Next Article in Journal
Formation of Spessartine and CO2 via Rhodochrosite Decarbonation along a Hot Subduction P-T Path
Next Article in Special Issue
Effective Utilization of Limonitic Nickel Laterite via Pressurized Densification Process and Its Relevant Mechanism
Previous Article in Journal
Fedorite from Murun Alkaline Complex (Russia): Spectroscopy and Crystal Chemical Features
Previous Article in Special Issue
Platinum Group Elements in Geosphere and Anthroposphere: Interplay among the Global Reserves, Urban Ores, Markets and Circular Economy
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

The Effect of Alkali Roasting Pretreatment on Nickel Extraction from Limonite Ore by Using Dissolved SO2-Air

by
Winny Wulandari
1,*,
Meiyer Marthen Kinda
2,
Rahmaditha Murida
1 and
Tjokorde Walmiki Samadhi
1
1
Chemical Engineering Product Design and Development Research Group, Department of Chemical Engineering, Faculty of Industrial Technology, Institut Teknologi Bandung, Bandung 40132, Indonesia
2
Department of Bioprocess Engineering, Faculty of Biotechnology, Institute of Technology Del, Toba Samosir 22381, Indonesia
*
Author to whom correspondence should be addressed.
Minerals 2020, 10(8), 701; https://doi.org/10.3390/min10080701
Submission received: 20 July 2020 / Revised: 30 July 2020 / Accepted: 30 July 2020 / Published: 7 August 2020
(This article belongs to the Special Issue The Processing of Alternative and Urban Ores)

Abstract

:
Extraction of limonite ore using dissolved SO2–air is an alternative hydrometallurgical method for nickel recovery. This process is carried out at atmospheric pressure and is shown to have good selectivity of nickel over iron, but with a low recovery yield. The literature refers to the application of alkali roasting as pretreatment in laterite ore leaching to increase nickel recovery. Thus, this study aims to apply the combination method of alkali roasting and leaching to extract nickel from limonite ore (1.33% Ni, 46.61% Fe) from the Southeast Sulawesi region. Three alkali compounds were included in the study (NaOH, Na2CO3 and Na2SO4). The batch-leaching process was carried out at pH 1 and 3 and temperatures of 55 and 80 ° C for 180 min. The leach liquors were sampled at 15, 60, 90 and 120 min, and concentrations of the extracted metals were measured by Atomic Absorption Spectrometry (AAS). A mineralogy characterization of the raw ore and its residue after leaching was undertaken by using X-Ray Diffraction (XRD), while the thermal decomposition behavior of the ore was characterized by Thermogravimetry Analyzer (TGA)/Differential Scanning Calorimetry (DSC). The addition of Na2CO3, Na2SO4 and NaOH in the ore pretreatment increases nickel recovery from 14.80% without alkali roasting to 23.99%, 28.15% and 39.22%, respectively. The optimum extraction condition for nickel recovery is at pH 1 and a temperature of 80 ° C. However, the highest Ni/Fe selectivity of 24,947 is obtained at pH 3 and a temperature of 80 ° C, preceded by roasting in the absence of alkali. Compared to other hydrometallurgical processes, the process studied in this work exhibits lower recovery, but provides an alternative to extract nickel from low-grade limonite ore.

1. Introduction

The depletion of high-grade nickel sulfide and the growing world demand of nickel have spurred an increasing focus on the processing of low-grade nickel laterite ores [1]. It is estimated that approximately 70% of global nickel resources exist as laterite ores [2]. The U.S. Geological Survey [3] reported that Indonesia has the globally largest nickel reserves of about 21 million tons in the form of laterite deposits (2018 data). These deposits comprise layers such as the limonite layer, which contains a significant amount of goethite (FeOOH), 0.5–1.7% nickel, 40–60% iron and low silica content; and the saprolite layer with containing about 1.5–3% nickel, with lower iron and higher silica contents [4].
Due to the complex mineralogy, heterogeneous nature and low nickel content, the physical beneficiation of Ni from limonitic laterite ore is very challenging [5]. On the other hand, saprolitic ore is more amenable to utilization via the pyrometallurgical route. In this context, the limonite ore becomes overburden and is generally underutilized. During recent decades, several studies on nickel extraction from limonitic laterite ores have been published, including high-pressure acid leaching (HPAL) [6], atmospheric acid leaching (AL) [7,8], biological leaching [9], heap leaching [10] and citric acid leaching [11]. High-pressure acid leaching (HPAL) is a proven hydrometallurgical technology, in which nickel leaching occurs at high temperature (250–253 °C) in an autoclave, while iron and aluminum are precipitated. However, high operating costs and safety risks are disadvantages of this process [6]. The atmospheric leaching (AL) process has been studied for the processing of various limonitic and saprolitic laterite ores. This process has low energy consumption and capital cost compared to HPAL [12], but often produces leach liquor containing a significant amount of impurities such as trivalent iron, aluminum and chromium ions [13]. An alternative citric acid leaching route was reported to able to extract nickel up to 96% in the laboratory scale; however, the leaching duration is very long, i.e., 15 days. The development of an economical industrial-scale laterite ore processing technology is therefore clearly still highly desirable.
The utilization of dissolved SO2–air during the extraction of nickel from laterite ore at atmospheric pressure has been known to provide a high nickel to iron selectivity [14]. Iron and other impurities may also be leached from laterite and are therefore regarded as unwanted byproducts in the nickel hydrometallurgical recovery process. Low SO2 concentration is the key in selectivity due to the selective complexation of the metal hydrous oxides with SO2 [15]. Moreover, the utilization of the SO2–air gas mixture as an oxidant is attractive because it is cheaper compared to other strong oxidants [16]. The dissolved SO2–air method does not require the use of strong acids. The dissolved SO2–air approach for limonitic ore extraction has been proved in a previous study by the Authors [14,17]. Conducted at very mild conditions, including a low temperature of 55 to 80 °C and atmospheric pressure, a leaching recovery as high as 21% was obtained. It was also found that at longer leaching duration (3 h), the iron content in the solution decreased due to iron precipitation, providing the possibility to increase the selectivity of nickel over iron in the leaching solution.
Several strategies have been attempted to improve the leaching process to increase the recovery of nickel from limonitic ore. Guo et al. [18] conducted a new extraction technology called the alkali roasting-acid leaching (ARAL) that was developed to process limonitic ore from Indonesia. The result showed the increase of recovery Ni and Co from 79.96% to 97.52% and 70.02% to 95.33% after alkali-roasting with the addition of Na2CO3. Alkali roasting activation pretreatment was thought to breaks the mineral lattices of laterites, thus Ni and Co are exposed which corresponds to the increasing of the recovery of these two metals under milder conditions [5]. In addition, Li et al. [19] also stated that pre-roasting can change the mineral structure and increase the surface and porosity of the raw ore, thus making it more amenable to leaching.
As the roasting pretreatment is hypothesized to disrupt the crystalline structure of the limonite minerals and expose Ni to leaching, it is important to study the pretreatment of nickel limonite ores to increase its recovery. This research aims to improve the recovery of nickel leaching from limonite ores adding alkali roasting pretreatment and studying its effect to the leaching process by using the SO2-dissolved air method. The alkali used in this study are Na2CO3, Na2SO4 and NaOH.

2. Materials and Methods

2.1. Limonite Laterite Nickel Ore

Limonite nickel ore was obtained from PT. Bhumi Karya Utama in North Konawe, Southeast Sulawesi. The ore is located at a depth of 3 m from the ground surface. The chemical composition of limonite nickel ore is shown in Table 1, presented the metals and oxides content. The sample limonite has high iron content (46.61%) and low nickel content (1.33%). The sulfur dioxide gas was obtained from CV Sangkuriang Gas Bandung.

2.2. Method

The experiments were conducted in two process steps, namely pretreatment and leaching. Two alternative routes were included in the pretreatment step, namely conventional roasting and alkali roasting. In the conventional roasting route, raw ore was roasted at 650 °C for 1 h in a Nabertherm P310 electric furnace. The roasted ore was then cooled down and transferred to the extraction step. In the alkali roasting route, 60% w/w of alkali (Na2CO3, Na2SO4, NaOH) was mixed with 6 g limonite nickel ore; the blend was then roasted under conditions identical to the conventional roasting route. After cooling, the alkali-roasted ore was then washed with distilled water.
The roasted ores are then transferred into a round-bottom flask 5-neck (see Figure 1) containing 250 mL hot water (55 or 80 °C) at a solid/liquid mass ratio of 2.4 wt%, then SO2 (99.98% pure) and air was bubbled through the suspension until the required pH is reached. The leaching process was carried out at pH 1 and 3, a temperature of 55 and 80 °C for 180 min. As a reference, the optimum condition of Ni selectivity over iron was identified as pH 3 and temperature of 80 °C in a previous study [14]. The current work investigates the effect of lower pH and temperature. Leach liquor sampled at 15, 90, 120 and 180 min using a syringe and filtered by 0.2-µL syringe filter (Whatman 42, GE Healthcare, Chicago, IL, USA). All filtrates were then analyzed by an AAS instrument (Agilent 8453 UV-visible Spectroscopy System, Agilent Technologies Deutschland GmbH, Waldbronn, Germany). Solid residues collected after the extraction step were characterized using an X-Ray Diffrraction (SmartLab XRD, Rigaku, Tokyo, Japan) to identify changes in mineral phases. The recovery metals after leaching as well as the nickel selectivity over iron were calculated the following formulas:
Metal   recovery = m a s s   o f   m e t a l   e x t r a c t e d   ( g ) m a s s   o f   m e t a l   i n   r a w   o r e   ( g )
Nickel   selectivity = N i / F e   i n   t h e   a q u o e u s N i / F e   i n   t h e   r a w   o r e

3. Results and Discussion

3.1. Roasting (No Alkali) Pretreatment

X-ray diffractograms in Figure 2 identify the crystalline phases present in the raw limonite ore, the conventionally roasted ore and the solid residue remaining after the leaching process. The raw limonite nickel ore composes of magnetite (Fe3O4) and goethite (FeOOH) as the major mineral phases. Goethite is assumed to have small nickel content in it with the formula of (Fe,Ni,Al)OOH. Upon roasting, hematite appears as a major phase. It is postulated that at a temperature of 650 °C, the hematite (Fe2O3) phase is formed due to the dehydroxylation of goethite [19], thus potentially liberating Ni from goethite. The residue from the leaching process shows enstatite (MgSiO3), quartz (SiO2), olivine (Mg2SiO4) and hematite (Fe2O3).
Figure 3 indicates nickel and iron recoveries as a function of time in various pH and temperature from the results of leaching of the conventionally roasted ore. The highest nickel recovery of 14.80% was obtained at pH 1 and temperature 80 °C after 180 min. In the early duration of the leaching process, 8.71% nickel was recovered from the ore at pH 1 and temperature of 80 °C; this result is higher than the nickel recovery in other conditions (Figure 3a). Leaching of iron decreases at increasing leaching time, with the recovery of 0.22% at 180 minutes at pH 1 and a temperature of 80 °C. Thus, the leaching process using SO2-dissolved air indicates high Ni/Fe selectivity.

3.2. Alkali Roasting Pretreatment

The diffractograms in Figure 4 compares the effect of conventional and alkali roasting on phase changes of the limonite ore. Several different phases form after the alkali roasting pretreatment step. Ore treated with Na2CO3 shows sodium iron silicon oxide [Na(FeSi)O2], quartz (SiO2), hematite and magnesium iron oxide (MgFeO). It is postulated that Na2CO3 decomposes into Na2O and CO2 during the roasting as indicated by Equation (3) [18]. Then, Na2O possibly reacts with iron, silicate, chrome and other minerals in the ore (Equations (4)–(6)).
Na2CO3 = Na2O + CO2
Na2O + Fe2O3 = 2NaFeO2
Na2O + Cr2O3 = 2NaCrO2
Na2O + SiO2 = Na2SiO3
The XRD of pretreated ore with Na2SO4 contains hematite as the major mineral as well as thenardite (Na2SO4). In a study that used reducing atmosphere [20], Na2SO4 is decomposed to form Na2O, Na2S and S; whereas it is claimed that Na2S and S are beneficial for nickel recovery through a magnetic separation due to the FeS formation. The present study shows that Na2SO4 is not decomposed into Na2O. For the XRD of pretreated ore with NaOH, the identified major mineral is sodium iron silicon oxide. The absence of goethite (Fe,Ni)(OOH) in those XRD spectra indicates that the goethite in the original ore has transformed to other major minerals, speculating to destruct the Ni that is bound in the limonite ore.
Figure 5 displays TGA/DSC thermograms of the raw limonite, limonite + Na2CO3 and limonite + Na2SO4 blends. All thermograms indicate an endothermic reaction at approximately 250–350 °C, which is due to the dehydroxylation of goethite to hematite [19].
X-ray diffractograms of the raw ore, after alkali roasting and after leaching are also shown in Figure 6a–c for alkali roasting with Na2CO3, Na2SO4 and NaOH, respectively. As can be seen in those figures, the goethite phase becomes diminished after alkali roasting. After leaching with SO2-dissolved air, the residue with Na2CO3 and Na2SO4 are dominated by the hematite phase. This condition may indicate that the iron in the ore is not dissolved in the leaching process due to its stability as the hematite phase. This may be advantageous in increasing the Ni/Fe selectivity. Zinc chromium iron oxide is present in the residue after leaching of NaOH-roasted limonite (Figure 6c).
Figure 7a–f show the recovery of nickel and iron after leaching with SO2-dissolved air. The increase in nickel recovery was observed at pH = 1 and temperature 80 °C in all pretreated ore. This result shows that the utilization of alkali roasting pretreatment enhances the recovery of nickel compared to roasting without alkali. Figure 7a,b present the Ni and Fe recoveries at pH 1 and temperature 80 °C with Na2CO3 addition, which reached 23.99% and 4.39%, respectively. In this condition, the nickel recovery was influenced by the leaching time. However, at pH 3 the nickel recovery was not affected by leaching time. Figure 7c,d present Ni and Fe recoveries with Na2SO4 roasting, which reached about 28.15% and 3.85%, respectively. Overall, the highest Ni and Fe recoveries were achieved by the addition of NaOH, which reached 39.22% and 18.60%, respectively (see Figure 7e,f).
However, these graphs also indicate that the recovery of unwanted Fe increases with the increasing leaching time. While alkali roasting activation pretreatment breaks the mineral lattices of laterites and increases the surface area of the raw ore, not only Ni and Co are exposed to the solvent, but also Fe.
The Ni/Fe selectivity was also investigated to determine the effectiveness of utilization of SO2–air in the leaching process. The summarized nickel selectivity presented in Table 2. The highest nickel selectivity of approximately 24,947 was obtained at pH 3 and temperature 80 °C for conventionally roasted ore. The second-highest selectivity of 16,172 was produced by alkali roasting using Na2SO4 followed by extraction at pH 3 and temperature of 55 °C. The alkali roasting pretreatment with NaOH and Na2CO3 generated low nickel selectivity as the Fe also was leached at prolonged leaching time. The higher basicity of NaOH is hypothesized to increase the extent of silicate structure disruption in the ore. This condition is unfavorable since it reduces the selectivity of the SO2–air extraction step.

3.3. Kinetic Analysis

The kinetics of nickel leaching from limonite at all method was investigated using the shrinking core model (SCM) approach for experimental data at pH 1 and temperature of 80 °C. This analysis aims to determine the leaching rate-controlling step in the nickel leaching process. In the SCM model, the leaching is described as involving three processes: surface diffusion, interface chemical reaction and diffusion of reactants or products. All standard kinetic equations derived from the SCM model were tested [15,21]. It is found that Equations (7) and (8), which describes the interface chemical reaction and diffusion of reactants or products, respectively, gives an excellent fit to the experimental data.
1 ( 1 X ) 1 3 = t τ
1 3 ( 1 X ) 2 3 + 2 ( 1 X ) = t τ
where X = conversion, t = time and τ = completing reaction time (min).
Figure 8a,b describe the fitting of two equations of the SCM model. Equations (7) and (8) provide a very good fit for the leaching of alkali-roasted ores, with coefficients of determination R 2 higher than 0.96. However, the kinetics of leaching of conventionally roasted ores cannot be fit by both models. The Equation (7) assumes that the leaching rate-controlling step is the chemical reaction occurring on the mineral particle surface while Equation (8) assumes the rate-controlling step to be the diffusion of leaching reagent through the product layer on the mineral particle surface [22]. Thus, the nickel leaching kinetics of alkali roasted limonite ore using SO2-dissolved air may be represented by two mechanisms simultaneously.
Table 3 summarizes key operating conditions and extraction yields from several published literatures on the recovery of nickel from limonite ores. These works mostly employ sulfuric acid, sodium sulfite, chlorination or hydrochloric acid. Nickel recovery varies from 82.3% to 93.1%. Compared to this range, the recovery obtained using dissolved SO2–air is considerably lower, i.e., 23.33–39.22%. This may be due to the nature of SO2 gas which is a much milder reductant compared to sulfuric acid or hydrochloric acid. Previous research on the SO2–air leaching method also indicates a nickel recovery of only 21%, but with a very high nickel selectivity [17]. A higher leaching temperature of 80 °C causes insufficient nickel leaching by SO2/air due to the low solubility of SO2 at elevated temperatures [15]. Another phenomenon that may hinder the recovery is the inclusion of nickel in the recrystallized iron oxide [23].
The overall results also show that alkali roasting has effect to increase the nickel recovery; however, it lowers the selectivity of nickel over iron. Adding alkali in the pretreatment process will also increase the operating cost of the overall hydrometallurgical process. While the recovery values summarized in Table 3 give the impression that the dissolved SO2–air to be not very promising, an economic assessment may nevertheless be needed to verify the overall economics of the processes in Table 3.
During the leaching process, there are proposed mechanism reaction of SO2 occurred in the solution [27] (Equations (9)–(14)). The formation of a peroxo–monosulfate species ( SO 5 · or HSO 5 ) is responsible for the fast oxidation. The final product of SO 5 · is sulfate via intermediate product HSO 5 or FeSO 5 + . However, the radical SO 3 · and SO 5 · also terminate by self-reaction to produce dithionate [26].
SO 2 · H 2 O     H S O 3 + H +
HSO 3     SO 3 2 + H +
Fe 3 + + SO 3 2     FeSO 3 +
FeSO 3 +     Fe 2 + + SO 3 ·
SO 3 · + O 2     SO 5 ·
SO 5 · + HSO 3     SO 3 · + HSO 5
The SO 4 · radical is known to be a very strong oxidant with a standard reduction potential of 2.43 V vs. SHE and is expected to rapidly oxidize sulfite and transition metal ions. (Equation (15)) [16].
SO 5 · + HSO 3     SO 4 · + HSO 4
The process may be improved by investigating the leaching mechanism; from dissolving SO2 gas and air, its reaction with water to form sulfite acid ions and the contact of the sulfite ions with the nickel-bearing ore. In addition, the roasting condition should be investigated to determine the optimum roasting temperature that yields the highest nickel recovery.

4. Conclusions

Nickel leaching from low-grade limonite ore using SO2-dissolved air with roasting and alkali roasting pretreatment has been carried out in this study. XRD results from roasting pretreatment indicate the formation of hematite due to the dehydroxylation of goethite, while those from alkali pretreatment indicate the formation of different mineral phases such as sodium iron silicon oxide [Na(FeSi)O2], quartz (SiO2), hematite and magnesium iron oxide (MgFeO) (for ore roasted with Na2CO3), hematite and thenardite (for ore roasted with Na2SO4) and sodium iron silicon oxide (for ore roasted with NaOH). The result shows that the highest nickel recovery of 39.22% was obtained by extraction at pH 1 and temperature of 80 °C with alkali roasting pretreatment using NaOH. The leaching kinetics of alkali roasted ore can be represented by interface chemical reaction and diffusion models. However, the nickel selectivity still low due to extensive breakup of the silica structure in the ore, which leads to increasing recovery of iron. The highest nickel selectivity of 24,946 was obtained by extraction limonite ore at pH 3 and temperature of 80 °C with no alkali roasting pretreatment, with the nickel recovery of 14.80%. While alkali roasting pretreatment increases the recovery of nickel, it also increases the recovery of iron, thereby decreasing the selectivity of nickel over iron.

Author Contributions

Conceptualization, W.W. and T.W.S.; methodology, M.M.K.; experimental work: M.M.K.; formal analysis: M.M.K., W.W. and R.M., Writing—Original draft preparation, M.M.K. and R.M.; Writing—Review and editing: W.W. and T.W.S.; funding acquisition, W.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Program Penelitian, Pengabdian Masyarakat, dan Inovasi (P3MI) (Research, Community Service and Innovation Program Grant) Institut Teknologi Bandung 2020.

Acknowledgments

We would like to thank PT. Bhumi Karya Utama for providing the ore samples.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Mudd, G.M.; Jowitt, S.M. A Detailed Assessment of Global Nickel Resource Trends and Endowments. Econ. Geol. 2014, 109, 1813–1841. [Google Scholar] [CrossRef]
  2. Fan, R.; Gerson, A.R. Mineralogical characterisation of Indonesian laterites prior to and post atmospheric leaching. Hydrometallurgy 2013, 134, 102–109. [Google Scholar] [CrossRef]
  3. U.S. Geological Survey. Mineral Commodity Summaries 2019; U.S. Geological Survey: Hunter Mill, VA, USA, 2019.
  4. Zhu, D.; Cui, Y.; Hapugoda, S.; Vining, K.; Pan, J. Mineralogy and crystal chemistry of a low grade nickel laterite ore. Trans. Nonferrous Met. Soc. China 2012, 22, 907–916. [Google Scholar] [CrossRef]
  5. Guo, Q.; Qu, J.K.; Han, B.B.; Wei, G.Y.; Zhang, P.Y.; Qi, T. Dechromization and dealumination kinetics in process of Na2CO3-roasting pretreatment of laterite ores. Trans. Nonferrous Met. Soc. China 2014, 24, 3979–3986. [Google Scholar] [CrossRef]
  6. Shibayama, K.; Yokogawa, T.; Sato, H.; Enomoto, M.; Nakai, O.; Ito, T.; Mizuno, F.; Hattori, Y. Taganito HPAL Plant Project. Miner. Eng. 2016, 88, 61–65. [Google Scholar] [CrossRef]
  7. McDonald, R.G.; Whittington, B.I. Atmospheric acid leaching of nickel laterites review: Part II. Chloride and bio-technologies. Hydrometallurgy 2008, 91, 56–59. [Google Scholar] [CrossRef]
  8. McDonald, R.G.; Whittington, B.I. Atmospheric acid leaching of nickel laterites review: Part I. Sulphuric acid technologies. Hydrometallurgy 2008, 91, 35–55. [Google Scholar] [CrossRef]
  9. Jang, H.-C.; Valix, M. Overcoming the bacteriostatic effects of heavy metals on Acidithiobacillus thiooxidans for direct bioleaching of saprolitic Ni laterite ores. Hydrometallurgy 2017, 168, 21–25. [Google Scholar] [CrossRef]
  10. Oxley, A.; Smith, M.E.; Caceres, O. Why heap leach nickel laterites? Miner. Eng. 2016, 88, 53–60. [Google Scholar] [CrossRef]
  11. Astuti, W.; Hirajima, T.; Sasaki, K.; Okibe, N. Comparison of atmospheric citric acid leaching kinetics of nickel from different Indonesian saprolitic ores. Hydrometallurgy 2016, 161, 138–151. [Google Scholar] [CrossRef]
  12. Luo, J.; Li, G.; Rao, M.; Peng, Z.; Zhang, Y.; Jiang, T. Atmospheric leaching characteristics of nickel and iron in limonitic laterite with sulfuric acid in the presence of sodium sulfite. Miner. Eng. 2015, 78, 38–44. [Google Scholar] [CrossRef]
  13. Wang, K.; Li, J.; Mcdonald, R.G.; Browner, R.E. Iron, aluminium and chromium co-removal from atmospheric nickel laterite leach solutions. Miner. Eng. 2018, 116, 35–45. [Google Scholar] [CrossRef]
  14. Wulandari, W.; Soerawidjaja, T.H.; Alifiani, D.; Rangga, D.A. The effect of pre-treatments to the nickel limonite leaching using dissolved gaseous SO2-air. IOP Conf. Ser. Mater. Sci. Eng. 2018, 285. [Google Scholar] [CrossRef]
  15. Gbor, P.K.; Ahmed, I.B.; Jia, C.Q. Behaviour of Co and Ni during aqueous sulphur dioxide leaching of nickel smelter slag. Hydrometallurgy 2000, 57, 13–22. [Google Scholar] [CrossRef]
  16. Mulaudzi, N.; Mahlangu, T. Oxidative precipitation of Mn(II) from cobalt leach solutions using dilute SO2/air mixture. J. South. Afr. Inst. Min. Metall. 2009, 109, 375–382. [Google Scholar]
  17. Wulandari, W.; Soerawidjaja, T.H.; Joshua, S.; Isradi, H.R. Extraction of nickel from nickel limonite ore using dissolved gaseous SO2-Air. AIP Conf. Proc. 2017, 1805, 070004. [Google Scholar] [CrossRef] [Green Version]
  18. Guo, Q.; Qu, J.; Qi, T.; Wei, G.; Han, B. Activation pretreatment of limonitic laterite ores. Miner. Eng. 2011, 24, 825–832. [Google Scholar] [CrossRef]
  19. Li, J.; Li, X.; Hu, Q.; Wang, Z.; Zhou, Y.; Zheng, J.; Liu, W.; Li, L. Effect of pre-roasting on leaching of laterite. Hydrometallurgy 2009, 99, 84–88. [Google Scholar] [CrossRef]
  20. Jiang, M.; Sun, T.; Liu, Z.; Kou, J.; Liu, N.; Zhang, S. Mechanism of sodium sulfate in promoting selective reduction of nickel laterite ore during reduction roasting process. Int. J. Miner. Process. 2013, 123, 32–38. [Google Scholar] [CrossRef] [Green Version]
  21. Levenspiel, O. Chemical Reaction Engineering. In Chemical Reaction Engineering, 3rd ed.; John Wiley & Sons: Hoboken, NJ, USA, 1998; pp. 569–576. [Google Scholar]
  22. Thubakgale, C.K.; Mbaya, R.K.K.; Kabongo, K. A study of atmospheric acid leaching of a south african nickel laterite. Miner. Eng. 2013, 54, 79–81. [Google Scholar] [CrossRef]
  23. O’Connor, F.; Cheung, W.H.; Valix, M. Reduction roasting of limonite ores: Effect of dehydroxylation. Int. J. Miner. Process. 2006, 80, 88–99. [Google Scholar] [CrossRef]
  24. Li, J.; Li, Y.; Gao, Y.; Zhang, Y.; Chen, Z. Chlorination roasting of laterite using salt chloride. Int. J. Miner. Process. 2016, 148, 23–31. [Google Scholar] [CrossRef]
  25. Ma, B.; Yang, W.; Pei, Y.; Wang, C.; Jin, B. Effect of activation pretreatment of limonitic laterite ores using sodium fluoride and sulfuric acid on water leaching of nickel and cobalt. Hydrometallurgy 2017, 169, 411–417. [Google Scholar] [CrossRef]
  26. Li, G.; Shi, T.; Rao, M.; Jiang, T.; Zhang, Y. Beneficiation of nickeliferous laterite by reduction roasting in the presence of sodium sulfate. Miner. Eng. 2012, 32, 19–26. [Google Scholar] [CrossRef]
  27. Zhang, W.; Singh, P.; Muir, D. Iron(II)/ oxidation by SO2/O2 in acidic media: Part I. Kinetics and mechanism. Hydrometallurgy 2000, 55, 229–245. [Google Scholar] [CrossRef]
Figure 1. Experiment setup for nickel leaching.
Figure 1. Experiment setup for nickel leaching.
Minerals 10 00701 g001
Figure 2. X-ray diffraction analysis of raw limonite ore, roasted ore and residue after leaching.
Figure 2. X-ray diffraction analysis of raw limonite ore, roasted ore and residue after leaching.
Minerals 10 00701 g002
Figure 3. Recovery of nickel and iron using conventional roasting pretreatment and leaching using SO2-dissolved air. (a) nickel recovery; (b) iron recovery.
Figure 3. Recovery of nickel and iron using conventional roasting pretreatment and leaching using SO2-dissolved air. (a) nickel recovery; (b) iron recovery.
Minerals 10 00701 g003
Figure 4. XRD pattern of limonite ore after roasting and alkali roasting. G—goethite; M—magnetite; H—hematite; Ss—sodium iron silicon oxide; Q—quartz; Mg—magnesium iron oxide; T—thenardite; Ns—sodium sulfate; Mn—manganese cyanide.
Figure 4. XRD pattern of limonite ore after roasting and alkali roasting. G—goethite; M—magnetite; H—hematite; Ss—sodium iron silicon oxide; Q—quartz; Mg—magnesium iron oxide; T—thenardite; Ns—sodium sulfate; Mn—manganese cyanide.
Minerals 10 00701 g004
Figure 5. TGA/DSC patterns of (a) Limonite ore, (b) ore + Na2CO3 and (c) ore + Na2SO4 alkali roasting.
Figure 5. TGA/DSC patterns of (a) Limonite ore, (b) ore + Na2CO3 and (c) ore + Na2SO4 alkali roasting.
Minerals 10 00701 g005
Figure 6. XRD patterns of (a) Ore + Na2CO3, (b) ore + Na2SO4 and (c) ore + NaOH after roasting and leaching with SO2–air.
Figure 6. XRD patterns of (a) Ore + Na2CO3, (b) ore + Na2SO4 and (c) ore + NaOH after roasting and leaching with SO2–air.
Minerals 10 00701 g006aMinerals 10 00701 g006b
Figure 7. Recovery of nickel and iron using alkali roasting pretreatment and leaching using SO2-dissolved air in water: (a,b) Ore + Na2SO4; (c,d) Ore + Na2SO4; (e,f) Ore + NaOH.
Figure 7. Recovery of nickel and iron using alkali roasting pretreatment and leaching using SO2-dissolved air in water: (a,b) Ore + Na2SO4; (c,d) Ore + Na2SO4; (e,f) Ore + NaOH.
Minerals 10 00701 g007aMinerals 10 00701 g007b
Figure 8. A linear fit of the nickel leaching kinetics at pH 1 and a temperature of 80 °C for (a) interface chemical reaction and (b) diffusion of reactants or products.
Figure 8. A linear fit of the nickel leaching kinetics at pH 1 and a temperature of 80 °C for (a) interface chemical reaction and (b) diffusion of reactants or products.
Minerals 10 00701 g008
Table 1. Metal and oxide content in limonite nickel ore.
Table 1. Metal and oxide content in limonite nickel ore.
Metal and OxideNiCoFeSiO2CaOMgOMnOCr2O3Al2O3P2O5TiO2SO3
Content (%)1.330.1446.614.070.021.181.072.7512.070.030.100.63
Table 2. The selectivity of nickel over iron in various pH and temperature.
Table 2. The selectivity of nickel over iron in various pH and temperature.
Operating ConditionNi/Fe Selectivity
pHT (°C)RoastingNa2CO3 RoastingNa2SO4 RoastingNaOH Roasting
1553.020.7156.661.25
8066.715.477.312.11
35510,5390.6116,172.382.32
8024,9460.487024.421.12
Table 3. Summary of leaching process of limonite ores literatures.
Table 3. Summary of leaching process of limonite ores literatures.
No.MethodType of OreExperiment ParametersNi Recovery (%)Reference
1Atmospheric leachingIndonesian lateriteT = 90 °C, 30-g/L Na2SO3,
t = 6 h, L/S ratio: 10:1.
82.3[12]
2Atmospheric leachingWest Papua limonite and saproliteT = 100 °C, H2SO4/ore ratio = 1.4:1, t (limonite) = 3 h.
t (saprolite) = 11 h
Limonite: 85
Saprolite: 50
[2]
4Chlorination roasting and water leachingLimoniteRoasting T = 1173 K, t = 1.5 h,
Chloride agent = NaCl + MgCl2.6H2O (mass ratio of 0.4)
87[24]
5Activation pretreatment and NaF and H2SO4 leachingPhilippines limoniteActivation T = 400 °C, t = 60 min,
H2SO4 dosage = 500 kg/ton, NaF dosage = 3%
85.3[25]
6Pre-roasting and leachingYunan, China lateriteT roasting = 300 °C, Ore + 4-mol/L HCl; S/L ratio = 1:6; T = 50 °C; t = 1 h93.1[19]
7Reduction roastingSulawesi, Indonesia lateriteReduction roasting T = 1100 °C, t = 60 min, sodium sulfate = 20 wt%83.01[26]
8Alkali roasting, SO2–air leachingIndonesia, limoniticT = 55–80 °C, pH: 1 and 3; t = 3 h23.99–39.22Current work
T—temperature; t—time; No.—number.

Share and Cite

MDPI and ACS Style

Wulandari, W.; Kinda, M.M.; Murida, R.; Samadhi, T.W. The Effect of Alkali Roasting Pretreatment on Nickel Extraction from Limonite Ore by Using Dissolved SO2-Air. Minerals 2020, 10, 701. https://doi.org/10.3390/min10080701

AMA Style

Wulandari W, Kinda MM, Murida R, Samadhi TW. The Effect of Alkali Roasting Pretreatment on Nickel Extraction from Limonite Ore by Using Dissolved SO2-Air. Minerals. 2020; 10(8):701. https://doi.org/10.3390/min10080701

Chicago/Turabian Style

Wulandari, Winny, Meiyer Marthen Kinda, Rahmaditha Murida, and Tjokorde Walmiki Samadhi. 2020. "The Effect of Alkali Roasting Pretreatment on Nickel Extraction from Limonite Ore by Using Dissolved SO2-Air" Minerals 10, no. 8: 701. https://doi.org/10.3390/min10080701

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop