; (c,d) distribution of C and Nb elements in (b).
Coatings 15 00626 g002
Figure 3. X-ray diffraction analysis patterns of TiC/Ti composites with different NbC contents [31].
Figure 3. X-ray diffraction analysis patterns of TiC/Ti composites with different NbC contents [31].
Coatings 15 00626 g003
Figure 4. SEM and EDS results showing the microstructure characteristics of TMCs with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Figure 4. SEM and EDS results showing the microstructure characteristics of TMCs with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Coatings 15 00626 g004aCoatings 15 00626 g004b
Figure 5. TEM Characterization of α-Ti and β-Ti phases in TMC3. (a) microstructural morphology image; (b) the selected area electron diffraction (SAED) pattern of the α-Ti phase; (c) the SAED pattern of the β-Ti phase.
Figure 5. TEM Characterization of α-Ti and β-Ti phases in TMC3. (a) microstructural morphology image; (b) the selected area electron diffraction (SAED) pattern of the α-Ti phase; (c) the SAED pattern of the β-Ti phase.
Coatings 15 00626 g005
Figure 6. TEM characterization of the interface between the TiC phase and the Ti matrix. (a) bright -field image; (b) HRTEM; (c) FFT of the corresponding transition region; (d) Inverse Fourier transform and atomic spacing.
Figure 6. TEM characterization of the interface between the TiC phase and the Ti matrix. (a) bright -field image; (b) HRTEM; (c) FFT of the corresponding transition region; (d) Inverse Fourier transform and atomic spacing.
Coatings 15 00626 g006
Figure 7. The calculated values of microhardness for TMC1–TMC4.
Figure 7. The calculated values of microhardness for TMC1–TMC4.
Coatings 15 00626 g007
Figure 8. The compressive stress–strain curve of TMC1–4 with different NbC additions.
Figure 8. The compressive stress–strain curve of TMC1–4 with different NbC additions.
Coatings 15 00626 g008
Figure 9. Compression fracture morphology of TMCs with different NbC additions. ((a,a1): 0 wt% NbC; (b,b1): 3wt% NbC; (c,c1): 6 wt% NbC; (d,d1): 9 wt% NbC).
Figure 9. Compression fracture morphology of TMCs with different NbC additions. ((a,a1): 0 wt% NbC; (b,b1): 3wt% NbC; (c,c1): 6 wt% NbC; (d,d1): 9 wt% NbC).
Coatings 15 00626 g009aCoatings 15 00626 g009b
Figure 10. Total deformation simulation results of TMC1–TMC4 with varying NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Figure 10. Total deformation simulation results of TMC1–TMC4 with varying NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Coatings 15 00626 g010
Figure 11. Equivalent stress distribution analysis in TMC1–TMC4 with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Figure 11. Equivalent stress distribution analysis in TMC1–TMC4 with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Coatings 15 00626 g011
Figure 12. Total deformation simulation profiles of TMC1–TMC4 at different NbC additions. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Figure 12. Total deformation simulation profiles of TMC1–TMC4 at different NbC additions. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Coatings 15 00626 g012
Figure 13. Equivalent stress simulation outcomes of TMC1–TMC4 with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Figure 13. Equivalent stress simulation outcomes of TMC1–TMC4 with different NbC contents. ((a), 0 wt% NbC; (b), 3wt% NbC; (c), 6 wt% NbC; (d), 9 wt% NbC).
Coatings 15 00626 g013
Table 1. Experimental raw materials (Wt %).
Table 1. Experimental raw materials (Wt %).
Material NameParticle SizePurity
Titanium particles3 × 3 mm99.9%
ZrC Powders1 μm99.9%
NbC Powders1 μm99.9%
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Wang, J.; Zhang, D.; Zhou, B.; Zhang, H.; Yang, Z. Microstructure Evolution and Properties of ZrC–NbC System Titanium Matrix Composites Based on Experiments and ANSYS Simulations. Coatings 2025, 15, 626. https://doi.org/10.3390/coatings15060626

AMA Style

Wang J, Zhang D, Zhou B, Zhang H, Yang Z. Microstructure Evolution and Properties of ZrC–NbC System Titanium Matrix Composites Based on Experiments and ANSYS Simulations. Coatings. 2025; 15(6):626. https://doi.org/10.3390/coatings15060626

Chicago/Turabian Style

Wang, Juan, Dayu Zhang, Baiqing Zhou, Haijun Zhang, and Zhong Yang. 2025. "Microstructure Evolution and Properties of ZrC–NbC System Titanium Matrix Composites Based on Experiments and ANSYS Simulations" Coatings 15, no. 6: 626. https://doi.org/10.3390/coatings15060626

APA Style

Wang, J., Zhang, D., Zhou, B., Zhang, H., & Yang, Z. (2025). Microstructure Evolution and Properties of ZrC–NbC System Titanium Matrix Composites Based on Experiments and ANSYS Simulations. Coatings, 15(6), 626. https://doi.org/10.3390/coatings15060626

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.