Next Article in Journal
Contribution of Second-Shell Residues to PLP-Dependent Transaminase Catalysis: A Case Study of D-Amino Acid Transaminase from Desulfomonile tiedjei
Next Article in Special Issue
Choline Acetate-, L-Carnitine- and L-Proline-Based Deep Eutectic Solvents: A Comparison of Their Physicochemical and Thermal Properties in Relation to the Nature and Molar Ratios of HBAs and HBDs
Previous Article in Journal
Integrated Multilayer Omics Reveals the Underlying Mechanisms in Xylazine-Related Heart Injury in Rats
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Dual Effects of In Situ Coal Combustion on CaO Pellets for CO2 Capture: High-Temperature Sintering and Ash Stabilization

State Key Laboratory of Coal Combustion, School of Power and Engineering, Huazhong University of Science and Technology, Wuhan 430074, China
*
Author to whom correspondence should be addressed.
Int. J. Mol. Sci. 2025, 26(17), 8535; https://doi.org/10.3390/ijms26178535
Submission received: 1 August 2025 / Revised: 31 August 2025 / Accepted: 2 September 2025 / Published: 2 September 2025

Abstract

High-temperature CaO-based CO2 capture technology, energized by in situ coal combustion, exhibits substantial promise owing to its high energy efficiency, strong compatibility, and maturity. However, sorbent deactivation mechanisms under complex coal combustion conditions, particularly for industrially required pelletized sorbents, are unclear. Pelletized sorbents were co-fired with four representative coals (differing in Na-K, S, and Al-Si content) in this study. Key factors were decoupled, and two competing mechanisms were revealed: (1) High-temperature sintering deactivation: Single co-firing triggers localized overheating (>900 °C), causing severe sintering and pore collapse. This reduces the specific surface area by 29% and pore volume by 50%, occludes meso-/macropores, and leads to a significant drop in initial CO2 capture capacity to 0.266–0.297 g/g. Coal types and minor residual surface impurities (<1.7%) are secondary factors. (2) Si-Al ash stabilization: During repeated co-firing (1–9 cycles), Si-Al ash components enrich on sorbents (0.1–7.6%), forming a thermally protective layer. After 20 adsorption–desorption cycles, the CO2 capture capacity loss drops from 17.6% to 3.9%, improving cycle stability. These findings clarify these dual mechanisms, providing a theoretical basis for system optimization and highlighting precise control of the combustion temperature field as critical for industrial deployment.

1. Introduction

Fossil fuels will maintain dominance in the global energy structure for decades. Their combustion is the primary source of carbon emissions, necessitating urgent development of efficient CO2 capture technologies [1,2,3,4]. Calcium looping (CaL) technology utilizes the reversible reaction of calcium-based sorbents, offering a promising path for efficient, low-cost, and environmentally friendly CO2 capture [5,6,7,8]. As shown in Figure 1a, this process captures CO2 in a carbonator (CaO + CO2 → CaCO3, 650 °C) and decomposes CaCO3 in a calciner (CaCO3 → CaO + CO2, 800–900 °C) [9,10,11]. This high-temperature requirement creates significant energy demands [12,13]. Using coal oxy-combustion for direct energy supply to the calciner offers three key advantages: stronger system compatibility, superior technological maturity, and favorable overall economics [9,14,15]. While the process incurs an energy penalty, studies indicate that this can be mitigated via thermal integration. For instance, Yang et al. showed that in a 600 MW coal-fired power plant, integrating CaL with waste heat recovery limits the net efficiency loss to within 3.8 percentage points [16]. However, the complex coal combustion environment, including temperature fluctuations, harmful gas emissions, and coal ash deposition, can accelerate the sintering of adsorbents, thereby leading to a decrease in CO2 capture performance.
Prior work demonstrates that coal combustion accelerates sorbent deactivation via two pathways: physical thermal sintering and chemical degradation (Figure 1b). Physically, localized overheating and thermal gradients during combustion drive rapid thermal sintering, which collapses the pore structure critical for efficient CO2 diffusion and surface reactivity [17,18,19]. Chemically, inorganic components in coal trigger reactions, including liquid-phase sintering (via volatile Na/K forming low-melting eutectics) [20,21], sulfation (SO2 reacting to form thermodynamically stable CaSO4) [22,23], and aluminosilicate formation (Si/Al oxides reacting with CaO) [24,25,26]. However, the complex interplay of these mechanisms obscures the dominant deactivation pathways under realistic industrial conditions, thereby hindering targeted optimization of sorbents. Existing studies predominantly rely on single coal sources with fixed compositions, which fails to disentangle the relative contributions of distinct pollutants to sorbent degradation, thus impeding the clear identification of key deleterious factors. Moreover, the industrial deployment of CaL necessitates the use of shaped sorbents; however, research on their CO2 capture performance and mechanical stability under in situ coal combustion conditions remains scarce [27,28,29].
Four types of coal with distinctly different contents of alkali metals (Na, K), sulfur (S), and aluminum (Al)–silicon (Si) were innovatively employed in this work to disentangle the individual effects of distinct pollutants on sorbent performance, and the dominant pathways governing sorbent deactivation under in situ coal combustion conditions were thereby identified (Figure 1c). The base material used was a pre-optimized, 10% Zr-doped limestone-based pelletized sorbent, which has been demonstrated in previous studies to exhibit enhanced cyclic stability and superior CO2 capture capacity [30]. Simulated coal combustion conditions were reproduced in a laboratory muffle furnace environment (Figure 1d). Combined performance testing and microstructure characterization reveal a dual mechanism through which coal influences the sorbent pellets: high-temperature sintering leads to performance degradation, while Al-Si components in the coal ash enhance the CO2 capture stability and mechanical strength. These insights provide critical guidance for the targeted design of high-performance calcium-based sorbents and facilitate the practical deployment of CaL for large-scale CO2 capture.

2. Results

2.1. Performance After First Co-Firing

Coal-contaminated sorbent pellets with a diameter of 0.90 to 1.25 mm were successfully prepared. As shown in Figure 2a, after one cycle of co-firing with coal, the pellets retained an intact spherical shape with partial porous structures remaining on their surface. After 20 carbonation/calcination cycles, the pore structure collapsed, and significant agglomeration and adhesion occurred on the surface. Mechanical properties, a key indicator for engineering applications, were evaluated. Figure 2b shows that the compressive strength (Pc) follows a normal distribution. The average compressive strength ( P c ¯ ) values of pellets corresponding to the TC, XHS, SX, and DT coal types are comparable (0.316 to 0.354 MPa), indicating that the coal type has a small effect on mechanical strength. Changes in CO2 capture capacity (Cn) are presented in Figure 2c. Over 20 cycles, the Cn of all pellets decreased continuously, consistent with the pore deterioration observed via SEM characterization. The initial Cn of coal-blended pellets was significantly lower than that of the coal-free reference sample Zr10. For instance, TC (0.297 g/g), XHS (0.299 g/g), SX (0.266 g/g), and DT (0.277 g/g) showed a ~40% decrease relative to Zr10 (0.508 g/g), indicating that pretreatment via coal co-firing causes significant deterioration in capture performance. Figure 2d shows that the Cn loss (Ln) and cumulative Cn over 20 cycles fall within comparable ranges: 16.1% to 17.6% and 5.120 g/g to 5.676 g/g, respectively. Their standard deviations account for 0.102 and 0.046 of the mean values, with minor dispersion, further confirming that the coal type has a limited effect on CO2 capture performance.
EDS mapping was used to analyze the surface chemical environment of the pellets. As shown in Figure 2e, the surface environments of TC and SX, which exhibit the largest difference in cumulative Cn, were compared. TC had residual Si (0.1%) and Mg (0.4%) on its surface, and SX had residual Na-K (1.2%), Al-Si (0.3%), and S (0.1%). Notably, TC (a high-alkali coal) showed minimal residual Na and K, while XHS (a high-sulfur coal) also had little residual S on the surface. This indicates that the coal type is not the dominant factor controlling surface composition; instead, the actual residual depends on the co-firing process. Meanwhile, this trace residual (total content < 1.7%) is significantly lower than that in powder sorbent, attributed to the high resistance to impurity adhesion on pelletized particle surfaces and their strong protection of internal pores. Previous studies attributed performance degradation in powder sorbent primarily to impurities, but this work shows that the extremely low impurity residue on particle surfaces is far from sufficient to explain the ~40% performance attenuation observed.
Further analysis of pore structure evolution was conducted. As shown in Figure 2f, the fresh Zr10 sample had a specific surface area and pore volume of 15.75 m2/g and 0.12 m3/g, respectively, which are 1.4 and 2.0 times those of the coal-contaminated sample. The pore size distribution in Figure 2g indicates that Zr10 is rich in more mesopores (2 to 50 nm) and macropores (50 to 100 nm), which serve as key channels for CO2 adsorption and diffusion [31]. Occlusion of these channels directly leads to capture performance deterioration. Excluding the influence of trace impurities, localized overheating on particle surfaces induced by coal co-firing at up to 900 °C, which results in pore channel closure, is the critical mechanism underlying the decline in CO2 capture performance.

2.2. Performance After Multiple Co-Firings

The TC with the highest cumulative CO2 capture capacity was selected for multiple co-firing experiments to simulate the repeated use process of the sorbent. As shown in Figure 3a, the trend of Cn over 20 cycles changed significantly with the number of co-firing cycles. First, as the number of co-firing cycles increased from one to three, five, seven, and nine, the Cn in the initial cycle gradually decreased from 0.297 to 0.261, 0.234, 0.215, and 0.210 g/g, respectively. Obvious self-activation occurred in subsequent cycles, and the degree of self-activation increased with the number of co-firing cycles. This is because coal combustion exposes the sorbent to high temperatures, promoting the formation of a rigid interconnected hard framework inside the sorbent [32]. Therefore, this framework hindered CO2 diffusion in the initial cycles, preventing the CO2 capture capacity from reaching the maximum. In subsequent cycles, the formation and decomposition of CaCO3 facilitated the growth of an external soft framework, accelerating the carbonation rate and increasing CO2 capture capacity, thereby inducing the self-activation of the sorbent [33]. Further analysis was conducted on Ln and cumulative Cn. As shown in Figure 3b, the cumulative Cn slightly decreased from 5.676 to 5.053 g/g with the increase in the number of co-firing cycles. Ln gradually decreased from 17.6% to 12.4%, 6.6%, and 3.5% as the number of co-firing cycles increased from one to three, five, and seven, with a slight increase to 3.9% at the ninth cycle. This indicates that increasing the number of co-firing cycles slows down the decrease in Cn, improving cycle stability. Compressive strength was further evaluated, as shown in Figure 3c. With the increase in the number of co-firing cycles from one to three, five, and seven, the average strength rose from 0.343 MPa to 0.401, 0.442, and 0.492 MPa, respectively, before slightly decreasing to 0.486 MPa at nine cycles. This indicates that more co-firing cycles enhance compressive strength.
The dynamic characteristics of Cn were further evaluated by analyzing the rate change curve (Vn). As shown in Figure 3d, Vn exhibits a peak-shaped curve that first increases and then decreases. The rate equation theory based on discrete three-dimensional product islands indicates that CO2 adsorption by CaO is a typical gas–solid reaction controlled by a combination of chemical reaction and product layer diffusion, involving three stages: chemical reaction, transition, and product layer diffusion [34,35]. As the number of cycles increased from 1 to 10 and then to 20, the peaks of Vn for all samples first increased and then decreased, consistent with the self-activation phenomenon of Cn mentioned above. With the increase in the number of co-firing cycles, the dynamic curves of Vn and Cn over time for the 10th and 20th cycles increasingly overlapped, further indicating enhanced cycle stability.
EDS mapping was used to analyze the effect of co-firing cycles on the surface chemical environment of sorbent pellets. As shown in Figure 4a, significant changes in the surface chemical environment occurred after five co-firing cycles, particularly the surface agglomeration of Al- and Si-based oxides. Figure 4b–e show the element energy spectra and content comparison. The energy spectrum intensity of Al and Si elements increased significantly with the number of co-firing cycles, with their contents increasing from 0.1% in the first co-firing to 3.6% in the fifth and further to 7.6% in the ninth. The contents of alkali metals, S, and Mg remained below 1.7%. This is attributed to the fact that silico-aluminum oxides account for 52.68–90.82% of coal ash. Notably, unlike powdered sorbents, silico-aluminum oxides only adhere to the surface of sorbent pellets, without consuming active CaO components.
Furthermore, gray correlation analysis was performed to investigate the relationships between four influencing factors (number of co-firing cycles, representing high temperature; Al and Si; Na and K; and S) and three performance metrics (Cn, cycle stability, and Pc). As shown in Figure 4f–h, the number of co-firing cycles and Al-Si content exhibited strong correlations with the performance metrics. The negative correlation degrees of co-firing cycles and Al/Si content with cumulative Cn were 0.91 and 0.93; their positive correlation degrees with cycle stability were 0.80 and 0.79; and their positive correlation degrees with Pc were 0.91 and 0.93, respectively. Therefore, the content of Al and Si increases with the increase in the number of co-firing cycles, leading to a slight decrease in cumulative Cn, a significant improvement in cycle stability, and a certain enhancement in mechanical properties. It is worth noting that the main reason for the improved cycle stability is the agglomeration of high-temperature-resistant Si-Al oxides on the surface of sorbent pellets, which plays a role in retarding sintering.

3. Discussion

Single co-firing significantly degrades the CO2 capture performance of sorbent pellets. The key influencing factors are the sintering and pore structure collapse of sorbent pellets induced by localized overheating during coal combustion, with a minor correlation with changes in the surface chemical environment or coal types (Figure 5). To meet the requirement of repeated use in practical applications, multiple cycles of co-firing were conducted. It was found that the content of Al and Si on the surface gradually increases, forming a high-temperature-resistant protective layer and significantly improving cycle stability (Figure 5). Considering the competing effects of temperature-induced degradation and stability enhancement by aluminosilicate oxides, future research should prioritize identifying a critical temperature window. This window can balance sintering suppression and stability promotion, which will be achieved through fixed-bed breakthrough experiments. Such studies will provide a theoretical basis for the long-term operation of sorbents. Notably, while the high temperatures of coal combustion degrade sorbent performance, activation strategies such as steam treatment can effectively revitalize these materials [36,37].

4. Materials and Methods

4.1. Coal Selection

Four types of coal were selected as research objects: Tianchi coal, Xiheishan coal, Datong coal, and Shanxi coal. The coal samples were pulverized via grinding and sieved to collect coal pellets smaller than 100 μm. After drying at 60 °C, the samples for combustion were obtained. The proximate and ultimate analysis results of the four coals are presented in Table 1. Ultimate analysis results show that Shanxi coal has the highest S content, reaching 4.65 wt%, while the S contents of the other coal samples are all below 1.20 wt%. Coal ash was obtained using plasma low-temperature ashing technology at temperatures below 200 °C with the aim of minimizing the loss of volatile alkali metals (Na and K) in the coal. The ash composition was analyzed via X-ray fluorescence spectroscopy (XRF, Bruker, Bremen, Germany), and the results are given in Table 2. Tianchi coal and Xiheishan coal have relatively high alkali contents (calculated as Na2O and K2O), exceeding 5.39 wt%. Datong coal has the lowest alkali content at 1.40 wt%, while Shanxi coal has a slightly higher alkali content of 2.76 wt%. Meanwhile, the content of silico-aluminum oxides is relatively low in Tianchi coal (52.48 wt%), whereas that in all the other coals exceeds 75.89 wt%.

4.2. In Situ Coal Combustion Simulation

First, pulverized coal was mechanically mixed with pelletized, Zr-loaded, limestone-derived sorbents (from previous work) at a specific ratio. The mixed samples were then placed in a muffle furnace and calcined at 900 °C for 2 h in an air atmosphere to simulate in situ coal calcination conditions. As shown in Figure 1d, after calcination, pelletized, limestone-derived sorbents with coal ash adhered to their surfaces were obtained, with a uniform particle size distribution of 0.9–1.25 mm. Sorbent pellets contaminated by Tianchi coal, Xiheishan coal, Datong coal, and Shanxi coal are designated as TC, XHS, DT, and SX, respectively. Multiple co-firing cycles involved re-adding coal followed by repeated calcination. Sorbent pellets after the third, fifth, seventh, and ninth calcination cycles were selected to investigate their CO2 capture performance. Under theoretical conditions, all heat released from complete coal combustion is used for the thermal decomposition of CaCO3. The formula for calculating the required coal mass is as follows:
m coal m CaCO 3 = H M CaCO 3 × 1000 Q
where m coal and m CaCO 3 are the masses of coal and the pelletized sorbent (converted to calcium carbonate), respectively, kg; ∆H is the heat absorption for the decomposition of 1 mol of CaCO3, 178 kJ/mol; M CaCO 3 is the molar mass of CaCO3, 100 g/mol; and Q is the low calorific value of coal, kJ/kg. The calculated mass ratios of added Tianchi coal, Xiheishan coal, Dadong coal, and Shanxi coal were 8.4 wt%, 10.4 wt%, 7.5 wt%, and 9.2 wt%, respectively.

4.3. CO2 Capture Capacity Testing

CO2 capture performance tests were conducted on a simultaneous thermal analyzer (STA 449 F5 Jupiter, NETZSCH, Selb, Germany), which enables simultaneous acquisition of mass and heat flow data for materials in a single test. Each sample underwent 20 cycles of carbonation (650 °C, 15 vol% CO2, 30 min) and calcination (850 °C, 100 vol% N2, 5 min), with N2 as the balance gas. The heating and cooling rates were 20 °C/min. Performance evaluation metrics included the CO2 capture capacity ( C n , g CO2/g sorbent), CO2 capture capacity loss ( L n , %), and CO2 adsorption rate ( V n , g CO2 g−1 sorbent min−1). The specific calculation formulas are as follows:
C n = m car , n m cal , n m cal , n   ×   100 %  
V n = d C n ( t ) dt
L n = C max C n C max × 100 %
where m car , n and m cal , n are the masses of the sample during the nth carbonation and calcination cycles, respectively, g; t is the carbonation time, min; C n ( t ) is the time-dependent C n , g/g; and L n is the percentage loss of the nth cycle C n relative to the maximum C n ( C max ), %.

4.4. Mechanical Property Testing

Mechanical properties were tested using a precision pressure testing machine (DL5 type intelligent particle strength tester, Dalian chemical engineering research and design institute, China), with the metric being the maximum compressive strength at particle breakage ( P c , i , MPa). P c , i is defined as the ratio of the maximum breaking force ( F max ) to the average cross-sectional area of the particle. Ten sorbent pellets with a particle size of 0.9–1.25 mm were subjected to breakage resistance tests. The average compressive strength ( P c ¯ ) is calculated as follows:
P c , i = F max π r 2
P c ¯ = i = 1 n P c , i / n
where F max is the maximum force required to crush a single particle, N, and r is the average radius of the CaO pellets, mm.

4.5. Gray Relational Analysis

First, dimensionless processing is performed on the data sequence of each factor. After processing, dimensionless data (such as x C n and x f a c t o r s in the formula) are obtained, which normalizes the values of different factors in proportion to facilitate subsequent comparison.
C n f a c t o r s ( t ) = x C n t x f a c t o r s t , t = 1,2 , 3
Next, the deviation sequence is calculated to quantify the differences between the reference sequences and the factor sequences. The reference sequences correspond to the target performance metrics of interest, namely, three items: Cn, cycling stability, and Pc. The factor sequences are the comparison sequences, namely, five items: co-firing times, Na-K, Al-Si, Mg, and S. Then, the global maximum deviation m a x and global minimum deviation m a x are identified.
m a x = m a x f a c t o r s ( m a x t x C n t x f a c t o r s t )
m i n = m i n f a c t o r s ( m i n t x C n t x f a c t o r s t )
The gray relational coefficients are then computed using the Formula (9). ρ is the resolution coefficient, typically set to 0.5.
ξ C n f a c t o r s ( t ) = m i n + ρ m a x C n f a c t o r s ( t ) + ρ m a x
Finally, the gray relational degree is computed to represent the overall correlation between a factor sequence and the reference sequences. The average of the gray relational coefficients across all points t is taken.
γ C n f a c t o r s = 1 / 3 t = 1 3 ξ C n f a c t o r s ( t )

4.6. Characterization

Semi-quantitative analysis was conducted with X-ray fluorescence (XRF, Bruker, Germany). The surface microtopography of samples before and after cycling was characterized using a Phenom Star benchtop scanning electron microscope (SEM, Phenom Star benchtop, Eindhoven, The Netherlands) operated at a 3 kV accelerating voltage. The elemental composition and distribution within samples were ascertained via energy-dispersive X-ray spectroscopy (EDX). The specific surface area and pore volumes were determined using a N2 adsorption-desorption analyzer (Micromeritics ASAP2020, Norcross, GA, USA), applying the Brunauer-Emmett-Teller (BET) method for surface area and the Barrett-Joyner-Halenda (BJH) method for pore volume calculations.

5. Conclusions

In this work, four coals representing three key compositional groups (alkali metals, sulfur, and Al/Si) were selected to explore the mechanisms governing the effects of single and multiple co-firing cycles between coal and pelletized sorbents. Single co-firing triggered particle sintering and pore collapse due to localized combustion overheating (900 °C), leading to a 29% reduction in the specific surface area and a 50% decrease in pore volume. Closure of mesopore/macropore channels caused a notable drop in initial CO2 capture capacity to 0.266–0.299 g/g. Importantly, neither trace surface impurity residues (<1.7%) nor differences in the coal type were primary causes of performance degradation. During multiple co-firing cycles, Al-Si oxides gradually accumulated on sorbent surfaces (rising from 0.1% to 7.6% after one to nine cycles), forming a high-temperature-resistant protective layer. This led to significant improvements in cyclic stability, with the CO2 capture capacity loss decreasing from 17.6% to 3.9% over 20 cycles. Thus, in situ coal combustion exerts dual effects on adsorbent particles: degradation induced by high-temperature sintering and cyclic stability enhanced by Si-Al components in the ash.

Author Contributions

Conceptualization, Y.L. and Z.Z.; Methodology, Y.L.; Software, R.X.; Validation, Y.L., C.W. and P.Z.; Formal Analysis, C.W. and P.Z.; Investigation, Y.L.; Resources, L.L.; Data Curation, R.X.; Writing—Original Draft Preparation, Y.L.; Writing—Review and Editing, C.W. and Z.Z.; Visualization, L.L.; Supervision, Z.Z. and M.X.; Project Administration, Z.Z.; Funding Acquisition, M.X. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the following funding sources: Natural Science Foundation of Wuhan (2023020201010045); Special Funds for Local Scientific and Technological Development by the Central Government of China (Hubei, 2024CSA088); and Huazhong University of Science and Technology Independent Innovation Research Fund (2025JYCXJJ046).

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Haszeldine, R.S. Carbon capture and storage: How green can black be? Science 2009, 325, 1647. [Google Scholar] [CrossRef]
  2. Kuramochi, T.; Ramírez, A.; Turkenburg, W.; Faaij, A. Comparative assessment of CO2 capture technologies for carbon-intensive industrial processes. Prog. Energy Combust. Sci. 2012, 38, 87. [Google Scholar] [CrossRef]
  3. Bui, M.; Adjiman, C.S.; Bardow, A.; Anthony, E.J.; Boston, A.; Brown, S.; Fennell, P.S.; Fuss, S.; Galindo, A.; Hackett, L.A. Carbon capture and storage (CCS): The way forward. Energy Environ. Sci. 2018, 11, 1062. [Google Scholar] [CrossRef]
  4. Deng, Z.; Zhu, B.; Davis, S.J.; Ciais, P.; Guan, D.; Gong, P.; Liu, Z. Global carbon emissions and decarbonization in 2024. Nat. Rev. Earth Environ. 2025, 6, 231. [Google Scholar] [CrossRef]
  5. Blamey, J.; Anthony, E.; Wang, J.; Fennell, P. The calcium looping cycle for large-scale CO2 capture. Prog. Energy Combust. Sci. 2010, 36, 260. [Google Scholar] [CrossRef]
  6. Witoon, T.; Mungcharoen, T.; Limtrakul, J. Biotemplated synthesis of highly stable calcium-based sorbents for CO2 capture via a precipitation method. Appl. Energy 2014, 118, 32. [Google Scholar] [CrossRef]
  7. Chen, J.; Duan, L.; Sun, Z. Review on the development of sorbents for calcium looping. Energy Fuels 2020, 34, 7806. [Google Scholar] [CrossRef]
  8. Zhou, L.; Duan, L.; Anthony, E.J. A calcium looping process for simultaneous CO2 capture and peak shaving in a coal-fired power plant. Appl. Energy 2019, 235, 480. [Google Scholar] [CrossRef]
  9. Perejón, A.; Romeo, L.M.; Lara, Y.; Lisbona, P.; Martínez, A.; Valverde, J.M. The Calcium-Looping technology for CO2 capture: On the important roles of energy integration and sorbent behavior. Appl. Energy 2016, 162, 787. [Google Scholar] [CrossRef]
  10. Armutlulu, A.; Naeem, M.A.; Liu, H.J.; Kim, S.M.; Kierzkowska, A.; Fedorov, A.; Müller, C.R. Multishelled CaO Microspheres Stabilized by Atomic Layer Deposition of Al2O3 for Enhanced CO2 Capture Performance. Adv. Mater. 2017, 29, 1702896. [Google Scholar] [CrossRef]
  11. Li, Z.; Fang, F.; Tang, X.; Cai, N.S. Effect of temperature on the carbonation reaction of CaO with CO2. Energy Fuels 2012, 26, 2473. [Google Scholar] [CrossRef]
  12. Ortiz, C.; Valverde, J.; Chacartegui, R.; Benítez-Guerrero, M.; Perejón, A.; Romeo, L. The Oxy-CaL process: A novel CO2 capture system by integrating partial oxy-combustion with the Calcium-Looping process. Appl. Energy 2017, 196, 1–17. [Google Scholar] [CrossRef]
  13. Wang, W.; Ramkumar, S.; Fan, L.-S. Energy penalty of CO2 capture for the carbonation-calcination Reaction (CCR) Process: Parametric effects and comparisons with alternative processes. Fuel 2013, 104, 561. [Google Scholar] [CrossRef]
  14. He, D.; Pu, G.; Qin, C.; Gong, R.; Tan, L.; Ran, J. Impacts and action mechanism of coal ash on CaO-based sorbents for CO2 capture under an oxy-fuel calcination environment. Ind. Eng. Chem. Res. 2017, 56, 15143. [Google Scholar] [CrossRef]
  15. Hughes, R.W.; Macchi, A.; Lu, D.Y.; Anthony, E.J. Changes in Limestone Sorbent Morphology during CaO-CaCO3 Looping at Pilot Scale. Chem. Eng. Technol. 2009, 32, 425. [Google Scholar] [CrossRef]
  16. Rolfe, A.; Huang, Y.; Haaf, M.; Rezvani, S.; MclIveen-Wright, D.; Hewitt, N. Integration of the calcium carbonate looping process into an existing pulverized coal-fired power plant for CO2 capture: Techno-economic and environmental evaluation. Appl. Energy 2018, 222, 169. [Google Scholar] [CrossRef]
  17. Chen, L.; Qian, N. The effects of water vapor and coal ash on the carbonation behavior of CaO-sorbent supported by γ-Al2O3 for CO2 capture. Fuel Process. Technol. 2018, 177, 200. [Google Scholar] [CrossRef]
  18. Soleimanisalim, A.H.; Sedghkerdar, M.H.; Karami, D.; Mahinpey, N. Pelletizing and coating of synthetic zirconia stabilized calcium-based sorbents for application in calcium looping CO2 capture. Ind. Eng. Chem. Res. 2017, 56, 5395. [Google Scholar] [CrossRef]
  19. Sun, J.; Liang, C.; Tong, X.; Guo, Y.; Li, W.; Zhao, C.; Zhang, J.; Lu, P. Evaluation of high-temperature CO2 capture performance of cellulose-templated CaO-based pellets. Fuel 2019, 239, 1046. [Google Scholar] [CrossRef]
  20. Sun, J.; Liu, W.; Hu, Y.; Wu, J.; Li, M.; Yang, X.; Wang, W.; Xu, M. Enhanced performance of extruded-spheronized carbide slag pellets for high temperature CO2 capture. Chem. Eng. J. 2016, 285, 293. [Google Scholar] [CrossRef]
  21. Werther, J.; Saenger, M.; Hartge, E.U.; Ogada, T.; Siagi, Z. Combustion of agricultural residues. Prog. Energy Combust. Sci. 2000, 26, 1–27. [Google Scholar] [CrossRef]
  22. Li, Z.; Wang, Y.; Li, Z.; Li, M.; Xu, K.; Liu, W.; Luo, G.; Yao, H. Limestone decomposition in an O2/CO2/steam atmosphere integrated with coal combustion. Energy Fuels 2016, 30, 5092. [Google Scholar] [CrossRef]
  23. Luo, C.; Zheng, Y.; Yin, J.J.; Qin, C.L.; Ding, N.; Zheng, C.G.; Feng, B. Effect of Sulfation during Oxy-Fuel Calcination Stage in Calcium Looping on CO2 Capture Performance of CaO-Based Sorbents. Energy Fuels 2013, 27, 1008. [Google Scholar] [CrossRef]
  24. Chen, H.; Khalili, N. Fly-ash-modified calcium-based sorbents tailored to CO2 capture. Ind. Eng. Chem. Res. 2017, 56, 1888. [Google Scholar] [CrossRef]
  25. Chen, H.; Wang, F.; Zhao, C.; Khalili, N. The effect of fly ash on reactivity of calcium based sorbents for CO2 capture. Chem. Eng. J. 2017, 309, 725. [Google Scholar] [CrossRef]
  26. He, D.; Qin, C.; Manovic, V.; Ran, J.; Feng, B. Study on the interaction between CaO-based sorbents and coal ash in calcium looping process. Fuel Process. Technol. 2017, 156, 339. [Google Scholar] [CrossRef]
  27. Alonso, M.; Arias, B.; Fernández, J.R.; Bughin, O.; Abanades, C. Measuring attrition properties of calcium looping materials in a 30 kW pilot plant. Powder Technol. 2018, 336, 273. [Google Scholar] [CrossRef]
  28. Sun, Z.; Sedghkerdar, M.H.; Saayman, J.; Mahinpey, N.; Ellis, N.; Zhao, D.; Kaliaguine, S. A Facile fabrication of mesoporous core–shell CaO-Based pellets with enhanced reactive stability and resistance to attrition in cyclic CO2 capture. J. Mater. Chem. A 2014, 2, 16577. [Google Scholar] [CrossRef]
  29. Sun, J.; Liu, W.; Hu, Y.; Li, M.; Yang, X.; Zhang, Y.; Xu, M. Structurally improved, core-in-shell, CaO-based sorbent pellets for CO2 capture. Energy Fuels 2015, 29, 6636. [Google Scholar] [CrossRef]
  30. Wang, C.; Liu, L.; Long, Y.; Zhou, Z.; Sun, J.; Liu, W.; Xu, M. Comparative investigation on CO2 uptake performance of limestone-derived sorbents with different supports synthesized by impregnated layer solution combustion method. Sep. Purif. Technol. 2024, 332, 125737. [Google Scholar] [CrossRef]
  31. Sun, J.; Liu, W.; Chen, H.; Zhang, Y.; Hu, Y.; Wang, W.; Li, X.; Xu, M. Stabilized CO2 capture performance of extruded-spheronized CaO-based pellets by microalgae templating. Proc. Combust. Inst. 2017, 36, 3977. [Google Scholar] [CrossRef]
  32. Kong, P.; Sun, J.; Li, K.; Jiang, L.; Sun, R.; Zhang, T.; Zhou, Z. Insight into the deactivation mechanism of CaO-based CO2 sorbent under in-situ coal combustion. Sep. Purif. Technol. 2024, 346, 127529. [Google Scholar] [CrossRef]
  33. Xu, R.; Sun, J.; Zhang, X.; Jiang, L.; Zhou, Z.; Zhu, L.; Zhu, J.; Tong, X.; Zhao, C. Strengthening performance of Al-stabilized, CaO-based CO2 sorbent pellets by the combination of impregnated layer solution combustion and graphite-moulding. Sep. Purif. Technol. 2023, 315, 123757. [Google Scholar] [CrossRef]
  34. Li, Z. General rate equation theory for gas-solid reaction kinetics and its application to CaO carbonation. Chem. Eng. Sci. 2020, 227, 115902. [Google Scholar] [CrossRef]
  35. Li, Z.; Sun, H.; Cai, N. Rate equation theory for the carbonation reaction of CaO with CO2. Energy Fuels 2012, 26, 4607. [Google Scholar] [CrossRef]
  36. Li, Z.; Liu, Y.; Cai, N. Understanding the enhancement effect of high-temperature steam on the carbonation reaction of CaO with CO2. Fuel 2014, 127, 88. [Google Scholar] [CrossRef]
  37. Bu, C.; Gómez-Barea, A.; Leckner, B.; Wang, X.; Zhang, J.; Piao, G. The effect of H2O on the oxy-fuel combustion of a bituminous coal char particle in a fluidized bed: Experiment and modeling. Combust. Flame 2020, 218, 42. [Google Scholar] [CrossRef]
Figure 1. Coal-integrated calcium looping system and experimental design. (a) Coal-powered calcium looping CO2 capture system. (b) Complex effects of coal combustion on calcium-based sorbents. (c) Inorganic component contents of representative coals. (d) Simulation of in situ coal combustion process.
Figure 1. Coal-integrated calcium looping system and experimental design. (a) Coal-powered calcium looping CO2 capture system. (b) Complex effects of coal combustion on calcium-based sorbents. (c) Inorganic component contents of representative coals. (d) Simulation of in situ coal combustion process.
Ijms 26 08535 g001
Figure 2. Single co-firing of coal and sorbent pellets. (a) Morphologies before and after cycling. (b) Mechanical strength. (c) Cn over 20 cycles. (d) Cn loss (Ln) and cumulative Cn over 20 cycles. (e) Inorganic component contents on TC and SX surfaces. (f) BET and BJH. (g) Pore size distribution.
Figure 2. Single co-firing of coal and sorbent pellets. (a) Morphologies before and after cycling. (b) Mechanical strength. (c) Cn over 20 cycles. (d) Cn loss (Ln) and cumulative Cn over 20 cycles. (e) Inorganic component contents on TC and SX surfaces. (f) BET and BJH. (g) Pore size distribution.
Ijms 26 08535 g002
Figure 3. Multiple co-firing of coal and sorbent pellets. (a) Cn over 20 cycles. (b) Cn loss (Ln) and cumulative Cn over 20 cycles. (c) Mechanical strength. (d) Cn (monotonic curve) and Vn (peaked curve) of the 1st, 10th, and 20th cycles.
Figure 3. Multiple co-firing of coal and sorbent pellets. (a) Cn over 20 cycles. (b) Cn loss (Ln) and cumulative Cn over 20 cycles. (c) Mechanical strength. (d) Cn (monotonic curve) and Vn (peaked curve) of the 1st, 10th, and 20th cycles.
Ijms 26 08535 g003
Figure 4. The 5th and 9th co-firing cycles. (a) SEM and EDS mapping for the 5th co-firing cycle. (b) Energy spectrum and (c) elemental contents for the 9th co-firing cycle. (d) Energy spectrum and (e) elemental contents. Gray relational analysis. (f) Cn vs. multiple factors. (g) Cyclic stability vs. multiple factors. (h) Mechanical strength vs. multiple factors.
Figure 4. The 5th and 9th co-firing cycles. (a) SEM and EDS mapping for the 5th co-firing cycle. (b) Energy spectrum and (c) elemental contents for the 9th co-firing cycle. (d) Energy spectrum and (e) elemental contents. Gray relational analysis. (f) Cn vs. multiple factors. (g) Cyclic stability vs. multiple factors. (h) Mechanical strength vs. multiple factors.
Ijms 26 08535 g004
Figure 5. Dual competing mechanisms: high-temperature sintering deactivation and Si-Al ash stabilization.
Figure 5. Dual competing mechanisms: high-temperature sintering deactivation and Si-Al ash stabilization.
Ijms 26 08535 g005
Table 1. Proximate and ultimate analyses of various coal samples (air-dried basis, wt%).
Table 1. Proximate and ultimate analyses of various coal samples (air-dried basis, wt%).
Proximate AnalysisUltimate AnalysisLow Calorific Value Q (kJ/kg)
MadVadAadFCadCadHadOadNadSad
Tianchi coal13.6233.9212.2240.2455.444.3738.570.551.0721,098
Xiheishan coal13.1526.9025.5334.4244.223.8850.960.540.4017,121
Datong coal2.1038.1027.2032.6075.004.6017.901.301.2023,862
Shanxi coal3.1416.5711.9568.3453.873.7736.840.874.6519,327
Mad stands for moisture content; Vad is volatile matter; Aad refers to ash content; FCad is fixed carbon; Cad denotes carbon content; Had is hydrogen content; Oad represents oxygen content (note: oxygen content is calculated according to the difference); Nad is nitrogen content; and Sad refers to sulfur content.
Table 2. XRF analysis results of low-temperature ash compositions of various coal samples (wt%).
Table 2. XRF analysis results of low-temperature ash compositions of various coal samples (wt%).
Na2OK2OMgOAl2O3SiO2P2O5ClCaOFe2O3
Tianchi coal6.900.752.7513.8238.861.181.1616.8317.74
Xiheishan coal3.741.653.9118.5457.351.150.744.908.03
Datong coal0.950.451.0435.4555.370.440.002.703.60
Shanxi coal1.731.031.5136.0951.650.470.003.893.62
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Long, Y.; Wang, C.; Xu, R.; Liu, L.; Zeng, P.; Zhou, Z.; Xu, M. Dual Effects of In Situ Coal Combustion on CaO Pellets for CO2 Capture: High-Temperature Sintering and Ash Stabilization. Int. J. Mol. Sci. 2025, 26, 8535. https://doi.org/10.3390/ijms26178535

AMA Style

Long Y, Wang C, Xu R, Liu L, Zeng P, Zhou Z, Xu M. Dual Effects of In Situ Coal Combustion on CaO Pellets for CO2 Capture: High-Temperature Sintering and Ash Stabilization. International Journal of Molecular Sciences. 2025; 26(17):8535. https://doi.org/10.3390/ijms26178535

Chicago/Turabian Style

Long, Yun, Changqing Wang, Ruichang Xu, Lei Liu, Pengxin Zeng, Zijian Zhou, and Minghou Xu. 2025. "Dual Effects of In Situ Coal Combustion on CaO Pellets for CO2 Capture: High-Temperature Sintering and Ash Stabilization" International Journal of Molecular Sciences 26, no. 17: 8535. https://doi.org/10.3390/ijms26178535

APA Style

Long, Y., Wang, C., Xu, R., Liu, L., Zeng, P., Zhou, Z., & Xu, M. (2025). Dual Effects of In Situ Coal Combustion on CaO Pellets for CO2 Capture: High-Temperature Sintering and Ash Stabilization. International Journal of Molecular Sciences, 26(17), 8535. https://doi.org/10.3390/ijms26178535

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop