Article

Improving the Wear Properties of Ductile Iron by Introducing Ultrafine Graphite Nodules

by
Chen Liu
,
Yuzhou Du
*,
Haohao Li
,
Caiyin You
,
Chao Yang
,
Na Tian
and
Bailing Jiang
School of Materials Science and Engineering, Xi’an University of Technology, Xi’an 710048, China
*
Author to whom correspondence should be addressed.
Lubricants 2025, 13(9), 399; https://doi.org/10.3390/lubricants13090399
Submission received: 4 August 2025 / Revised: 4 September 2025 / Accepted: 7 September 2025 / Published: 9 September 2025
(This article belongs to the Special Issue Advances in Wear-Resistant Fe-Based Materials)

Abstract

The tribological behavior of ferritic ductile iron without ultrafine graphite nodules (FDI) and ferritic ductile iron with ultrafine graphite nodules (FDI-UG) was investigated in the present study. Ultrafine graphite nodules with a count of 3400 nod/mm2 were introduced by annealing treatment of quenched ductile iron, which effectively reduced the friction coefficient of ferritic ductile iron from approximately 0.3 to 0.15. This improvement was attributed to the ultrafine graphite nodules, which, due to their small spacing, facilitated a more uniform distribution on the tribological surface. Additionally, the formation of ultrafine graphite nodules in ferritized ductile iron refined the grain size (15 μm) and enhanced the hardness of ferritic ductile iron (183 HV), thereby significantly reducing abrasive wear. The more uniform graphite lubrication on the tribosurface and high hardness of fine ferrite grains in FDI-UG further enhanced wear resistance between the frictional pairs, effectively suppressing adhesion wear at high loads (6 N). Consequently, the ferritic ductile iron containing ultrafine graphite nodules and fine ferrite grains exhibited a superior wear resistance (6.84 × 10−3 mm3 and 9.47 × 10−3 mm3) compared to its untreated counterpart (9.22 × 10−3 mm3 and 11.95 × 10−3 mm3). These findings suggest that the incorporation of ultrafine graphite nodules was an effective strategy to enhance the tribological properties of ductile iron.

1. Introduction

Solid lubricants play a crucial role in reducing friction and wear of components. Graphite or graphene, as a widely used solid lubricant, is commonly employed to add to the friction contact surface to reduce friction coefficient. For example, graphite as dry lubricant was used in rail wheels, which reduced friction and wear of the rail wheels and extended their lifespan [1]; graphene platelets as dry lubricants applied on the surfaces of angular contact ball bearings demonstrated superior friction and wear performance [2]; However, with the improvement of component accuracy matching and operating speed, it is difficult to add external lubricants to effectively lubricate. Therefore, graphite was introduced into metal to fabricate self-lubricant metal matrix composites to reduce friction coefficient [3]. Al-graphite composites fabricated by 3D printing exhibit a rather low friction coefficient (0.2 ± 0.02) and wear rate (6.64 × 10−4 mm3/N·m) due to the formation of graphite lubricating film on the contact surface [4]. It is worth noting that the content and morphology of graphite are crucial for wear resistant performances of metal-graphite composites. Li et al. [5] investigated the tribological properties of graphite/Cu composites with varying graphite content, revealing that the friction coefficient and wear rate exhibited an initial increase followed by a decrease as the graphite content increased. Wu et al. [4] researched the tribological performance of graphite/aluminum composites with graphite in various morphologies into skeletons with various orientations, which indicated that fiber graphite exhibited the worst wear performance while spherical graphite obtained optimal friction and wear performance.
The spheroidal graphite in ductile iron was formed by spheroidization and incubation treatment for Fe molten during solidification [6,7]. Ductile iron containing spheroidal graphite not only exhibits comprehensive strength-plasticity matching, but also has potential in wear resistance due to the self-lubricating effect by graphite [8]. Notably, the count, size and distribution of spheroidal graphite are critical factors affecting the physical and mechanical properties of ductile iron. It is accepted that fine spheroidal graphite with high count and uniform distribution in ductile iron was favorable to enhance physical and mechanical properties [9,10,11]. Especially for friction and wear performance, ductile iron with high graphite nodule count could effectively reduce the friction coefficient, which is beneficial for improving friction and wear performance. For example, Abedi et al. [12] investigated tribological behavior of ductile cast iron with different graphite nodule count. The result indicated that the ductile iron with a higher density of graphite nodules exhibited a lower wear rate. Unfortunately, the spheroidal graphite from solidification process usually exhibits a large size (10~30 μm), low count (100~500 nod/mm2) and large spacing (20~50 μm) [13,14,15], which is not conducive to effectively reducing the friction coefficient.
In the past decades, some interesting studies have involved introducing small-sized graphite (3~10 μm) into free cutting steels by graphite annealing treatment to increase their wear resistance [16,17]. The formation of graphite in steels by graphite annealing usually required the addition of some graphitizing elements (Al and Si) [18,19]. Besides, it was found that the initial matrix structure of medium carbon steel had a significant impact on the formation of small-sized graphite [20]. The martensitic structure containing supersaturated carbon atom solid solution and more grain boundaries, which provided very favorable conditions for the formation of the small-sized and high-density graphite nodules during the annealing process [21].
Refer to the graphitization annealing conditions of medium carbon steel, the chemical composition of ductile iron typically contains high levels of C and Si elements [22]. Meanwhile, the C elements content in matrix of ductile iron can be tailored by austenization treatment [23]. These factors can provide the basic compositional conditions for precipitation of high count and small-sized graphite in matrix of ductile iron by solid phase transformation. Hence, it is inferred that the formation high density and small-sized graphite nodules can also be achieved in ductile iron. In the work, an initial martensitic structure was obtained in ductile iron, followed by annealing treatment to precipitate the small-sized graphite in matrix and reveal the formation mechanism of small-sized graphite nodules in ductile iron with a martensitic matrix, with the aim of obtaining high density graphite nodules to its reduce friction coefficient and improve wear performance.

2. Experimental Procedures

The chemical composition of as-cast ductile iron with a dimension of Ø 70 mm × 300 mm was measured by a spark optical emission spectrometer in the present study and the result is shown in Table 1. Two cylindrical specimens were cut from the cast profiles. Figure 1 shows the two annealing treatment process. Austenitizing a cylindrical specimen at 900 °C and maintaining it for 90 min, then cooling the specimen in a furnace, resulted in ferrite ductile iron without ultrafine graphite nodules as the comparison group (Figure 1A). Another cylindrical specimen was austenitized at 900 °C and maintained for 90 min. Afterwards, the specimen was quenched into oil to achieve a martensitic matrix (Figure 1B). The specimens with the dimensions of 10 mm × 10 mm × 10 mm was machined from the directly oil quenched samples and annealed at 700 °C from 0, 20 and 60 min, respectively to observe the formation of ultrafine graphite nodules in ductile iron (Figure 1B). The ferrite ductile iron without ultrafine graphite nodules (FDI) and ferrite ductile iron with ultrafine graphite nodules (FDI-UG) were named FDI and FDI-UG, respectively in the following text.
Standard metallographic specimens were etched with 4% nital solution. The microstructure was observed by an optical microscope (OLYMPUS GX71, Olympus, Tokyo, Japan) and scanning electron microscopy (JSM-6700F, JEOL, Tokyo, Japan). The micro-hardness of FDI and FDI-UG was tested by the microhardness tester (HVS-1000A, Shandong Shancai Testing Instrument Co., Ltd., Yantai, China) with a load of 25 g and holding time of 15 s. Each sample was tested with five indentations, and the average was taken as the final test result to maintain accuracy.
Disc specimens with a dimension of Ø 30 mm × 4 mm were machined from two ferritized samples to conduct friction and wear testing. Before testing, samples were ground and polished. The friction and wear properties of the ferritized samples were evaluated by a ball-on-disk tribometer (FHC-1D, Xi’an Rui’an Instrument Equipment Co., Ltd., Xi’an, China), as shown in Figure 2. GCr15 steel balls with a diameter of 9.0 mm and a hardness exceeding 60 HRC were used as the grinding material. Normal loads of 3 N and 6 N were applied and the corresponding to mean contact pressure was calculated as 430 MPa and 543 MPa according to Hertzian elastic contact theory [24,25]. The sliding speed was 200 r/min and the rotation diameter was 14 mm. The test took 20 min to complete. Three samples were performed for wear tests under each condition to ensure repeatability. The worn surfaces and the longitudinal sections were observed by SEM. The wear profiles of samples were determined using a profile-meter. The worn volume loss was V was determined as follows:
V = π · d · A
where d represents diameter of the wear trace (mm), A represents the section area of the wear track (mm2), and V represents the worn volume loss (mm3).

3. Results and Discussion

The optical micrographs of FDI and FDI-UG were illustrated in Figure 3. There were obvious differences for the two annealing samples. The FDI contained spheroidal graphite with a diameter of about 15 ± 3 μm and a graphite nodule count was about 350 ± 20 nod/mm2 distributing homogeneously around the matrix (Figure 4a). However, ultrafine graphite nodules could be observed in the FDI-UG besides the original spheroidal graphite (Figure 4b). The count and the diameter of the ultrafine spheroidal graphite nodules were estimated to 3400 ± 200 nod/mm2 and 0.8 ± 0.08 μm, respectively. The grain size of ferrite was measured approximately 29 ± 2.3 μm for FDI and 15 ± 1.7 μm for FDI-UG (Figure 4c,d). The result mainly because the low annealing temperature (700 °C) reduced the tendency for ferrite grain growth for FDI-UG compared to FDI with the high annealing temperature (900 °C), which resulted in the formation of finer ferrite grains in FDI-UG. The microhardness of FDI and FDI-UG were measured to be 156 ± 3 HV and 183 ± 5 HV, respectively. The increase in microhardness of FDI-UG was mainly attributed to the strengthening of ferrite grain refinement. It was worth emphasizing that the increase in ferrite hardness was beneficial for the wear resistance of FDI-UG.
In order to observe the formation process of ultrafine graphite nodules, the microstructural evolution of FDI-UG was presented in Figure 4. The matrix of the quenched sample exhibited the typical acicular martensite (Figure 4a). When the quenched sample was annealed for 20 min, the martensite decomposed into granular carbides and ferrite formed (Figure 4b). Additionally, some fine spheroidal particles with white contrast and ultrafine spheroidal graphite with dark contrast could be observed in the region of ferrite (Figure 4b). After annealing 60 min, all carbides and fine spheroidal particles with white contrast transformed into ultrafine spheroidal graphite with dark contrast (Figure 4c).
Figure 5 shows SEM images and EDS analysis of quenched ductile iron annealed at 700 °C for 20 min. The carbides with white contrast in the region A of Figure 5a were enlarged in Figure 5b. It could be seen that carbides appeared in granular and aggregated to form chains. The corresponding EDS analysis in the D area of Figure 5b was shown in Figure 5c. EDS confirmed the atomic ratio of Fe to C was about 3:1, which indicated that carbides were Fe3C. The result was consistent to previous literature [26], which reported that martensite easily decomposed into ferrite and Fe3C at high temperature (>500 °C). The area in Figure 5a with fine spheroidal particles and the ultrafine spheroidal graphite nodules were enlarged in Figure 5c. The size of fine spheroidal particles and the ultrafine spheroidal graphite nodules was estimated about 0.8 μm. It could be seen that the fine spheroidal particles with white contrast were surrounded by granular Fe3C with white contrast, which implied that the fine spheroidal particles with white contrast were transformed from the decomposition of granular Fe3C. It should be noted that there was almost no granular Fe3C around ultrafine spheroidal graphite with dark contrast (Figure 5c), which demonstrated that the Fe3C had totally transformed into ultrafine spheroidal graphite. The results of EDS analysis in the E, F and G areas of Figure 5c further confirmed the transformation process from Fe3C to ultrafine spheroidal graphite (Figure 5E–G). It should be mentioned that the boundary of ferrite grains migration was accompanied by the aggregation and growth of Fe3C during the recovery process of ferrite [27]. From aggregated Fe3C to fine spheroidal particles and then to ultrafine graphite, the composition containing C atoms gradually increased while the Fe atoms decreased (Figure 5D,E), which indicated that the aggregated Fe3C gradually decomposed into C atoms and Fe atoms, and the C atoms gradually aggregated to form graphite, while the Fe atoms moved into the matrix. Therefore, the fine spheroidal particles with white contrast were the transition phase from Fe3C transforming to ultrafine graphite nodules (Figure 5c). Additionally, it should be noted that the Si atoms content of Fe3C transforming to ultrafine graphite gradually decreased (Figure 5D,E), which indicated a close relationship between Si elements and the transformation Fe3C into ultrafine graphite nodules. Some literature has reported that the binding ability between Si atoms and Fe atoms was higher than that between C atoms and Fe atoms [28,29], which resulted in a reduction of Si content from Fe3C transforming into ultrafine graphite. The presence of Si element made the Fe3C easy to decompose and transform into the stable graphite phase.
Figure 6 presents fiction coefficient curves of FDI and FDI-UG under different normal loads. The frictional resistance generated by the asperities of the contact surface first led to an increase in the friction coefficient curve of FDI. As the asperities gradually flattened, graphite was gradually dragged to the contact surface, and the friction coefficient curve of FDI reached a stable value. However, the fiction coefficient curves of FDI-UG first showed a downward trend and then directly entered steady stage. The ultrafine graphite nodules in ductile iron could be quickly dragged out to the tribosurface and effectively exert their lubricating effect in the early stages, resulting in a rapid decrease in the friction curve and reaching a stable state. It could be seen that the FDI-UG exhibited a lower friction coefficient value compared to FDI. The friction coefficient value of FDI at steady state was 0.31 ± 0.020 and 0.28 ± 0.015 at 3 N and 6 N, respectively. However, the values were 0.15 ± 0.010 and 0.13 ± 0.008 for FDI-UG, which was only half of FDI at the same normal load. The steady-state friction coefficient values of FDI-UG was similar to the friction coefficient values (0.1~0.2) of graphene platelets with 6~15 nm thicknesses used as dry lubricants in high load rolling bearings in the previous study [30]. The result was related to the lubricating effect of ultrafine graphite nodules in FDI-UG. Additionally, it could be seen that the FDI and FDI-UG exhibited a lower friction coefficient value at higher normal load (6 N) compared to the value at lower normal load (3 N), which was attributed to the varying amount of graphite dragged out onto the tribosurface. More graphite could be dragged out to the tribosurface and played a lubricating role under high normal load (6 N) compared to the low normal load (3 N), giving rise to a lower friction coefficient value at 6 N.
Figure 7 illustrates the profiles of wear track for FDI and FDI-UG at 3 N and 6 N. As shown in Figure 7a,b, both the width and depth of the wear profiles for FDI and FDI-UG increased with the increase in normal loads, primarily due to the higher load resulting in more severe wear. Furthermore, under the same normal load, the wear track dimensions for FDI were larger than those of FDI-UG. For instance, the width and depth of the worn track for FDI were 1.05 mm and 28.38 μm at 3 N, respectively, while the corresponding values were measured as 0.84 mm and 23.82 μm for FDI-UG. These results indicated that FDI-UG exhibited relatively lower wear compared to FDI. The roughness (Ra) of the friction-discs interface (FDI) was evaluated as 1.2 ± 0.23 μm and 1.5 ± 0.26 μm at normal loads of 3 N and 6 N, respectively. In contrast, the Ra values for the FDI-UG were 0.86 ± 0.18 μm and 1.1 ± 0.19 μm at the same loads. Both Ra values for FDI and FDI-UG increased with increasing normal loads, primarily due to more severe wear occurring on the tribo-surface under higher loads. Notably, FDI-UG exhibited a lower Ra than FDI at equivalent loads, indicating enhanced wear resistance in FDI-UG. This superior wear resistance resulted in less wear on the tribo-surface compared to FDI. Furthermore, the lower Ra of FDI-UG contributed to a reduced friction coefficient during friction and wear.
Figure 8 illustrates the worn volume loss for FDI and FDI-UG at 3 N and 6 N. The worn volume loss for FDI and FDI-UG increased with increasing normal load. Notably, the worn volume loss for FDI was greater than that of FDI-UG at the same load. Specifically, at 3 N, the worn volume loss for FDI was measured at (9.22 ± 0.26) × 10−3 mm3, while at 6 N, it increased to (11.95 ± 0.34) × 10−3 mm3. In contrast, the worn volume loss for FDI-UG was (6.84 ± 0.16) × 10−3 mm3 at 3 N and (9.47 ± 0.23) × 10−3 mm3 at 6 N. These results demonstrate that FDI-UG exhibited superior wear resistance compared to FDI, which was related to the effective reduction of the friction coefficient in FDI-UG due to the ultrafine graphite nodules distributing on the tribological surface. Besides, the FDI-UG with a hardness of 183 ± 5 HV was higher than FDI with a hardness of 156 ± 3 HV due to the strengthening effect of fine grains. According the Archard’s equation as follows [31]:
V = K N L H
where K is wear coefficient, N is normal load, L is sliding distance and H is the hardness of material. The volume loss of (V) is proportional to normal load (N) disproportional to the hardness of material (H). Therefore, the FDI-UG exhibited the less volume loss compared to FDI. Meanwhile, the volume loss of FDI-UG and FDI increased with the increasing normal loads.
Figure 9 shows the worn surface for FDI and FDI-UG at 3 N and 6 N. The wear of contact surface gradually became severe and the amount of graphite worn out gradually increased with the increasing loads (Figure 9a–d). The proportion of graphite coverage in worn surface for FDI was estimated about 15% and 20% at 3 N and 6 N, while the values were about 31% and 38% for FDI-UG at 3 N and 6 N (Figure 9). Therefore, the friction coefficients of FDI and FDI-UG were low at 6 N compared to 3 N due to the higher graphite coverage on the tribosurface at 6 N (Figure 6 and Figure 9). Additionally, the FDI-UG exhibited higher graphite coverage on the tribosurface compared to the FDI, which resulted in a low friction coefficient of FDI-UG compared to FDI (Figure 6).
Figure 10 presents longitudinal section of worn track of FDI and FDI-UG at 3 N and 6 N. The ferrite matrix underwent varying degrees of deformation with the increasing normal loads. The deformation layer depth increased from about 5 μm to 10 μm when the load increased from 3 N to 6 N (Figure 10). Spheroidal graphite and ultrafine graphite nodules in the ferrite were squeezed and dragged to the tribosurface to act as lubricants, which was mainly responsible for reducing the friction coefficient. More graphite were squeezed and dragged to the tribosurface with the increasing load from 3 N to 6 N (Figure 10a–d), which resulted in a decrease in the fiction coefficient with the increasing loads. Additionally, the ultrafine graphite nodules exhibited a small size (0.8 μm) and high nodule count (3400 ± 163 nod/mm2) distribution in ferrite compared to initial spheroidal graphite (15 ± 3 μm and 350 ± 20 nod/mm2), and therefore more ultrafine graphite nodules could be easily dragged out to the tribosurface (Figure 10a–d). Therefore, the graphite lubricating layer was more easily formed in FDI-UG compared to FDI, which resulted in a lower friction coefficients for FDI-UG. It should be emphasized that the matrix distributing around the original graphite was easily to be plastically deformed due to the weak strength of graphite, which would promote the formation of abrasive during wear test. This would be discussed in the following.
Figure 11 shows worn surface of FDI and FDI-UG at 3 N and 6 N. The grooves and spalling could be observed in the worn surface of FDI and FDI-UG, which indicated that the mainly abrasive failure and surface fatigue occurred (Figure 11). Additionally, it should be mentioned that the adhesive wear also occurred for FDI under high loads (6 N). Some cracks could be found in region of spalling, which was responsible for the occurrence of spalling on worn surface (Figure 11a–c). The more wear debris acted as abrasive particles on the worn surface of FDI compared to FDI-UG (Figure 11), which resulted in more deep and wide grooves in the worn surface of FDI compared to FDI-UG (Figure 11a–d). The formation of ultrafine graphite nodules in ferritized ductile iron during annealing refined the grain of ferrite, which resulted in an increase in hardness of FDI-UG (183 ± 5 HV) compared to FDI (156 ± 3 HV). Therefore, the abrasive particles was prevented forming grooves in ferrite matrix, which reduced abrasive wear in the tribosurface of FDI-UG. Therefore, the relatively less abrasive wear occurred and only shallow and fine grooves were observed in worn surfaces of FDI-UG (Figure 11c,d). Besides, the initial spheroidal graphite could observed in worn surfaces of FDI and FDI-UG, while the additional precipitated ultrafine graphite nodules could be seen in the worn of FDI-UG (Figure 11). The ultrafine graphite nodules in the tribosurface further effectively lubricated, which resulted in lower frictional force on the contact surface. Additionally, the adhesion occurred in the worn surface of FDI at 6 N (Figure 11b), while this phenomenon has hardly been observed in the worn surface of FDI-UG (Figure 11d). Meanwhile, a lot of ultrafine graphite distributed on the worn surface of FDI-UG (Figure 11d). More ultrafine graphite in FDI-UG would be dragged out to the worn surface and reduced the direct contact area between the GCr15 ball and the FDI-UG at 6 N. Thus, the adhesive wear was suppressed in FDI-UG and the friction coefficient decreased.
Figure 12 presents a schematic diagram of FDI and FDI-UG during the friction and wear process. The microstructure of FDI was composed of initial spheroidal graphite and ferrite (Figure 12a). The ferrite, characterized with low hardness and high plasticity, readily underwent plastic deformation under normal loads (Figure 12b). During the friction and wear process, the initial graphite within the ferrite matrix was squeezed and transported to the tribological surface, playing a certain lubricating role and reducing the friction coefficient (Figure 12b). In contrast, the microstructure of FDI-UG included initial spheroidal graphite, ultrafine graphite nodules, and ferrite (Figure 12c). Under normal load, the ferrite in FDI-UG also underwent plastic deformation, leading to the squeezing and dragging of initial spheroidal graphite and ultrafine graphite nodules to the tribosurface. This resulted in a greater amount of graphite at the tribosurface of FDI-UG compared to FDI (Figure 12d). Consequently, the distribution of denser graphite on the tribosurface of FDI-UG, which more effectively reduced the friction coefficient compared to FDI.

4. Conclusions

In the work, the friction and wear performance of ferritized ductile iron was improved through introducing of ultrafine graphite nodules via solid phase transformation, which provided a new idea to designing the microstructure and enhancing the wear resistance of ductile iron. The results were expected to be applied to the design and production of anti-friction and wear-resistant ductile iron components. The following conclusions could be drawn.
(1)
The fine ferrite grains with the size of 15 μm and ultrafine graphite nodules with a count of 3400 nod/mm2 was obtained in ductile iron by annealing treatment in the present.
(2)
The formation of these ultrafine graphite nodules in ductile iron was primarily attributed to the instability of Fe3C, which was influenced by Si. This instability facilitated the graphitization of carbon atoms originating from the decomposition of Fe3C.
(3)
The presence of ultrafine graphite nodules supposed to be the main reason for reducing the friction coefficient of ductile iron by about 50% during wear test.
(4)
The high hardness of fine ferrite grains combined with low friction coefficient in ferritic ductile iron reduced abrasive wear and suppressed adhesion at high normal loads, thereby reducing the wear loss of ductile iron by about 20% during wear test.
(5)
This study provided a new method to enhancing the wear resistance of ductile iron through introducing the ultrafine graphite nodules and refine ferrite grains via solid phase transformation and was expected to be applied in the production of friction reducing and wear-resistant ductile iron.

Author Contributions

Conceptualization, B.J. and C.Y.; methodology, H.L.; software, C.Y.; validation, N.T., H.L. and C.Y.; formal analysis, C.L.; investigation, C.L.; resources, Y.D.; data curation, C.Y.; writing—original draft preparation, C.L.; writing—review and editing, Y.D.; visualization, H.L.; supervision, N.T.; project administration, C.Y.; funding acquisition, B.J. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Key Research and Development Project in Shaanxi Province (No. 2023QCY-LL-20) and Shaanxi Province Technical Innovation Guidance Special Project (No. 2023GXLH-040). And The APC was funded by the Key Research and Development Project in Shaanxi Province.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chen, K.; Li, H.; Jiang, Z.; Liu, F.; Kang, C.; Ma, X. Multiphase microstructure formation and its effect on fracture behavior of medium carbon high silicon high strength steel. J. Mater. Sci. Technol. 2021, 72, 81–92. [Google Scholar] [CrossRef]
  2. Pape, F.; Poll, G. Investigations on graphene platelets as dry lubricant and as grease additive for aliding contacts and rolling bearing application. Lubricants 2020, 8, 3. [Google Scholar] [CrossRef]
  3. Rohatgi, P.K.; Ray, S.; Liu, Y. Tribological properties of metal matrix-graphite particle composites. Int. Mater. Rev. 1992, 37, 129–152. [Google Scholar] [CrossRef]
  4. Wu, H.; Zhang, H.; Gao, A.; Gong, L.; Ji, Y.; Zeng, S. Friction and wear performance of aluminum-based self-lubricating materials derived from the 3D printed graphite skeletons with different morphologies and orientations. Tribol. Int. 2024, 195, 109614. [Google Scholar] [CrossRef]
  5. Li, H.; Liu, Y.; Zheng, B.; Wang, S.; Yi, Y.; Zhang, Y. On the tribological behaviors of Cu matrix composites with different Cu-coated graphite content. J. Mater. Res. Technol. 2023, 25, 83–94. [Google Scholar] [CrossRef]
  6. Tewary, U.; Paul, D.; Mehtani, H.K.; Bhagavath, S.; Alankar, A.; Mohapatra, G. The origin of graphite morphology in cast iron. Acta Mater. 2022, 226, 117660. [Google Scholar] [CrossRef]
  7. Vicente, A.D.A.; Sartori Moreno, J.R.; Santos, T.F.D.A.; Espinosa, D.C.R.; Tenorio, J.A.S. Nucleation and growth of graphite particles in ductile cast iron. J. Alloys Compd. 2019, 775, 1230–1234. [Google Scholar] [CrossRef]
  8. Hu, Z.; Liu, C.; Du, Y.; Wang, X.; Zhu, X.; Jiang, B. Effects of tempering temperature on mechanical and tribological behavior of ductile iron. Lubricants 2022, 10, 326. [Google Scholar] [CrossRef]
  9. Liu, C.; Du, Y.; Ying, T.; Zhang, L.; Zhang, X.; Wang, X. Effects of graphite nodule count on mechanical properties and thermal conductivity of ductile iron. Mater. Today Commun. 2022, 31, 103522. [Google Scholar] [CrossRef]
  10. Pedersen, K.M.; Tiedje, N.S. Graphite nodule count and size distribution in thin-walled ductile cast iron. Mater. Charact. 2008, 59, 1111–1121. [Google Scholar] [CrossRef]
  11. Rebasa, N.; Dommarco, R.; Sikora, J. Wear resistance of high nodule count ductile iron. Wear 2002, 253, 855–861. [Google Scholar] [CrossRef]
  12. Abedi, H.R.; Fareghi, A.; Saghafian, H.; Kheirandish, S.H. Sliding wear behavior of a ferritic-pearlitic ductile cast iron with different nodule count. Wear 2010, 268, 622–628. [Google Scholar] [CrossRef]
  13. Azeem, M.A.; Bjerre, M.K.; Atwood, R.C.; Tiedje, N.; Lee, P.D. Synchrotron quantification of graphite nodule evolution during the solidification of cast iron. Acta Mater. 2018, 155, 393–401. [Google Scholar] [CrossRef]
  14. Ghassemali, E.; Hernando, J.C.; Stefanescu, D.M.; Dioszegi, A.; Jarfors, A.E.W.; DluhoS, J. Revisiting the graphite nodule in ductile iron. Scr. Mater. 2019, 161, 66–69. [Google Scholar] [CrossRef]
  15. Shinde, V.D.; Ravi, B.; Narasimhan, K. Solidification behaviour and mechanical properties of ductile iron castings with varying thickness. Int. J. Cast. Metals Res. 2012, 25, 364–373. [Google Scholar] [CrossRef]
  16. He, K.; Daniels, H.R.; Brown, A.; Brydson, R.; Edmonds, D.V. An electron microscopic study of spheroidal graphite nodules formed in a medium-carbon steel by annealing. Acta Mater. 2007, 55, 2919–2927. [Google Scholar] [CrossRef]
  17. Lu, S.Y.; Chung, T.F.; Chen, J.J.; Lai, Y.W.; Hsiao, C.N.; Chen, C. Development of microstructures-properties in Fe-0.4C/0.2C-2Si-3Mn carbide-free bainite steels. Mater. Charact. 2023, 24, 112670. [Google Scholar] [CrossRef]
  18. Inam, A.; Brydson, R.; Edmonds, D.V. Raman spectroscopy study of the crystallinity of graphite formed in an experimental free-machining steel. Mater. Charact. 2020, 163, 25–30. [Google Scholar] [CrossRef]
  19. Inam, A.; Brydson, R.; Edmonds, D.V. Effect of starting microstructure upon the nucleation sites and distribution of graphite particles during a graphitising anneal of an experimental medium-carbon machining steel. Mater. Charact. 2015, 106, 86–92. [Google Scholar] [CrossRef]
  20. Kim, Y.J.; Park, S.H. Effect of initial microstructure on graphitization behavior of Fe-0.55C-2.3Si steel. J. Mater. Res. Technol. 2021, 15, 4529–4540. [Google Scholar] [CrossRef]
  21. Li, Q.; Li, R.; Yue, X.; Chang, G.; Zhai, Q. Effect of electropulsing on the formation of graphite during solid-state graphitization of spherical graphite iron. Mater. Chem. Phys. 2008, 112, 402–406. [Google Scholar] [CrossRef]
  22. Liu, C.; Du, Y.Z.; Li, P.C.; Wang, X.; Sun, W.T.; You, C.Y. Formation of Ultrafine Graphite Nodules in Ductile Iron and its Effects on Mechanical Properties. J. Mater. Eng. Perform. 2023, 33, 10485–10494. [Google Scholar] [CrossRef]
  23. Nishikawa, A.S.; Miyamoto, G.; Furuhara, T.; Tschiptschin, A.P.; Goldenstein, H. Phase transformation mechanisms during Quenching and Partitioning of a ductile cast iron. Acta Mater. 2019, 179, 1–16. [Google Scholar] [CrossRef]
  24. Johnson, K.L.; Kendall, K.; Roberts, A.D. Surface Energy and the Contact of Elastic Solids. Proc. R. Soc. Lond. 1971, 324, 301–313. [Google Scholar] [CrossRef]
  25. Tang, Y.; Ji, P.; Li, B.; Zhang, G.; Ma, W. Effect of loading on microstructure and friction and wear behavior of an austenite lightweight steel. Tribol. Int. 2023, 177, 108006. [Google Scholar] [CrossRef]
  26. Saha, D.C.; Biro, E.; Gerlich, A.P.; Zhou, Y. Martensite tempering kinetics: Effects of dislocation density and heating rates. Mater. Charact. 2020, 168, 110564. [Google Scholar] [CrossRef]
  27. Li, S.; He, M.; Hu, G.; Tian, Y.; Wang, C.; Jing, B. Pearlite formation via martensite. Compos. Part B Eng. 2022, 238, 109859. [Google Scholar] [CrossRef]
  28. Kim, K.H.; Lee, J.S.; Lee, D.L. Effect of silicon on the spheroidization of cementite in hypereutectoid high carbon chromium bearing steels. Met. Mater. Int. 2010, 16, 871–876. [Google Scholar] [CrossRef]
  29. Vélez, J.M.; Garboggini, A.; Tschiptschin, A.P. Effect of silicon on kinetics of bainitic reaction in austempered ductile cast iron. Mater. Sci. Technol. 1996, 12, 329–337. [Google Scholar] [CrossRef]
  30. Pape, F. Investigation of graphene platelet-based dry lubricating film formation in tribological contacts. Coatings 2024, 14, 360. [Google Scholar] [CrossRef]
  31. Archard, J.F. Contact and rubbing of flat surfaces. J. Appl. Phys. 1953, 24, 981–998. [Google Scholar] [CrossRef]
Figure 1. Schematic diagram of two annealing processes (A) ductile iron directly annealed at 900 °C, (B) quenched ductile iron and annealed at at 700 °C.
Figure 1. Schematic diagram of two annealing processes (A) ductile iron directly annealed at 900 °C, (B) quenched ductile iron and annealed at at 700 °C.
Lubricants 13 00399 g001
Figure 2. Schematic diagram of the friction experiments.
Figure 2. Schematic diagram of the friction experiments.
Lubricants 13 00399 g002
Figure 3. Microstructure of FDI and FDI-UG after annealing: (a,b) low and (c,d) high magnifications; (a,c) FDI and (b,d) FDI-UG.
Figure 3. Microstructure of FDI and FDI-UG after annealing: (a,b) low and (c,d) high magnifications; (a,c) FDI and (b,d) FDI-UG.
Lubricants 13 00399 g003
Figure 4. Microstructure of the quenched ductile iron after annealing at 700 °C for (a) 0 min, (b) 20 min and (c) 60 min.
Figure 4. Microstructure of the quenched ductile iron after annealing at 700 °C for (a) 0 min, (b) 20 min and (c) 60 min.
Lubricants 13 00399 g004
Figure 5. Microstructure of the quenched sample annealed at 700 °C for 20 min: (a) low magnifications; (b,c) are high magnifications of corresponding regions of B and C at (a); D, E, F and G are the EDS point analysis of the corresponding area in (b,c).
Figure 5. Microstructure of the quenched sample annealed at 700 °C for 20 min: (a) low magnifications; (b,c) are high magnifications of corresponding regions of B and C at (a); D, E, F and G are the EDS point analysis of the corresponding area in (b,c).
Lubricants 13 00399 g005
Figure 6. Fiction coefficient curves of FDI and FDI-UG at different normal loads.
Figure 6. Fiction coefficient curves of FDI and FDI-UG at different normal loads.
Lubricants 13 00399 g006
Figure 7. The profiles of wear track of FDI and FDI-UG at 3 N and 6 N: (a) FDI and (b) FDI-UG.
Figure 7. The profiles of wear track of FDI and FDI-UG at 3 N and 6 N: (a) FDI and (b) FDI-UG.
Lubricants 13 00399 g007
Figure 8. Worn volume loss of FDI and FDI-UG at 3 N and 6 N.
Figure 8. Worn volume loss of FDI and FDI-UG at 3 N and 6 N.
Lubricants 13 00399 g008
Figure 9. Optical images of worn surface under the loads of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Figure 9. Optical images of worn surface under the loads of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Lubricants 13 00399 g009
Figure 10. Longitudinal section of worn track under the load of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Figure 10. Longitudinal section of worn track under the load of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Lubricants 13 00399 g010
Figure 11. SEM images of worn surface under the load of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Figure 11. SEM images of worn surface under the load of (a,c) 3 N and (b,d) 6 N for (a,b) FDI and (c,d) FDI-UG.
Lubricants 13 00399 g011
Figure 12. Schematic diagram of the wear process of ductile iron with (a,b) FDI and (c,d) FDI-UG.
Figure 12. Schematic diagram of the wear process of ductile iron with (a,b) FDI and (c,d) FDI-UG.
Lubricants 13 00399 g012
Table 1. Chemical compositions of as cast ductile iron (wt. %).
Table 1. Chemical compositions of as cast ductile iron (wt. %).
CSiMnPSMgREFe
3.522.450.10.0220.0150.0490.011Bal.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Liu, C.; Du, Y.; Li, H.; You, C.; Yang, C.; Tian, N.; Jiang, B. Improving the Wear Properties of Ductile Iron by Introducing Ultrafine Graphite Nodules. Lubricants 2025, 13, 399. https://doi.org/10.3390/lubricants13090399

AMA Style

Liu C, Du Y, Li H, You C, Yang C, Tian N, Jiang B. Improving the Wear Properties of Ductile Iron by Introducing Ultrafine Graphite Nodules. Lubricants. 2025; 13(9):399. https://doi.org/10.3390/lubricants13090399

Chicago/Turabian Style

Liu, Chen, Yuzhou Du, Haohao Li, Caiyin You, Chao Yang, Na Tian, and Bailing Jiang. 2025. "Improving the Wear Properties of Ductile Iron by Introducing Ultrafine Graphite Nodules" Lubricants 13, no. 9: 399. https://doi.org/10.3390/lubricants13090399

APA Style

Liu, C., Du, Y., Li, H., You, C., Yang, C., Tian, N., & Jiang, B. (2025). Improving the Wear Properties of Ductile Iron by Introducing Ultrafine Graphite Nodules. Lubricants, 13(9), 399. https://doi.org/10.3390/lubricants13090399

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Article metric data becomes available approximately 24 hours after publication online.
Back to TopTop