Next Article in Journal
The Evolution and Distribution of Microstructures in High-Energy Laser-Welded X100 Pipeline Steel
Next Article in Special Issue
Mechanically Robust and Repairable Superhydrophobic Zinc Coating via a Fast and Facile Method for Corrosion Resisting
Previous Article in Journal
Effect of Adjusted Gas Nitriding Parameters on Microstructure and Wear Resistance of HVOF-Sprayed AISI 316L Coatings
Previous Article in Special Issue
Lotus-Inspired Multiscale Superhydrophobic AA5083 Resisting Surface Contamination and Marine Corrosion Attack
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Optimization of Cathodic Protection Design for Pre-Insulated Pipeline in District Heating System Using Computational Simulation

School of Advanced Materials Engineering, Sungkyunkwan University, 300 Chunchun-Dong, Jangan-Gu, Suwon 440-746, Korea
*
Author to whom correspondence should be addressed.
Materials 2019, 12(11), 1761; https://doi.org/10.3390/ma12111761
Submission received: 13 May 2019 / Revised: 24 May 2019 / Accepted: 28 May 2019 / Published: 30 May 2019
(This article belongs to the Special Issue Advanced Coatings for Corrosion Protection)

Abstract

:
Cathodic protection (CP) has been used as a primary method in the control of corrosion, therefore it is regarded as the most effective way for protecting buried pipelines. However, it is difficult to apply CP to a pipeline for district heating distribution systems, because the pipeline has thermally insulated coatings which could disturb the CP. Theoretical calculation and field tests alone are not enough for a reliable CP design, and therefore additional CP design methods such as computational analysis should be used. In this study, the CP design for pre-insulated pipelines is tested considering several environmental factors, such as temperature and coating defect ratio. Additionally, computational analysis is performed to verify and optimize the CP design. The simulation results based on theoretical methods alone failed to satisfy the CP criteria. Then, a re-design is conducted considering the IR drop. Consequently, all of the simulation results of defective pipelines satisfied the CP criteria after adding the proper CP current.

1. Introduction

In district heating (DH) systems, heated water is distributed through a double-pipe network and transferred to buildings for use in space heating, hot water generation, and process heating [1]. DH systems have three main elements: the heat source, the distribution system, and the customer interface. The distribution system supplies hot water from the heat source to the heat consumer and returns with temperatures in the range of 40 °C to 120 °C [2]. Generally, pipelines in DH distribution systems use a thermally insulated coating to minimize heat loss during transfer. As shown in Figure 1, the coating consists of two layers: an inner layer of polyurethane foam (PUR) to reduce heat loss, and an outer layer of high-density polyethylene (HDPE) to protect the PUR [3]. The coatings effectively mitigate corrosion by blocking the outer environment, which contains corrosive elements such as water, oxygen, and chloride ions, when the coating is maintained perfectly. However, the HDPE is susceptible to unpredictable mechanical damage, and the PUR can be vanished by heat, humidity, and oxygen during its long operational life [4,5]. Several studies have reported that the main source of corrosion is groundwater introduced through failure of the HDPE and PUR [5,6,7].
Cathodic protection (CP) has been used as the primary method in the control of corrosion, in conjunction with protective coatings. CP can reduce the corrosion rate, and a properly maintained system will provide protection in accordance with the designed structural life [8]. The impressed current CP (ICCP) system has a power supply (rectifier) that generates larger potential differences between the anode and the structure [9]. For this reason, ICCP is applied to many industrial pipelines. However, despite the availability of CP, there are still several limitations in applying CP to pre-insulated pipelines [10]. The National Association of Corrosion Engineers (NACE) reported that the CP design for pre-insulated pipelines is ineffective because the protection current cannot reach the corroded area through the insulating layer [11]. Additionally, according to previous studies, the corrosion rate of PUR-insulated carbon steel is much lower than that of uninsulated (bare) steel, even when the PUR is fully immersed in groundwater [12]. Therefore, CP for pre-insulated pipelines may be unnecessary when the PUR layer is intact. However, the immersed PUR layer can deteriorate and vanish during long operating periods, causing exposure of the bare carbon steel to the corrosive environment. For this reason, it is important to apply CP to operating pipelines with external coating defects, as a precaution against sudden fracture. Nevertheless, it is difficult to design CP systems for operating pipelines using only theoretical methods and a limited number of standards. It is also difficult to verify the appropriate protecting current required to reach the external surface of the pipeline with proper CP potential. For this reason, additional CP design methods, such as computational analysis, should be applied to optimize the design [13,14,15]. To improve the reliability of simulation results, several essential factors should be considered, such as polarization data for real materials and appropriate environmental information.
In this study, a CP system was designed for an existing pipeline with damaged insulation, taking into consideration environmental factors, such as corrosion properties of real materials, operating temperatures, and structural effects. Additionally, electrochemical tests were performed in synthetic groundwater to obtain input data for the computer simulation. Finally, a computational analysis was performed to verify and optimize the CP design of pre-insulated pipelines.

2. Materials and Methods

2.1. Materials and Test Conditions

The corrosion environment used was synthetic groundwater. Table 1 gives the chemical composition of the synthetic groundwater, and HNO3 was used to control the pH of the solution. A welded carbon steel specimen consisting of a base metal, heat affected zone, and a weld metal was used during testing to calculate the required CP current. Table 2 shows the chemical composition of the SPW400 (carbon steel), and Table 3 shows the welding methods used in all experiments. The surface of the specimen was polished with 600-grit silicon carbide (SiC) paper, degreased with ethanol, and dried with N2.

2.2. Electrochemical Test Methods

All electrochemical experiments were performed using a three-electrode system, in a 1000 mL Pyrex glass corrosion cell connected to an electrochemical apparatus. The test specimens were connected to a working electrode, a graphite rod was used as the counter electrode, and a saturated calomel electrode (SCE) was used as the reference electrode. The area of the test specimen exposed to the electrolyte was 2.25 cm2 (1.5 cm × 1.5 cm). An open-circuit potential (OCP) was established within three hours to carry out the electrochemical test. Potentiodynamic polarization tests were carried out in accordance with ASTM G5-14 (Standard Reference Test Method for Making Potentiodynamic Anodic Polarization Measurements), using a VMP2 (Bio-Logic Science Instruments, Seyssinet-Pariset, France) with a potential sweep of 0.166 mV/sec, from an initial potential of −2000 mV versus the reference to a final potential of 200 mV versus the OCP. The electrochemical tests were performed at 80 °C, because a previous study found that the highest protection current for carbon steel was required at this temperature [7].

2.3. CP Design and Computational Analysis Method

The computational analysis tool BEASY S/W (BEASY Ltd., Southampton, England), which is based on the boundary element method (BEM), was used to conduct 3D modeling and computational analysis of the pre-insulated pipeline. The required CP current (Ireq) for the pipeline was calculated, taking into consideration the current density of real material measured by electrochemical tests. The cathodic polarization curve, which was used as input data for the simulation, was obtained from the potentiodynamic polarization test, which incorporated the environmental information.

3. Results and Discussion

3.1. Potentiodynamic Polarization Tests

The applied current density (iapp) for the pre-insulated pipeline was calculated using the Evans diagram, as shown in Figure 2. According to the diagram, anodic current density is under activation control (activation polarization), and cathodic current density is limited at a higher current density (concentration polarization). As the applied current density for CP is increased, the potential and the corrosion current density are reduced simultaneously [16,17]. According to the previous study, since the pre-insulated pipeline has a high corrosion rate at 80 °C, the reasonable maximum CP potential is −1350 mVSCE [7]. Figure 3 shows the results of the potentiodynamic polarization test in synthetic groundwater at 80 °C. The corrosion current density was determined using the Tafel extrapolation method. Table 4 shows the calculated CP current density, which will apply to the CP design. The applied current density was calculated as the difference between the anodic polarization curve and cathodic polarization curve at −1350 mVSCE, as shown in Figure 2. The cathodic polarization curve, which contains the corrosion properties of real material, was used as the input data for computational analysis.

3.2. Cathodic Protection Design and Computational Analysis

The pre-insulated pipeline was connected every 6 m by welds, therefore, the CP design was preformed to 6 meters of 600 A pipe (Figure 1). In addition, ICCP anodes were installed at both edges of the pipeline, which are the parts most sensitive to corrosion because it will connect using welding. In this study, the CP design was applied to operating pipelines with slight defects. Therefore, the CP design was tested at a range of defect ratios (1, 5, 10, 20%), and it is assumed that the insulating part of the pipeline has no defect. Figure 4 shows the 3D modeling of the pipeline according to defect ratio. For modeling and calculations, the approach was based on the assumption that the crevice between the coating and pipeline was not effective as a CP [18]. Table 5 shows the basic design parameters related to the structural factors. The surface area of the pipe used in the CP design was 12.62 m2, which included an additional 10% safety factor. The resistivity of soil was assumed to be 1000 Ω∙cm, corresponding to a highly corrosive environment. The required current (Ireq) for CP was calculated from the following equation [19,20]:
Ireq = Cdefect · iapp · Apipe,
where Cdefect is the defect ratio of the pipeline, iapp is the applied current density of the pipe material calculated from the electrochemical test, Apipe is the surface area of the pipe. Ireq is calculated with the defect ratio, as listed in Table 6.
The computational analysis was performed using the cathodic polarization curve data, obtained from the electrochemical tests. Figure 5 shows the simulation results for CP. All of the simulation results failed to satisfy the CP criteria for pre-insulated pipelines (under −1350 mVSCE) because the IR drop caused by soil and structural factors was not considered in the CP design.
The additional CP current required to satisfy the CP criteria should be calculated taking into consideration the polarization curve, as shown in Figure 6. The maximum CP potentials were defined based on the simulation results according to the defect ratio. Then, the applied current densities were calculated at the maximum CP potential from the simulation results, using the same method as above. To obtain the additional CP current densities, the difference was calculated between the calculated applied current densities, according to the defect ratio and applied current density at −1350 mVSCE. The additional CP currents were then calculated using Equation (1). The calculated values are listed in Table 7.
Then, the entire simulation was re-conducted. Figure 7 shows the optimized simulation results, and it was verified that all of the pipelines with different defect ratios satisfied the CP criteria. Another important point is over-protection due to the low CP criteria of district pipelines. The simulation results show that the minimum CP potentials have a range from −1.7 VSCE to −2.6 VSCE. This is quite a low potential value, which could cause hydrogen embrittlement risk. However, according to the international standards, such as NACE (RP0169-96), ARAMCO (SAES-X-400), and BSI (BS 7361-1), the over protection range of the steel pipeline ranges from −2.5 VSCE to −5 VSCE. Therefore, the simulation results can apply up to 10% of the defect ratio, which has a minimum potential of about −2.49 VSCE. When the CP applies over 10% of the defect ratio, the site of defect should be previously investigated. Then, the anode should be installed as close as possible to the defect area, to avoid over protection and reduce CP current requirement. Therefore, the investigation of the defect area is one of the significant design parameters in practical CP installation.

4. Conclusions

In this study, a credible CP design method for existing pre-insulated pipelines was conducted, taking into consideration the environmental factors, and computational analysis was performed to verify and optimize the CP design. According to the results, the following conclusions were drawn:
The results of the simulations using the theoretical method failed to satisfy the CP criterion determined for heating pre-insulated pipeline. To solve the problem, a re-design was conducted, taking into consideration the IR drop caused by soil and structural factors. Consequently, after adding the proper CP current, all of the simulation results of defective pipelines satisfied the CP criteria.
Incorporating practical corrosion properties of metal and environmental factors in the computational analysis improves the reliability of the CP design for a pipeline. For this reason, application of CP is recommended for pre-insulated pipelines, to mitigate external corrosion and reduce maintenance costs. The computational analysis is an essential step for credible CP design.

Author Contributions

Conceptualization, M.-S.H.; methodology, Y.-S.S.; software, M.-S.H.; validation, M.-S.H. and J.-G.K.; formal analysis, M.-S.H. and Y.-S.S.; investigation, M.-S.H.; resources, M.-S.H.; data curation, M.-S.H. and Y.-S.S.; writing—original draft preparation, M.-S.H.; writing—review and editing, M.-S.H. and J.-G.K.; visualization, M.-S.H.; supervision, J.-G.K.; project administration, M.-S.H. and J.-G.K.

Funding

This research was supported by the program for fostering next-generation researchers in engineering of National Research Foundation of Korea (NRF) funded by the Ministry of Science and ICT (2017H1D8A2031628).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Skagestad, B.; Mildenstein, P. District Heating and Cooling Connection Handbook; Netherlands Agency for Energy and the Environment: Amsterdam, The Netherlands, 2002; pp. 23–50. [Google Scholar]
  2. Eliseev, K. District Heating System in Finland and Russia. Ph.D. Thesis, Mikkeli University of Applied Sciences, Mikkeli, Finland, 2011; pp. 4–20. [Google Scholar]
  3. Choi, S.Y.; Yoo, K.Y.; Lee, J.B.; Shin, C.B.; Park, M.J. Mathematical modeling and control of thermal plant in the district heating system of Korea. Appl. Therm. Eng. 2010, 30, 2067–2072. [Google Scholar] [CrossRef]
  4. Yarahmadi, N.; Sällström, J.H. Improved maintenance strategies for district heating pipe lines. In Proceedings of the 14th International Symposium on District Heating and Cooling, Stockholm, Sweden, 7–9 September 2014. [Google Scholar]
  5. Choi, Y.-S.; Chung, M.-K.; Kim, J.-G. Effects of cyclic stress and insulation on the corrosion fatigue properties of thermally insulated pipeline. Mater. Sci. Eng. A 2004, 384, 47–56. [Google Scholar] [CrossRef]
  6. Rassoul, E.-S.A.; Abdel-Samad, A.; El-Naqier, R. On the cathodic protection of thermally insulated pipelines. Eng. Fail. Anal. 2009, 16, 2047–2053. [Google Scholar] [CrossRef]
  7. Kim, J.G.; Kim, Y.W. Cathodic protection criteria of thermally insulated pipeline buried in soil. Corros. Sci. 2001, 43, 2011–2021. [Google Scholar] [CrossRef]
  8. Shreir, L. Design and Operational Guidance on Cathodic Protection of Offshore Structures, Subsea Installations and Pipelines; The Marine technology directorate limited publication: London, UK, 1990. [Google Scholar]
  9. Von Baeckmann, W.; Schwenk, W.; Prinz, W. Handbook of Cathodic Corrosion Protection; Elsevier: Huston, TX, USA, 1997. [Google Scholar]
  10. Gummow, R. Cathodic protection criteria—A critical review of NACE standard RP-01-69. Mater. Perform. 1986, 25, 9–16. [Google Scholar]
  11. Effectiveness of Cathodic Protection on Thermally Insulated Underground Metallic Surfaces; NACE Technical Committee Report No. 24156; NACE Publication: Huston, TX, USA, 1992.
  12. Kim, J.-G.; Kim, Y.-W.; Kang, M.-C. Corrosion Characteristics of Rigid Polyurethane Thermally Insulated Pipeline with Insulation Defects. Corrosion 2002, 58, 175–181. [Google Scholar] [CrossRef]
  13. Parsa, M.; Allahkaram, S.; Ghobadi, A. Simulation of cathodic protection potential distributions on oil well casings. J. Pet. Sci. Eng. 2010, 72, 215–219. [Google Scholar] [CrossRef]
  14. DeGiorgi, V.G.; Wimmer, S.A. Geometric details and modeling accuracy requirements for shipboard impressed current cathodic protection system modeling. Eng. Anal. Bound. Elem. 2005, 29, 15–28. [Google Scholar] [CrossRef]
  15. Hong, M.-S.; Hwang, J.-H.; Kim, J.H. Optimization of the Cathodic Protection Design in Consideration of the Temperature Variation for Offshore Structures. Corrosion 2017, 74, 123–133. [Google Scholar] [CrossRef]
  16. Roberge, P.R. Handbook of Corrosion Engineering; McGraw-Hill: New York, NY, USA, 2000. [Google Scholar]
  17. Kim, Y.-S.; Lee, S.; Kim, J.-G. Influence of anode location and quantity for the reduction of underwater electric fields under cathodic protection. Ocean Eng. 2018, 163, 476–482. [Google Scholar] [CrossRef]
  18. Fessler, R.R.; Markworth, A.J.; Parkins, R.N. Cathodic Protection Levels under Disbonded Coatings. Corrosion 1983, 39, 20–25. [Google Scholar] [CrossRef]
  19. Veritas, D.N. Cathodic Protection Design, Recommended Practice DNV-RP-B401; DNV: Oslo, Norway, 2010. [Google Scholar]
  20. Pedeferri, P. Cathodic protection and cathodic prevention. Constr. Build. Mater. 1996, 10, 391–402. [Google Scholar] [CrossRef]
Figure 1. Schematic diagram of the pre-insulated coated pipe (600 A).
Figure 1. Schematic diagram of the pre-insulated coated pipe (600 A).
Materials 12 01761 g001
Figure 2. Evan’s diagram, indicating the relationship between the applied current density and protection potential [16].
Figure 2. Evan’s diagram, indicating the relationship between the applied current density and protection potential [16].
Materials 12 01761 g002
Figure 3. Potentiodynamic polarization curves in the synthetic groundwater at 80 °C.
Figure 3. Potentiodynamic polarization curves in the synthetic groundwater at 80 °C.
Materials 12 01761 g003
Figure 4. 3D modeling of pipeline according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Figure 4. 3D modeling of pipeline according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Materials 12 01761 g004
Figure 5. Simulation results (averaged protection potential, mVSCE) according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Figure 5. Simulation results (averaged protection potential, mVSCE) according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Materials 12 01761 g005
Figure 6. Calculation of additional current caused by IR drop in the polarization curve: potential difference of (a) 1%, (b) 5%, (c) 10%, (d) 20% defected pipelines.
Figure 6. Calculation of additional current caused by IR drop in the polarization curve: potential difference of (a) 1%, (b) 5%, (c) 10%, (d) 20% defected pipelines.
Materials 12 01761 g006
Figure 7. Optimized simulation results (averaged protection potential, mVSCE) according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Figure 7. Optimized simulation results (averaged protection potential, mVSCE) according to the defect ratio: (a) 1%, (b) 5%, (c) 10%, (d) 20%.
Materials 12 01761 g007
Table 1. Chemical composition of synthetic groundwater.
Table 1. Chemical composition of synthetic groundwater.
CaCl2 (ppm)MgSO4∙7H2O (ppm)NaHCO3 (ppm)H2SO4 (ppm)HNO3 (ppm)pHResistivity (kΩ∙cm)
133.2592088522.26.81.736
Table 2. Chemical composition of SPW400 (wt.%).
Table 2. Chemical composition of SPW400 (wt.%).
FeCPS
Balance0.25
Max.
0.04
Max.
0.04
Max.
Table 3. Welding procedure specification.
Table 3. Welding procedure specification.
Welding ProcessGTAW
Joint designSingle V joint with a 60° included angle and a 1.6 mm root face
ElectrodeGTAW ER70S-G
Voltage12–15 V
Current100–180 A
PolarityDirect Current Straight Polarity (DCSP)
Travel speed20–30 cm/min
Welding atmosphereAr, 15–25 L/min
Table 4. Results of Potentiodynamic Polarization Test at 80 °C in the Synthetic Groundwater.
Table 4. Results of Potentiodynamic Polarization Test at 80 °C in the Synthetic Groundwater.
Corrosion Potential (Ecorr, mVSCE)Corrosion Current Density (icorr, A/m2)Βc (mV)Βa (mV)Applied Current Density (iapp, A/m2)
−6490.493258.378.214.45
Table 5. Basic design parameters related to the structural factors.
Table 5. Basic design parameters related to the structural factors.
Pipeline
(600 A)
Diameter609.6 mm
Length6 m
Surface Area11.48 m2
Resistivity of Soil1000 Ω∙cm
Temperature on the Pipeline80 °C
CP CriteriaUnder −1350 mV
Table 6. Required current calculation for cathodic protection (CP).
Table 6. Required current calculation for cathodic protection (CP).
Applied Current Density (iapp)Surface Area with 10% Safety Factor (Apipe)Defect Ratio (Cdefect)Required Current (Ireq)
14.45 A/m212.62 m21%0.011.824 A
5%0.059.120 A
10%0.118.241 A
20%0.236.483 A
Table 7. Results of calculated additional CP current and optimized current for CP.
Table 7. Results of calculated additional CP current and optimized current for CP.
Defect
Ratio
Max. Potential
in Previous Results
Additional
Current Density
Additional
Current
Optimized
Current for CP
1%−1243.5 mV7.079 A/m20.893 A2.717 A
5%−1214.6 mV12.589 A/m27.944 A17.064 A
10%−1208.8 mV13.804 A/m217.420 A35.661 A
20%−1218.1 mV12.303 A/m231.052 A67.535 A

Share and Cite

MDPI and ACS Style

Hong, M.-S.; So, Y.-S.; Kim, J.-G. Optimization of Cathodic Protection Design for Pre-Insulated Pipeline in District Heating System Using Computational Simulation. Materials 2019, 12, 1761. https://doi.org/10.3390/ma12111761

AMA Style

Hong M-S, So Y-S, Kim J-G. Optimization of Cathodic Protection Design for Pre-Insulated Pipeline in District Heating System Using Computational Simulation. Materials. 2019; 12(11):1761. https://doi.org/10.3390/ma12111761

Chicago/Turabian Style

Hong, Min-Sung, Yoon-Sik So, and Jung-Gu Kim. 2019. "Optimization of Cathodic Protection Design for Pre-Insulated Pipeline in District Heating System Using Computational Simulation" Materials 12, no. 11: 1761. https://doi.org/10.3390/ma12111761

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop