Next Article in Journal
Organo-Modified Vermiculite: Preparation, Characterization, and Sorption of Arsenic Compounds
Next Article in Special Issue
Petrographical and Geochemical Signatures Linked to Fe/Mn Reduction in Subsurface Marine Sediments from the Hydrate-Bearing Area, Dongsha, the South China Sea
Previous Article in Journal
Reuse of Dunite Mining Waste and Subproducts for the Stabilization of Metal(oid)s in Polluted Soils
Previous Article in Special Issue
Can Primary Ferroan Dolomite and Ankerite Be Precipitated? Its Implications for Formation of Submarine Methane-Derived Authigenic Carbonate (MDAC) Chimney
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Simultaneous Leaching of Seafloor Massive Sulfides and Polymetallic Nodules

1
Department of Geoscience and Petroleum, NTNU Norwegian University of Science and Technology, S. P. Andersens veg 15a, 7031 Trondheim, Norway
2
GeMMe, University of Liege, Allée de la Découverte 9, 4000 Liège, Belgium
*
Author to whom correspondence should be addressed.
Minerals 2019, 9(8), 482; https://doi.org/10.3390/min9080482
Submission received: 9 July 2019 / Revised: 7 August 2019 / Accepted: 8 August 2019 / Published: 10 August 2019
(This article belongs to the Special Issue Marine Geology and Minerals)

Abstract

:
Simultaneous leaching of seafloor massive sulfides (SMS) from Loki’s Castle on the Arctic Mid-Ocean Ridge (AMOR) and polymetallic nodules (PN) from Clarion Clipperton Zone (CCZ) of the Central Pacific Ocean was studied. Leaching tests were conducted using sulfuric acid and sodium chloride, at a temperature of 80 °C for 48 h under reflux. The effect of PN-to-SMS ratio was examined. It was shown that simultaneous leaching of two different types of marine resources was possible resulting in high dissolution rates of metals. The proposed process has many advantages as it does not require pyrometallurgical pretreatment, and yields solid products (i.e., silica, barite, elemental sulfur, albite, microcline, muscovite), which might be utilized for various industrial applications.

Graphical Abstract

1. Introduction

Polymetallic nodules (PN), iron-manganese crusts (Fe-MnC) and seafloor massive sulfides (SMS) deposits, due to their high content of various economically important metals (i.e., Cu, Ag, Zn, Mn, REE, etc.), have been identified as important marine mineral resources for the future [1,2]. Each type of deposit presents individual challenges at every stage of exploration, exploitation, and metal extraction cycle [3]. SMS are metallic sulfide ores, while PN and Fe-MnC are metallic oxide ores, thus their processing requires different methodologies. Whereas sulfides are conventionally processed by flotation [4], leaching has become an efficient method for the extraction of metals from oxides [5].
The complex mineralogy and rapid oxidation of SMS provide challenges to conventional beneficiation by flotation [6,7,8], thus a new process to extract metals simultaneously by leaching of SMS and PN is proposed in this paper. The simultaneous leaching of manganese dioxide and sulfides such as chalcopyrite [9,10], sphalerite [11], and pyrite [12] in acid media has been investigated. In our previous paper [8], we showed that the dissolution rate of metals from SMS was accelerated in the presence of MnO2 in the H2SO4-NaCl media. This acceleration was interpreted to be a result of galvanic interactions between the sulfide minerals of the SMS ore, such as chalcopyrite (CuFeS2), isocubanite (CuFe2S3), sphalerite ((Zn,Fe)S), pyrite/marcasite (FeS2), and manganese dioxide (MnO2). We suggested that polymetallic nodules might serve as a potential source of MnO2 acting as an oxidant for leaching of metals from SMS. Furthermore, PN contain not only manganese and iron but also other economically important metals such as copper, nickel, cobalt etc., which can be recovered during leaching of a mixture of SMS and PN. However, to date, no paper has been published on simultaneous leaching of SMS and PN. Our approach considers the mixed H2SO4-NaCl system, which is efficient and less expensive than leaching in pure chloride systems [13,14,15]. The successful development of such a process offers an attractive alternative to pyrometallurgical processing, as it offers the prospect of eliminating gas emission, production of potentially recoverable solid residues and generation of acid, which could be recycled to the head of the process. The new approach holds promise for efficient processing of marine mineral resources.

2. Materials and Methods

2.1. Materials

This study utilizes an SMS sample collected from the Loki’s Castle active hydrothermal vent field at the Arctic Mid-Ocean Ridge (AMOR), which occurs on the Mohn’s Ridge at a depth of approximately 2400 m [16]. The SMS samples were collected as a part of the MarMine cruise [17]. More than 200 kg of loose boulders from the mound flanks were collected via grab sampling. The location and areas of operation are described elsewhere [7,17,18]. In order to prevent oxidation of sulfides, the collected rock samples were bagged, flushed with nitrogen, vacuum sealed, and stored at −21 °C.
The polymetallic deep-sea nodules (PN) studied in this research were collected in the license area of Global Sea Mineral Resources (GSR) from Clarion Clipperton Zone (CCZ) of the Central Pacific Ocean. The samples were stored in plastic bags.
Mili-Q water® and analytically grade H2SO4 and NaCl were used in the experiments.

2.2. Methods

Prior to characterization and leaching experiments, the SMS sample was unpacked and dried at room temperature (25 °C), while the PN samples were dried in a drying cabinet at 60 °C. Then, the individual rock samples were crushed using a jaw crusher (Retsch GmbH, Haan, Germany), ground in a disc mill (Retsch GmbH, Haan, Germany), and sieved to obtain 100% finer than 50 µm, with a d50 of 10 µm.
A known mass of feed for leaching (7.5 ± 0.05 g) consisting of either pure SMS, PN or their mixtures at different ratios, together with 150 cm3 of 1.0 M sulfuric acid (H2SO4) and 1 M sodium chloride (NaCl) were added to 250 cm3 reaction flasks. Then, the flasks were placed in the Carousel 6 Plus reaction station from Radley’s Innovation Technology, stirred at 700 rpm, and heated to 80 °C. Leaching experiments were conducted for 48 h under reflux.
Leachate was collected periodically, filtered using a 32 mm syringe filter with 0.2 µm Supor® membrane, diluted 10-times using 1.0% (v/v) HNO3, and then analyzed at NTNU using inductively coupled plasma mass spectroscopy (ICP-MS, PerkinElmer SCIEX-ELAN DRC II, Waltham, MA, USA).
The leaching residues were dried at 60 °C prior to chemical and mineralogical analyses. The bulk chemical composition of the leaching feed and residues was analyzed at NTNU with ICP-MS and X-ray fluorescence (XRF, ThermoScientific, Waltham, USA). A 2 g of solid sample and 20 cm3 of concentrated nitric acid were added to a 100 cm3 closed Erlenmeyer flask. The mixture was placed on a hot plate and heated to 85 °C for 20 h. After digestion, the sample was cooled to the room temperature, filtered, diluted to 50 cm3, and then analyzed.
The mineralogy was determined by using semi-quantitative X-ray diffraction (XRD) at NTNU, and automated mineralogy (AM) at GeMMe. The XRD patterns were collected using a Bruker D8 Advanced XRD (Billerica, MA, USA), using CuK alpha radiation with a wavelength of 0.154056 nm taking measurements between 3–65° 2θ at a step size of 0.01° 2θ s−1. The mineral phases were identified by the use of diffract.Eva software. For automated mineralogy, ca. 1 g of representative sample was embedded in a mixture of 0.4 g carbon powder, 15 cm3 epoxy resin and 2 cm3 hardener in order to obtain blocks of 2.5 cm, which were then polished [19]. The polished blocks were observed by optical microscopy and analyzed using a ZEISS Sigma 300 field emission scanning electron microscope fitted with two Bruker xFlash 6|30 X-ray detectors for energy-dispersive X-ray spectroscopy (EDX) analysis. The mineral composition was analyzed using Mineralogical Mining System from Zeiss Ltd. (Oberkochen, Germany). The operating conditions for data acquisition were as follows: 20 kV acceleration voltage, 3 µm step size, and 30.000 number of analyzed particles. More details about the AM can be found elsewhere [20].
The leaching efficiency (recovery) of metals was calculated based on the amount of leached metal in the leachate with respect to the concentration of metal in the feed. The results were obtained from at least three determinations at a 95% confidence interval.

3. Results and Discussion

3.1. Material Characterization

Figure 1 illustrates the mineralogical phases of SMS sample, while Figure 2 and Table 1 show the SEM-EDS analyses of the leaching feed for a mixture of PN (67%) and SMS (33%), as an example. Mineralogy of this particular leaching feed is discussed in Section 3.3.
The investigated SMS sample represents the hydrothermal vent fragments. Each collected sample represents different bulk chemistry and mineralogy. A detailed characterization of SMS rock samples from AMOR is provided by Snook et al. [18]. The SMS samples were characterized using ICP-MS, XRD, XRF, optical microscopy, and automated mineralogy. Briefly, the SMS sample investigated in this work was very porous and heterogeneous comprising the following mineralogical phases determined by XRD: Quartz (SiO2, ca. 36.8%) with trace barite (BaSO4, ca. 1.0%), pyrite/marcasite (ca. 38.2%), sphalerite (ca. 12.1%), galena (ca. 1.0%), isocubanite (ca. 4.7%), chalcopyrite (ca. 2.5%) and others (ca. 3.7%). Chalcopyrite, isocubanite and sphalerite showed complex intergrowth textures with chalcopyrite lamellae within isocubanite, and sphalerite (Figure 1 and Figure 2). Homogenous sphalerite contained up to 20% of Fe (Table 1). In this work, the sample containing 2.0% Cu, 7.4% Zn, 21.0% Fe, 26.9% S, 2.8% Pb, 12.0% Si, 0.1% Ba, was used.
Figure 2b shows that polymetallic nodules represent the typical heterogeneous layer growth structure with the crystal structure of Mn-oxides and Mn-Fe(oxy) hydroxides being intergrown on a submicron scale. The major minerals for manganese and iron are todorokite (Na,Ca,K)2(Mn4+,Mn3+)6O12·3–4.5(H2O), birnessite (Na,Ca,K)0.5(Mn4+,Mn3+)2O4·1.5H2O), buserite (Na4Mn14O27·21H2O), manganite (MnOOH), vernadite (Mn4+,Fe3+,Ca,Na)(O,OH)2·nH2O, goethite (FeOOH), magnetite (Fe3O4) or hematite (Fe2O3) ([21], chemical formulae based on [22]). Muscovite (KAl2(Si3Al)O10(OH,F)2), microcline (KAlSi3O8), albite (NaAlSi3O8) and quartz (SiO2) were the analysed silicates (chemical formulae based on [22]). The investigated PN contained 27.7% Mn, 5.5% Fe, 1.3% Ni, 1.1% Cu, 0.12% Zn.

3.2. Leaching

Our previous study [8] investigated various factors such as the temperature, H2SO4 concentration, and dosage of NaCl, that could influence dissolution of metals from SMS rock samples in the presence of pure manganese dioxide, as an oxidant. In this paper, we only emphasized changes in time and dosage of polymetallic nodules, while other leaching parameters, such as 1 M H2SO4, 1 M NaCl, 80 °C, 700 rpm, solid-to-liquid ratio of 50 g/L, were kept constant.
The leaching recoveries of copper and manganese at various times and PN-to-SMS ratios are shown in Figure 3 and Figure 4. The results show that copper was not extracted from SMS in the aqueous solution of H2SO4 (1 M) and NaCl (1 M) without polymetallic nodules. We interpret this to be due to the absence of an oxidizing agent, that is MnO2. The addition of polymetallic nodules resulted in the increased leaching of metals within the first two hours. The mechanism behind this could be either an increased dissolution due to a source of manganese dioxide, Fe as well as Cu and Ni or the result of rapid desorption of metals from the PN structure. One can see that two different stages of leaching kinetics can be distinguished (Figure 3). In the first stage, before 2 h, copper dissolved rapidly, while after two hours, it dissolved at a relatively slow rate, ultimately reaching plateau. The leaching recovery of metals increased, and at the same time the content of metal in the residue decreased (Figure 4). Under the investigation conditions, Ni dissolved rapidly (Figure 3c), while Zn followed the Cu pattern (Figure 3d). Thus, for the sake of clarity, we only discuss the data for Cu and Mn.
The kinetics of copper dissolution varied with the concentration of MnO2 (Figure 3a and Figure 4a). For the first two hours, the copper recovery changed significantly from ca. 50% to ca. 70% as the dosage of PN increased from 33% to 67%. We interpret this to be due to increased concentration of MnO2, as an oxidizing agent, from ca. 7 and 14.5 g/L, respectively. A higher concentration of MnO2 and longer leaching time improved the leaching reaction of copper from chalcopyrite, isocubanite, sphalerite/chalcopyrite intergrowths as well as from the PN matrix.
The results clearly indicate that there was only partial dissolution of manganese in the absence of SMS (PN dosage of 100%, which corresponds to 22 g/L of MnO2) (Figure 3 and Figure 4). Thus, in order to dissolve manganese from PN, it was necessary to use a reducing agent. In the presence of SMS, as a source of Fe(II), irrespective of the SMS-to-PN ratio, manganese from polymetallic nodules dissolved rapidly, and almost the whole manganese was leached out within 30 min. One can clearly see that dissolution of copper was slower than that of Mn (Figure 3). After two hours of the process, the recovery of copper was increasing slowly with the leaching time, while manganese was already dissolved. It indicates the preferential dissolution of manganese over copper under-investigated conditions. For PN, initial dissolution of major elements such as Mn and Fe affects further dissolution of minor constituents such as Cu and Ni which are finely disseminated in the PN matrix [24].
Simultaneous leaching of SMS and PN in the H2SO4-NaCl media was found to occur due to three possible routes: (i) Galvanic interactions between manganese dioxide and primary marine minerals of SMS (i.e., pyrite, isocubanite, chalcopyrite, sphalerite), (ii) the action of the Fe3+/Fe2+ couple, as well as iii) possible action of chlorine gas generated in the mixed sulfate–chlorite media in the presence of MnO2, which has been readily utilized in the redox reaction. The possible dissolution mechanism was described in detail elsewhere [8].
Briefly, complete dissolution of Mn results in reduction of manganese(IV) to manganese(II) by ferrous (Fe2+) ions in the aqueous solution of H2SO4 according to the simplified reaction:
MnO2 + 2Fe2+ + 4H+ Mn2+ + 2Fe3+ + 2H2O
In the mixed sulfate–chloride media and the solution containing dissolved MnO2, ferrous (Fe2+) ions could be oxidized to ferric (Fe3+) ions, which then acted as an oxidizing agent for chalcopyrite isocubanite and sphalerite/chalcopyrite intergrowths as well as PN matrix. In the MnO2-H2SO4-NaCl system, dissolution of copper was also possible due to mineral surface complexation with Cl according to the reactions:
CuFeS2 + 4Fe3+ Cu2+ + 5Fe2+ + 2S0
CuFe2S3 + 6Fe3+ Cu2+ + 8Fe2+ + 3S0
2CuFeS2 + 5Cl2 2CuCl2+ + 2FeCl3 + 4S0
CuFe2S3 + 4Cl2 CuCl2+ + 2FeCl3 + 3S0
Based on the XRD data of the leachate residue (Figure 5) the leaching process yielded sulfur in its elemental form, confirming the aforementioned reactions.
The results also indicate that copper was dissolved from PN in the mixed sulfate–chlorite media without SMS, while the recovery of manganese remained very low in the absence of the reducing agent (Figure 3 and Figure 4). High copper recovery may result from involvement of H+ and Cl in the surface reaction and dissolution of copper oxide according to the simplified reaction:
CuO + 2H+ Cu2+ + H2O
Moreover, the presence of ferric(III) oxyhydroxide (goethite) in the PN matrix, which dissolves according to the reaction:
FeOOH + 3H+ Fe3+ + 2H2O
could facilitate complete dissolution of copper oxide species from PN. Low recovery of Mn resulted from the existence of stable MnO2, Mn3O4, MnOOH species [24].

3.3. Mineralogical Analyses of Feed and Residues

The mineralogy of the feed, consisting of 67% PN and 33% SMS, and leaching residues was investigated to reveal the effect of time on mineral phase changes during simultaneous leaching of SMS and PN. The XRD and automated mineralogy (Zeiss Mineralogic Mining, AM) analyses, in the form of mineral abundance, are presented in Figure 5 and Figure 6, respectively. Due to the complex structure of PN, with typical grain size less than the 3 µm analytical step size (pixel spacing) in AM, it was impossible to distinguish different types of silicates using AM. Since the leaching feed sample was very amorphous, the presented XRD results are semi-quantitative. Thus, both methods have been used to strengthen the results and discussion. Furthermore, AM provides information on the elemental deportment, which can be found in Figure 7.
According to the XRD analyses (Figure 5), the feed sample (depicted as 0) contained significant quantities of pyrite/marcasite/pyrrhotite (ca. 21%), chalcopyrite (ca. 5.4%), isocubanite (ca. 4.3%) with silicates (ca. 53%) such as quartz, albite, muscovite and microcline as a gangue material. The automated mineralogy analyses revealed the presence of ca. 1% goethite in the feed sample, which was not found by XRD. As shown in Figure 2c,d, the typical heterogeneous layer growth structure of nodules, that is the crystal structure of Mn-oxides and Mn-Fe(oxy) hydroxides, were intergrown on a submicron scale. Thus, the polymetallic nodule structure was depicted by the automated mineralogy as a mixed polymetallic (Poly) phase (Figure 6). The analyzed by XRD silicate minerals were grouped into one group in the AM analysis (Figure 6).
The distribution of elements in the leaching feed, obtained from the automated mineralogy, revealed that manganese occurs only within the heterogeneous layer growth structure of nodules (Figure 7), and its content ranges from ca. 40 to ca. 51%. Copper was found to be distributed among chalcopyrite (ca. 24%) and isocubanite (ca. 63%), in addition to being associated with Fe-silicates (ca. 13%), being a part of the PN matrix. The submicron inclusions of chalcopyrite in sphalerite were not detected by automated mineralogy (3 µm pixel spacing), thus no copper deportment in sphalerite was reported. Zinc occurs mainly in sphalerite (ca. 95%) with minor presence in Fe-silicates. Iron was distributed among iron sulfides (pyrite/marcasite ca. 38%, pyrrhotite ca. 6%), silicates (ca. 18%), goethite (ca. 15%), sphalerite (ca. 14%), isocubanite (ca. 7%) and chalcopyrite (ca. 1%).
As indicated by the XRD and AM findings, the mineral composition of residues changed with the leaching time (Figure 5, Figure 6, Figure 7 and Figure 8). The leaching caused a significant reduction in the amount of sulfides in the solid phase and resulted in concentrations of 15%, 7%, 3% and 1% after 2, 12, 24 and 48 h, respectively (XRD, Figure 5 and Figure 7a). Pyrite/marcasite, pyrrhotite, and goethite were rapidly dissolved being utilized for leaching of Mn-oxide species from PN (Figure 5 and Figure 6). The proportion of iron deportment in the leaching residues changed significantly. In the residue after 48 h, iron occurred mostly in silicates (ca. 75%), with only a minor proportion (<1 wt %) attributed to sulfides (Figure 7).
The XRD results show that the leaching process yielded elemental sulfur (Figure 5). The sulfides were readily oxidized to form elemental sulfur, which comprised ca. 22–24% of the leaching residues. Some sulfur might also get oxidized to sulfates, generating sulfuric acid. It should be noted that elemental sulfur was only detected by XRD (a lack of S0 detection by MA might be a result of either its rapid oxidation or removal during the sample preparation for MA). One should also note that jarosite was not found by either mineralogical method. Thus, it confirms the aforementioned reactions, and proves that in the mixed sulfate–chloride systems in the presence of MnO2 jarosite does not precipitate and elemental sulfur is the only product of sulfides dissolution.
The silicates were more abundant compared to the feed sample, and their proportion increased with the leaching time (Figure 6 and Figure 7). As revealed by mineralogical observations, after 48 h of leaching, the residue sample was mostly composed of silicates, elemental sulfur, and barite. These mineralogical phases are not reactive to the leaching process.
After leaching there was only a slight reduction in the grain size (from d50 10 to 8 µm). The remaining grains were extremely fine and locked in coarser grains of silicates (Figure 8).

4. Conclusions

Simultaneous processing of seafloor massive sulfides (SMS) and polymetallic nodules (PN) was studied in this paper. Leaching experiments were conducted using sulfuric acid and sodium chloride at different ratios of PN-to-SMS. It was shown that simultaneous leaching of two different types of marine resources was possible, resulting in high extraction of metals. The mineralogical investigations revealed that leaching residues consisted of silicates (quartz, muscovite, microcline, albite) in addition to elemental sulfur and barite, with trace abundance in sulfides (<1 wt %). These products might be purified using physical and physicochemical methods, and then utilized for various applications, including: Electronics and glass/ceramic production (silicates), oil and gas drilling (baryte) as well as sulfuric acid production and polymeric materials (sulfur, [25]). They could also be utilized as heavy metal absorbents (e.g., [26]). Metals from the leachate might be extracted through different methods among which solvent extraction and electrowinning are widely used. The leach solution would be recycled to the head of the process. The simplified conceptual flowsheet is presented in Figure 9.
Simultaneous leaching of marine minerals has many advantages as it results in high extraction of metals, and also the need for additional oxidizing and reducing agents is reduced resulting in a less expensive and more environmentally friendly process. For SMS-PN in the mixed sulfate–chloride system, the process does not require pyrometallurgical pretreatment, thus the environmental impact can be significantly reduced. Moreover, due to high costs of hydrochloric acid, the addition of sodium chloride offers the possibility of an efficient and less expensive leaching process.

Author Contributions

Conceptualization, P.B.K.; methodology, P.B.K.; formal analysis, P.B.K.; investigation, P.B.K. and H.B.; writing—original draft preparation, P.B.K.; writing—review & editing, P.B.K., H.B., R.A.K., K.A.; visualization, P.B.K.; supervision, R.A.K.; funding acquisition, K.A.

Funding

This work was funded by the Research Council of Norway (Norges Forskningsråd, NFR) Project No. 247626/O30. The industrial partners are acknowledged for co-funding the project.

Acknowledgments

The authors gratefully acknowledge Torill Sørløkk and Laurentius Tijhuis, NTNU for their technical assistance with XRF, ICP-MS and XRD, as well as Ben Snook and Kristian Drivenes for their help in mineralogical characterization of the SMS and PN samples. Further thanks go to Global Sea Mineral Resources (GSR), DEME Group and Aleksandra Lang for providing the polymetallic nodule samples. The authors would also like to thank five anonymous reviewers for their detailed and constructive comments.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Lusty, P.A.J.; Murton, B.J. Deep-ocean mineral deposits: metal resources and windows into Earth processes. Elements 2018, 14, 301–306. [Google Scholar] [CrossRef]
  2. Sharma, R. Deep-Sea Mining: Current Status and Future Considerations. In Deep-Sea Mining Resource Potential, Technical and Environmental Considerations; Sharma, R., Ed.; Springer International Publishing AG: Cham, Switzerland, 2018. [Google Scholar]
  3. Lodge, M.W.; Verlaan, P.A. Deep-sea mining: International regulatory challenges and responses. Elements 2018, 14, 331–336. [Google Scholar] [CrossRef]
  4. Drzymala, J. Mineral Processing. Foundations of Theory and Practice of Metallurgy; Oficyna Wydawnicza Politechniki Wroclawskiej: Wroclaw, Poland, 2007. [Google Scholar]
  5. Gupta, C.K. Chemical Metallurgy: Principles and Practice; John Wiley & Sons: New Jersey, NJ, USA, 2006. [Google Scholar]
  6. Nakajima, Y.; Uto, S.; Kanada, S.; Yamamoto, J.; Takahashi, J.; Otabe, S.; Sadaki, J.; Okaya, K.; Matsuo, S.; Fujita, T. Concept of seafloor mineral processing for development of seafloor massive sulfides. In Proceedings of the ASME 30th International Conference on Ocean, offshore and Arctic Engineering, Rotterdam, The Netherlands, 19–24 June 2011. [Google Scholar]
  7. Kowalczuk, P.B.; Snook, B.; Kleiv, R.A.; Aasly, K. Efficient extraction of copper and zinc from seafloor massive sulphide rock samples from the Loki’s Castle area at the Arctic Mid-Ocean Ridge. Miner. Eng. 2018, 115, 106–116. [Google Scholar] [CrossRef]
  8. Kowalczuk, P.B.; Manaig, D.O.; Drivenes, K.; Snook, B.; Aasly, K.; Kleiv, R.A. Galvanic leaching of seafloor massive sulphides using MnO2 in H2SO4-NaCl media. Minerals 2018, 8, 235. [Google Scholar] [CrossRef]
  9. Havlik, T.; Laubertova, M.; Miskufova, A.; Kondas, J.; Vranka, F. Extraction of copper, zinc, nickel and cobalt in acid oxidative leaching of chalcopyrite at the presence of deep-sea manganese nodules as oxidant. Hydrometallurgy 2005, 77, 51–59. [Google Scholar] [CrossRef]
  10. Nakazawa, H.; Hareyama, W. Galvanic leaching of chalcopyrite using manganese oxides in spent zinc-carbon batteries. Resour. Process. 2016, 63, 3–11. [Google Scholar] [CrossRef]
  11. Wang, S.F.; Xiao, L.; Li, Y.Q.; Fang, Z.; Qiu, G.Z.; Li, J. Electronegative leaching for sphalerite-MnO2 in the presence of acidithiobacillus ferrooxidants. J. Therm. Anal. Calorim. 2009, 95, 601–604. [Google Scholar] [CrossRef]
  12. Nayak, B.B.; Mishra, K.G.; Paramguru, R.K. Kinetics and mechanism of MnO2 dissolution in H2SO4 in the presence of pyrite. J. Appl. Electrochem. 1999, 29, 191–200. [Google Scholar] [CrossRef]
  13. Lu, Z.Y.; Jeffrey, M.I.; Lawson, F. The effect of chloride ions on the dissolution of chalcopyrite in acidic solutions. Hydrometall. 2000, 56, 189–202. [Google Scholar] [CrossRef]
  14. Dutrizac, J.E.; MacDonald, R.J.C.; Ingraham, T.R. The kinetics of dissolution of cubanite in aqueous acidic ferric sulfate solutions. Metall. Trans. 1970, 1, 3083–3088. [Google Scholar]
  15. Veloso, T.C.; Peixoto, J.J.M.; Pereira, M.S.; Leao, V.A. Kinetics of chalcopyrite leaching in either ferric sulphate or cupric sulphate media in the presence of NaCl. Int. J. Miner. Process. 2016, 148, 147–154. [Google Scholar] [CrossRef]
  16. Pedersen, R.B.; Rapp, H.T.; Thorseth, I.H.; Lilley, M.D.; Barriga, F.J.A.S.; Baumberger, T.; Flesland, K.; Fonseca, R.; Fruh-Green, G.L.; Jorgensen, S.L. Discovery of a black smoker vent field and vent fauna at the Arctic Mid-Ocean Ridge. Nat. Commun. 2010, 1, 126. [Google Scholar] [CrossRef]
  17. Ludvigsen, M.; Aasly, K.; Ellefemo, S.; Hilario, A.; Ramirez-Llodra, E.; Søreide, F.; Falcon-Suarez, I.; Juliani, C.; Kieswetter, A.; Lim, A.; et al. NTNU Cruise Reports 2016 No 1 MarMine Arctic Mid Ocean Ridge 15.08.2016–05.09.2016; NTNU: Trondheim, Norway, 2016; ISSN 2535-2520. [Google Scholar]
  18. Snook, B.; Drivenes, K.; Rollinson, G.; Aasly, K. Characterisation of Mineralised Material from the Loki’s Castle Hydrothermal Vent on the Mohn’s Ridge. Minerals 2018, 8, 576. [Google Scholar] [CrossRef]
  19. Bouzahzah, H.; Benzaazoua, M.; Mermillod-Blondin, R.; Pirard, E. A novel procedure for polished section preparation for automated mineralogy avoiding internal particle settlement. In Proceedings of the 12th International Congress for Applied Mineralogy (ICAM), Istanbul, Turkey, 10–12 August 2015. [Google Scholar]
  20. Santoro, L.; Tshipeng, S.; Pirard, E.; Bouzahzah, H.; Kaniki, A.; Herrington, R. Mineralogical reconciliation of cobalt recovery from the acid leaching of oxide ores from five deposits in Katanga (DRC). Miner. Eng. 2019, 137, 277–289. [Google Scholar] [CrossRef]
  21. Abramovski, T.; Stefanova, V.P.; Causse, R.; Romanchuk, A. Technologies for the processing of polymetallic nodules from Clarion Clipperton Zone in the Pacific Ocean. J. Chem. Technol. Metall. 2017, 52, 258–269. [Google Scholar]
  22. Mineralogy Database. Available online: http://webmineral.com/ (accessed on 5 July 2019).
  23. Whitney, D.L.; Evans, B.W. Abbreviations for names of rock-forming minerals. Am. Miner. 2010, 95, 185–187. [Google Scholar] [CrossRef]
  24. Senanayake, G. Acid leaching of metals from deep-sea manganese nodules-A critical review of fundamentals and applications. Miner. Eng. 2011, 24, 1379–1396. [Google Scholar] [CrossRef]
  25. Chung, W.J.; Griebel, J.J.; Kim, E.T.; Yoon, H.; Simmonds, A.G.; Ji, H.J.; Dirlam, P.T.; Glass, R.S.; Wie, J.J.; Nguyen, N.A.; et al. The use of elemental sulfur as an alternative feedstock for polymeric materials. Nat. Chem. 2013, 5, 518–524. [Google Scholar] [CrossRef] [PubMed]
  26. Vu, N.H.; Kristianová, E.; Dvořák, P.; Abramowski, T.; Dreiseitl, I.; Adrysheva, A. Modified Leach Residues from Processing Deep-Sea Nodules as Effective Heavy Metals Adsorbents. Metals 2019, 9, 472. [Google Scholar] [CrossRef]
Figure 1. (a) Photomicrographs (under reflected light) demonstrating seafloor massive sulfides (SMS) mineralogy and texture, (b) sphalerite and isocubanite-chalcopyrite texture, sphalerite (grey) with strong chalcopyrite disease (yellow), the centre yellow grain is an intergrowth of isocubanite and chalcopyrite (after [8]). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Gn—galena, Py—pyrite. Icb is isocubanite.
Figure 1. (a) Photomicrographs (under reflected light) demonstrating seafloor massive sulfides (SMS) mineralogy and texture, (b) sphalerite and isocubanite-chalcopyrite texture, sphalerite (grey) with strong chalcopyrite disease (yellow), the centre yellow grain is an intergrowth of isocubanite and chalcopyrite (after [8]). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Gn—galena, Py—pyrite. Icb is isocubanite.
Minerals 09 00482 g001
Figure 2. Scanning electron microscope (SEM) (a,c) images and energy dispersive spectroscopy (EDS) analyses (b,d) with displayed distribution of selected elements. (a,b) Isocubanite with lamellae of chalcopyrite, (c,d) heterogeneous layer growth structure of nodules.
Figure 2. Scanning electron microscope (SEM) (a,c) images and energy dispersive spectroscopy (EDS) analyses (b,d) with displayed distribution of selected elements. (a,b) Isocubanite with lamellae of chalcopyrite, (c,d) heterogeneous layer growth structure of nodules.
Minerals 09 00482 g002
Figure 3. Effect of polymetallic nodules dosage (%) on recovery of (a) copper, (b) manganese, (c) nickel and (d) zinc (1 M H2SO4, 1 M NaCl, 80 °C).
Figure 3. Effect of polymetallic nodules dosage (%) on recovery of (a) copper, (b) manganese, (c) nickel and (d) zinc (1 M H2SO4, 1 M NaCl, 80 °C).
Minerals 09 00482 g003
Figure 4. Leaching recovery and content in residue of (a) copper and (b) manganese in the presence of various amounts of polymetallic nodules (PN, in %) and corresponding MnO2 (g/L) (1 M H2SO4, 1 M NaCl, 80 °C, 48 h).
Figure 4. Leaching recovery and content in residue of (a) copper and (b) manganese in the presence of various amounts of polymetallic nodules (PN, in %) and corresponding MnO2 (g/L) (1 M H2SO4, 1 M NaCl, 80 °C, 48 h).
Minerals 09 00482 g004
Figure 5. Mineral distribution (semi-quantitative XRD) in the feed (0) and leaching residues (1 M H2SO4, 1 M NaCl, 80 °C, 67% PN, 33% SMS). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Gn—galena, Py—pyrite, Mrc—marcasite, Qz—quartz, Ms—muscovite, Mc—microcline, Ab—albite, Brt—barite. Iso is isocubanite, and S0 is elemental sulfur.
Figure 5. Mineral distribution (semi-quantitative XRD) in the feed (0) and leaching residues (1 M H2SO4, 1 M NaCl, 80 °C, 67% PN, 33% SMS). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Gn—galena, Py—pyrite, Mrc—marcasite, Qz—quartz, Ms—muscovite, Mc—microcline, Ab—albite, Brt—barite. Iso is isocubanite, and S0 is elemental sulfur.
Minerals 09 00482 g005
Figure 6. Mineral distribution (automated mineralogy) in the feed (0) and leaching residues (1 M H2SO4, 1 M NaCl, 80 °C, 67% PN, 33% SMS). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Py—pyrite, Po—pyrrhotite, Gth—goethite, Brt—barite. Poly represents heterogeneous layer growth structure of nodules, while Iso is isocubanite.
Figure 6. Mineral distribution (automated mineralogy) in the feed (0) and leaching residues (1 M H2SO4, 1 M NaCl, 80 °C, 67% PN, 33% SMS). Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Py—pyrite, Po—pyrrhotite, Gth—goethite, Brt—barite. Poly represents heterogeneous layer growth structure of nodules, while Iso is isocubanite.
Minerals 09 00482 g006
Figure 7. Mn, Fe, Cu and Zn deportment (calculated by automated mineralogy) in (a) feed (PN (67%) and SMS (33%)), and (b) leaching residue after 48 h. Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Py—pyrite, Po—pyrrhotite, Gth—goethite. Poly is heterogeneous layer growth structure of nodules, Iso is isocubanite.
Figure 7. Mn, Fe, Cu and Zn deportment (calculated by automated mineralogy) in (a) feed (PN (67%) and SMS (33%)), and (b) leaching residue after 48 h. Abbreviations after [23]: Ccp—chalcopyrite, Sp—sphalerite, Py—pyrite, Po—pyrrhotite, Gth—goethite. Poly is heterogeneous layer growth structure of nodules, Iso is isocubanite.
Minerals 09 00482 g007
Figure 8. False-color mineral maps as obtained by automated mineralogy of selected areas of (a,b) feed (PN (67%) and SMS (33%)) and(c,d) residue after 48 h.
Figure 8. False-color mineral maps as obtained by automated mineralogy of selected areas of (a,b) feed (PN (67%) and SMS (33%)) and(c,d) residue after 48 h.
Minerals 09 00482 g008
Figure 9. Simplified conceptual flowsheet of simultaneous leaching of seafloor massive sulfides (SMS) and polymetallic nodules (PN).
Figure 9. Simplified conceptual flowsheet of simultaneous leaching of seafloor massive sulfides (SMS) and polymetallic nodules (PN).
Minerals 09 00482 g009
Table 1. EDS analyses (in %) on selected particles of a mixture of PN (67%) and SMS (33%). Point locations are indicated in Figure 1. Points 14–16 represent isocubanite with lamellae of chalcopyrite, point 20 is sphalerite with a high concentration of Fe, points 17–19, 21 are from heterogeneous layer growth structure of nodules.
Table 1. EDS analyses (in %) on selected particles of a mixture of PN (67%) and SMS (33%). Point locations are indicated in Figure 1. Points 14–16 represent isocubanite with lamellae of chalcopyrite, point 20 is sphalerite with a high concentration of Fe, points 17–19, 21 are from heterogeneous layer growth structure of nodules.
PointOFNaMgAlSiPSClKCaTiMnFeCoNiCuZn
14 35.47 44.94 19.32
15 35.55 45.12 19.3
16 34.44 44.86 20.7
1730.29 2.121.260.763.460.40.80 0.444.171.0539.1015.530.63
1834.372.022.091.720.581.37 0.710.170.771.830.1845.253.110.143.261.960.46
1937.87 1.912.020.430.97 0.110.111.11.49 51.05 0.872.06
20 33.18 2.1916.95 47.68
2146.86 10.26 11.9830.9

Share and Cite

MDPI and ACS Style

Kowalczuk, P.B.; Bouzahzah, H.; Kleiv, R.A.; Aasly, K. Simultaneous Leaching of Seafloor Massive Sulfides and Polymetallic Nodules. Minerals 2019, 9, 482. https://doi.org/10.3390/min9080482

AMA Style

Kowalczuk PB, Bouzahzah H, Kleiv RA, Aasly K. Simultaneous Leaching of Seafloor Massive Sulfides and Polymetallic Nodules. Minerals. 2019; 9(8):482. https://doi.org/10.3390/min9080482

Chicago/Turabian Style

Kowalczuk, Przemyslaw B., Hassan Bouzahzah, Rolf Arne Kleiv, and Kurt Aasly. 2019. "Simultaneous Leaching of Seafloor Massive Sulfides and Polymetallic Nodules" Minerals 9, no. 8: 482. https://doi.org/10.3390/min9080482

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop