Principles of Stress-Strength Modelling of the Highly Thermally Loaded Materials—The Influence of an Effect of Strength Differential on the Material Effort
Next Article in Special Issue
Effect of Conditioning on PU Foam Matrix Materials Properties
Previous Article in Journal
Modeling of the Effective Permittivity of Open-Cell Ceramic Foams Inspired by Platonic Solids
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Study of the Mechanical, Sound Absorption and Thermal Properties of Cellular Rubber Composites Filled with a Silica Nanofiller

1
Centre of Polymer Systems, Tomas Bata University in Zlin, Třída Tomáše Bati 5678, 760 01 Zlin, Czech Republic
2
Faculty of Technology, Tomas Bata University in Zlin, Nám. T.G. Masaryka 275, 760 01 Zlin, Czech Republic
3
Faculty of Mechanical Engineering, VŠB-Technical University of Ostrava, 17. listopadu 15/2172, Poruba, 708 00 Ostrava, Czech Republic
*
Author to whom correspondence should be addressed.
Materials 2021, 14(23), 7450; https://doi.org/10.3390/ma14237450
Submission received: 15 November 2021 / Revised: 29 November 2021 / Accepted: 2 December 2021 / Published: 4 December 2021
(This article belongs to the Special Issue Advanced Materials Structures for Sound and Vibration Damping)

Abstract

:
This paper deals with the study of cellular rubbers, which were filled with silica nanofiller in order to optimize the rubber properties for given purposes. The rubber composites were produced with different concentrations of silica nanofiller at the same blowing agent concentration. The mechanical, sound absorption and thermal properties of the investigated rubber composites were evaluated. It was found that the concentration of silica filler had a significant effect on the above-mentioned properties. It was detected that a higher concentration of silica nanofiller generally led to an increase in mechanical stiffness and thermal conductivity. Conversely, sound absorption and thermal degradation of the investigated rubber composites decreased with an increase in the filler concentration. It can be also concluded that the rubber composites containing higher concentrations of silica filler showed a higher stiffness to weight ratio, which is one of the great advantages of these materials. Based on the experimental data, it was possible to find a correlation between mechanical stiffness of the tested rubber specimens evaluated using conventional and vibroacoustic measurement techniques. In addition, this paper presents a new methodology to optimize the blowing and vulcanization processes of rubber samples during their production.

Graphical Abstract

1. Introduction

Natural rubber (NR) comes from a tree called “Hevea brasiliensis” that is grown in many countries around the world, e.g., in Malaysia, Indonesia, India, Vietnam and Thailand. This tree produces a milky liquid called natural rubber latex [1]. Natural rubber latex is a dispersion of rubber particles in aqueous medium containing approximately 33% cis-1,4-polyisoprene rubber particles dispersed in water. This latex is obtained from the tree by making a cut in its bark in tropical countries of its origin [2]. The rubber is prepared by coagulation of the latex with acids. The obtained precipitate is subsequently dried and pressed into packaging. Natural rubber is very important in the rubber industry due to its elasticity, tensile strength and self-reinforcing character, which is said to originate from its strain-induced crystallization (SIC). SIC is caused by its linear chains, which are able to orient under stress. Rubbers with a macromolecular structure like polychloroprene rubber (CR) and polyisoprene rubber (IR) similar to NR can crystallize under stress. Due to the SIC behavior, these rubbers have excellent mechanical properties and good resistance to crack growth [3,4,5]. The advantages of NR also include low heat build-up [6].
However, unvulcanized rubbers without ingredients are not often used because they do not have the required properties. Additionally, additives (fillers, vulcanizing agents, UV stabilizers, etc.) are added to these rubbers to achieve the required properties. NR with additives is referred to as a rubber compound that is plastic and malleable. The composition of rubber compounds is given in units of phr (i.e., parts per hundred rubber). Crosslinking process occurs during high-temperature heating, when the rubber compound turns into an elastic material, i.e., vulcanizate [7,8]. Sulphur is one of the most commonly used curing agents [7]. Peroxides usually for ethylene propylene diene methylene (EPDM) and oxides of divalent metals for CR rubbers are also used. The main components of rubber compounds are fillers because they reduce the cost of rubber products and modify physical and mechanical properties of vulcanizates, such as tensile strength and abrasion [8]. The stiffening effect of rubber compounds generally depends on filler particle sizes. The highest stiffness is usually achieved with rubber compounds containing filler particle sizes from 10 to 100 nm that are characterized by a large specific surface area. In practice, carbon black and silica nanofillers are most commonly used as reinforcing fillers [9]. Silica is obtained from silica rocks by natural mining of minerals in various parts of the world and by the subsequent grinding or crushing of these raw materials. Such silica is called ground silica and is characterized by a low reinforcing effect due to the large primary particles. By chemical treatment of the mined material, it is possible to obtain silica with small particle sizes, which have a stiffening effect comparable to that of carbon black filler. The smallest primary particle sizes (i.e., from 1 to 3 nm) are obtained by pyrolysis process. Such silica is called fumed silica [10]. These primary particles form aggregates of size from 100 to 250 nm. Silica is characterized by the best stiffening effect due to its large specific surface area (i.e., from 50 to 400 m2·g−1) [11]. Larger particle sizes (>40 nm) are obtained by precipitation of sodium silicate (Na2SiO3) with acids. Such silica is called precipitated silica [10,12].
Other additives are also added to rubber compounds. Nucleating agents are used to improve the cell morphology of rubber compounds (i.e., increasing cell density, decreasing cell size and narrowing cell-size distribution) by providing heterogeneous nucleation sites [13]. Blowing agents are added in order to produce foam rubber products. Along with urethane and polyvinyl chloride rubber materials, the foam rubber products are competitive with cushioning or padding plastic foams such as cloth, polyester fiberfill, hair, jute and the like. Foam rubber products are very important in many applications due to their unique structural properties such as their low weight, performance, impact damping, thermal and acoustic insulation properties, moderate energy absorption and low price [14,15,16]. In general, foam rubbers can be divided into sponge, cellular and microcellular rubbers. Sponge rubber has a similar structure to a real sea sponge. It consists of open and interconnected cavities. The channels thus formed allow a high absorption of liquids and release the absorbed liquid after their compression. Cellular rubber is characterized by a higher specific weight compared to sponge rubber. Its structure, characterized by cell size, cell density and expansion ratio [17], consists of smaller cavities that are not interconnected. The cellular rubber is thus more compressible, non-absorbent and achieves excellent damping properties [14]. Microcellular rubbers are characterized by cell densities greater than 109 cells/cm3 and cells smaller than 10 μm [18]. These rubber types are produced by using physical or chemistry blowing agents. Physical blowing is performed with blowing liquids (e.g., pentane and hexane) and is based on the liquid–vapor transition. The essence of chemical blowing is the chemical decomposition of the blowing agent or the reaction to release gases. In the rubber blowing process, it is important that the blowing process takes place before vulcanization. Once the cellular structure is formed, vulcanization should occur to fix this cellular structure [14,19,20]. Another type of foam rubber is latex foam, which is obtained from natural rubber latex by mechanical whipping and subsequent vulcanization. New applications of the NR latex foam rubbers allow their use as absorbent materials for oils and carbon dioxide (CO2). NR latex foam rubber filled with silica can serve as a CO2 absorbing material [21].
Many studies have already investigated various properties of silica-filled rubber composites. The aim of this research is to investigate the mechanical, sound absorption and thermal properties of cellular rubber composites that were produced with various concentrations of silica nanofiller and the same blowing agent concentration. Mechanical properties of rubber materials can be determined by conventional measurement techniques such as tensile, shear, hardness, permanent deformation, rebound resilience and viscoelasticity tests. In this research, the mechanical stiffness of the investigated silica-filled rubber composites determined from permanent deformation and rebound resilience measurements is verified by non-conventional methods for determining the stiffness of these materials, namely by vibration damping and sound absorption methods. The latter two methods are relatively simple, inexpensive, fast and non-destructive compared to the conventional methods used to determine the mechanical stiffness of solids. Therefore, the vibration damping and sound absorption methods can also be easily applied to compare the mechanical stiffness of different materials. In addition, the rubber molding process is optimized using rubber processing analysis, where the rubber blowing phase should generally take place before the vulcanization phase for a given rubber recipe.

2. Materials and Methods

2.1. Materials

Natural rubber SMR (Standard Malaysian Rubber)–20 was used as the base for rubber compounds. Silica Perkasil KS–408 from WR Grace & Co. (Columbia, MD, USA) with the specific surface area of 175 m2·g−1 and bulk density of 0.17 g·cm−3 was used as a nanofiller in rubber compounds. The additives, including activator ZnO from SlovZink a.s. (Košeca, Slovakia), activator stearic acid from Setuza a.s. (Ústí nad Labem, Czech Republic), antiozonant N-(1,3-dimethylbutyl)-N’-phenyl-p-phenylenediamine (Vulkanox 4020) from Lanxess AG (Brussel, Belgium), plasticizer (paraffinic oil Nyflex 228) from Nynas AB (Stockholm, Sweden), blowing agent azodicarbonamide C2H4N4O2 (Porofor ADC) from Lanxess AG (Brussel, Belgium), accelerator N-tert-butyl-benzothiazole sulfonamide (TBBS) from Duslo a.s. (Šal’a, Slovakia) and curing agent sulphur type Crystex OT33 from Eastman Chemical company (Kingsport, TN, USA), were also compounded. Five rubber compounds with different silica concentrations were prepared. Their recipe is detailed in Table 1.
The optimization of mechanical properties of rubber compounds is highly dependent on the silica concentration. During the mixing process of rubber compounds, the viscosity of these compounds generally increases with increasing the silica concentration. High concentrations of silica filler (i.e., over 30 phr) in rubber compounds lead to a difficult mixing process, a lower dispersion of additives and an increase in curing time [22]. For this reason, rubber samples produced with the highest silica concentration of 45 phr are characterized by an imperfect blowing process, which results in a reduction in damping properties of cellular rubbers.
In the first stage of the production of rubber composites, the basic rubber compounds (i.e., SMR–20, ZnO, Vulkanox 4020, stearic acid, silica and Nyflex 228) were mixed in a two-roll mill (150 mm × 330 mm, Farrel, Milan, Italy) at a rotation speed ratio of 15/20 at a temperature of 50 °C. After mixing these ingredients, a three-minute homogenization took place on the two-roll mill and subsequently the compound was withdrawn from this mill. The mixing process in the second stage, in which the remaining ingredients (i.e., Porofor ADC, TBBS and sulphur OT33) were mixed, followed after a 20-min pause on the two-roll mill under the same conditions as in the first stage. After this mixing, a five-minute homogenization was performed, and the obtained rubber compounds were subsequently withdrawn from the mill.
The rubber compounds were compression-molded at a temperature of 170 °C using a hydraulic hot press during the time tm, which is given by the equation:
t m = t 90 + c m · t
where cm = 0.5 min/mm is the molding constant, t90 (min) is the optimum cure time (see Chapter 3.1) and t (mm) is the sample thickness.
Finally, rubber specimens of two different diameters of 20 and 100 mm and three different thicknesses of 4, 8 and 12 mm were produced.

2.2. Measurement Methodology

2.2.1. Curing Characteristics

Curing characteristics were measured according to ASTM D 5289 standard on the Premier MDR moving die rheometer from Alpha Technology (Hudson, OH, USA) at a constant temperature of 170 °C. Minimum (ML) and maximum (MH) torques, scorch (ts1) and optimum cure (t90) times were subsequently evaluated.

2.2.2. Rubber Processing Analysis

The rubber processing (RP) analysis, which is based on cone-cone principle, was performed on the Premier RPA rubber process analyzer from Alpha Technology (Hudson, OH, USA). As a result of RP analysis, time dependencies of pressure curves during isothermal vulcanization were determined. The rate of blowing was subsequently obtained from the first time derivative of the pressure curve.

2.2.3. Optical Microscopy

Pore sizes on cut surfaces of the investigated rubber specimens were evaluated using an optical microscope “Carl Zeiss Stemi 2000–C” from Carl Zeiss Microimaging GmbH (Jena, Germany) [23]. The magnification of the microscope objective was from 0.65× to 5× and the stereo angle was set to 11°.

2.2.4. Rebound Resilience

The rebound resilience was measured according to ISO 4662 standard. Rubber specimens measuring 12 mm in thickness were examined. Average values of the rebound resilience and their standard deviations were subsequently determined from six measured values. The measurements were carried out at an ambient temperature of 22 °C.

2.2.5. Compression Testing

Experimental measurements of permanent deformation of cellular rubber composites were performed according to ČSN EN ISO 1856 standard based on compression tests. These measurements were carried out on rubber samples measuring 12 mm in thickness and 20 mm in diameter. The samples were compressed to 50% initial thickness (t1) for 24 h at three different temperatures (i.e., 24, 40 and 65 °C). After compression, the samples were released for 30 min, and their thicknesses (t2) were measured again. Finally, the compression set CS (%) of the rubber samples was determined from the equation [24]:
C S = t 1 t 2 t 1 × 100
Average values of the compression set, including their standard deviations, were determined from five measured values.

2.2.6. Mechanical Vibration Damping Testing

The ability of a material to dampen harmonically excited mechanical vibration is expressed by the displacement transmissibility Td (–) that is defined for a linear single degree of freedom as follows [25,26]:
T d = y 2 y 1 = a 2 a 1 = k 2 + ( c ω ) 2 ( k m ω 2 ) 2 + ( c ω ) 2 = 1 + ( 2 ζ r ) 2 ( 1 r 2 ) 2 + ( 2 ζ r ) 2
where y is the displacement amplitude on the input (1) and output (2) sides of the harmonically loaded sample, a is the acceleration amplitude on input (1) and output (2) sides of the harmonically loaded sample, k is the stiffness (spring constant), c is the viscous damping coefficient, m is the mass, ω is the frequency of oscillation, ζ is the damping ratio and r is the frequency ratio. The damping and frequency ratios are expressed by the equations [27,28,29]:
ζ = c 2 · k · m
r = ω ω n = ω · m k
where ωn is the natural frequency. There are three different types of mechanical vibration depending on the displacement transmissibility value, namely damped (Td < 1), undamped (Td = 1) and resonance (Td > 1) vibration. Under the condition dTd/dr = 0 in Equation (3), it is possible to determine the frequency ratio r0, at which the displacement transmissibility reaches a maximum value [25]:
r 0 = 1 + 8 ζ 2 1 2 ζ
It is apparent from Equation (6) that the local extreme of the displacement transmissibility (Tdmax) is generally shifted to lower values of the frequency ratio r with an increase in the damping ratio ζ.
The mechanical vibration damping testing of the investigated rubber composites was performed by the forced oscillation method. The displacement transmissibility Td was experimentally measured using a BK 4810 shaker in combination with a BK 3560-B-030 signal pulse multi-analyzer and a BK 2706 power amplifier (Brüel & Kjær, Nærum, Denmark) in the frequency range of 2–1500 Hz. Harmonic sine waves were generated by the shaker. The displacement transmissibility was determined from Equation (3) based on the acceleration amplitudes a1 and a2 on the input and output sides of the investigated samples by means of BK 4393 accelerometers (Brüel & Kjær, Nærum, Denmark). Measurements of the displacement transmissibility were performed for different inertial masses m (i.e., 0, 90 and 500 g), which were located on the upper side of the harmonically loaded investigated samples. Furthermore, vibration damping testing of the investigated rubber samples with a ground plane dimension of 60 mm × 60 mm was performed for three different sample thicknesses (i.e., 4, 8 and 12 mm). Each measurement was repeated five times at an ambient temperature of 23 °C.

2.2.7. Sound Absorption Measurements

Sound absorption properties of materials are characterized by the sound absorption coefficient α (–), which is defined by the ratio [30]:
α = P d P i
where Pd is the dissipated acoustic power and Pi is the incident acoustic power. The ability of a material to absorb sound is generally affected by different factors, namely by excitation frequency of acoustic waves, material thickness, structure, density, temperature, humidity and so on. Sound absorption properties of materials are also characterized by the noise reduction coefficient NRC (−), which considers the excitation frequency influence on the sound absorption coefficient. This coefficient is defined as the average value of the sound absorption coefficients of a given material at the excitation frequencies of 250, 500, 1000 and 2000 Hz [31]:
N R C = α 250 + α 500 + α 1000 + α 2000 4
Sound absorption measurements can also be used to determine the longitudinal elastic coefficient K of a powder bed. This coefficient is similar to Young´s modulus of elasticity and is defined by the formula [32,33]:
K = c 2 · ρ b = ( 4 · h · f p 1 ) 2 · ρ b
where c is the speed of sound of elastic wave propagated through a powder bed, ρb is the powder bulk density, h is the powder bed height and fp1 is the primary absorption peak frequency.
Frequency dependencies of the normal incidence sound absorption coefficient α of the tested rubber samples and the loose silica powder were determined by the transfer function method ISO 10534-2 [34] using a BK 4206 two-microphone impedance tube in combination with a BK 3560-B-030 signal pulse multi-analyzer and a BK 2706 power amplifier (Brüel & Kjær, Nærum, Denmark) in the frequency range of 150–6400 Hz. The transfer function method is based on the partial standing wave principle. In this case, the normal incidence sound absorption coefficient α is expressed by the equation [35]:
α = 1 | H 12 e k 0 · ( x 1 x 2 ) · j e k 0 · ( x 1 x 2 ) · j H 12 . e 2 k 0 · x 1 · j | 2
where H12 is the complex acoustic transfer function, k0 is the wave number, x1 and x2 are the distances of two microphone positions from the reference plane (x = 0) and j is the imaginary unit. The complex acoustic transfer function is defined as follows:
H 12 = p 2 p 1 = e k 0 · x 2 · j + r · e k 0 · x 2 · j e k 0 · x 1 · j + r · e k 0 · x 1 · j
where p1 and p2 are the complex acoustic pressures at two microphone positions. Sound damping properties of the tested rubber samples and the silica powder bed were investigated in the impedance tube having inside diameter of 30 mm for different sample thicknesses (i.e., 4, 8 and 12 mm) of the studied rubber composites and various silica powder bed heights (ranging from 10 to 40 mm). Experimental measurements of the sound absorption coefficient were realized at an ambient temperature of 22 °C.

2.2.8. Thermal Conductivity

Experimental measurements of the thermal conductivity over the range of 0.01–10 W·m−1·K−1 of the rubber composites were carried out according to ČSN 72 1105 standard using a C-Therm TCi thermal conductivity analyzer (C-Therm Technologies, Frederiction, NB, Canada). Average values of the thermal conductivity and their standard deviations were subsequently determined from five measured values.

2.2.9. Thermogravimetric Analysis

Thermogravimetric properties of the investigated cellular rubber samples were realized on a thermal analyzer DTG/60 (Shimadzu, Japan). Experimental measurements were performed at a heating rate of 10 °C/min under nitrogen atmosphere (50 mL/min) in the temperature range from 30 to 500 °C. Thermogravimetric analysis, which consisted in measurements of the weight loss ∆m of the tested rubber samples, was evaluated using ta60 Version 1.40 (Shimadzu, Japan) software. The measured results were performed in triplicate.

3. Results and Discussion

3.1. Curing Characteristics

Curing curves of the tested rubber composites are demonstrated in Figure 1. Curing parameters of these materials are shown in Table 2. It is visible (see Figure 1) that the minimum (ML) and maximum (MH) torques increase with an increase in the silica concentration due to a higher mechanical stiffness of the rubber composites at higher silica concentrations. Similarly, the optimum cure time t90 increases with increasing the silica concentration. Table 2 also shows the scorch time ts1, which is characterized by the fact that the rubber composite was still plastic during this time. Therefore, the blowing process of the tested rubbers should also be carried out during the time ts1.

3.2. Rubber Processing Analysis

Time dependencies of pressure curves and the rate of blowing of the investigated rubber composites are shown in Figure 2 and Figure 3. It is evident from these figures that the blowing process of the rubbers took place in three phases. In the first phase (i.e., preheating), the rubber composite is heated, its viscosity is reduced to a minimum and the blowing agent was not decomposed. In addition, a skin is formed in order to prevent profile collapse. In the second stage (i.e., expansion), the blowing agent was decomposed with increasing the vulcanization rate. A relative balance between pressure gas and vulcanizate formation created a cell structure. The degree of vulcanization reached its maxima in the third stage (i.e., curing). If the decomposition of the blowing agent starts late, the production of released gas from the decomposition of the blowing agent could be limited during the curing process, which could lead to imperfect cellular structures of rubbers. It is evident from Figure 2 that a rapid increase in pressure (i.e., blowing) took place in the second phase, when the decomposition of the blowing agent occurs only with the increasing rate of vulcanization. As shown in Figure 3, the fastest decomposition of the blowing agent occurred at the maximum rate of blowing. The vulcanization and blowing processes of the rubber composite containing 45 phr of silica were more difficult due to higher filler content. These processes were slower because the silica filler bound the vulcanization system due to the content of polar groups. Therefore, the rubber composite containing 45 phr of silica became more viscous during the blowing process, and thus the blowing of this rubber composite was imperfect.

3.3. Optical Microscopy

As can be seen from the optical microscopy images (see Figure 4), it is possible to observe distinct cavities caused by evaporation of the blowing agent. It is evident that the most distinct cavities are observed for the rubber composite containing 0 phr of silica. Smaller cavities are observable in the rubber samples containing 10, 20 and 30 phr of silica. The size of these cavities is still sufficient to ensure good thermal insulation properties of these rubbers. It is also obvious from Figure 4 that there was practically no cellular structure of the rubber composite containing 45 phr of silica. This is due to the fact that silica is reinforcing filler, which increases the viscosity of rubber composites at high silica concentrations. Therefore, sufficiently large cavities were not created during the blowing process in the rubber composite with 45 phr of silica. This fact also corresponds with the time dependence of the rate of blowing (see Figure 3), where the maximum rate of blowing for the rubber composite containing 45 phr of silica was lower compared to the maximum rate of blowing of the rubber composite with 30 phr of silica. For this reason, the rubber composite containing 45 phr of silica was not suitable in terms of thermal insulation properties.

3.4. Mechanical Properties

3.4.1. Rebound Resilience

The results of the average values of the rebound resilience and their standard deviations are shown in Table 3. The rebound resilience decreased from 51% to 35% for S0 and S45 rubber composites, respectively. It can be concluded that higher silica concentrations in rubber composites led to a higher ability to transform mechanical energy into heat, and thus to a decrease in the rebound resilience.

3.4.2. Compression Testing

Dependencies of permanent deformation vs. silica concentration for three different temperatures (i.e., 25, 40 and 65 °C) are demonstrated in Figure 5. It can be observed that the compression set generally increased with increasing temperature. It is also evident that the permanent deformation decreased at higher silica concentrations. This was due to the higher silica content in rubber composites and the formation of smaller cavities that were able to return the rubber composites to their original state [24]. The highest compression set values (i.e., 52.2 and 48.7%) at the given compression temperatures (i.e., 65 and 40 °C) were obtained for the rubber composites containing 10 phr of silica. At the compression temperature of 25 °C, the highest compression set of 36.2% was found for the rubber composite containing 20 phr of silica.

3.4.3. Mechanical Vibration Damping Testing

Frequency dependencies of the displacement transmissibility of the tested rubber composites measuring t = 4 mm in thickness and containing different concentrations of silica are shown in Figure 6. In addition, the rubber samples were loaded with an inertial mass of 90 g. It is evident from this comparison that the concentration of silica had a significant influence on vibration damping properties of the tested composite materials. The ability of a material to damp mechanical vibration is generally decreasing with increasing the concentration of silica, which was in accordance with measurements of the rebound resilience and the permanent deformation. It was again due to higher stiffness k (or lower damping ratio ζ) of the rubber composites, which were produced with higher concentrations of silica. These facts resulted in a lower transformation of input mechanical energy into heat during forced oscillations [36], and in an increase in the values of the damped and undamped natural frequencies (see Equation (6)) [37]. Therefore, the first resonance frequency (fR1) value was shifted to the right (see Figure 6) with increasing concentration of silica, namely from 218 Hz (i.e., sample S0) to 721 Hz (i.e., sample S45), as indicated in Table 4.
The vibration damping properties of the investigated harmonically loaded rubber samples were also influenced by their thickness t, the inertial mass m and the excitation frequency f.
The effect of the inertial mass on vibration damping properties for the S20 rubber type measuring t = 4 mm in thickness is shown in Figure 7a. It is visible that better vibration damping properties were generally observed for higher inertial masses m. For this reason, the inertial mass had a positive influence on mechanical vibration damping, which is reflected in a shift of the first resonance frequency peak position to lower excitation frequencies, i.e., in the decrease of the frequency fR1 (see Table 4) from 434 Hz (m = 0 g) to 120 Hz (m = 500 g). This finding is consistent with Equations (4) and (6). It should be noted that the magnitude of inertial mass is limited only to the range of elastic deformations of the harmonically loaded rubber specimens.
The effect of the sample thickness on vibration damping properties is shown in Figure 7b for the S45 rubber type loaded by an inertial mass of 90 g. It is visible that a higher material thickness led to lower values of the frequency fR1, i.e., from 721 Hz (t = 4 mm) to 457 Hz (t = 12 mm), as indicated in Table 4. For this reason, the rubber thickness generally has a positive effect on vibration damping and leads to a higher transformation of input mechanical energy into heat during dynamic loading.
It is also visible from Figure 6 and Figure 7 that the vibration damping properties were also significantly influenced by the excitation frequency f. It is evident from these frequency dependencies that the resonant mechanical vibration (i.e., Td > 1) was achieved at low excitation frequencies depending on the rubber composite type, its thickness t and the inertial mass m. For example, for the S45 rubber type measuring 4 mm in thickness and without inertial mass (i.e., m = 0 g), the resonant mechanical vibration was observed over the entire frequency range. In the case of the S0 rubber type measuring 12 mm in thickness and loaded with the highest inertial mass (i.e., m = 500 g), the resonant mechanical vibration was observed at significantly lower excitation frequencies (namely at f < 86 Hz). On the contrary, the damped mechanical vibration (i.e., Td < 1) was generally obtained at higher excitation frequencies (see Figure 6 and Figure 7).

3.5. Sound Absorption Properties

Frequency dependencies of the sound absorption coefficient of the loose silica powder depending on its height are shown in Figure 8. The obtained results of acoustical and mechanical quantities from sound absorption measurements are shown in Table 5. It is clear from the calculated values of the noise reduction coefficient NRC (see Equation (8)) that sound damping properties of the tested loose silica filler generally increased with increasing the powder bed height. As is shown in Figure 8, sound absorption properties of the silica powder were similar at higher excitation frequencies (i.e., at f > 2 kHz) independently of the powder bed height. It is also visible that the maximum value of the sound absorption coefficient, which is proportional to the primary absorption peak frequency fp1 (i.e., αmax = αfp1), generally shifted towards lower excitation frequencies with increasing the powder bed height (see Figure 8). The speed of sound c and the longitudinal elastic coefficient K were subsequently determined from Equation (9). It was found that a higher powder bed height led to a higher speed of sound c, and thus, to higher values of the longitudinal elastic coefficient K. For this reason, the mechanical stiffness of the studied silica filler generally increased with increasing the silica bed height h.
Frequency dependencies of the sound absorption coefficient of the tested rubber composites measuring t = 12 mm in thickness with different concentrations of silica are shown in Figure 9a. It is evident that sound absorption properties generally increased with decreasing silica concentrations. This fact was influenced by the rubber stiffness, which increases with increasing the silica concentration, as well as the longitudinal elastic coefficient of the loose powder beds (see Table 5). For this reason, better sound damping properties were obtained for rubber samples containing lower silica concentrations, at which the rubber samples exhibit lower stiffness and their structure is more spongy-like. This finding is consistent with the fact that porous, spongy and fiber materials belong to suitable materials in order to absorb sound [38]. The above-mentioned phenomena were also in good agreement with the vibration damping measurements, when a better ability of damp mechanical vibrations was generally obtained in rubber composites containing lower concentrations of silica.
It was also found that sound damping properties increase with increasing the sample thickness (see Figure 9b), especially at lower excitation frequencies. This finding was confirmed on the basis of the noise reduction coefficient. As indicated in Table 6, the noise reduction coefficient generally increased with an increase in rubber thickness and the decreasing concentration of silica. Its value ranges from 0.028 (S45, t = 4 mm) to 0.182 (S0, t = 12 mm). For these reasons, sound absorption properties of the investigated rubber composites were relatively low.

3.6. Thermal Properties

3.6.1. Thermal Conductivity

The effect of silica concentration on thermal conductivity of the studied rubber composites is shown in Figure 10. Observed data show an exponential increase in thermal conductivity with the increasing silica concentration. Low silica content led to larger pore sizes in rubber composites, which is accompanied by lower values of thermal conductivity. Therefore, rubber composites containing pores of larger sizes can be used as thermal insulators. As shown in Figure 10, a significant increase in thermal conductivity was achieved at higher concentrations (>30 phr) of silica. In these cases, the rubber composite is too stiff and viscous, which prevented the formation of larger pores. The thermal conductivity of 0.508 W·m−1·K−1 for the rubber composite containing 45 phr of silica was approximately double compared to the thermal conductivity of the rubber composite with 30 phr of silica. For this reason, a porous structure of the rubber composite containing 45 phr of silica was practically not formed, which led to a significant decrease in thermal insulation properties of rubber composites containing high concentrations (i.e., over 45 phr) of silica.

3.6.2. Thermogravimetric Analysis

As illustrated in Figure 11, the rubber composites were characterized by a two-step symmetric degradation of similar curve shapes, regardless of filler amount. The first declination on thermogravimetric curves started above 150 °C and continued until 300 °C with the corresponding weight loss of about 10% (w/w). Exceeding this temperature limit (i.e., about 300 °C), a rapid degradation occurred, and was accompanied by a noticeable decrease in the sample weight. At the temperatures from 420 to 440 °C, the degradation process stopped, while the degradation extent was apparently dependent on the filler concentration.
As is obvious from Table 7, higher reduction in the weight loss ∆m was generally observed at lower filler concentrations. It was found that the rubber sample without any silica filler (i.e., 0 phr) exhibited the weight loss of 90.42% (w/w) in the entire temperature range. On the other hand, the rubber sample containing the highest filler concentration (i.e., 45 phr) showed the highest thermal stability at the weight loss ∆m = 66.63% (w/w). Therefore, higher concentrations of the silica filler generally led to a higher thermal stability of the investigated rubber composites.

4. Conclusions

Rubber composites are widely applied in many areas at the present time. It is often necessary to optimize rubber properties for given purposes. This research was focused on the study of mechanical, sound absorption and thermal properties of cellular rubber composites that were filled with different concentrations of silica nanofiller. Nevertheless, the tested rubber composites were produced with the same blowing agent concentration. In addition, the production of the rubber samples was carried out according to a new methodology in order to optimize the blowing and vulcanization processes of these samples. Based on this research, it can be concluded that the concentration of silica filler in the rubber composites had a significant influence on the mechanical stiffness of the rubbers, and thus on their sound absorption and thermal properties.
The mechanical properties examined included rebound resilience, compression testing and mechanical vibration damping properties of the investigated rubber composites. It was found that the mechanical stiffness of the rubber composites generally increased with increasing concentration of silica filler. The rebound resilience of the rubber composite containing 45 phr of silica was approximately 32% lower compared to the rubber composite containing 0 phr of silica. Similarly, the compression set of the rubber composites with 45 phr of silica was approximately 16% lower compared to those of the rubber composites with 0 phr of silica. These findings were in good agreement with vibration damping measurements that were performed using the non-destructive forced oscillation method based on the displacement transmissibility. It can be stated that the first resonance frequency peak position increased with an increase in mechanical stiffness leading to lower vibration damping properties of the rubber composites. Therefore, a higher concentration of silica filler in rubber composites generally led to a lower transformation of input mechanical energy into heat under dynamic loading of these rubbers. The mechanical properties of the investigated rubber composites were also in agreement with their sound absorption properties. It was found based on the sound damping measurements that higher concentrations of the loose silica powder led to higher values of the longitudinal elastic coefficient, and thus to a higher mechanical stiffness of the silica filler. Furthermore, sound absorption properties of the rubber composites generally decreased with increasing silica concentration. For this reason, a higher ability to damp sound was found for the rubber composites of more spongy-like structure, which is typical for rubbers containing lower concentrations of silica filler.
It was also found that higher concentrations of silica nanofiller generally led to a decrease in thermal degradation and an increase in thermal conductivity of the investigated rubber composites. Therefore, in practice, rubber composites containing lower concentrations of silica filler can be used as thermal insulators.
From the experimental data, it can be concluded that the mechanical stiffness of the tested silica-filled rubber composites can be also evaluated by the non-conventional methods of mechanical vibration damping and sound absorption. These methods are relatively simple, inexpensive, fast and non-destructive, which are their undeniable advantages compared to conventional methods used to determine the mechanical stiffness.
The investigated silica-filled rubber composites can be used in applications where higher shape recovery, stiffness-to-weight ratio and thermal conductivity are required, e.g., in the manufacture of rubber components in automotive, aerospace and footwear industries.

Author Contributions

Conceptualization, M.V. and M.P.; methodology, M.V. and M.P.; software, M.V. and M.P.; validation, M.V. and M.P.; formal analysis, M.V. and M.P.; investigation, M.V. and M.P.; resources, M.V. and M.P.; data curation, M.V. and M.P.; writing—original draft preparation, M.V. and M.P.; writing—review and editing, M.V. and M.P.; visualization, M.P.; supervision, M.V.; project administration, M.V. and M.P.; funding acquisition, M.V. and M.P. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Ministry of Education, Youth and Sports of the Czech Republic—DKRVO (RP/CPS/2020/004); as well as with direct support of the European Regional Development Fund in the Research Centre of Advanced Mechatronic Systems project, project number CZ.02.1.01/0.0/0.0/16_019/0000867 within the Operational Programme Research, Development and Education.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors would like to thank the Ministry of Education, Youth and Sports of the Czech Republic for its direct support of this research through the project DKRVO (RP/CPS/2020/004), as well as the European Regional Development Fund in the Research Centre of Advanced Mechatronic Systems for its financial support of this research through the project number CZ.02.1.01/0.0/0.0/16_019/0000867 within the Operational Programme of Research, Development, and Education. Authors would like to express their special thanks to Ing. T. Valenta, and D. Měřínská, (both from Faculty of Technology, Tomas Bata University in Zlin) for thermal measurements.

Conflicts of Interest

The authors declare that they have no conflict of interest.

References

  1. Shizok, K. Natural Rubber: From the Odyssey of the Hevea Tree to the Age of Transport, 1st ed.; A Smithers Group Company: Shawbury, UK, 2015; pp. 3–4. [Google Scholar]
  2. Gent, A.N.; Kawahara, S.; Zhao, J. Crystalization and strength of natural rubber and synthetic cis-1,4 polyisoprene. Rubber Chem. Technol. 1998, 71, 668–678. [Google Scholar] [CrossRef]
  3. Parrella, F.W.; Gaspari, A.A. Natural rubber latex protein reduction with an emphasis on enzyme treatment. Methods 2002, 27, 77–86. [Google Scholar] [CrossRef]
  4. Nie, Y.; Gu, Z.; Wei, Y.; Hao, T.; Zhou, Z. Features of strain-induced crystallization of natural rubber revealed by experiments and simulations. Polym. J. 2017, 49, 309–317. [Google Scholar] [CrossRef]
  5. Chenal, J.-M.; Gauthier, C.; Chazeaur, L.; Guy, L.; Bomaly, Y. Parameters governing strain induced crystallization in filled natural rubber. Polymer 2007, 48, 6893–6901. [Google Scholar] [CrossRef] [Green Version]
  6. Sarkawi, S.; Dierkes, W.K.; Noordermeer, J.W.M. Reinforcement of natural rubber by precipitated silica: The influence of processing temperature. Rubber Chem. Tech. 2014, 87, 103–119. [Google Scholar] [CrossRef] [Green Version]
  7. Morton, M. Rubber Technology, 3rd ed.; Springer Science+Business Media: Dordrech, OH, USA, 1999; pp. 30–47. [Google Scholar]
  8. Alan, N.G. Engineering with Rubber—How to Design Rubber Components, 3rd ed.; Hanscher Publischers: Ohio, OH, USA, 2012; pp. 18–20. [Google Scholar]
  9. Thomas, S.; Stephen, R. Rubber Nanocomposites Preparation, Properties and Applications, 1st ed.; John Wiley & Sons Pte Ltd.: Singapore, 2010; pp. 21–39. [Google Scholar]
  10. Hewitt, N. Compositeing Precipitated Silica in Elastomers, 1st ed.; William Andrew Publishing/Plastics Design Library: New York, NY, USA, 2007; pp. 1–9. [Google Scholar]
  11. Cassagnau, P. Melt rheology of organoclay and fumed silica nanocomposites. Polymer 2008, 49, 2183–2196. [Google Scholar] [CrossRef] [Green Version]
  12. Wilgis, T.A.; Heinrich, G.K. Reinforcement of Polymer Nano-Composites—Theory, Experiments and Applications, 1st ed.; Cambridge University Press: Cambridge, UK, 2009; pp. 96–100. [Google Scholar]
  13. Leung, S.N.; Wong, A.; Park, C.B.; Zhong, J.H. Ideal surface geometries of nucleating agents to enhance cell nucleation in polymeric foaming processes. J. Appl. Polym. Sci. 2008, 108, 3997–4003. [Google Scholar] [CrossRef]
  14. Arthur, H.L. Handbook of Plastics Foams, 1st ed.; Elsevier Books: Cambridge, UK, 1995; pp. 246–250. [Google Scholar]
  15. Nijib, N.N.; Ariff, Z.M.; Manan, N.A.; Bakar, A.A.; Sipaut, C.S. Effect of blowing agent concentration on cell morphology and impact properties of natural rubber foam. J. Phys. Sci. 2009, 20, 13–25. [Google Scholar]
  16. Gayathri, R.; Vasanthakumari, R.; Padmanabhan, C. Sound absorption, thermal and mechanical behavior of polyurethane foam modified with nano silica, nano clay and crumb rubber fillers. Int. J. Sci. Eng. Res. 2013, 4, 301–308. [Google Scholar]
  17. Pang, Y.; Cao, Y.; Zheng, W.; Park, C.B. A comprehensive review of cell structure variation and general rules for polymer microcellular foams. Chem. Eng. J. 2021, 430, 132662. [Google Scholar] [CrossRef]
  18. Park, C.B.; Baldwin, D.F.; Suh, N.P. Effect of the pressure drop rate on cell nucleation in continuous processing of microcellular polymers. Polym. Eng. Sci. 1995, 35, 432–440. [Google Scholar] [CrossRef]
  19. Bayat, H.; Fasihi, M.; Zare, Y.; Rhee, K.Y. An experimental study on one-step and two-step foaming of natural rubber/silica nanocomposites. Nanotechnol. Rev. 2020, 9, 427–435. [Google Scholar] [CrossRef]
  20. Sun, X.; Zhang, G.; Zhang, G.; Shi, Q.; Tang, B.; Wu, Z. Study on foaming water-swellable EPDM rubber. J. App. Polym. Sci. 2002, 84, 3712–3717. [Google Scholar] [CrossRef]
  21. Panploo, K.; Chalermsinsuwan, B.; Poompradus, S. Natural rubber latex foam with particulate fillers for carbon dioxide adsorption and regeneration. RSC Adv. 2019, 9, 28916–28923. [Google Scholar] [CrossRef] [Green Version]
  22. Sombatsompop, N.; Thongsang, S.; Markpin, T.; Wimolmala, E. Fly ash particles and precipitated silica as fillers in rubbers. I. Untreated fillers in natural rubber and styrene–butadiene rubber compounds. J. Appl. Polym. Sci. 2004, 93, 2119–2130. [Google Scholar] [CrossRef]
  23. Rodriguez-Vear, R.; Genovese, K.; Rayas, J.A.; Mendoza-Santoyo, F. Vibration Analysis at Microscale by Talbot Fringe Projection Method. Strain 2009, 45, 249–258. [Google Scholar] [CrossRef]
  24. Prasopdee, T.; Smitthipong, W. Effect of fillers on the recovery of rubber foam: From theory to applications. Polymer 2020, 12, 2745. [Google Scholar] [CrossRef]
  25. Rao, S.S. Mechanical Vibrations, 5th ed.; Pearson Education, Inc.: Upper Saddle River, NJ, USA, 2011; pp. 281–287. [Google Scholar]
  26. Carrella, A.; Brennan, M.J.; Waters, T.P.; Lopes, V., Jr. Force and displacement transmissibility of a nonlinear isolator with high-static-low-dynamic-stiffness. Int. J. Mech. Sci. 2012, 55, 22–29. [Google Scholar] [CrossRef]
  27. Liu, K.; Liu, J. The damped dynamic vibration absorbers: Revisited and next result. J. Sound Vib. 2005, 284, 1181–1189. [Google Scholar] [CrossRef]
  28. Stephen, N. On energy harvesting from ambient vibration. J. Sound Vib. 2006, 293, 409–425. [Google Scholar] [CrossRef] [Green Version]
  29. Vette, A.H.; Wu, N.; Masani, K.; Popovic, M.R. Low-intensity functional electrical stimulation can increase multidirectional trunk stiffness in able-bodied individuals during sitting. Med. Eng. Phys. 2015, 37, 777–782. [Google Scholar] [CrossRef] [PubMed]
  30. Sgard, F.; Castel, F.; Atalla, N. Use of a hybrid adaptive finite element/modal approach to assess the sound absorption of porous materials with meso-heterogeneities. Appl. Acoust. 2011, 72, 157–168. [Google Scholar] [CrossRef]
  31. Tiwari, W.; Shukla, A.; Bose, A. Acoustic properties of cenosphere reinforced cement and asphalt concrete. Appl. Acoust. 2004, 65, 263–275. [Google Scholar] [CrossRef]
  32. Okudaira, Y.; Kurihara, Y.; Ando, H.; Satoh, M.; Miyanami, K. Sound absorption measurements for evaluating dynamic physical properties of a powder bad. Powder Tech. 1993, 77, 39–48. [Google Scholar] [CrossRef]
  33. Yanagida, T.; Matchett, A.J.; Coulthard, J.M.; Asmar, B.N.; Langston, P.A.; Walters, J.K. Dynamic measurements for the stiffness of loosely packed powder beds. AIChE J. 2002, 48, 2510–2517. [Google Scholar] [CrossRef]
  34. International Organization for Standardization. ISO 10534-2, Acoustics-Determination of Sound Absorption Coefficient and Impedance in Impedance Tubes-Part 2: Transfer-Function Method; ISO/TC 43/SC2 Building Acoustics; CEN, European Committee for Standardization: Brussels, Belgium, 1998; pp. 10534–10542. [Google Scholar]
  35. Han, F.S.; Seiffert, G.; Zhao, Y.Y.; Gibbs, B. Acoustic absorption behaviour of an open-celled alluminium foam. J. Phys. D Appl. Phys. 2003, 36, 294–302. [Google Scholar] [CrossRef] [Green Version]
  36. Júnior, J.H.S.A.; Júnior, H.L.O.; Amico, S.C.; Amado, F.D.R. Study of hybrid intralaminate curaua/glass composites. Mater. Des. 2012, 42, 111–117. [Google Scholar] [CrossRef]
  37. Rajoria, H.; Jalili, N. Passive Vibration Damping Enhancement using Carbon Nanotube-epoxy Reinforced Composites. Compos. Sci. Tech. 2005, 65, 2079–2093. [Google Scholar] [CrossRef]
  38. Kalauni, K.; Pawar, S.J. A review on the taxonomy, factors associated with sound absorption and theoretical modeling of porous sound absorbing materials. J. Porous Mater. 2019, 26, 1795–1819. [Google Scholar] [CrossRef]
Figure 1. Time dependencies of vulcanization characteristics.
Figure 1. Time dependencies of vulcanization characteristics.
Materials 14 07450 g001
Figure 2. Time dependencies of pressure curves.
Figure 2. Time dependencies of pressure curves.
Materials 14 07450 g002
Figure 3. Time dependencies of rate of blowing.
Figure 3. Time dependencies of rate of blowing.
Materials 14 07450 g003
Figure 4. Optical microscopy images of the studied rubber samples.
Figure 4. Optical microscopy images of the studied rubber samples.
Materials 14 07450 g004
Figure 5. Effect of silica concentration on compression set of the investigated rubber composites under different compression temperatures.
Figure 5. Effect of silica concentration on compression set of the investigated rubber composites under different compression temperatures.
Materials 14 07450 g005
Figure 6. Effect of silica concentration on frequency dependencies of the displacement transmissibility of the tested rubber composites measuring t = 4 mm in thickness and loaded with inertial mass m = 90 g.
Figure 6. Effect of silica concentration on frequency dependencies of the displacement transmissibility of the tested rubber composites measuring t = 4 mm in thickness and loaded with inertial mass m = 90 g.
Materials 14 07450 g006
Figure 7. Frequency dependencies of the displacement transmissibility: (a) Rubber samples containing 20 phr of silica measuring t = 4 mm in thickness and loaded with different inertial masses; (b) rubber samples of various thicknesses containing 45 phr of silica and loaded with inertial mass m = 90 g.
Figure 7. Frequency dependencies of the displacement transmissibility: (a) Rubber samples containing 20 phr of silica measuring t = 4 mm in thickness and loaded with different inertial masses; (b) rubber samples of various thicknesses containing 45 phr of silica and loaded with inertial mass m = 90 g.
Materials 14 07450 g007
Figure 8. Frequency dependencies of the sound absorption coefficient of the silica powder for different loose powder bed heights.
Figure 8. Frequency dependencies of the sound absorption coefficient of the silica powder for different loose powder bed heights.
Materials 14 07450 g008
Figure 9. Frequency dependencies of the sound absorption coefficient: (a) Rubber samples measuring t = 12 mm in thickness at different concentrations of silica filler; (b) rubber samples of various thicknesses with 30 phr of silica filler.
Figure 9. Frequency dependencies of the sound absorption coefficient: (a) Rubber samples measuring t = 12 mm in thickness at different concentrations of silica filler; (b) rubber samples of various thicknesses with 30 phr of silica filler.
Materials 14 07450 g009
Figure 10. Effect of silica concentration on thermal conductivity of the tested rubber composites.
Figure 10. Effect of silica concentration on thermal conductivity of the tested rubber composites.
Materials 14 07450 g010
Figure 11. Thermogravimetric analysis results of the studied silica/rubber composites.
Figure 11. Thermogravimetric analysis results of the studied silica/rubber composites.
Materials 14 07450 g011
Table 1. Recipe of the investigated rubber compounds.
Table 1. Recipe of the investigated rubber compounds.
IngredientsRubber Designation
S0S10S20S30S45
Loading (phr)
SMR–20100100100100100
Silika KS–408010203045
ZnO22222
Vulkanox 402011111
Porofor ADC55555
Nyflex 2281010101010
Stearic acid11111
TBBS11111
Sulphur OT3322222
Table 2. Curing parameters of the studied rubber composites.
Table 2. Curing parameters of the studied rubber composites.
Rubber
Type
MH
[dN·m]
ML
[dN·m]
ts1
[min]
t90
[min]
S01.670.200.541.76
S102.450.370.571.73
S202.670.411.092.31
S305.281.030.873.36
S457.143.370.313.54
Table 3. Values of rebound resilience of the tested rubber composites.
Table 3. Values of rebound resilience of the tested rubber composites.
Rubber
Type
Resilience
[%]
S051 ± 1
S1048 ± 1
S2044 ± 1
S3041 ± 1
S4535 ± 1
Table 4. First resonance frequency (fR1) in Hz of the studied rubber composites as induced by harmonic force vibration depending on rubber thickness (t) and inertial mass (m).
Table 4. First resonance frequency (fR1) in Hz of the studied rubber composites as induced by harmonic force vibration depending on rubber thickness (t) and inertial mass (m).
Rubber
Type
t
[mm]
m [g]
090500
S04399 ± 13218 ± 10100 ± 5
8192 ± 8115 ± 562 ± 3
12176 ± 680 ± 355 ± 2
S104417 ± 15251 ± 11106 ± 4
8235 ± 10122 ± 470 ± 3
12220 ± 9103 ± 459 ± 2
S204434 ± 14279 ± 12120 ± 5
8294 ± 12178 ± 677 ± 3
12257 ± 11146 ± 473 ± 3
S304525 ± 15468 ± 18196 ± 6
8436 ± 16343 ± 11140 ± 4
12396 ± 13278 ± 9119 ± 4
S4541239 ± 25721 ± 20284 ± 9
8804 ± 19548 ± 15201 ± 7
12545 ± 14457 ± 12154 ± 5
Table 5. Results of measured and calculated acoustical and mechanical quantities for different loose powder bed heights of the applied silica filler.
Table 5. Results of measured and calculated acoustical and mechanical quantities for different loose powder bed heights of the applied silica filler.
Quantityh [mm]
1015203040
NRC [–]0.2590.3590.3020.4580.384
fp1 [Hz]696480364244184
αfp1 [–]0.7090.8540.9110.8790.784
c [m·s−1]27.828.829.129.329.4
K [MPa]0.1320.1410.1440.1460.147
Table 6. Values of noise reduction coefficient (NRC) of the studied rubber composites.
Table 6. Values of noise reduction coefficient (NRC) of the studied rubber composites.
Rubber
Type
t [mm]
4812
S00.0860.1130.182
S100.0660.1070.158
S200.0650.0980.110
S300.0470.0670.084
S450.0280.0300.037
Table 7. Values of weight loss (∆m) of the investigated rubber composites containing different silica concentrations in the temperature range of 30 to 500 °C as the results of thermogravimetric analysis.
Table 7. Values of weight loss (∆m) of the investigated rubber composites containing different silica concentrations in the temperature range of 30 to 500 °C as the results of thermogravimetric analysis.
Rubber
Type
m
[% w/w]
S090.42 ± 0.40
S1083.29 ± 0.53
S2079.34 ± 0.43
S3073.33 ± 0.58
S4566.63 ± 0.83
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Pöschl, M.; Vašina, M. Study of the Mechanical, Sound Absorption and Thermal Properties of Cellular Rubber Composites Filled with a Silica Nanofiller. Materials 2021, 14, 7450. https://doi.org/10.3390/ma14237450

AMA Style

Pöschl M, Vašina M. Study of the Mechanical, Sound Absorption and Thermal Properties of Cellular Rubber Composites Filled with a Silica Nanofiller. Materials. 2021; 14(23):7450. https://doi.org/10.3390/ma14237450

Chicago/Turabian Style

Pöschl, Marek, and Martin Vašina. 2021. "Study of the Mechanical, Sound Absorption and Thermal Properties of Cellular Rubber Composites Filled with a Silica Nanofiller" Materials 14, no. 23: 7450. https://doi.org/10.3390/ma14237450

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.