The Effect of Mold Structure and Cooling Parameters on Heat Transfer during Billet High-Speed Continuous Casting
Previous Article in Journal
High-ZT Due to the Influence of Copper in Ti(Ni1-xCux)Sn
Previous Article in Special Issue
Fluid Flow in Continuous Casting Mold for Ultra-Wide Slab
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Crystallization of Slag Films of CaO-Al2O3-BaO-CaF2-Li2O-Based Mold Fluxes for High-Aluminum Steels’ Continuous Casting

School of Materials and Energy Engineering, Guizhou Institute of Technology, Guiyang 550003, China
*
Authors to whom correspondence should be addressed.
Materials 2023, 16(5), 1903; https://doi.org/10.3390/ma16051903
Submission received: 1 December 2022 / Revised: 2 January 2023 / Accepted: 24 February 2023 / Published: 25 February 2023
(This article belongs to the Special Issue Metallurgical Process Simulation and Optimization2nd Volume)

Abstract

:
In this study, solidified films of CaO-Al2O3-BaO-CaF2-Li2O-based mold fluxes with different contents of Al2O3 addition were acquired by immersing an improved water-cooled copper probe in bulk molten slags. This probe can obtain films with representative structures. Different slag temperatures and probe immersion times were employed to investigate the crystallization process. The crystals in the solidified films were identified using X-ray diffraction, the morphologies of the crystals were observed using optical microscopy and scanning electron microscopy, and the kinetic conditions, especially the activation energy of devitrified crystallization in glassy slags, were calculated and discussed based on the differential scanning calorimetry. The results indicated that after adding extra Al2O3, the growing speed and thickness of the solidified films increased, and more time was required for the film thickness to reach a steady state. In addition, fine spinel (MgAl2O4) precipitated in the films at the early stage of solidification after adding 10 wt% of extra Al2O3. Together with LiAlO2, spinel (MgAl2O4) acted as nuclei for the precipitation of BaAl2O4. The apparent activation energy of initial devitrified crystallization decreased from 314.16 KJ/mol (original slag) to 297.32 KJ/mol (5 wt% Al2O3 added) and 269.46 KJ/mol (10 wt% Al2O3 added). The crystallization ratio of the films also increased after adding extra Al2O3.

1. Introduction

Mold fluxes are essential materials applied in the continuous casting of steels, which are added to molds during casting and melted to form a slag pool on liquid steel [1,2,3]. Under the action of mold oscillation, molten fluxes in the slag pool flow into the gap between the initial steel shells and water-cooled molds to form the liquid slag film (at the steel shell side) and solid slag film (initially, as a glassy state and then devitrified, at the mold side). The liquid film lubricates the contact between the mold and steel shells for a smooth manufacturing process, whereas the solid film controls the heat flux from the steel shells to the mold for high-quality slab surfaces [4,5,6]. Thus, the structure and properties of the slag films of mold fluxes are of critical importance.
In the continuous casting of high-Al transformation-induced plasticity (TRIP) and twinning-induced plasticity (TWIP) steels, the Al in liquid steel can react with some components in the molten mold flux, especially SiO2, dramatically changing the composition of the liquid slag pool and the characteristics of the slag films [7,8,9]. To solve this problem, non-reactive mold fluxes without SiO2 and with low content of other active components have been developed; for example, CaO-Al2O3-based mold fluxes have been proposed as substitutes for conventional CaO-SiO2-CaF2-based ones. The properties of CaO-Al2O3-based mold fluxes have been reported, including viscosity–temperature features, solidification processes, heat conduction of solid slag films, and the reaction of molten slags with steels [10,11,12,13,14,15,16]. Numerous CaO-Al2O3-based mold fluxes have similar viscosity and melting temperature to the conventional CaO-SiO2-CaF2-based slags. However, their lubricating effect is insufficient during the continuous casting of high-Al steels as sticking or breakout occurs, which significantly limits the industrial applications of CaO-Al2O3-based mold fluxes. One accepted explanation for the insufficient lubrication is that the overdeveloped slag rims block the slag channel at the meniscus and prevent the liquid slag in pools from flowing into this channel for efficient lubrication [17,18]. In addition, transferring the slag system from CaO-SiO2-CaF2 to CaO-Al2O3 changes the structures of solid slag films despite the similar physical properties of the slags. This phenomenon has been reported in our previous work on conventional mold fluxes for peritectic steels and fluorine-free mold fluxes [19,20].
Therefore, it is critical to understand the slag film evolution of CaO-Al2O3-based mold fluxes. Researchers have attempted to explore the solidification and devitrification of CaO-Al2O3-based slag films [11,12,13]. However, structures of solid films strongly depend on the cooling conditions. The conventional “water-cooled probe” cannot obtain slag films with representative or similar structures to the films obtained in casting molds [21,22]. Thus, there are very limited reports on the structural evolution, such as thickness growth speed, devitrification features, the roughness of surfaces in contact with molds, and the porosity of the solid slag films of CaO-Al2O3-based mold fluxes under cooling conditions similar to those in molds.
Crystallization in solid slag films (containing devitrified and solidified crystals) plays a key role in controlling the heat flux by reflecting and scattering infrared rays from steel shells [23]. In addition, crystallization in glassy films potentially increases the roughness of CaO-Al2O3-based film surfaces in contact with the mold wall (although this is insignificant in CaO-SiO2-CaF2-based slag films) [19]. Thus, this work aims to reveal the crystallization, especially the devitrified crystallization features, of typical CaO-Al2O3-based slag films similar in cooling conditions to films in molds and their possible influence on the casting process.
To obtain slag films with representative structures and study their evolution process, an optimized water-cooled copper probe was adopted in this work. It has been proven to yield solid slag films with structures similar to those obtained in molds. The structure, characteristics, and advantages of this optimized water-cooled probe can be found in previous studies [21,22].

2. Materials and Methods

A typical CaO-Al2O3-based mold flux was selected as the basis of this study (No. 1 slag in Table 1). To adjust the physical properties of the slag, fusion agents (BaO, CaF2, LiF, Li2O, B2O3, and MgO) were added. As endogenous inclusions containing Al2O3 in liquid steel can be absorbed by molten mold fluxes and increase the actual Al2O3 content in slag films, 5 wt% and 10 wt% of extra Al2O3 were added to the typical CaO-Al2O3-based mold fluxes (as No. 2 and No. 3, respectively) to reveal the effect of Al2O3 absorption on the crystallization process. The slags for the experiments were prepared using analytical-grade reagents (CaCO3, Al2O3, BaCO3, CaF2, LiF, Li2CO3, B2O3, and MgO). The reagents were loaded into a high-purity graphite crucible and pre-melted in a resistance furnace at 1300 °C, which were then poured and quenched in a water-cooled copper plate.
For each solidification experiment, 300 g of pre-melted slag lump was loaded into a high-purity graphite crucible with an inner diameter of 60 mm and melted in a resistance furnace. The optimized water-cooled copper probe with a large width–thickness ratio (20 mm wide, 15 mm tall, and 6.35 mm thick) was immersed in liquid slag to acquire a solid slag film. To study the effect of slag temperature on film crystallization, three different slag temperatures (1300 °C, 1350 °C, and 1400 °C) were used. In addition, different probe immersion times (7, 15, 30, 60, and 90 s) were adopted to investigate the evolution processes.

Measurements and Analysis

The thickness of the slag films was measured using a point micrometer. For each film sample acquired on the wide face of the probe, six measurements near the film center were adopted. The average value of these six measurements was taken as the film thickness. The crystallization process was investigated by inspecting the cross-sections of the films using optical microscopy and scanning electron microscopy (SEM, FEI Company, Nova Nanosem 450, Hillsboro, OR, USA) with energy-dispersive spectroscopy (EDS). Cross-section samples for SEM measurements were prepared by mounting solid films into resin, polishing with alumina suspensions, and coating with Au. The crystals in the films were identified through X-ray diffraction (XRD, Cu Kα, Rigaku Miniflex 600, Tokyo, Japan) after grinding the solid films into powder. The precipitation ratio of various crystals in the slag films was measured using EDS on a cross-section area of 4 mm2 for each sample.
The kinetic conditions of the film devitrification were investigated using differential scanning calorimetry (DSC, NETZSCH STA 449 F3, Selb, Germany). Samples for DSC measurements were prepared by grinding pre-melted slag (quenched in a glassy state) into a powder with a diameter of less than 74 μm. Four different heating rates (5, 15, 25, and 35 °C/min) were applied for DSC measurements. The crystallization activation energy of glassy slag can be calculated using the Kissinger equation [24], as shown in Equation (1).
l n β T p 2 = A E K R T P
where β is the heating rate, TP is the temperature of the first peak on the DSC heating curve (the temperature of the obvious initial crystallization), A is a constant related to the system characteristics, EK is the apparent activation energy of devitrified crystallization, and R is the gas constant.

3. Results and Discussion

3.1. Evolution of Thickness and Devitrification of Slag Films

The thicknesses of the obtained slag films are listed in Table 2. When the solidification time was short, especially 7 s, some films could not be obtained because they did not tightly adhere to the water-cooled probe, or the adhered film was incomplete. As shown in Figure 1, when the slag temperature was 1350 °C, the thickness of No. 1 slag films reached a steady state after approximately 60 s solidification. As the Al2O3 content increased from No. 1 slag to No. 3 slag, the thickness of the solid films increased dramatically and an extended time was required to reach a steady thickness. With a decrease in slag temperature, the film thickness increased significantly, indicating that the temperature fluctuation of the liquid slag could cause unevenness of the solidified slag films, especially for No. 3 slag.
Figure 2 shows a typical devitrification layer in a solid slag film. In addition to the labeled devitrified crystallization layer, fine crystals started to precipitate on the probe side (Figure 2b). Obvious cracks with healing signs and isolated flat hole chains were evident, consistent with the observation in F-free slag films in previous works [25]. The formation and healing of these cracked surfaces could cause heat flux fluctuations, especially during the early stage of solidification. This was partly due to the shrinkage of the nearby devitrified crystallization. Notably, some devitrified crystals were dispersed in the glassy films, as shown in Figure 3; thus, it is difficult to measure the thickness of the devitrification layer.

3.2. Crystals in Slag Films

The XRD patterns of typical slag film powders are shown in Figure 4 and the major crystal phases are summarized in Table 3. Calcium fluoride, lithium aluminate, and barium aluminate were the major crystals in most of the films. In the films with an extra 10% alumina (No. 3 slag), spinel (MgAl2O4) with a high melting temperature was detected.
To verify the existence of spinel, the cross-section of No. 3 slag film (devitrified parts) was inspected using SEM-EDS. Typical backscattered SEM images and the corresponding elemental maps are shown in Figure 5 and Figure 6, respectively. Based on the previous X-ray diffraction results presented in Table 3 (to identify the kind of precipitated crystals in films) and the corresponding elemental maps shown in Figure 6, precipitated calcium fluoride (containing Ca and F) and spinel (containing Mg, Al and O) were identified. The dark area around the calcium fluoride indicated that the crystals did not solidify in the liquid slag but precipitated in the glassy film. In addition to the labeled spinel, very fine spinel crystals were observed in the film (circle in Figure 5). The EDS map (Figure 6) revealed that Mg, Al, and O were concentrated in the circled area. The fine spinel particles precipitated at the solidification front, especially in the liquid slag film, could increase the apparent viscosity of the film, which was unfavorable for lubrication. This increased viscosity was also one of the reasons for the fast-growing film thickness.
In this study, only 2 wt% MgO was added and fine spinel crystals were detected in the slag, indicating that the absorption of Al2O3 from liquid steel or MgO from raw materials of slags and corroded refractory should be restricted.
It should be noted that massive cracks were observed around nearly all calcium fluoride crystals. Further research is required to investigate the effects of cracks on the thermal resistance of the solid slag films.
Table 3 reveals the precipitation sequence of crystals. For No. 1 slag, CaF2 and LiAlO2 precipitated first followed by BaAl2O4 when the probe immersion time exceeded 60 s. For No. 3 slag, spinels precipitated at a very early stage with CaF2 and LiAlO2 followed by BaAl2O4. Because barium ions are larger than the other ions, their diffusion for crystallization requires more energy and time. This is one of the reasons that barium oxide can partially replace calcium oxide to decrease the crystallization capacity of mold fluxes under certain circumstances, especially mold fluxes for alloy steel casting to dissolve various non-metallic inclusions. Figure 7 shows BaAl2O4 precipitated on the LiAlO2 core (only Al and O were detected at this core using EDS point analysis). As Li cannot be detected using EDS, a distribution map of Li is not presented.

3.3. Kinetic Conditions of Crystallization

Typical DSC curves of the No. 1 mold flux powder (glassy state) at different heating rates are shown in Figure 8. With an increase in heating rates from 5 °C/min to 35 °C/min, the initial temperature of apparent devitrification increased from 622 °C to 664 °C. Based on the Kissinger relationship in Equation (1), the plot between ln(β/Tp2) and 1/TP is shown in Figure 9. For No. 1 slag, the calculated apparent activation energy of devitrified crystallization was 314.16 KJ/mol. Based on the same methods, the calculated apparent activation energies of devitrification for slags 2 and 3 were 297.32 and 269.46 KJ/mol, respectively, indicating that the devitrification capacity of the slag increased after adding Al2O3. The increase in devitrification capacity provided more nuclei for crystallization, which partially contributed to the increased crystal ratio of films, which is discussed later.
The DSC results also indicate that the heating rate can affect the softening temperature zone of glassy films. In Figure 8, when the heating rate reached 35 °C/min and the temperature exceeded 700 °C, the slag began to absorb heat and became soft or melted. This feature was not observed at lower heating rates. Slow heating rates provided better kinetic conditions and allowed sufficient time for LiAlO2 and CaF2 to precipitate in the glassy film. The consumption of Li, Ca, and F ions in the nearby glass matrix significantly decreased the Li2O and CaF2 fusion agents in the remaining glass. Consequently, the softening or melting temperatures of the nearby glass matrix increased. The softening of solid slag films could decrease the surface roughness of solid films in contact with the water-cooled copper wall, which was also observed in our previous study [19]. This phenomenon could affect the capacity of heat transfer control of solid slag films during solidification; in addition, it could be utilized in the design of the property of the solid slag film for high-Al steels. Detailed research on this topic is ongoing.
The area ratio of a specific crystal on the cross-section was determined as the crystal ratio. The measured crystal ratios in the typical slag films are listed in Table 4 and Figure 10. A comparison of the No. 1 and No. 3 slag films indicated that extra Al2O3 increased the crystal ratio and crystallization capacity of the films. Consistent with the previous discussion on Figure 7, during the crystallization of slag films, the initial precipitated LiAlO2 and MgAl2O4 usually acted as nuclei for the further precipitation of BaAl2O4 (also see Figure 11). Thus, the low apparent activation energy of the devitrified crystallization of No. 3 slag could provide more nuclei at a very early stage of film solidification, promoting the precipitation of crystals in the glassy film and liquid slag with a relatively high viscosity near the solidification front.

4. Conclusions

The crystallization process of slag films of typical mold fluxes for casting high-Al steels was studied in this work, and the following conclusions can be drawn:
(1)
After adding extra Al2O3, the growing speed and thickness of the slag films increased significantly, especially for films with 10 wt% Al2O3 addition, and more time was required to reach a steady state of film thickness.
(2)
LiAlO2, CaF2, and BaAl2O4 were the major crystals precipitated in slag films of No. 1 and No. 2. BaAl2O4 usually precipitated and used initial crystal particles as their nuclei. Spinel (MgAl2O4) precipitated in the films when an extra 10 wt% of Al2O3 was added. The results suggest that the MgO in the slag or the absorption of Al2O3 from liquid steels should be controlled.
(3)
For the glassy state of No. 1 slag, when the heating rate reached 35 °C/min during devitrification, the softening temperature decreased to approximately 700 °C. Lower heating rates were associated with higher softening temperatures.
(4)
The apparent activation energy of initial devitrification crystallization for the original slag (No. 1) was 314.16 KJ/mol. After adding Al2O3, this activation energy decreased to 297.32 KJ/mol and 269.46 KJ/mol for 5 wt% and 10 wt% Al2O3 addition, respectively. The crystallization ratio of the slag films also increased after adding extra Al2O3.

Author Contributions

Methodology, X.L. (Xiao Long); investigation, X.L. (Xiao Long), C.T., J.X. and W.L.; resources, S.L., W.L. and X.L. (Xiang Li); writing—original draft preparation, X.L. (Xiao Long); writing—review and editing, X.L. (Xiao Long) and Y.N. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China (51904083), Natural Science Foundation of Guizhou Province (Qian Ke He Ji Chu [2020]1Y221), Growth Project of Young Scientific and Technological Talents in Universities of Guizhou Province [Qian Jiao He KY Zi (2021)262], and Guizhou Institute of Technology high-level talent research launch project [XJGC20190963].

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Mills, K.C.; Fox, A.B. The role of mould fluxes in continuous casting-so simple and yet so complex. ISIJ Int. 2003, 43, 1479–1486. [Google Scholar] [CrossRef]
  2. Cho, J.W.; Emi, T.; Shibata, H.; Suzuki, M. Heat transfer across mold flux film in mold during initial solidification in continuous casting of steel. ISIJ Int. 1998, 38, 834–842. [Google Scholar] [CrossRef]
  3. Yoon, D.W.; Cho, J.W.; Kim, S.H. Controlling radiative heat transfer across the mold flux layer by the scattering effect of the borosilicate mold flux system with metallic iron. Metall. Mater. Trans. B 2017, 48, 1951–1961. [Google Scholar] [CrossRef]
  4. Susa, M.; Mills, K.C.; Richardson, M.J.; Taylor, R. Thermal properties of slag films taken from continuous casting mould. Ironmak. Steelmak. 1994, 21, 279–286. [Google Scholar]
  5. Mills, K.C. Structure and Properties of slags used in the continuous casting of steel: Part 1 conventional mould powders. ISIJ Int. 2016, 56, 1–13. [Google Scholar] [CrossRef] [Green Version]
  6. Bhagurkar, A.G.; Qin, R. The Microstructure formation in slag solidification at continuous casting mold. Metals 2022, 12, 617. [Google Scholar] [CrossRef]
  7. Kim, M.S.; Park, M.S.; Kang, Y.B. A reaction between high Mn–high Al steel and CaO-SiO2-type molten mold flux: Reduction of additive oxide components in mold flux by Al in steel. Metall. Mater. Trans. B 2020, 50, 2077–2082. [Google Scholar] [CrossRef]
  8. Wang, W.; Lu, B.; Xiao, D. A review of mold flux development for the casting of high-Al steels. Metall. Mater. Trans. B 2016, 47, 384–389. [Google Scholar] [CrossRef]
  9. XYan, X.; Pan, W.; Wang, X.; Zhang, X.; He, S.; Wang, Q. Electrical conductivity, viscosity and structure of CaO–Al2O3-based mold slags for continuous casting of high-Al steels. Metall. Mater. Trans. B 2021, 52, 2526–2535. [Google Scholar]
  10. Ou, G.L.; Liu, Y.C.; Yen, S.Y.; Wang, H.Y.; Su, Y.H.; Lu, M.J.; Lin, S.K. Reactivity and thermo-physical properties of MnO-modified CaO-Al2O3-based mold fluxes for advanced high-strength steels. J. Mater. Res. Technol. 2020, 9, 12091–12101. [Google Scholar] [CrossRef]
  11. Gao, E.; Wang, W.; Zhang, L. Effect of alkaline earth metal oxides on the viscosity and structure of the CaO-Al2O3 based mold flux for casting high-al steels. J. Non-Cryst. Solids 2017, 473, 79–86. [Google Scholar] [CrossRef]
  12. SShirayama, S.; Aoki, H.; Yanaba, Y.; Kim, Y.; Morita, K. Relationship between thermal conductivity and structure of the CaO–BO1.5–AlO1.5 System. ISIJ Int. 2020, 60, 392–399. [Google Scholar] [CrossRef] [Green Version]
  13. Zhang, K.; Liu, J.; Cui, H. Simulation for mass transfer kinetics at slag-steel interface during high Al steel continuous casting. ISIJ Int. 2019, 59, 2256–2263. [Google Scholar] [CrossRef] [Green Version]
  14. Zhao, B.; Zhang, J.; Yan, B. Interfacial phenomena and reaction kinetics between high Al molten steel and CaO-SiO2-type flux. Metals 2022, 12, 391. [Google Scholar] [CrossRef]
  15. Gu, S.; Wen, G.; Ding, Z.; Tang, P.; Liu, Q. Effect of shear stress on isothermal crystallization behavior of CaO-Al2O3-SiO2-Na2O-CaF2 slags. Materials 2018, 11, 1085. [Google Scholar] [CrossRef] [Green Version]
  16. Leng, M.; Lai, F.; Li, J. Effect of cooling rate on phase and crystal morphology transitions of CaO–SiO2-based systems and CaO–Al2O3-based systems. Materials 2019, 12, 62. [Google Scholar] [CrossRef] [Green Version]
  17. Perrot, C.; Pontoire, J.N.; Marchionni, C.; Ridolfi, M.R.; Sancho, L.F. Several slag rims and lubrication behaviours in slab casting. Metall. Res. Technol. 2005, 102, 887–896. [Google Scholar] [CrossRef]
  18. He, S.; Li, Z.; Chen, Z.; Wu, T.; Wang, Q. Review of mold fluxes for continuous casting of high-alloy (Al, Mn, Ti) steels. Steel Res. Int. 2019, 90, 180042. [Google Scholar] [CrossRef] [Green Version]
  19. Long, X.; Wang, Q.; He, S.; Pistorius, P.C. Structure evolution of slag films of ultrahigh-basicity mold flux during solidification. Metall. Mater. Trans. B 2017, 48, 1938–1942. [Google Scholar] [CrossRef]
  20. Long, X.; He, S.; Wang, Q.; Pistorius, P.C. Structure of solidified films of mold flux for peritectic steel. Metall. Mater. Trans. B 2017, 48, 1652–1658. [Google Scholar] [CrossRef]
  21. Assis, K.L.S.; Pistorius, P.C. Improved cold-finger measurement of heat flux through solidified mould flux. Ironmak. Steelmak. 2018, 45, 502–508. [Google Scholar] [CrossRef]
  22. Assis, K.L.S. Heat Transfer through Mold Fluxes: A New Approach to Measure Thermal Properties of Slags; Carnegie Mellon University: Pittsburgh, PA, USA, 2016. [Google Scholar]
  23. Nakada, H.; Susa, M.; Seko, Y.; Hayashi, M.; Nagata, K. Mechanism of heat transfer reduction by crystallization of mold flux for continuous casting. ISIJ Int. 2008, 48, 446–453. [Google Scholar] [CrossRef] [Green Version]
  24. Xiao, L.O.N.G.; He, S.P.; Xu, J.F.; Huo, X.L.; Qian, W.A.N.G. Properties of high basicity mold fluxes for peritectic steel slab casting. J. Iron Steel Res. Int. 2012, 19, 39–45. [Google Scholar]
  25. Zeng, J.; Long, X.; You, X.; Li, M.; Wang, Q.; He, S. Structure of solidified films of CaO-SiO2-Na2O based low-fluorine mold flux. Metals 2019, 9, 93. [Google Scholar] [CrossRef] [Green Version]
Figure 1. Average thickness of slag films solidified in slag bulk at a temperature of 1350 °C.
Figure 1. Average thickness of slag films solidified in slag bulk at a temperature of 1350 °C.
Materials 16 01903 g001
Figure 2. Optical images of cross-sections of solid slag films with different solidification times, (a) 15 s, (b) 30 s of No. 1 slag (bulk temperature 1300 °C).
Figure 2. Optical images of cross-sections of solid slag films with different solidification times, (a) 15 s, (b) 30 s of No. 1 slag (bulk temperature 1300 °C).
Materials 16 01903 g002
Figure 3. Optical image of crystals dispersed in glassy film (slag bulk temperature 1300 °C).
Figure 3. Optical image of crystals dispersed in glassy film (slag bulk temperature 1300 °C).
Materials 16 01903 g003
Figure 4. Typical XRD patterns of slag film powders: (a) No. 1 slag; (b) No. 2 slag; (c) No. 3 slag. Bulk slag temperature for film solidification: 1350, and solidification time: 30 s.
Figure 4. Typical XRD patterns of slag film powders: (a) No. 1 slag; (b) No. 2 slag; (c) No. 3 slag. Bulk slag temperature for film solidification: 1350, and solidification time: 30 s.
Materials 16 01903 g004
Figure 5. Backscattered SEM image of typical morphology of the devitrified crystals in the No. 3 slag film solidified in molten slag at 1300 °C.
Figure 5. Backscattered SEM image of typical morphology of the devitrified crystals in the No. 3 slag film solidified in molten slag at 1300 °C.
Materials 16 01903 g005
Figure 6. EDS mapping of CaF2 and spinel (MgAl2O4) crystals.
Figure 6. EDS mapping of CaF2 and spinel (MgAl2O4) crystals.
Materials 16 01903 g006
Figure 7. Backscattered SEM image and EDS area scanning of LiAlO2 and LiAlO2 cores for the precipitation of BaAl2O4 in the film solidified in molten slag at 1300 °C.
Figure 7. Backscattered SEM image and EDS area scanning of LiAlO2 and LiAlO2 cores for the precipitation of BaAl2O4 in the film solidified in molten slag at 1300 °C.
Materials 16 01903 g007
Figure 8. DSC curves of quenched glassy powder of No. 1 slag with different heating rates.
Figure 8. DSC curves of quenched glassy powder of No. 1 slag with different heating rates.
Materials 16 01903 g008
Figure 9. Relationship between ln(β/Tp2) and 1/TP of No. 1 slag.
Figure 9. Relationship between ln(β/Tp2) and 1/TP of No. 1 slag.
Materials 16 01903 g009
Figure 10. Crystallization ratio evolution of typical slag films solidified in molten slag at 1400 °C.
Figure 10. Crystallization ratio evolution of typical slag films solidified in molten slag at 1400 °C.
Materials 16 01903 g010
Figure 11. A typical crystal (BaAl2O4) precipitated using initial crystals as nuclei (backscattered image, the No. 3 slag film solidified in molten slag at 1300 °C).
Figure 11. A typical crystal (BaAl2O4) precipitated using initial crystals as nuclei (backscattered image, the No. 3 slag film solidified in molten slag at 1300 °C).
Materials 16 01903 g011
Table 1. Composition of mold fluxes (wt%).
Table 1. Composition of mold fluxes (wt%).
No.CaOAl2O3BaOFLi2OB2O3MgO
12432151064.52
22437151064.52
32442151064.52
(All components are represented as oxides, except for F).
Table 2. Average thickness of slag films with different solidification times and slag bulk temperatures.
Table 2. Average thickness of slag films with different solidification times and slag bulk temperatures.
Solidification Time, sNo. 1 SlagNo. 2 SlagNo. 3 Slag
Bulk Temperature of Molten Slag, °C
140013501300140013501300140013501300
Average Film Thickness, mm
7------1.612.093.35
15--2.541.672.013.291.882.514.37
301.732.322.991.892.773.971.983.245.60
602.232.954.452.683.224.332.626.12-
902.453.015.562.714.136.212.977.809.17
Table 3. Major crystal phases in films with different solidification times and slag bulk temperatures.
Table 3. Major crystal phases in films with different solidification times and slag bulk temperatures.
Solidification Time, sNo. 1 SlagNo. 2 SlagNo. 3 Slag
Bulk Temperature of Molten Slag, °C
140013501300140013501300140013501300
Crystal Phase
7------GGAC
15--BGABABBCABCABC
30ABABABABABABDABCABCDABCD
60ABDABDABDABDABDABDABCDABCD-
90ABDABDABDABDABCDABDABCDABCDABCD
(A-CaF2, B-LiAlO2 C-MgAl2O4; D-BaAl2O4; G-totally glassy state).
Table 4. Typical crystal ratios of films solidified at different times (%).
Table 4. Typical crystal ratios of films solidified at different times (%).
Slag No.Solidified Time, sCaF2Spinel (MgAl2O4)LiAlO2BaAl2O4Crystal Ratio of Film
No. 1302010012
608013627
909015731
No. 3700000
15038011
305311019
607414732
90124161143
The film was solidified in molten slag at 1400 °C.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Long, X.; Long, S.; Luo, W.; Li, X.; Tu, C.; Na, Y.; Xu, J. Crystallization of Slag Films of CaO-Al2O3-BaO-CaF2-Li2O-Based Mold Fluxes for High-Aluminum Steels’ Continuous Casting. Materials 2023, 16, 1903. https://doi.org/10.3390/ma16051903

AMA Style

Long X, Long S, Luo W, Li X, Tu C, Na Y, Xu J. Crystallization of Slag Films of CaO-Al2O3-BaO-CaF2-Li2O-Based Mold Fluxes for High-Aluminum Steels’ Continuous Casting. Materials. 2023; 16(5):1903. https://doi.org/10.3390/ma16051903

Chicago/Turabian Style

Long, Xiao, Shaolei Long, Wenbo Luo, Xiang Li, Changping Tu, Yunhao Na, and Jinxin Xu. 2023. "Crystallization of Slag Films of CaO-Al2O3-BaO-CaF2-Li2O-Based Mold Fluxes for High-Aluminum Steels’ Continuous Casting" Materials 16, no. 5: 1903. https://doi.org/10.3390/ma16051903

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.