Communication

Study on Formability and Microstructure Evolution of Usibor®2000 Sheet Under Different Forming Temperatures in Deep Drawing Process

School of Materials Science and Engineering, Shanghai University of Engineering Science, Shanghai 201620, China
*
Author to whom correspondence should be addressed.
Materials 2025, 18(10), 2224; https://doi.org/10.3390/ma18102224
Submission received: 23 March 2025 / Revised: 1 May 2025 / Accepted: 6 May 2025 / Published: 12 May 2025
(This article belongs to the Section Manufacturing Processes and Systems)

Abstract

:
Due to the need for weight reduction in the automobile structure, effective and accurate forming is demanded to take advantage of ultrahigh-strength steels. Research on the deep-drawing formability of Usibor®2000 has an important impact on the application of lightweight automotive bodies. The microstructure and formability of Usibor®2000 sheets at different temperatures were investigated by the Swift test. The positive effects of increasing the temperature on improving the forming limit and forming quality of Usibor®2000 were demonstrated by LDR results, thickness, and hardness measurement. The microstructure evolution of Usibor®2000 steel plates under warm forming and hot forming conditions was discussed in terms of microstructure characterization and precipitate morphology. The phase composition of the sample deformed at 860 °C is analyzed by two-step etching metallographic analysis and numerical simulation, which provides a reference for the application of Usibor®2000 ultrahigh-strength steel in automotive lightweight.

1. Introduction

With the increasingly stringent automobile emission regulations around the world and the continuous demand for vehicle impact resistance, higher requirements are put forward for advanced steel in both automotive lightweight and safety [1]. Ultrahigh strength steel (UHSS), an advanced steel with a strength grade higher than 1500 MPa, has outstanding advantages in strength, toughness, wear resistance, and other aspects. Various steel manufacturing enterprises have paid great attention to the development of UHSS in recent decades, such as 22MnB5 developed by SSAB of Sweden [2], Usibor®1500 by ArcelorMittal of Luxembourg [3], and B1500H by Baosteel of China [4].
ArcelorMittal’s new generation of UHSS, Usibor®2000, has broad application prospects due to its superior resistance and mechanical properties [5]. However, UHSS frequently experiences issues with shape and dimensional stability during the forming process, including cracking and springback, resulting in great difficulties in installation and debugging. Solving the problem of improving the formability and quality of UHSS is a key challenge to promote its broad application. Hot forming technology has become an effective approach to achieve efficient and high-quality processing of UHSS due to its superior formability and low flow stress at high temperatures [6,7,8].
The profitable hot forming process of UHSS has received great enrichment and optimization in response to the large and rapidly growing market demand for steel applications. The rich variety of research results on the hot forming technology of UHSS has been achieved in the heating method [9,10,11], process window [12,13,14], numerical simulation [15,16], and microstructure evolution [17,18]. The majority of research on Usibor®2000 processing and application has only focused on the constitutive model [19], soft zone design [20], and thermal processing process window [21], and failed to address the microscopic deformation mechanism of Usibor®2000 under the complex action of temperature and force. The plasticity and formability of Usibor®2000 in the hot forming process are superior to those in the warm forming process, due to not only the occurrence of deformation and recrystallization, but also the evolution of the second precipitated phase [22]. Recent studies indicate that the matrix of commercial 38MnB5 was effectively reinforced through the uniform dispersion of (Nb, Ti)C nanoparticles as a second phase [23]. Nevertheless, the phase transition law and the second phase precipitation behavior in Usibor®2000 steel still call for an explanation in detail. The mechanical properties and formability of UHSS such as Usibor®2000 are intricately linked to its microstructural constituents and alloying element distribution. The steel’s high strength is primarily attributed to the presence of hard martensitic phases, which are significantly affected by its chemical composition, including carbon, boron, and microalloying elements such as Nb, Ti, and Mo. These elements influence the austenite stability, delay phase transformations, and promote precipitation strengthening via (Nb,Ti)C or (Ti,Nb)(C,N) carbides. During thermomechanical processing, these factors govern the kinetics and morphology of phase transitions, especially the competition between ferrite, bainite, and martensite formation depending on cooling rates. Understanding these mechanisms is essential for optimizing forming processes at various temperatures. Furthermore, modeling these phase transformations in real deep-drawing conditions provides valuable predictive insights for practical manufacturing, allowing for virtual process tuning and reducing the cost of trial-and-error experimentation. However, comprehensive studies linking microstructural evolution, mechanical response, and numerical simulations of thermal-mechanical behavior under deep drawing conditions remain scarce, particularly for Usibor®2000.
Despite recent advances in processing technology and phase transformation modeling of Usibor®2000, the fundamental question of how microscopic deformation mechanisms and precipitate evolution govern formability across different thermal regimes remains unresolved. Therefore, this study hypothesized that the formability and final mechanical properties of Usibor®2000 in the deep drawing process could be significantly influenced by temperature-induced microstructural evolution, particularly through the behavior of second-phase precipitates. The main objective was to elucidate the thermomechanical deformation mechanisms of Usibor®2000 under different forming temperatures, integrating microstructural characterization, phase composition analysis, and numerical simulation to bridge the gap between macro-scale forming outcomes and underlying microstructural processes.

2. Numerical Simulation

The phase transition behavior in sheet metal during the hot forming process was calculated theoretically to study the deformation mechanism of Usibor®2000 and analyze the phase composition evolution. The CCT curves for Usibor®2000 steel, provided by the JMatPro software v7.61 in Figure 1, show that varying cooling rates lead to different phase compositions. As the cooling rate increases, the martensitic content in the transformed microstructure also rises. The critical cooling rate required to achieve a fully martensitic phase falls between 1 °C/s and 10 °C/s. However, coupled with the in-die heating system, the cooling method adopted in this study basically relies on mold pressure cooling quenching, which is relatively slow, and fails to achieve the full martensitic transformation of Usibor®2000 in the hot forming process.
In this study, the cooling phase transformation of Usibor®2000 steel during the hot stamping process at an austenitizing temperature of 860 °C is illustrated in Figure 2 for two different cooling rates: 1 °C/s and 10 °C/s. Because the initial sheet temperature did not reach the austenitizing temperature of the material, 86.89% of the initial structure is austenite, with the remaining 12.62% ferrite, according to JMatPro. The ferritic transition begins at 800 °C and slowly increases, eventually stopping at 500 °C. At this point, the bainite transition begins and continues until it stops at 340 °C and then turns to a martensitic transition until almost all of the austenite is transformed. At a cooling rate of 1.0 °C/s, the final microstructure consists of 37.53% martensite, 24.66% ferrite, 37.46% bainite, and 0.35% residual austenite. In contrast, when the cooling rate is increased to 10 °C/s, the rapid temperature drop prevents austenite from transforming into ferrite and bainite. Instead, it reaches the martensitic transformation temperature range, resulting in the formation of martensite. Consequently, at a cooling rate of 10 °C/s, the final microstructure shows a significant shift compared to that at 1.0 °C/s, comprising 85.85% martensite, 13.85% ferrite, 0.17% bainite, and 0.14% residual austenite. The martensite content of Usibor®2000 after press hardening should be within the range of these two conditions, and the specific content and proportion need to be determined on the formed samples.
The numerical simulation analysis of the Swift cylinder drawing process in the 860 °C hot forming scheme was carried out by Autoform R8 software. The specific geometric model and mesh division of the deep drawing die are shown in Figure 3a. Under ideal conditions, the martensitic structure is formed in most areas of the sheet metal after thermoforming cooling; especially, the rounded corner area is the best quenching effect and the complete martensitic structure can be achieved, as shown in Figure 3b.
To validate the simulation results, the predicted phase fractions were compared with experimental data obtained from a two-step color metallographic analysis. The simulation estimated a martensite content ranging between 37.53% and 85.85% depending on the cooling rate, and the experimentally measured martensite content in the 860 °C formed samples was 65.89%, which falls within the predicted range, demonstrating good agreement between the simulation and the experiment.
Although in situ techniques such as dilatometry or thermal imaging were not employed in this study, the boundary conditions for the numerical simulation were carefully defined based on the actual processing parameters used in the thermoforming tests, including the austenitizing temperature, holding time, and in-die cooling method. Cooling rates of 1 °C/s and 10 °C/s were selected to represent the lower and upper bounds of industrial press hardening conditions. These parameters ensured that the simulation results closely reflect the expected microstructural transformations during forming.

3. Materials and Methods

The experimental material used in this study is an as-received Usibor®2000 steel sheet (ARCELORMITTAL, Luxembourg) with a thickness of 1.8 mm. Its chemical composition (in weight percentage) is Fe-0.36C-0.19Si-0.8Mn-0.28Cr-0.36Mo-0.04Nb-0.0032B. According to JMatPro software, the calculated austenitizing temperature is 952.18 °C. Therefore, the sheet was heated to 950 °C and maintained for 5 and 10 min before quenching. The resulting martensitic structures are illustrated in Figure 4a,b. It can be observed that the ferrite can be completely transformed into austenite, and then formed into a martensitic structure through a quenching and cooling transformation. By comparison, the uniform microstructure of martensite was obtained after a phase transition when the holding time is 10 min, as austenite has more time to form and grow.
Figure 4c,d shows SEM images of martensitic structures obtained after Usibor®2000 was held at 950 °C for 5 min followed by a quenching duration of 10 min. In both images, the martensite slats are arranged parallelly in a bundle and group, as well as the interlaced sheet martensite in different sizes, which constitute the mixed martensitic structure. The coarser-lath martensite groups and longer-sheet martensite are obtained when the material is held at an austenitizing temperature for 10 min, as shown in Figure 4d.
The formability for the Usibor®2000 sheet at different temperatures was evaluated using a KOMATSU H1F60 servo press (KOMATSU, Komatsu, Ishikawa, Japan) equipped with an in-die heating system. Figure 5a illustrates the die setup used for the Swift cup tests, while Figure 5b presents an approximate timeline of the thermoforming process across various temperature conditions. According to the GB/T 4156–2020 standard [24], the limiting drawing ratio (LDR) is defined as the ratio between the limiting blank diameter (D) and the punch diameter ( d p = 2 6.24 mm). Additional details regarding the testing procedure and parameters are available in previous work [25]. Deep drawing experiments were conducted within a temperature range of 100 °C to 860 °C, using 100 °C intervals. The stamping speed is set at 40 mm/s, and the blank holder force is maintained at 8 MPa.
The thickness profile of the formed cups was evaluated by taking an average of three measurements at each point. A digital Vickers microhardness tester was used, applying a 50 g load for 10 s. Microstructural analysis was conducted using a scanning electron microscope (SEM, Zeiss Gemini Sigma 300, Carl Zeiss AG, Oberkochen, Germany), and the elemental composition of the precipitates was identified using an energy-dispersive spectroscopy (EDS) system.
The microstructure of the drawn sample was characterized by two-step color metallographic etching. This technology was developed by De et al. [26] to identify different metallographic structures and the distribution of each phase by different colors after corrosion and coloring in multiphase steel. Bardelcik and George et al. [27,28] also employed this method to analyze the phase composition and friction distribution in hot-stamping processes.
The color metallurgical etching analysis is carried out in two stages. Initially, a solution of 4% picric acid (4 g dissolved in 100 mL of ethanol) is mixed with 1 mL of hydrochloric acid. This mixture is then used to etch the polished sample for around 20 s, and then immediately clean the sample with a large amount of water and wipe it with alcohol. After that, the sample is etched for roughly 10 s using a 10% sodium metabisulfite solution. Under the metallography microscope, the sample’s martensite will appear yellowish brown, the bainite black, and the ferrite white [29]. The different color proportions can be calculated and analyzed by image processing software ImageJ 1.53k through image region and pixel statistics to distinguish the phases in the metallographic photos. In this paper, martensite is marked red, ferrite is marked blue, and bainite is marked green.

Lubrication and Tooling Surface Treatment

To minimize interfacial friction during the deep drawing process, a high-temperature solid lubricant, specifically a boron nitride-based coating, was applied to both the punch and die surfaces before each forming test. This lubricant was selected for its effectiveness in high-temperature applications and its ability to reduce direct metal-to-tool contact. Additionally, the forming tools were polished to a surface roughness (Ra) of less than 0.2 μm to further reduce frictional resistance and ensure consistent material flow during deformation. These lubrication and surface treatment conditions were maintained consistently throughout all tests to ensure uniformity in the experimental setup.

4. Results and Discussions

4.1. Formability Analysis

To analyze the influence of temperature on the drawing process of the Usibor®2000 sheet, Figure 6a,b show a comparison of the cup height formed at 500 °C and 860 °C, respectively. The height of the cylindrical part formed at 860 °C increases by 53% compared to that at 500 °C. The LDR value at 860 ℃ was 2.05, which was 16.5% higher than that at 500 ℃ (1.76).
The thickness distribution of formed samples under drawing temperatures was assessed, as illustrated in Figure 6c. The maximum thinning area is located at the tangent point between the cylinder wall and the rounded corner of the drawn cup, which is in good agreement with the splitting position in the broken parts. The similar curves of thickness distribution indicate that the drawing performance of sheet metal is improved under the condition of hot forming. However, it can be seen from Figure 6d that the hardness of the hot drawing formed part is almost twice that of the warm drawing due to the martensitic phase transition, which means that the hot forming part obtains more ideal strength and forming quality.
The microstructure and compositional distribution of the specimens were further investigated, as shown in Figure 7, on which elemental mapping analysis of Nb, Mo, V, and C was induced, as depicted in Figure 7c,d. The large-size segregation component of Nb, Mo, and a little V, with an average diameter of 1.1 µm, was identified as Nb-rich (Nb, Ti) C carbide that is not solidly dissolved into the matrix during warm drawing at 500 °C, as shown in Figure 7c. The (Ti, Nb) (C, N) carbonitride remaining at 500°C can be considered as the crack source of the forming sheet [30]. As the temperature increases, most of the second phase has been dissolved into the matrix and has no time to precipitate in the form of a large-scale solid solution because of the high rapid cooling. In addition, the small-sized precipitates can be used as the martensitic nucleus substrate to promote the solid solution strengthening of sheet metal during deep drawing at 860 °C [31]. To further support these findings, a quantitative analysis of the precipitates was performed on representative SEM images using ImageJ. For the sample formed at 500 °C, the average diameter of (Nb,Ti)C precipitates was approximately 1.12 ± 0.28 μm, with an estimated number density of ~2.5 × 109 particles/cm2. In contrast, precipitates in the 860 °C sample were more dispersed and finer, with an average diameter of 0.38 ± 0.11 μm and a number density of ~6.8 × 109 particles/cm2. These quantitative differences further illustrate the enhanced dissolution and redistribution of alloying elements at higher temperatures, promoting a more favorable martensitic transformation and strengthening behavior.

4.2. Phase Composition Analysis

A two-step color metallographic etching technique was employed to analyze the phase distribution and composition within the sidewall structure of the drawn sample formed at 860 °C, as illustrated in Figure 8. The sidewall of the drawn sample formed at 860 °C exhibits a multiphase microstructure due to quenching during the forming process. Color etching reveals the coexistence of martensite, bainite, and ferrite. Martensite is arranged in an irregular, slat-like pattern, while bainite is characterized by a ferrite matrix with dispersed cementite particles [32].
The distribution of martensite, bainite, and ferrite in the sidewall microstructure of the sample drawn at 860°C was quantified through image analysis of the color metallographic image. Based on the processed data shown in Figure 8b, the area fractions for martensite, ferrite, and bainite are 65.89%, 21.25%, and 12.86%, respectively. Some ferrite and bainite phases formed before the martensitic phase transformation, resulting in a mixed microstructure in the sample. This structure, achieved at the cooling rate used in this test, provides an optimal balance of strength, toughness, and enhanced application potential. The result is basically consistent with the predicted martensite content range obtained by numerical simulation calculation.
The experimental results obtained from two-step color metallographic etching showed good agreement with the phase fractions predicted by simulation, particularly in the proportions of martensite, bainite, and ferrite. This consistency indirectly validates the phase transformation behavior modeled in the simulation and supports the use of CCT-based simulation as a reliable tool for predicting microstructure evolution under practical forming conditions.
To further interpret the observed increase in hardness at 860 °C, the hardness contribution of each phase was estimated using a rule-of-mixtures approach. Based on literature values, the Vickers hardness of martensite, bainite, and ferrite in boron-added ultrahigh strength steel is approximately 550 HV, 350 HV, and 200 HV, respectively [33]. Using the measured phase area fractions (65.89% martensite, 12.86% bainite, and 21.25% ferrite), the estimated average hardness is:
Havg = 0.6589 × 550 + 0.1286 × 350 + 0.2125 × 200 = 451.3 HV
which agrees well with the experimentally measured hardness (~460 HV). This result quantitatively supports the assertion that martensite formation dominates the observed hardening behavior at higher forming temperatures.

5. Conclusions

This study demonstrates that Usibor®2000 exhibited significantly improved formability and mechanical properties under hot stamping conditions. Specifically, deep drawing at 860 °C resulted in a limiting drawing ratio (LDR) of 2.05–16.5% higher than that at 500 °C— and a 53% increase in cup height. The enhanced performance could be attributed to the formation of a predominantly martensitic microstructure (65.89%), complemented by bainite and ferrite, as confirmed by two-step color metallography and consistent with numerical predictions. Compared to conventional press hardening steels, such as 22MnB5, Usibor®2000 demonstrated superior hardenability and strength-formability synergy due to its alloying with Nb, Mo, and Cr, promoting refined and stable austenite formation during heating and efficient martensitic transformation during quenching. Additionally, its capacity to achieve uniform phase distribution and solid solution strengthening under optimized forming conditions makes it a strong candidate for automotive structural components requiring high crashworthiness and weight reduction. These findings highlight the practical potential of Usibor®2000 in advanced hot forming applications and contribute to the ongoing efforts in lightweight, high-strength automotive design. It is acknowledged that the inclusion of temperature-dependent uniaxial tensile tests could further clarify the relationship between microstructure evolution and mechanical properties. Future research should concentrate on integrating such data to enhance the understanding of the thermal-mechanical response of Usibor®2000 during forming. Future research integrating temperature-dependent tensile testing and simulation will further elucidate the microstructure–property–process relationships in this material system.

Author Contributions

Conceptualization, Y.W. and P.D.; methodology, P.D.; software, Y.W. and J.H.; validation, Y.W., J.H. and Y.S.; formal analysis, Y.W. and J.H.; investigation, J.H. and J.S.; resources, P.D.; data curation, J.H.; writing—original draft preparation, Y.W. and J.H.; writing—review and editing, P.D.; visualization, Y.W.; supervision, Y.W. and P.D.; project administration, P.D. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

This work was supported by the Class III Peak Discipline of Shanghai—Materials Science and Engineering (High-Energy Beam Intelligent Processing and Green Manufacturing). The authors would like to thank the Shiyanjia Lab (www.shiyanjia.com) for the SEM tests.

Conflicts of Interest

The authors declare that they have no conflicts of interest.

References

  1. Merklein, M.; Wieland, M.; Lechner, M.; Bruschi, S.; Ghiotti, A. Hot stamping of boron steel sheets with tailored properties: A review. J. Mater. Process. Technol. 2016, 228, 11–24. [Google Scholar] [CrossRef]
  2. Barcellona, A.; Palmeri, D. Effect of Plastic Hot Deformation on the Hardness and Continuous Cooling Transformations of 22MnB5 Microalloyed Boron Steel. Metall. Mater. Trans. A 2009, 40, 1160–1174. [Google Scholar] [CrossRef]
  3. Eriksson, M.; Oldenburg, M.; Somani, M.C.; Karjalainen, L.P. Testing and evaluation of material data for analysis of forming and hardening of boron steel components. Model. Simul. Mater. Sci. Eng. 2002, 10, 277. [Google Scholar] [CrossRef]
  4. Liu, Y.; Lian, J.; Han, X.; Yang, Y.; Yuan, H. Hydrogen embrittlement studies of hot-stamped boron steel with different prior austenite grain sizes. J. Mater. Sci. 2023, 58, 18187–18206. [Google Scholar] [CrossRef]
  5. Valentini, R.; Tedesco, M.M.; Corsinovi, S.; Bacchi, L.; Villa, M. Investigation of Mechanical Tests for Hydrogen Embrittlement in Automotive PHS Steels. Metals 2019, 9, 934. [Google Scholar] [CrossRef]
  6. Karbasian, H.; Tekkaya, A.E. A review on hot stamping. J. Mater. Process. Technol. 2010, 210, 2103–2118. [Google Scholar] [CrossRef]
  7. Li, Y.; Li, S.; He, J.; Chen, Y.; Yue, L. Identification methods on blank-die interfacial heat transfer coefficient in press hardening. Appl. Therm. Eng. 2019, 152, 865–877. [Google Scholar] [CrossRef]
  8. Abe, Y.; Ohmi, T.; Mori, K.; Masuda, T. Improvement of formability in deep drawing of ultra-high strength steel sheets by coating of die. J. Mater. Process. Technol. 2014, 214, 1838–1843. [Google Scholar] [CrossRef]
  9. Gu, Z.; Lü, M.; Lu, G.; Li, X.; Xu, H. Effect of Contact Pressure during Quenching on Microstructures and Mechanical Properties of Hot-stamping Parts. J. Iron Steel Res. Int. 2015, 22, 1138–1143. [Google Scholar] [CrossRef]
  10. Kolleck, R.; Veit, R.; Merklein, M.; Lechler, J.; Geiger, M. Investigation on induction heating for hot stamping of boron alloyed steels. CIRP Ann. 2009, 58, 275–278. [Google Scholar] [CrossRef]
  11. Mori, K.; Maki, S.; Tanaka, Y. Warm and Hot Stamping of Ultra High Tensile Strength Steel Sheets Using Resistance Heating. CIRP Ann. 2005, 54, 209–212. [Google Scholar] [CrossRef]
  12. Merklein, M.; Lechler, J.; Geiger, M. Characterisation of the Flow Properties of the Quenchenable Ultra High Strength Steel 22MnB5. CIRP Ann. 2006, 55, 229–232. [Google Scholar] [CrossRef]
  13. Merklein, M.; Lechler, J. Investigation of the thermo-mechanical properties of hot stamping steels. J. Mater. Process. Technol. 2006, 177, 452–455. [Google Scholar] [CrossRef]
  14. Mori, K.; Maeno, T.; Yamada, H.; Matsumoto, H. 1-Shot hot stamping of ultra-high strength steel parts consisting of resistance heating, forming, shearing and die quenching. Int. J. Mach. Tools Manuf. 2015, 89, 124–131. [Google Scholar] [CrossRef]
  15. Merklein, M.; Lechler, J. Determination of Material and Process Characteristics for Hot Stamping Processes of Quenchenable Ultra High Strength Steels with Respect to a FE-based Process Design. SAE Int. J. Mater. Manuf. 2009, 1, 411–426. [Google Scholar] [CrossRef]
  16. Geiger, M.; Merklein, M.; Hoff, C. Basic Investigations on the Hot Stamping Steel 22MnB5. Adv. Mater. Res. 2005, 6–8, 795–804. [Google Scholar] [CrossRef]
  17. Liu, H.; Jin, X.; Dong, H.; Shi, J. Martensitic microstructural transformations from the hot stamping, quenching and partitioning process. Mater. Charact. 2011, 62, 223–227. [Google Scholar] [CrossRef]
  18. Liu, H.; Lu, X.; Jin, X.; Dong, H.; Shi, J. Enhanced mechanical properties of a hot stamped advanced high-strength steel treated by quenching and partitioning process. Scr. Mater. 2011, 64, 749–752. [Google Scholar] [CrossRef]
  19. Palmieri, M.E.; Tricarico, L. Comparison of Flow Behaviors at High Temperature of Two Press Hardening Boron Steels with Different Hardenability. Metals 2022, 12, 1935. [Google Scholar] [CrossRef]
  20. Palmieri, M.E.; Galetta, F.R.; Tricarico, L. Study of Tailored Hot Stamping Process on Advanced High-Strength Steels. J. Manuf. Mater. Process. 2022, 6, 11. [Google Scholar] [CrossRef]
  21. Palmieri, M.E.; Tricarico, L. Process Window Definition to Predict Mechanical Properties of Press Hardened Parts of Boron Steel with Tailored Properties. Key Eng. Mater. 2022, 926, 635–644. [Google Scholar] [CrossRef]
  22. Hou, J.; Deng, P.; Wang, Y.; Xu, H.; Shi, Y.; Wang, Y.; Li, J. Investigation of microstructure evolution and recrystallization refinement of Usibor®2000 press hardening steel sheets during deep drawing process. J. Mater. Sci. 2024, 59, 16292–16308. [Google Scholar] [CrossRef]
  23. Liang, J.; Lu, H.; Zhang, L.; Li, F.; Cao, R.; Liu, K.; Pan, H.; Teng, H.; Li, X.; Guo, A.; et al. A 2000 MPa grade Nb bearing hot stamping steel with ultra-high yield strength. Mater. Sci. Eng. A 2021, 801, 140419. [Google Scholar] [CrossRef]
  24. GB/T 4156–2020; Metallic Materials—Sheet and Strip—Erichsen Cupping Test. Standards Press of China: Beijing, China, 2020.
  25. Hou, J.; Deng, P.; Wang, S.; Xu, H.; Shi, Y. Study on formability and microstructure evolution of hot deep drawing manufactured 7005 aluminum alloy sheet metal. Mater. Today Commun. 2023, 36, 106794. [Google Scholar] [CrossRef]
  26. De, A.K.; Speer, J.G.; Matlock, D.K. Color tint-etching for multiphase steels. Adv. Mater. Amp. Process. 2003, 161, 27–31. [Google Scholar]
  27. Bardelcik, A.; Worswick, M.J.; Wells, M.A. The influence of martensite, bainite and ferrite on the as-quenched constitutive response of simultaneously quenched and deformed boron steel—Experiments and model. Mater. Des. 2014, 55, 509–525. [Google Scholar] [CrossRef]
  28. George, R.; Bardelcik, A.; Worswick, M.J. Hot forming of boron steels using heated and cooled tooling for tailored properties. J. Mater. Process. Technol. 2012, 212, 2386–2399. [Google Scholar] [CrossRef]
  29. Grajcar, A.; Radwański, K.; Krztoń, H.J. Microstructural Analysis of a Thermomechanically Processed Si-Al TRIP Steel Characterized by EBSD and X-Ray Techniques. Solid State Phenom. 2013, 203–204, 34–37. [Google Scholar] [CrossRef]
  30. Hong, S.G.; Kang, K.B.; Park, C.G. Strain-induced precipitation of NbC in Nb and Nb–Ti microalloyed HSLA steels. Scr. Mater. 2002, 46, 163–168. [Google Scholar] [CrossRef]
  31. Grajcar, A. Thermodynamic analysis of precipitation processes in Nb–Ti-microalloyed Si–Al TRIP steel. J. Therm. Anal. Calorim. 2014, 118, 1011–1020. [Google Scholar] [CrossRef]
  32. Bhadeshia, H.K.D.H.; Christian, J.W. Bainite in steels. Metall. Trans. A 1990, 21, 767–797. [Google Scholar] [CrossRef]
  33. Saeidi, N.; Ekrami, A. Comparison of mechanical properties of martensite/ferrite and bainite/ferrite dual phase 4340 steels. Mater. Sci. Eng. A 2009, 523, 125–129. [Google Scholar] [CrossRef]
Figure 1. CCT curve of Usibor®2000.
Figure 1. CCT curve of Usibor®2000.
Materials 18 02224 g001
Figure 2. Usibor®2000 quenching phase transition at different cooling rates at the austenitizing temperature of 860 °C (a) 1.0 °C/s (b) 10 °C/s.
Figure 2. Usibor®2000 quenching phase transition at different cooling rates at the austenitizing temperature of 860 °C (a) 1.0 °C/s (b) 10 °C/s.
Materials 18 02224 g002
Figure 3. Numerical simulation results of deep drawing Usibor®2000 (a) Deep drawing mold structure (b) Martensitic phase distribution.
Figure 3. Numerical simulation results of deep drawing Usibor®2000 (a) Deep drawing mold structure (b) Martensitic phase distribution.
Materials 18 02224 g003
Figure 4. (a,b) OM and (c,d) SEM images of martensitic tissue obtained from Usibor®2000 quenching after holding at 950 °C (a,c) for 5 min and (b,d) for 10 min.
Figure 4. (a,b) OM and (c,d) SEM images of martensitic tissue obtained from Usibor®2000 quenching after holding at 950 °C (a,c) for 5 min and (b,d) for 10 min.
Materials 18 02224 g004
Figure 5. (a) Die structure and (b) time-temperature changing curve for one shot.
Figure 5. (a) Die structure and (b) time-temperature changing curve for one shot.
Materials 18 02224 g005
Figure 6. Cup height of drawn samples at (a) 500°C and (b) 860°C. (c) Thickness distribution of molded cylinders at different temperatures (d); hardness distribution of molded cylinders at different temperatures. The interval of warm and hot forming cylindrical parts was 0.75 mm and 0.85 mm, respectively.
Figure 6. Cup height of drawn samples at (a) 500°C and (b) 860°C. (c) Thickness distribution of molded cylinders at different temperatures (d); hardness distribution of molded cylinders at different temperatures. The interval of warm and hot forming cylindrical parts was 0.75 mm and 0.85 mm, respectively.
Materials 18 02224 g006
Figure 7. SEM and EDS images of samples formed at (a,c) 500 °C and (b,d) 860 °C, and the top right corner is images for elemental mapping. (e) Morphology type of the precipitates in (c). (f) Compositional profile of the matrix in (d).
Figure 7. SEM and EDS images of samples formed at (a,c) 500 °C and (b,d) 860 °C, and the top right corner is images for elemental mapping. (e) Morphology type of the precipitates in (c). (f) Compositional profile of the matrix in (d).
Materials 18 02224 g007
Figure 8. Phase distribution and proportion of the side wall tissue of the specimen drawn at 860 °C (a) Color metallography obtained by two-step dyeing (b) phase area statistics and phase fractions.
Figure 8. Phase distribution and proportion of the side wall tissue of the specimen drawn at 860 °C (a) Color metallography obtained by two-step dyeing (b) phase area statistics and phase fractions.
Materials 18 02224 g008
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Wang, Y.; Hou, J.; Deng, P.; Shi, Y.; Song, J. Study on Formability and Microstructure Evolution of Usibor®2000 Sheet Under Different Forming Temperatures in Deep Drawing Process. Materials 2025, 18, 2224. https://doi.org/10.3390/ma18102224

AMA Style

Wang Y, Hou J, Deng P, Shi Y, Song J. Study on Formability and Microstructure Evolution of Usibor®2000 Sheet Under Different Forming Temperatures in Deep Drawing Process. Materials. 2025; 18(10):2224. https://doi.org/10.3390/ma18102224

Chicago/Turabian Style

Wang, Yuxuan, Jinyu Hou, Peiran Deng, Yongze Shi, and Jiacheng Song. 2025. "Study on Formability and Microstructure Evolution of Usibor®2000 Sheet Under Different Forming Temperatures in Deep Drawing Process" Materials 18, no. 10: 2224. https://doi.org/10.3390/ma18102224

APA Style

Wang, Y., Hou, J., Deng, P., Shi, Y., & Song, J. (2025). Study on Formability and Microstructure Evolution of Usibor®2000 Sheet Under Different Forming Temperatures in Deep Drawing Process. Materials, 18(10), 2224. https://doi.org/10.3390/ma18102224

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop