Next Article in Journal
Time-Domain Impedance Analysis on Passivation Quality of 316L Stainless Steel with Portable-Probe-Measured Potential Step Transient
Previous Article in Journal
Mechanistic Insights into Full Solid-Waste Activators for Enhancing the Performance of Blast Furnace Slag–Fly Ash Cementitious Composites
Previous Article in Special Issue
Microstructure and Mechanical Properties of As-Cast Al-10Ce-3Mg-xZn Alloys
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Study of the Influence of Gas Tungsten Arc (GTA) Welding on the Microstructure and Properties of Mg–Al–RE-Type Magnesium Alloys

by
Katarzyna N. Braszczyńska-Malik
Department of Materials Engineering, Faculty of Production Engineering and Materials Technology, Czestochowa University of Technology, 19 Armii Krajowej Ave., 42-200 Czestochowa, Poland
Materials 2025, 18(14), 3277; https://doi.org/10.3390/ma18143277
Submission received: 29 May 2025 / Revised: 4 July 2025 / Accepted: 9 July 2025 / Published: 11 July 2025
(This article belongs to the Collection Alloy and Process Development of Light Metals)

Abstract

The effects of the gas tungsten arc (GTA) welding process on the microstructure and microhardness of two Mg-5Al-3RE and Mg-5Al-5RE experimental alloys (RE—rare earth elements) are presented. Both alloys were gravity-cast in a steel mould and GTA-welded in the same conditions. Analyses of the alloys’ microstructure were carried out by scanning electron microscopy (SEM+EDX) as well as X-ray diffraction (XRD). In as-cast conditions; both alloys were mainly composed of α-Mg; Al11RE3; and Al10RE2Mn7 intermetallic phases. Additionally; α+γ eutectic (where γ is Al12Mg17) in the Mg-5Al-3RE alloy and an Al2RE phase in the Mg-5Al-5RE material were revealed. The same phase composition was revealed for both alloys after the GTA welding process. The results of the dendrite arm size (DAS) and Vickers microhardness measurements were also described. Both welded materials exhibited an intensive size reduction of the structural constituents after GTA welding. About 75% smaller values of the dendrite arm spacing were revealed in the fusion zones of the investigated materials than in the as-cast conditions. The GTA welding process also influenced the microhardness of the experimental alloys and increased them by about 21% compared to the base metal; which was the consequence of the refinement of the structural constituents.

1. Introduction

The development of magnesium alloys forces the search for modern technical solutions that cause a change in their microstructure and properties. Among them, welding technologies including laser welding [1,2,3,4,5,6,7], friction stir welding [8,9,10,11,12], tungsten inert gas (TIG) welding [13,14,15], or electron beam welding [16,17] processes have been recently widely investigated for magnesium alloys. Gas tungsten arc (GTA) welding (presented schematically in Figure 1) deserves special attention due to its economy and utility. This process is characterised by a flexibility of operation and short processing time, which results in time and energy saving, as well as processing precision [18,19,20,21]. The relatively small cost of equipment necessary for the GTA welding technique is also an undeniable advantage of using this process. Additionally, thanks to the very good quality of welds obtained in products after GTA welding, complications arising from weld defects such as weld spatter, porosity, and undercuts are minimized [22,23,24,25]. On the other hand, the fusion zone geometry can be designed thanks to the wide range of possible changes to the GTA welding parameters, which directly affects linear energy. Additionally, the choice of suitable welding parameters allowed the achievement of different size reductions of the microstructure in the fusion zone, which depends on the solidification conditions, especially the cooling rate [26]. It should also be added that magnesium alloys especially require special care during welding processes because of their high reactivity. Although shielding gas is typically used during the GTA process, its effect on the fusion zone in magnesium alloys has also been reported. Argon, helium, hydrogen, and nitrogen are used very often for GTA welding. Nevertheless, Marya et al. [27] concluded that helium, as a consequence of its high first ionization potential (24.6 eV), increases the constant-current voltage and creates a larger fusion zone than argon (15.6 eV).
Although there are several reports [1,18,28,29,30,31] describing the influence of GTA welding technology on magnesium alloys, the large majority of those investigations were concerned with commercial magnesium. In the presented work, the effect of the GTA welding process on the microstructure of two experimental Mg–Al–RE-type (RE—rare earth elements) alloys is presented. Even though aluminium constitutes a very important alloying element owing to its low price and advantageous effect on the strength properties or corrosion behaviour of magnesium alloys, it does not provide high-temperature strength, especially the poor creep properties of these alloys [32]. This set of properties results from the presence of a γ phase in the microstructure of Mg–Al-type alloys. The γ phase (also sometimes called β phase) is an intermetallic compound with an α-Mn-type cubic unit cell and a stoichiometric composition of Mg17Al12 (at 43.95 wt% Al). In the microstructure of Mg–Al-type alloys, a fully or partially divorced α+γ eutectic (where α is a magnesium solid solution) forms at a relatively low temperature equal to 710 K [32]. In order to especially improve the high-temperature properties of magnesium alloys, several alloy systems, focused on Mg–Al–third metal alloys, have been developed [33,34,35,36,37,38]. In Mg–Al–RE-type alloys, the γ phase is suppressed by the formation of mainly Al11RE3 (especially advantageous) and Al2RE intermetallic compounds. The real phase composition of an Mg–Al–RE-type alloy depends on the Al/RE ratio in its chemical composition and solidification conditions. These alloys are characterised by higher mechanical properties (especially after the high-pressure die casting process), including higher creep properties than those of Mg–Al-type alloys. They have also been investigated as a matrix alloy for magnesium composites [38,39,40]. It should also be noted that there are several reports describing the microstructure and properties of different Mg-Al-RE-type alloys based on single rare earth elements (Ce, La, Nd, Pr, etc.) [41,42,43,44,45,46]; however, using rare earth elements in the form of mischmetal is more economical. Additionally, it was reported [2] that rare earth elements reduced the tendency for porosity and cracking in magnesium castings. The main aim of this study is to analyse the microstructure and microhardness of two experimental cast Mg-5Al-3RE and Mg-5Al-5RE alloys after the GTA welding process. Two main commercial alloys from the Mg–Al–RE system, i.e., the AE42 and AE44 alloy (precisely, Mg-4Al-2.5RE-0.1Mn and Mg-4Al-3.9RE-0.3Mn, respectively), are the most common [47,48], although extensive research is being carried out on many experimental alloys with different ratios of aluminium to rare earth elements. Most of these studies concern the description of the primary microstructure (in as-cast conditions), including that obtained after the high-pressure casting process [35,48,49]. Nevertheless, it should also be noted that recent research also concerned the welding processes of various different magnesium alloys with rare-earth elements [50,51,52,53]. This work presents for the first time the results obtained after GTA welding of the new experimental alloys (from the Mg-Al-RE-type system with RE/Al ratios equal to 0.6 and 1) in order to illustrate both the possibility of applying the process to them and describing the obtained microstructure.

2. Materials and Methods

Two experimental alloys (Mg-5Al-3RE and Mg-5Al-5RE) with 5 wt% aluminium and 3 and 5 wt% rare earth elements were used in this study. The chemical composition of the investigated alloys is given in Table 1. Rare earth elements in the form of cerium-rich mischmetal (the composition according to the attestation was 54.8 wt% Ce, 23.8 wt% La, 16 wt% Nd, 5.4 wt% Pr, 0.16 wt% Fe, and 0.19 wt% Mg) were used. Additionally, a low volume fraction (i.e., 0.4 wt%) of manganese in magnesium with aluminium alloys was also used in order to reduce the iron content (as a harmful impurity) in the casts. The alloys were gravity-cast in steel moulds under the same conditions. The gas tungsten arc (GTA) welding process was conducted by means of a Falting 315 AC/DC instrument (OZAS, Opole, Poland) on a clean cast plate (free of oil and grease) of the dimensions 140 × 25 × 15 mm. The tungsten electrodes used in this study had a diameter of 2.4 mm (WT20 according to the DIN Standard). The shielding gas was helium with a flow rate of 20 L/min. The investigations were conducted utilizing the following welding parameters: 13 V voltage, 250 A current, and 12 mm/s welding speed.
A Brucker D8 Advance diffractometer (Bruker Corporation, Billerica, MA, USA) with CuKα X-ray radiation was employed in order to ascertain the phase composition of the investigated alloys after GTA welding. Reflexes from particular phases were identified according to ICDD PDF-4ţ cards [54]. For the GTA-welded materials, X-ray diffraction patterns were obtained from the fusion zone areas perpendicular to their depth, according to Figure 2.
Microstructure observations of the alloys in the initial stage and after GTA welding were carried out by means of a JOEL JSM-6610LV scanning electron microscope (SEM) (JOEL Ltd., Tokyo, Japan) with an energy-dispersive X-ray spectrometer (EDX) (Oxford Instruments, Abingdon, UK). The specimens for the microstructure investigations were prepared by standard metallographic procedures and, to reveal the microstructure, the specimens were etched in a 1% solution of HNO3 in C2H5OH for about 60 s.
The linear method of stereology was also used in order to determine the DAS (dendrite arm size) parameter, which can describe the microstructure changes caused by the GTA welding process. In this case, due to the kind of obtained microstructure, the DAS parameter corresponded to the average α-Mg phase size. Additionally, Vickers microhardness was determined by means of a Future-Tech FM-7 microhardness tester (Future-Tech Corp., Kawasaki, Japan) (load: 490.3 mN; time: 10 s). Average values were calculated based on 12 measurements for each material.

3. Results and Discussion

Figure 3 presents representative SEM micrographs of the microstructure of the investigated alloys in the initial stage (as-cast conditions). They consist of an α-Mg solid solution and an Al11RE3 intermetallic compound. In the microstructure of the Al-5Al-3RE alloy, a small volume fraction of the α+γ divorced eutectic is also visible, whereas this structural compound is practically below quantity sensitivity in the microstructure of the Al-5Al-5RE alloy. On the other hand, some amounts of the Al2RE intermetallic compound can be observed in the microstructure of the Al-5Al-5RE alloy, while this phase does not exist in the microstructure of the Al-5Al-3RE alloy. In the microstructure of both alloys, a ternary Al10RE2Mn7 intermetallic compound also formed owing to the presence of a low weight fraction of manganese in the chemical composition of the investigated materials.
The results presented in Figure 3 also illustrate the morphology of particular phases, which was identified by the EDX analyses. It should be noted, however, that the above-mentioned phases in the investigated alloys were also confirmed by XRD and TEM techniques because the high electron beam penetration during the EDX analyses of magnesium alloys prevents precise identification. The results of these examinations were presented in detail in previous works [34]. Nonetheless, thanks to the EDX results (presented in Figure 3) combined with the morphology analyses, a detailed description of individual structural constituents is possible. The Al11RE3 phase in the magnesium alloys has an acicular morphology, whereas the Al2RE and Al10RE2Mn7 intermetallic compounds are characterized by a blocky morphology [34,36]. As can also be easily seen by comparing Figure 3a,b and Figure 3c,d, with a decreasing Al/RE ratio, the volume fraction of the main Al11RE3 phase increases significantly. Additionally, the size of the DAS parameter also decreases, which is clearly visible during the comparison of Figure 3a with Figure 3c. The DAS parameters determined by quantitative metallography for the Al-5Al-3RE alloy was equal to 20.8 µm, while for the Al-5Al-5RE alloy, it was only 10.2 µm.
Figure 4a,b shows the SEM micrographs of the fusion boundary, fusion zone, and base material microstructure of the Mg-5Al-3RE alloy after GTA welding. Analogical images of the Mg-5Al-5RE alloy microstructure after GTA welding are presented in Figure 4c,d. In both cases, the fusion boundary is clearly visible.
Additionally, the fusion boundaries for both alloys are also presented at higher magnification in Figure 5a,b. It should also be noted that for the presented experimental alloys, distinct partially melted zones were not observed. In Mg–Al-type alloys, a wide partially melted zone (PMZ), located from the fusion boundary to the base metal, is observed very often [15,17,26,28,29], resulting from the low-melting point nature of the eutectic transformation, TE, of only 710 K (and also of the γ phase—about 723 K). For non-uniform solidified Mg-Al-type alloys, the difference between the liquidus (TL) and solidus temperatures (TE) is equal to about 463-433 K (depending on the Al weight fraction), which has an influence on the heat distribution below the fusion zone. Generally, in the partially melted zones, the α+γ eutectic is remelted and resolidified (varying in morphology), whereas the central areas of primary α-Mg dendrites do not change [26]. PMZ was also observed by Wagner et al. [13] in the Mg-6Zn alloy, which is also characterized by a very wide solidification range. In the presented Mg-5Al-3RE and Mg-5Al-5RE alloys, the γ phase is suppressed by the formation of mainly the Al11RE3 intermetallic phase. The calculated equilibrium liquidus temperature (according to ThermoCalc data [54]) is equal to 891 K for the Mg-5Al-3RE alloy and 888 K for the Mg-5Al-5RE alloy. The solidus temperature (according to the equilibrium condition) is 844 and 855 K for the Mg-5Al-3RE and Mg-5Al-5RE alloys, respectively. Therefore, the solidification range for the investigated alloys is considerably narrower (i.e., only 47–33 K) than for binary Mg-Al- or Mg–Zn-type alloys. Hence, the material was remelted only in the fusion zone.
Figure 6 displays the microstructure in the fusion zones of the investigated materials after the GTA welding process. It is clearly visible that the microstructure of both examined alloys in the fusion zone has a dendritic morphology. A higher magnification of the SEM allowed a detailed observation of particular phases, as shown in Figure 7, which also presents the results of EDX analyses from designated points marked on the relevant microstructure micrographs.
As a consequence of the high width and depth of the electron beam penetrating the magnesium alloys during the investigations, the obtained results from the EDX analyses are limited by some errors, such as the presence of magnesium in every examined point. In spite of this, based on the analyses of the presence of individual elements in the analysed structural constituents and their morphology, it is possible to identify the individual phases. Nevertheless, XRD investigations were carried out to confirm the phase composition of the fusions zones, the results of which are presented in Figure 8. The X-ray diffraction patterns obtained from the fusion zones did not reveal different phases to those observed in the base metals either, and confirmed the same structural constituents. During these analyses, the individual intermetallic compounds were identified based on the following phases: Al11Ce3 phase (Immm space group, a = 0.4389 nm, b = 1.0072 nm, and c = 1.3011 nm [54]), Al2Ce phase (Fd-3m space group, a = b=c = 0.8015 nm [54]), and Al10Ce2Mn7 phase (R-3m space group, a = b = 0.9040 nm, c = 1.3170 nm [54]).
By comparing the microstructure of the base metal (Figure 3) and fusion zone shown in Figure 6, it is also clearly visible that the dendrite arm size (DAS) was substantially reduced after GTA welding. The growth of dendrites in the fusion zones was hampered by the rapid cooling during GTA welding. Additionally, the cooling speed was induced by the good thermal conductivity and low capacity of magnesium alloys [26]. Figure 9 presents the differences in the DAS parameter between the base metal and fusion zone for both investigated alloys. As stated above, the difference in the DAS parameter between both studied alloys in as-cast conditions was 51%. The same influence of rare earth elements on the DAS values is also visible in the alloys after GTA welding. The difference in the DAS parameter between the welded alloys was 49% and the Mg-5Al-5RE alloy also exhibited a lower DAS value than the Mg-5Al-3RE alloy after GTA welding. It is well known that the DAS parameter depends on the solidification conditions, especially the cooling rate. Because both alloys were cast and GTA-welded under the same conditions, the influence of rare earth elements on the DAS value is unequivocal. Nonetheless, the GTA welding process caused a decrease in DAS by 74-75% in comparison to the as-cast investigated alloys.
Additionally, it can be noted that the dendrite arm size in the fusion zone of both experimental alloys was smaller than those obtained for the commercial Mg-Al alloy (AZ91) welded using the same GTA parameters, which was presented in a previous study [26]. On the other hand, the size of the other structural constituents was also significant reduced. The Al11RE3 intermetallic phase was visibly significantly finer in the fusion zones than in the base metals for both investigated alloys. Nonetheless, it should also be noted that the microstructure of the researched alloys after the GTA welding process was more homogeneous than that obtained after the high-pressure die casting process (in which a biomodal grain size distribution occurs very often). Nevertheless, the Mg-5Al-5RE alloy showed a greater microstructure refinement than the Mg-5Al-3RE alloy after both the GTA welding process presented in this paper and the high-pressure die-casting process described in [55]. Analogical relationships were obtained for different parameters described in [56].
Both the volume fraction of the Al11RE3 phase and the size of the microstructural constituents also affected in direct proportion the Vickers microhardness of the alloys. Figure 10 presents the differences between the HV0.05 values for the investigated alloys in as-cast conditions and after the GTA welding process. An increase in the mass fraction of rare earth elements in the Mg-5Al-3RE alloy in as-cast conditions caused a rise in this property by 12% in comparison to the Mg-5Al-3RE alloy. The same dependence between the microhardness values and rare earth elements in the alloys was observed in the fusion zone. The microhardness measured in the fusion zone of the AME505 alloy was 9% higher than in the fusion zone of the AME503 alloy. After the welding process, the Mg-5Al-3RE alloy had a microhardness equal to 75 HV0.05, whereas this property for the Mg-5Al-5RE alloy was equal to 85 HV0.05. The standard deviations of these values were 3.1 and 2.7 HV0.05, respectively. However, it should be noted that the GTA welding process caused growth in the microhardness by about 21% in comparison to the base metal for both investigated alloys. The obtained dependencies show that for the studied alloys, the degree of microstructure refinement (obtained after the GTA welding process) is also a significant factor influencing microhardness.
The presented results of analyses of the two experimental alloys from the Mg-Al-RE-system indicate that this type of magnesium alloy can be successfully surface-remelted by the gas tungsten arc welding process. Both alloys exhibited the same influence of the GTA welding process on the microstructure refinement and microhardness. Although the obtained growth in the microhardness of the Mg-5Al-3RE and Mg-5Al-5RE experimental alloys was not very high (about 21%), it should be taken into consideration that this result corresponds to those received for different magnesium alloys. Future studies should investigate in detail the influence of the GTA welding process on the corrosion resistance and tribological properties of this type of alloy.

4. Conclusions

The influence of the GTA welding process on the microstructure characterization of the Mg-5Al-3RE and Mg-5Al-5RE experimental alloys was investigated and the following results were revealed:
1. Two experimental Mg-Al-RE-type alloys were successfully GTA-welded and exhibited an intensive structure constituent size reduction. The DAS parameter in the melted zone for both alloys was about 75% lower than for the base metal.
2. The chemical composition of the examined alloys influenced the solidification range and prevented the formation of a partially melted zone observed in binary Mg–Al- or Mg–Zn-type alloys.
3. The GTA welding process caused an increase in microhardness by about 21% in comparison to the base metal for both investigated alloys.

Funding

This research received no external funding.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed at the corresponding author.

Conflicts of Interest

The author declares no conflicts of interest.

References

  1. Cao, X.; Jahazi, M.; Immarigeon, J.P.; Wallace, W. A review of laser welding techniques for magnesium alloys. J. Mater. Proc. Tech. 2006, 171, 188–204. [Google Scholar] [CrossRef]
  2. Abderrazak, K.; Kriaa, W.; Salem, W.B.; Mhiri, H.; Lepalec, G.; Autic, M. Numerical and experimental studies of molten pool formation during an interaction of a pulse laser (Nd:YAG) with a magnesium alloy. Opt. Laser Technol. 2009, 41, 470–480. [Google Scholar] [CrossRef]
  3. Jun, Y.; Sun, G.P.; Wang, H.-Y.; Jia, S.Q.; Jia, S.S. Laser (Nd:YAG) cladding of AZ91D magnesium alloys with Al + Si + Al2O3. J. Alloys Compd. 2006, 407, 201–207. [Google Scholar] [CrossRef]
  4. Xu, N.; Shen, J.; Xie, W.; Wang, L.; Wang, D.; Min, D. Abnormal distribution of microhardness in tungsten inert gas arc butt-welded AZ61 magnesium alloy plates. Mater. Charact. 2010, 61, 713–719. [Google Scholar] [CrossRef]
  5. DuPoint, J.N. On optimization of the powder plasma arc surfacing process. Metal. Mater. Trans. B 1998, 29, 932–934. [Google Scholar] [CrossRef]
  6. Quan, Y.J.; Chen, Z.H.; Gong, X.S.; Yu, Z.H. Effects of heat input on microstructure and tensile properties of laser welded magnesium alloy AZ31. Mater. Charact. 2008, 59, 1491–1497. [Google Scholar] [CrossRef]
  7. Zhu, J.; Li, L.; Liu, Z. CO2 and diode laser welding of AZ31 magnesium alloy. App. Sur. Sci. 2005, 247, 300–306. [Google Scholar] [CrossRef]
  8. Liang, G.L.; Zhou, G.; Yuan, S.Q. Study on hybrid heat source overlap welding of magnesium alloy AZ31B. Mater. Sci. Eng. A 2009, 499, 93–96. [Google Scholar] [CrossRef]
  9. Cao, X.; Jahazi, M. Effect of welding speed on the quality of friction stir welded butt joints of a magnesium alloy. Mater. Des. 2009, 30, 2033–2042. [Google Scholar] [CrossRef]
  10. Xie, G.M.; Ma, Z.Y.; Geng, L.; Chen, R.S. Microstructural evolution and mechanical properties of friction stir welded Mg–Zn–Y–Zr alloy. Mater. Sci. Eng. A 2007, 471, 63–68. [Google Scholar] [CrossRef]
  11. Chowdhury, S.M.; Chen, D.L.; Bhole, S.D.; Cab, X.; Powidajko, E.; Weckman, D.C.; Zhou, Y. Tensile properties and strain-hardening behavior of double-sided arc welded and friction stir welded AZ31B magnesium alloy. Mater. Sci. Eng. A 2010, 527, 2951–2961. [Google Scholar] [CrossRef]
  12. Sato, Y.S.; Hwan, S.; Park, C.; Michiuchi, M.; Kokawa, H. Constitutional liquation during dissimilar friction stir welding of Al and Mg alloys. Scripta Mater. 2004, 50, 1233–1236. [Google Scholar] [CrossRef]
  13. Wagner, D.C.; Chai, X.; Tang, X.; Kou, S. Liquation cracking in arc and friction-stir welding of Mg-Zn Alloys. Matall. Mater. Trans. A 2015, 46, 315–327. [Google Scholar] [CrossRef]
  14. Huang, R.-S.; Liu, L.-M.; Song, G. Infrared temperature measurement and interference analysis alloys in hybrid laser-TIG welding process. Mater. Sci. Eng. A 2007, 447, 239–243. [Google Scholar] [CrossRef]
  15. Min, D.; Shen, J.; Lai, S.; Chen, J. Effect of heat input on the microstructure and mechanical properties of tungsten inert gas arc butt-welded AZ61 magnesium alloy plates. Mater. Charact. 2009, 60, 1583–1590. [Google Scholar] [CrossRef]
  16. Chi, C.-T.; Chao, C.-G.; Liu, T.-F.; Wang, C.-C. A study of weldability and fracture modes in electron beam weldments of AZ series magnesium alloys. Mater. Sci. Eng. A 2006, 435–436, 672–680. [Google Scholar] [CrossRef]
  17. Luo, Y.; Liu, J. Microstructural evolution in AZ91D magnesium alloy during electron beam welding. Vacuum 2011, 85, 1004–1010. [Google Scholar] [CrossRef]
  18. Srinivasan, S.; Ravi Bharath, R.; Atrens, A.; Srinivasan, P.B. Fusion Welding of Magnesium Alloys: Process Variants, Metallurgical Challenges, and Structure–Property Relationships—A Critical Review. JMEP 2025, 34, 9247–9280. [Google Scholar] [CrossRef]
  19. Shen, J.; You, G.; Long, S.; Pan, F. Abnormal macropore formation during double-sided gas tungsten arc welding of magnesium AZ91D alloy. Mater. Charact. 2008, 59, 1059–1065. [Google Scholar] [CrossRef]
  20. Liu, L.; Dong, C. Gas tungsten-arc filler welding of AZ31 magnesium alloy. Mater. Letters 2006, 60, 2194–2197. [Google Scholar] [CrossRef]
  21. Strzelecka, M.; Iwaszko, J.; Malik, M.; Tomczyński, S. Surface modification of the AZ91 magnesium alloy. Arch. Civ. Mech. Eng. 2015, 15, 854–861. [Google Scholar] [CrossRef]
  22. Wenbin, D.; Haiyan, J.; Xiaoqin, Z.; Dehui, L.; Shoushan, Y. Microstructure and mechanical properties of GTA surface modified composite layer on magnesium alloy AZ31 with SiCP. J. Alloys Compd. 2007, 429, 233–241. [Google Scholar] [CrossRef]
  23. Winzer, N.; Xu, P.; Bender, S.; Gross, T.; Unger, W.E.S.; Cross, C.E. Stress corrosion cracking of gas-tungsten arc welds in continuous-cast AZ31Mg alloy sheet. Corros. Sci. 2009, 51, 1950–1963. [Google Scholar] [CrossRef]
  24. Stern, A.; Munitz, A. Partially melted zone microstructural characterization from gas tungsten-arc bead on plate welds of magnesium AZ91 alloy. J. Mater. Sci. Letters 1999, 18, 853–855. [Google Scholar] [CrossRef]
  25. Liao, J.; Yamamoto, N.; Nakata, K. Gas tungsten arc welding of fine-grained AZ31B magnesium alloys made by powder metallurgy. Mater. Des. 2014, 56, 460–467. [Google Scholar] [CrossRef]
  26. Braszczyńska-Malik, K.N.; Mróz, M. Gas-tungsten arc welding of AZ91 magnesium alloy. J. Alloys Compd. 2011, 509, 9951–9958. [Google Scholar] [CrossRef]
  27. Marya, M.; Edwords, G.R.; Liu, S. An investigation on the effects of gases in GTA welding of a wrought AZ80 magnesium alloy. Weld. J. July 2004, 83, 203-S. [Google Scholar]
  28. Zhu, T.; Chen, Z.W.; Gao, W. Microstructure formation in partially melted zone during gas tungsten arc welding of AZ91 Mg cast alloy. Mater. Charact. 2008, 59, 1550–1558. [Google Scholar] [CrossRef]
  29. Munitz, A.; Cotler, C.; Stern, A.; Kohn, G. Mechanical properties and microstructure of gas tungsten arc welded magnesium AZ91D plates. Mater. Sci. Eng. A 2001, 302, 68–73. [Google Scholar] [CrossRef]
  30. Ben-Hamu, G.; Eliezer, D.; Cross, C.E.; Böllinghaus, T. The relation between microstructure and corrosion behavior of GTA welded AZ31B magnesium sheet. Mater. Sci. Eng. A 2007, 452–453, 210–218. [Google Scholar] [CrossRef]
  31. Zhou, W.; Le, Q.; Shi, Y.; Liao, Q.; Wang, T.; Zou, Q.; Aranas, C., Jr. Enhencement of mechanical properties of GTAW joints for AZ63 magnesium Alloys by post weld hat treatment. J. Mater. Sci. Techn. 2024, 169, 251–263. [Google Scholar] [CrossRef]
  32. Braszczyńska-Malik, K.N. Precipitates of α-Mg17Al12 phase in AZ91 alloy. In Magnesium Alloys—Design, Processing and Properties; Czerwinski, F., Ed.; INTECH Open Access Publisher: London, UK, 2011; Chapter 5; pp. 95–112. [Google Scholar]
  33. Dieringa, H.; Hort, N.; Kainer, K.U. Investigation of minimum creep rates and stress exponents calculated from tensile and compressive creep data of magnesium alloy AE42. Mater. Sci. Eng. A 2009, 510–511, 382–386. [Google Scholar] [CrossRef]
  34. Braszczyńska-Malik, K.N.; Grzybowska, A. Microstructure of Mg-5Al-0.4Mn-xRE (x = 3 and 5 wt.%) alloys in as-cast conditions and after annealing. J. Alloys Compd. 2016, 663, 172–179. [Google Scholar] [CrossRef]
  35. Dargusch, M.S.; Zhu, S.M.; Nie, J.F.; Dunlop, G.L. Microstructural analysis of the improved creep resistance of a die-cast magnesium–aluminium–rare earth alloy by strontium additions. Scr. Mater. 2009, 60, 116–119. [Google Scholar] [CrossRef]
  36. Braszczyńska-Malik, K.N.; Grzybowska, A. Influence of phase composition on microstructure and properties of Mg-5Al-0.4Mn-xRE (x = 0, 3 and 5 wt.%) alloys. Mater. Charact. 2016, 115, 14–22. [Google Scholar] [CrossRef]
  37. Nami, B.; Razavi, H.; Mirdamadi, S.; Shabestari, S.G.; Miresmaeili, S.M. Effect of Ca and rare earth elements on impression creep properties of AZ91 magnesium alloy. Metal. Mater. Trans. A 2010, 41, 1973–1982. [Google Scholar]
  38. Braszczyńska-Malik, K.N. Types of component interfaces in metal matrix composites on the example of magnesium matrix composites. Materials 2021, 14, 5182. [Google Scholar] [CrossRef]
  39. Braszczyńska-Malik, K.N.; Przełożyńska, E. The influence of Ti particles on microstructure and mechanical properties Of Mg-5Al-5RE matrix alloy composite. J. Alloys Compd. 2017, 728, 600–606. [Google Scholar] [CrossRef]
  40. Braszczyńska, K.N. Contribution of SiC particles to the formation of the structure of Mg-3 wt.% RE cast composites. Z. Für Met. 2003, 94, 144–148. [Google Scholar] [CrossRef]
  41. Wang, X.; Du, W.; Liu, K.; Wang, Z.; Li, S. Microstructure, tensile properties and creep behaviors of as-cast Mg–2Al–1Zn–xGd (x = 1, 2, 3, and 4 wt.%) alloys. J. Alloys Compd. 2012, 522, 78–84. [Google Scholar] [CrossRef]
  42. Qiu, W.; Han, E.; Liu, L. Microstructure and mechanical properties of Mg-3Al-1Zn-xRE alloys. J. Mater. Sci. Technol. 2009, 25, 356–360. [Google Scholar]
  43. Zhang, J.; Liu, S.; Leng, Z.; Zhang, M.; Meng, J.; Wu, R. Microstructure and mechanical properties of heat-resistant HPDC Mg-4Al-based alloys containing cheap misch metal. Mater. Sci. Eng. A 2011, 528, 2670–2677. [Google Scholar] [CrossRef]
  44. Zheng, X.; Wang, L.; Wang, J.; Wu, Y.; Ning, Z. Microstructure and mechanical properties of Mg-4Al-4Nd-0.5Zn-0.3Mn alloy. Mater. Sci. Eng. A 2009, 515, 98–101. [Google Scholar] [CrossRef]
  45. Braszczyńska-Malik, K.N. Some mechanical properties of experimental Mg-Al-RE-Mn magnesium alloys. Arch. Foundry Eng. 2014, 14, 13–16. [Google Scholar] [CrossRef]
  46. Zhang, J.; Liu, K.; Fang, D.; Qiu, X.; Tang, D.; Meng, J. Microstructure, tensile properties and creep behavior of high-pressure die-cast Mg-4Al-4RE-0.4Mn (RE = La, Ce) alloys. J. Mater. Sci. 2009, 44, 2046–2054. [Google Scholar] [CrossRef]
  47. Huang, Y.D.; Dieringa, H.; Hort, N.; Maier, P.; Kainer, K.U.; Liu, Y.L. Evolution of microstructure and hardness of AE42 alloy after heat treatment. J. Alloys Comp. 2008, 463, 238–245. [Google Scholar] [CrossRef]
  48. Feng, L.; Dong, X.; Xia, M.; Zhu, X.; Ji, G.; Yang, H.; Wang, B.; Nyberg, E.A.; Ji, S. Development of high thermal conductivity, enhanced strength and cost-effective die-cast Mg alloy compared with AE44 alloy. J. Mater. Res. Technol. 2023, 22, 2955–2966. [Google Scholar] [CrossRef]
  49. Braszczyńska-Malik, K.N. Mg-Al-RE magnesium alloys for high-pressure die-casting. Arch. Foundry Eng. 2014, 14, 49–52. [Google Scholar] [CrossRef]
  50. Lakshmikhanth, R.S.; Lakshminarayanan, A.K. On the mechanical, microstructural, and corrosion properties of pulsed gas tungsten arc and friction stir welded RZ5 rare earth grade magnesium alloy. Mater. Res. Express 2022, 9, 126507. [Google Scholar] [CrossRef]
  51. Eftekhar, A.H.; Sadrossadat, S.M.; Reihanian, M. Effect of heat input on microstructure and mechanical properties of TIG-welded semisolid cast AXE622 Mg alloy. Mater. Charact. 2022, 184, 111692. [Google Scholar] [CrossRef]
  52. Wang, Q.; Tong, X.; Wu, G.; Zhan, J.; Qi, F.; Zhang, L.; Liu, W. Microstructure and strengthening mechanism of TIG welded joints of a Mg-Nd-Gd alloy: Effects of heat input and pulse current. Mater. Sci. Eng. A 2023, 869, 144816. [Google Scholar] [CrossRef]
  53. Zhou, W.; Le, Q.; Liao, Q.; Shi, Y.; Wang, T.; Hu, W. Study of GTA-welded joints of ZW61 magnesium alloy—effect of welding current on the microstructure and mechanical properties. Weld. J. 2025, 104, 17–24. [Google Scholar] [CrossRef]
  54. Powder Diffraction File; PDF-4 + 2015; International Centre for Diffraction Data (ICDD): Pennsylvania, PA, USA, 2015.
  55. Braszczyńska-Malik, K.N. Effect of high-pressure die casting on structure and properties of Mg-5Al-0.4Mn-xRE (x = 1, 3 and 5wt%) experimental alloys. J. Alloys Compd. 2017, 694, 841–847. [Google Scholar] [CrossRef]
  56. Braszczyńska-Malik, K.N. Magnesium Alloys and Composites on Their Matrix (Oryg. Title: Stopy Magnezu i Kompozyty na Ich Osnowie), 1st ed.; Czestochowa University Publisher: Czestochowa, Poland, 2017; pp. 82–133. ISBN 978-83-7193-674-6. (In Polish) [Google Scholar]
Figure 1. Scheme of gas tungsten arc (GTA) welding.
Figure 1. Scheme of gas tungsten arc (GTA) welding.
Materials 18 03277 g001
Figure 2. Scheme of researched areas.
Figure 2. Scheme of researched areas.
Materials 18 03277 g002
Figure 3. Microstructure of Mg-5Al-3RE alloy ((a,b): SEM micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): SEM micrographs taken at different magnifications) under as-cast conditions with EDX results obtained from designated points.
Figure 3. Microstructure of Mg-5Al-3RE alloy ((a,b): SEM micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): SEM micrographs taken at different magnifications) under as-cast conditions with EDX results obtained from designated points.
Materials 18 03277 g003
Figure 4. SEM micrographs presenting base metal, fusion boundary, and fusion zone after GTA welding of Mg-5Al-3RE alloy ((a,b): micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): micrographs taken at different magnifications).
Figure 4. SEM micrographs presenting base metal, fusion boundary, and fusion zone after GTA welding of Mg-5Al-3RE alloy ((a,b): micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): micrographs taken at different magnifications).
Materials 18 03277 g004
Figure 5. Microstructure of fusion boundary after GTA welding of Mg-5Al-3RE alloy (a) and Mg-5Al-5RE alloy (b), SEM.
Figure 5. Microstructure of fusion boundary after GTA welding of Mg-5Al-3RE alloy (a) and Mg-5Al-5RE alloy (b), SEM.
Materials 18 03277 g005
Figure 6. Microstructure of Mg-5Al-3RE alloy ((a,b): micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): micrographs taken at different magnifications) after GTA welding process (areas form fusion zones), SEM.
Figure 6. Microstructure of Mg-5Al-3RE alloy ((a,b): micrographs taken at different magnifications) and Mg-5Al-3RE alloy ((c,d): micrographs taken at different magnifications) after GTA welding process (areas form fusion zones), SEM.
Materials 18 03277 g006
Figure 7. SEM micrographs of Mg-5Al-3RE alloy ((a,b): SEM micrographs taken from different areas of fusion zone) and Mg-5Al-3RE alloy ((c,d): SEM micrographs taken at different areas of fusion zone) after GTA welding process with EDX results obtained from designated points.
Figure 7. SEM micrographs of Mg-5Al-3RE alloy ((a,b): SEM micrographs taken from different areas of fusion zone) and Mg-5Al-3RE alloy ((c,d): SEM micrographs taken at different areas of fusion zone) after GTA welding process with EDX results obtained from designated points.
Materials 18 03277 g007
Figure 8. X-ray diffraction patterns of Mg-5Al-3RE and Mg-5Al-5RE alloys after GTA welding process (from fusion zones).
Figure 8. X-ray diffraction patterns of Mg-5Al-3RE and Mg-5Al-5RE alloys after GTA welding process (from fusion zones).
Materials 18 03277 g008
Figure 9. Comparison of DAS parameter values of investigated alloys in as-cast conditions and after GTA welding process with detailed results obtained from fusion zones of Mg-5Al-3RE and Mg-5Al-5RE alloy.
Figure 9. Comparison of DAS parameter values of investigated alloys in as-cast conditions and after GTA welding process with detailed results obtained from fusion zones of Mg-5Al-3RE and Mg-5Al-5RE alloy.
Materials 18 03277 g009
Figure 10. Comparison of microhardness values of investigated alloys in as-cast conditions and after GTA welding process.
Figure 10. Comparison of microhardness values of investigated alloys in as-cast conditions and after GTA welding process.
Materials 18 03277 g010
Table 1. Nominal chemical composition of investigated magnesium alloy.
Table 1. Nominal chemical composition of investigated magnesium alloy.
AlloyChemical Composition wt%
AlREMnMg
Mg-5Al-3RE530.4balance
Mg-5Al-5RE550.4balance
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Braszczyńska-Malik, K.N. Study of the Influence of Gas Tungsten Arc (GTA) Welding on the Microstructure and Properties of Mg–Al–RE-Type Magnesium Alloys. Materials 2025, 18, 3277. https://doi.org/10.3390/ma18143277

AMA Style

Braszczyńska-Malik KN. Study of the Influence of Gas Tungsten Arc (GTA) Welding on the Microstructure and Properties of Mg–Al–RE-Type Magnesium Alloys. Materials. 2025; 18(14):3277. https://doi.org/10.3390/ma18143277

Chicago/Turabian Style

Braszczyńska-Malik, Katarzyna N. 2025. "Study of the Influence of Gas Tungsten Arc (GTA) Welding on the Microstructure and Properties of Mg–Al–RE-Type Magnesium Alloys" Materials 18, no. 14: 3277. https://doi.org/10.3390/ma18143277

APA Style

Braszczyńska-Malik, K. N. (2025). Study of the Influence of Gas Tungsten Arc (GTA) Welding on the Microstructure and Properties of Mg–Al–RE-Type Magnesium Alloys. Materials, 18(14), 3277. https://doi.org/10.3390/ma18143277

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.