Next Article in Journal
Grain Knowledge Graph Representation Learning: A New Paradigm for Microstructure-Property Prediction
Next Article in Special Issue
Basaltic Glass Fibers from Industrial Wastes: A Laboratory-Scale Technical Feasibility Study
Previous Article in Journal
Two Polynuclear Manganese(II) Complexes Based on Multidentate N-Heterocyclic Aromatic Ligand and V-Shaped Polycarboxylate Ligand: Synthesis, Crystal Structure Analysis and Magnetic Properties
Previous Article in Special Issue
Self-Assembled Nanocomposites and Nanostructures for Environmental and Energy Applications
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Modifying HKUST-1 Crystals for Selective Ethane Adsorption Using Ionic Liquids as Synthesis Media

by
Gregory S. Deyko
1,*,
Lev M. Glukhov
1,
Vera I. Isaeva
1,*,
Vladimir V. Chernyshev
2,3,
Vadim V. Vergun
1,
Danil A. Archipov
1,
Gennady I. Kapustin
1,
Olga P. Tkachenko
1,
Vera D. Nissenbaum
1 and
Leonid M. Kustov
1,3,*
1
N.D. Zelinsky Institute of Organic Chemistry, Russian Academy of Sciences, 47 Leninsky Prospect, 119991 Moscow, Russia
2
A.N. Frumkin Institute of Physical Chemistry and Electrochemistry, Russian Academy of Sciences, Building 4, 31 Leninsky Prospect, 119071 Moscow, Russia
3
Department of Chemistry, M.V. Lomonosov Moscow State University, 1-3 Leninskie Gory, 119991 Moscow, Russia
*
Authors to whom correspondence should be addressed.
Crystals 2022, 12(2), 279; https://doi.org/10.3390/cryst12020279
Submission received: 7 January 2022 / Revised: 12 February 2022 / Accepted: 16 February 2022 / Published: 18 February 2022

Abstract

:
Novel adsorbents for methane and ethane based on HKUST-1 metal-organic framework were synthesized by microwave (MW) assisted technique using ionic liquids (ILs) as synthesis media. It was found that the MW synthesis time remarkably impacts both the product yield and the physico-chemical characteristics of the produced HKUST-1 material. The crystalline phase purity, crystallite size/dispersion and textural properties of the synthesized HKUST-1 matrices determine their performance in methane and ethane adsorption. Therefore, the HKUST-1 material produced in MW fields for 3 min only shows the highest phase purity and the largest surface area (BET) and porosity, along with a rather small crystallite size (below ~300 nm), demonstrating high methane and ethane adsorption capacity in the pressure range 1–30 atm.

1. Introduction

Natural gas is the cleanest fuel among fossil-based resources [1]. It consists mainly of methane (>90%) and other hydrocarbons (mostly ethane, up to 10%). It is mainly used as a fuel in industry and households, as well as in internal combustion engines. However, the combustion of methane–ethane mixture is not an optimal method because ethane is a promising precursor in the petrochemical synthesis for producing a number of valuable products, such as plastics [2]. Therefore, more efficient methods for the separation of components of natural gas are demanded.
To date, methods for natural gas processing based on the cryoseparation techniques, which involve liquefaction of natural gas at high pressures and low temperatures (10–15 bar, 100 K), are used [3]. An alternate strategy, gas adsorption on porous materials, allows one to perform separation at room temperature and relatively low pressures (usually 0.1–5 bar) [4].
A novel type of hybrid nanoporous adsorbents, metal-organic frameworks (MOFs), are currently studied as promising materials for storage and separation of a large number of different gases [5]. MOF materials are crystalline coordination polymers composed of metal cations and polydentate organic molecules (linkers) [6]. Due to these unique properties, MOF matrices show a better configuration for the specific task (i.e., gas separation, catalysis, sensors) than their inorganic and carbon counterparts. In particular, the reason for adsorption/separation applications of MOFs is their record-high specific surface area and porosity, open-pore system, diverse chemical composition and tunable pore geometry and functionality [7].
A lot of efforts is devoted to the application of MOF materials in natural gas purification [8]. In particular, some methods are recognized as promising candidates for the separation of methane and ethane, i.e., HKUST-1 [9,10], SBMOF-1 and SBMOF-2 [11], DUT-49 [12], DUT-75 [12] and ZnSDB (isostructural analogue of SBMOF-1) [13]. For instance, DUT materials show the highest methane adsorption capacity [12], e.g., 240 mg/g for DUT-75 (90 atm, 298 K), and that of DUT-76 matrix is 308 mg/g under the same conditions, which is record-breaking today. However, most published works deal with single gas, methane or ethane, so it is rather problematic to evaluate the real separation performance of the reported MOF adsorbents due to different adsorption conditions in each cited work, e.g., pressure and temperature.
The HKUST-1 material is the most promising adsorbent known to date [12] for the purposes of separating natural gas components due to its high capacity for both methane and ethane, as well as the rather low cost of synthesis in comparison, for example, with the DUT-75 matrix.
HKUST-1 (Cu3(btc)2) metal-organic framework consists of Cu-Cu dimers, which are connected by benzene-1,3,5-tricarboxylate (btc) linkers to form a three-dimensional network with micropores in the range of 0.7–0.9 nm. Due to this structure, the HKUST-1 matrix features promising adsorption characteristics [13,14].
In particular, the HKUST-1 material shows the adsorption capacity of 4.5 mmol/g (1 MPa, 303K) [15] for methane and about 3.5 mmol/g (1 bar, 313 K) for ethane [16]. Note, this capacity value of HKUST-1 for methane meets the requirements of DOE (Department of Energy, Washington, DC, USA) for the capacity of solid sorbents relevant to their industrial use.
Currently, a number of different methods are proposed for the synthesis of the HKUST-1 material, i.e., solvothermal procedure [17,18], MW-assisted solvothermal technique using templates [19], solvent-free vacuum growth [20], mechanochemical method [21], etc. All these methods can significantly affect most physicochemical properties of the produced HKUST-1 material, such as crystallinity, surface area (BET), pore volume, morphology, etc. Therefore, the correct choice of synthesis procedure may be a key factor which has a serious impact on the gas separation performance of the HKUST-1 adsorbent.
The crystal size and dispersion of the MOF product are determined by an appropriate choice of synthesis procedure. It is well-established that efficient nanocrystal size control is a key factor governing the possibility of application of the material, including MOF matrices for the specific task [22]. Various procedures are used to tune both the size and morphology of MOF materials, but the modification of the solvent composition is one of the most convenient methods [23].
Conventional solvents for MOF formation include water, N,N-dimethylformamide (DMF), N,N-diethylformamide, dimethyl sulfoxide and N-methylpyrrolidone. In particular, the use of mixed solvents based on water or ethanol (e.g., DMF/ethanol and DMF/water) was found to influence crystal growth through solvent-induced effects [24].
Currently, ionic liquids (ILs) are proposed as alternatives to traditional organic solvents for the ionothermal synthesis of MOF materials [25,26]. Ionic liquids are molten salts with a melting point below 100 °C, consisting of organic cations (usually dialkylimidazolium or tetraalkylmmonium) and various organic or inorganic anions, such as acetate CH3COO, triflate CF3SO3, tetrafluoroborate BF4. In addition, ILs also feature versatility in choosing the cation and anion combination, highly tunable properties, high thermal stability, low vapor pressure and recyclability. The polar ILs provide a high solubility of both organic and inorganic reagents. In addition, the presence of cation and anion groups in the solvent can serve as charge compensating moieties during MOF synthesis [27]. Additionally, ILs are environmentally friendly solvents primarily due to their easy recovery.
In addition, using ILs as a solvent system makes it possible to reduce the MOF crystallite size efficiently. For instance, the use of ionic liquid microemulsions (ILMEs) is a relatively new technique for tuning the particle size distributions of MOFs [28].
Despite its advantages, ionothermal MOF synthesis usually requires a high temperature (>100 °C) and long reaction time (3–12 days) to overcome the high enthalpies of the product formation or account for the slow kinetics of nucleation [29]. To conquer these obstacles, it was proposed in [30] to utilize CO2 as an activator to promote HKUST-1 material crystallization as ultra-small nanoparticles (NPs) in 1-butyl-3-methylimidazolium tetrafluoroborate ([BMIM]BF4) at room temperature.
On the other hand, in the context of the efficient control of the morphology of MOF crystallites, MW-assisted synthesis shows particular potential. This technique is recognized as a promising strategy to efficiently manipulate the key physico-chemical characteristics of produced MOF materials [31,32,33].
MW-assisted synthesis using ILs as solvents is expected, under certain conditions, to provide enhanced physico-chemical properties of produced MOF materials. It is known that ILs are appropriate templates for microporous materials [34] and ideal microwave absorbers [35]. Furthermore, the heating rate in MW fields is significantly increased compared to traditional organic solvents since the ILs have a significantly higher ionic conductivity [36,37].
Recently, we reported the impact of MW-assisted synthesis in the H2O-DMF system at an atmospheric pressure using a household MW oven on the structural, compositional, morphological and textural characteristics of the produced HKUST-1 material and thereby on its performance in liquid phase adsorption [32].
This work presents an attempt to combine the “power” of MW-assisted synthesis and advantages of ILs as reaction media for the efficient control and improvement of the morphological and textural characteristics of the produced HKUST-1 material and thereby its behavior in methane and ethane adsorption. For this purpose, HKUST-1 materials were synthesized in ionic liquids via both MW technique and solvothermal procedure. Available alkylmethylimidazolium ILs with different alkyl groups, with triflate CF3SO3 (OTf) and bis(trifluoromethylsulfonyl)imide (CF3SO2)2N (Tf2N) anions, were chosen as IL components in order to probe the alkyl chain effect on the properties of the formed MOF materials. The anion choice was dictated by thermal stability and reactivity. ILs with halogen or carboxylate anions are not thermally stable enough, while inorganic fluorinated complex anions such as BF4 or PF6 may be prone to decomposition in the presence of metal ions involved in MOF synthesis with the formation of metal fluorides at an elevated temperature.
The HKUST-1 materials synthesized in an IL medium under MW and solvothermal conditions were comparatively studied in methane and ethane adsorption at low and elevated pressures. To the best of our knowledge, there are no publications on high-pressure ethane adsorption. Therefore, we report, for the first time, the data on the high-pressure (>20 bar) adsorption of ethane for the HKUST-1 material.

2. Materials and Methods

The main reagents, i.e., 1-ethyl-3-methylimidazolium chloride, 1-methylimidazole, n-butyl chloride, n-octyl chloride, benzene-1,3,5-tricarboxylic acid (H3btc), copper nitrate trihydrate, copper acetate monohydrate and lithium bis(trifluoromethylsulfonyl)imide, are commercial products (Acros). All solvents were purified via common methods before use.

2.1. Synthesis of Ionic Liquids

1-Butyl-3-methylimidazolium triflate (BMIM OTf), 1-octyl-3-methylimidazolium triflate (OMIM OTf) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (EMIM Tf2N) were synthesized via well-known procedures with slight modification [38]. BMIMCl and OMIMCl were prepared by alkylation of 1-methylimidazole with corresponding alkyl chlorides in acetonitrile. ILs with the triflate anion were synthesized by ion exchange from the corresponding alkylmethylimidazolium chlorides and potassium triflate in acetonitrile. Then, the crude products were dissolved in CH2Cl2, and the halide impurities were extracted with water until a negative reaction with silver nitrate was noted. The EMIMTf2N was prepared via ion exchange with lithium bis(trifluoromethylsulfonyl)imide in water–CH2Cl2 mixture. All obtained ionic liquids were dried in a vacuum at 80 °C for 6 h. The detailed procedures are provided in supplementary materials.

2.2. Synthesis of HKUST-1 Materials

Sample mw1 was synthesized according to the procedure reported in [32].
Sample solv1 was synthesized according to the procedure reported in [32].
Samples 3–8 were synthesized in IL media by a solvothermal method and in MW fields according to original procedures. Furthermore, when using ILs as a non-boiling solvent, it is crucial to effectively stir the reaction mixture to achieve homogenization of the reactant concentrations in the reaction volume.
The reagents (H3btc and Cu2+ source) were preliminarily thoroughly ground in an agate mortar. The exact amounts of reagents, type of solvent, reaction conditions and yields are presented in Table 1.
A conventional household inverter microwave oven Panasonic NN-GD366M with the standard frequency of 2450 MHz was used for microwave-assisted syntheses at a power setting of 200 W. The upper level of the liquid inside the glass reactor was 3 cm lower than the upper plane of the oven camera. The temperature of the solution was measured with a thermocouple immediately after turning off the microwave irradiation to prevent temperature measurement error.
Each reagent was mixed with ½ of a necessary volume of the selected solvent, and then the mixtures were combined in the reaction tube. The reaction mixture was stirred during microwave irradiation with a glass overhead stirrer. The exact reaction times are presented in Table 1.
The reaction mixture (both after solvothermal and MW syntheses) was diluted with ethanol (~20 mL). The product was separated by centrifugation and thoroughly washed with ethanol (3 × 30 mL). The obtained crystalline product was dried under a vacuum (RT, 2 h and 140 °C, 6 h).
To study the recyclability of ILs, the reaction mixture was diluted with ethanol after MW-synthesis, and the HKUST-1 product was centrifuged; the supernatant was collected and then rotary evaporated to remove ethanol. The residue was analyzed via NMR.

2.3. Material Characterization

The microstructure and morphology of the synthesized samples were studied by field emission scanning electron microscopy (FE SEM) with a Hitachi SU8000 field-emission instrument. The target-oriented approach was utilized for the optimization of the analytical measurements [38]. The images were recorded in the secondary electron mode at an accelerating voltage of 2 kV and a working distance of 5–6 mm. The morphology of the samples was studied with a correction applied to the surface effects of conduction layer sputtering. X-ray powder diffraction data were collected in a reflection mode using an EMPYREAN instrument (PANalytical, Malvern, UK) equipped with a linear X’celerator detector and non-monochromated Cu Kα radiation (α = 1.5418 Å), measurement parameters: tube voltage/current 40 kV/35 mA, divergence slits of 1/8 and 1/4°, 2θ range 4–40°, speed 0.2° min−1. Porous structure characteristics of the synthesized materials were obtained using a standard adsorption isotherm of N2 at 77 K measured using ASAP 2020 Plus instrument (Micromeritics). The specific surface area (BET) was calculated from the adsorption data over the relative pressure range between 0.05 and 0.20. The total pore volume (VΣ) was evaluated at p/po = 0.95, taking into account the asymptotic behavior of the isotherm at relative pressures approaching 1. The thickness of the adsorbed multilayer generally appears to increase without limit when p/po= 1. The cumulative volume at adsorption in the BJH method was taken as a mesopore volume (Vmeso).
1H NMR spectra were recorded using a Bruker AM300 instrument at a frequency of 300 MHz using deuterated DMSO-d6.
Thermogravimetric analysis was performed using a Derivatograph-C instrument (MOM Company, Budapest, Hungary). Diffuse–reflectance infrared Fourier-transform spectra (DRIFTS) were recorded at room temperature with a Nicolet 460 Protégé spectrometer equipped with a diffuse–reflectance attachment. The samples were placed in the ampoules with a KBr window. The CaF2 powder was used as a standard. For a satisfactory signal-to-noise ratio, 500 spectra were collected. The spectra were measured at ambient temperature in the range of 6000–750 cm−1 in 4 cm−1 steps. The IR spectra of ionic liquids (OMIM OTf and EMIM Tf2N) were collected with the same spectrometer in a transmission mode. The KF glass slide was used as a standard.

2.4. Gas Adsorption Experiments

Adsorption of methane and ethane was studied in a classic Sieverts-type apparatus [39]. Adsorption was calculated from pressure measurements over 12–16 points using high precision empirical equations of state for each gas [40,41]. The parameters of the equations of states and other experimental details are provided in the supplementary information. Before measurements, the samples were evacuated at 140°C directly in the setup for 4 h. The typical sample weight was 0.3–0.6 g; the volume of samples was measured via helium pycnometry at room temperature.

3. Results

3.1. Synthesis of HKUST-1 Material in the IL Medium

In order to optimize the reaction time, the heating rates of selected ionic liquids and the DMF–water (v/v) = 1:1 system as reaction media under MW radiation were evaluated (Figure S1 in the Supplementary Materials). Figure S1 show clearly that the heating rate of the BMIM OTf is rather constant along with a temperature increase until 300 °C, while the DMF–water mixture can be heated up to its boiling point (104 °C). The IL heating rate is much higher than that of the DMF–water system due to the ionic conductivity and lower heat capacity of the IL. Therefore, using ILs as solvent systems, the reaction time was decreased to 5 min to prevent possible overheating of the reaction mixture and the formation of impurity phases.
The effect of the synthesis time on the yield of the HKUST-1 material was evaluated. Figure S2 show the linear increase in the HKUST-1 yield along with time with a maximum of ~3 min under MW radiation. Prolonged heating leads to lower HKUST-1 yields (70% at 7 min). After 7 min of heating, the color of the reaction mixture turns from dark blue to black. However, after cooling to room temperature and diluting the reaction mixture with ethanol (20 mL), the color of the suspension soon turns back to dark blue.
Efficient utilization of ILs (as a reaction medium) dictates increasing concentrations of the reagents for HKUST-1 synthesis as compared to its synthesis in common solvents (e.g., 1solv sample) due to the rather higher cost of IL. It was found that the optimal IL solvent quantity (independently of its kind) in the reaction mixture was 10 mL.
A further increase in the volume of IL to 10 mL (Table 2, 5mw sample) led to an almost quantitative yield (99%). Therefore, the fast (3 min) synthesis of HKUST-1 proceeds in an economical way in terms of the solvent:reagents ratio, i.e., over 1 mol of reactants per 1 L of the solvent. Therefore, the optimal conditions for the HKUST-1 material synthesis in ILs are those described for the 5mw sample.
The 3solv and 2solv samples were prepared under solvothermal conditions using 5 mL of IL per 7 mmol of H3btc with yields of 40–50%, correspondingly. In more dilute systems (8solv sample), a HKUST-1 yield as high as 99% was achieved.
According to elemental analysis data (Table S1 in the Supplementary Materials), the synthesized HKUST-1 samples contain only trace amounts of ILs, except for 2solv and 3solv samples before extra-rinsing. Fluorine and nitrogen contents in these materials allow one to evaluate the presence of ILs cations and anions, correspondingly. In the 3solv and 2solv samples, the HKUST-1 matrix contains more anions than cations. However, extra-rinsing with DMF allows one to remove ILs almost completely from these materials affording 2solv-after-rinsing and 3solv-after-rinsing samples.
One of the main advantages of ILs over traditional organic solvents is the ease of purification via rotary evaporation due to the fact that ionic liquids are non-volatile. After the synthesis of sample 5mw under microwave conditions, the recyclability of the ionic liquid, e.g., OMIMOTf, was studied. Figure S3 show the comparison between the spectra of neat IL OMIMOTf and the IL recovered after MW synthesis. As can be seen, both spectra are almost identical, with the exception of two peaks corresponding to traces of ethanol, indicating the high thermal stability of IL under harsh synthesis conditions (microwave irradiation associated with a high temperature). Therefore, the proposed method allows one to easily reuse ionic liquids as the reaction media.

3.2. XRD Analysis of the HKUST-1 Material

The efficiency of the synthesis method was further justified by XRD data.
Powder diffraction patterns of all samples prove the presence of the HKUST-1 crystalline phase as the main phase.
A comparison of XRD patterns of the samples HKUST-1DMF-MW synthesized by the MW technique in DMF as a unique solvent and 1mw (Figure S4) clearly show discrepancies in the relative heights of small-angle peaks, thus indicating the differences in the content of the voids in both samples. The Pawley fitting also led to slightly different values of the cubic unit cell parameter a in HKUST-1DMF-MW and 1mw – 26.292(5) and 26.321(5) Å, respectively.
Note that the mixed solvent system, i.e., DMF-H2O, was selected in order to carry out this reaction in a more “green” way by reducing the content of toxic and rather expensive DMF in the synthesis medium.
Three samples, 5mw, 7mw and 8solv, synthesized in pure ILs, demonstrate no extra peaks from any additional phases (Figure 1).
At the same time, the other samples are not single-phase materials. For example, the 3solv material contains at least two additional crystalline phases. One of them is most probably copper oxalate hydrate with characteristic peaks at 2θ of 22.9 and 36.2° (its content is about 10%) and near 5% of unknown phase(s) with the peaks at 10.7, 12.6, 14.2, 27.4° and some other 2θ angles (Figure S5).
Additional rinsing of the 3solv sample, as a result of which 3solv-after-rinsing material was obtained, allowed one to reduce the content of the copper oxalate hydrate phase in the sample down to 3% and completely remove unknown phase(s) (Figure S6).
Additional rinsing of the sample 2solv also did not lead to single-phase sample 2solv-after-rinsing, whose XRD pattern (Figure S7) contains characteristic peaks of two crystalline side phases, copper oxalate hydrate (2θ 22.9°) and copper nitrate hydroxide (2θ 12.8, 25.8, 33.6°), with the total content of these side phases of about 4%.
Coming back to single-phase samples, 5mw, 7mw and 8solv, we should pay attention to the proximity of the values of their cubic unit cell parameter a (26.313(2), 26.314(2) and 26.304(2) Å, respectively) obtained in the Pawley fittings [42] performed with the program MRIA [43]. At the same time, it is worthy to note the essential difference in the heights of some low-angle peaks of 5mw (for example, at 2θ angles 6.8 and 15°, Figure 1) as compared with 7mw and 8solv. This difference is most probably related to the pore content, which, in turn, may impact the adsorption properties of these materials.
According to XRD results, the highest phase purity and crystallinity are observed for the samples 5mw and 8solv, synthesized in a more diluted IL solution using the same reaction mixture composition by MW and solvothermal technique, correspondingly.
It could be suggested that the optimal synthesis time for the HKUST-1 material under MW activation conditions is 3 min. Both synthesis time shortening (2 min) and increasing (7 min) result in the appearance of additional peaks on the XRD pattern of the corresponding 4mw and 6mw samples. In this case, the effect of the reaction time is accompanied by the effect of the more concentrated reaction mixture.
By comparing the XRD data for 5mw, 7mw and 8solv materials, it could be concluded that the reaction mixture composition, in particular, the IL content, has the dominating effect on the phase purity and crystallinity of the synthesized samples.
In order to study the possibility to produce the HKUST-1 material under scale-up conditions, it was synthesized using 10-fold quantities of the reagents as compared to the 1mw sample prepared using the MW technique in the DMF-H2O mixed solvent. XRD results (Figure S8) show that its structural characteristics are nearly identical to the structural characteristics of the 1mw sample.
To probe the stability of the HKUST-1 materials produced by different methods, the chemical stability of 1mw and 5mw, along with 3solv-after washing and 8solv materials, was studied by soaking them in water and methanol followed by the XRD measurements (Figures S9 and S10). It was found that these HKUST-1 samples produced by MW and solvothermal techniques retain their structural characteristics almost intact after contacting with these solvents (4 h, 22 °C).
These data confirmed the possibility of the practical implementation of the HKUST-1 based adsorbents synthesized by the described methods.

3.3. Morphology of the HKUST-1 Materials

The morphology of the synthesized HKUST-1 materials was studied by the SEM method. It was found that synthesis conditions, i.e., heating mode, solvent and reaction time, impact remarkably on the crystallite size. The 1mw material synthesized in MW fields in a DMF-H2O system shows the largest crystal size (~25 µm, Figure S11a) [32]. Note, the 1solv material obtained under solvothermal conditions in the DMF-H2O-EtOH system is composed of smaller crystallites (~8 µm, Figure S11b). Probably, the crystal growth rate prevails over the rate of nucleation under conditions of MW radiation.
According to the literature data [29] and this work’s results, microwave-assisted ionothermal synthesis is a more effective method for crystallization time shortening. The local superheating could facilitate the reagent conversion [21]. For instance, local superheating accelerated the crystallization of the ZIF-8 material under conditions of MW-assisted ionothermal synthesis [29].
Using IL as a synthesis medium results in particle size reduction both for solvothermal and MW samples. All materials synthesized in ILs are composed of crystallites with sizes varying in the range of 200–800 nm. This IL effect could be explained by preventing crystal growth by IL interacting with HKUST-1 crystallization sites [32].
Probably, in the case of the usage ILs as reaction medium for the HKUST-1 synthesis, they can act as surfactants [44] and capping agents. Therefore, anions and cations in their structures can bind with Cu2+ open sites and btc linkers (coordinated partially) in HKUST-1 nanoparticles preventing crystal growth in this manner. In addition, Cu(II) complexes with IL anions, such as Tf2N (which is a constituent of the 2solv and 7mw samples), are reported in [45].
Again, the dominating factor for the phase purity of the synthesized HKUST-1 materials is the IL content in the reaction mixture. Therefore, the HKUST-1 particle size is almost the same for 5mw (~290 nm) (Figure 2a) and 8solv (~360 nm) (Figure S12a) samples synthesized in a more diluted solution in MW fields and by the solvothermal technique. The 2solv-after-rinsing and 3solv-after-rinsing samples obtained in a more concentrated solution than the 8solv material have more than twice the crystallite size (Figure S12b,c).
In the case of MW synthesis, the reaction time is an additional factor. Therefore, the 4mw sample synthesized using BMIMOTf in MW fields in the shortest time period (~2 min) has the smallest particle size (~200 nm) (Figure 2b)). Probably, for the MW synthesis, a reaction time as short as 2 min is crucial for the dramatic reduction of the HKUST-1 crystal size. As a result, the 6mw material synthesized in the same IL (BMIMOTF) as the 4mw sample, but in a more concentrated reaction solution and for two-fold prolonged reaction time (5 min), has around a three-fold larger crystal size—750 nm (Figure S13a). The 7mw sample prepared with the same reaction time of ~ 7 min and in the most concentrated reaction mixture as 6mw is composed of a smaller particle size (around 570 nm, Figure S13b).
The comparison of the HKUST-1 materials synthesized in the IL medium by the MW technique and under solvothermal conditions clearly shows the differences in their morphology. Furthermore, the crystallite habit of the solvothermal samples (prepared within the same reaction time) depends on the IL nature. In particular, the 8solv sample obtained in BMIMOTF is composed of rather well-shaped distorted cubic crystals (Figure S12a). The 2solv-after-rinsing and 3solv-after-rinsing samples synthesized under solvothermal conditions using different ionic liquids, i.e., EMIMTf2N and OMIMOTf, respectively, are shaped as octahedra (2solv-after-rinsing) (Figure S12b) and rhombohedra (3solv-after-rinsing) (Figure S12c) after post-treatment with solvents.
In contrast, the 6mw and 7mw materials produced in MW fields using BMIMOTF and EMIMTf2N, correspondingly, are composed of the crystallite concretions with an irregular shape (Figure S13a,b).
It can be suggested that the differences in the habit of the HKUST-1 materials synthesized by different activation methods in the IL medium may be related to the specific mechanisms of crystallization in MW fields and under solvothermal conditions.

3.4. Textural Properties and Particle Size of the Synthesized HKUST-1 Materials

The HKUST-1 samples differ remarkably in the specific surface area and pore volume depending on the synthesis mode (Table 2). According to XRD results, the synthesis method significantly affects the HKUST-1 phase purity.
The 8solv material synthesized in a more diluted (twice) reaction mixture in the OMIMOTf medium has a specific surface area that is even larger than that of the 1solv material synthesized in the DMF-H2O system (Table 2). Moreover, the specific surface area of 8solv is even larger than that of the 1solv sample synthesized in the EtOH-H2O system. On the contrary, its porosity is slightly decreased compared to the 1solv sample. However, the mesopore fractions in both 1solv and 8solv materials are rather similar.
According to elemental analysis data (Table S1), 2solv and 3solv materials synthesized in a concentrated reaction mixture contain around 8–10 wt. % of IL. It is likely that IL used as a synthesis medium is located in the mesopores or intercrystalline space in these materials. Therefore, the specific surface area and pore volume of these samples are much smaller than these characteristics obtained for other synthesized HKUST-1 materials (Table 2).
Additional treatment of the 2solv and 3solv samples with EtOH results in a remarkable increase of the specific surface area and porosity. Simultaneously, the mesopore content in the corresponding 2solv-after-rinsing and 3solv-after-rinsing materials increases.
The 2solv-after-rinsing and 3solv-after-rinsing samples show a lower surface areas, which is possibly due to the presence of IL residues entrapped in their pores. The 2solv-after-rinsing sample has the highest mesopore content, and a reduced specific surface area among solvothermal HKUST-1 materials, probably due to the nature of IL (EMIMTf2N) used as a solvent. This phenomenon could indicate that IL plays the role of the structure-directing agent in the formation of the HKUST-1 matrix. A similar suggestion was made for the ionothermal synthesis of the zeolitic imidazolate framework ZIF-8 in the MW fields [29].
The 4mw material has a higher mesopore content and decreased surface area compared to its other counterparts. The decreased surface areas and porosity of 4mw and 6mw systems are probably related to the use of a more concentrated reaction solution leading to the presence of additional crystalline phases according to XRD results. Additionally, the mesopore content in the 4mw material could probably be attributed to its small particle size (~200 nm).
The heating mode does not remarkably impact the textural properties of the produced HKUST-1 material. Therefore, the 5mw, 7mw and 8solv samples have specific surface areas comparable with the best HKUST-1 samples reported to date, such as the HKUST-1 material synthesized in the DMF-H2O system in MW fields with the highest surface area [32].
In particular, 5mw and 7mw materials synthesized in OMIMOTf and EMIMTf2N, respectively, have almost the same specific surface area (BET) and porosity, which are highest among HKUST-1 materials obtained in ILs (Table 2).
In spite of differences in the specific surface area and pore volume, HKUST-1 materials synthesized in IL media show almost a similar micropore width (Table 2).

3.5. Thermal Stability of the HKUST-1 Materials

The thermal stability of representative HKUST-1 materials obtained by changing synthesis variables, 1mw, 5mw, 7mw and 8solv samples was probed by the TGA method. The results of this study (Figure S14) show that all samples maintain network integrity until 320–330 °C. However, the mass loss could be associated with different pore content in the studied HKUST-1 materials. This observation is in accordance with XRD data (Section 3.2). The solvent residues may be responsible for the differences in mass loss of the studied HKUST-1 materials under TGA measurements. These results confirm the stability of the HKUST-1 materials during their preparation at elevated temperatures under conditions of the MW-activation of the reaction mass.

3.6. DRIFTS Study of the Synthesized HKUST-1 Materials

Pore chemistry of the synthesized HKUST-1 materials was studied using the DRIFTS method (ESI). Note that the obtained results could indicate the absence of IL residues in the synthesized HKUST-1 (5mw, 7mw and 8solv) materials. Furthermore, the DRIFTS study revealed the absence of adsorbed or coordinated water in 5mw, 7mw and 8solv samples.

3.7. Adsorption Performance

All adsorption isotherms measured for the synthesized HKUST-1 materials using pure CH4 and C2H6 exhibit type I shapes (Figures S21 and S22). Moreover, the methane adsorption isotherm for the 1solv sample synthesized in the DMF–water system is similar to the literature data [15]. The 1mw material produced in MW fields in the same mixed solvent shows rather similar adsorption properties as solvothermal one (Figure 3).
The results of the adsorption measurements for the synthesized HKUST-1 materials show that the main factors affecting their capacities are the specific surface area, pore volume and crystallite size. Furthermore, the combination of these factors is required for optimal performance. Therefore, the 5mw material with a high specific surface area and micropore volume associated with the small (~280 nm) size of the crystallites demonstrates the best adsorption capacity for ethane and methane within the entire pressure range. According to Figure 3 and Table 3, the 5mw material exhibits ~ 20% higher adsorption of methane and ethane than the samples synthesized in a DMF-H2O medium (1mw and 1solv). The maximum adsorption value for the sample 5mw is 11.4 mmol/g for ethane (at 20 atm) and 9.37 mmol/g for methane (at 20 atm).
In particular, the methane adsorption value obtained for the 5mw material is almost identical to the methane capacity of best DUT-like adsorbents [12], such as DUT-76, i.e., 9.5 mmol/g (20 atm). The adsorption capacities of 2solv and 3solv samples are markedly improved after extra-rinsing (Figure 4, Table 3), along with an increase in the specific surface area and porosity (2solv-after-rinsing and 3solv-after-rinsing samples) (Table 2). The 7mw and 8solv samples posessing almost the same specific surface area and crystallite size (Table 2) show very close and high adsorption capacities both for methane and ethane, which are slightly inferior to the capacity measured for the 5mw material with a higher dispersion and smaller nanoparticle size (Table 3).
On the other hand, the 4mw sample with the smallest particle size, but with the decreased specific surface area and porosity as compared with 5mw, 7mw and 8solv materials (Table 2), is inferior to them concerning adsorption capacity (Table 3). A further decrease in the adsorption capacity (Table 3) is observed for 6mw, 2solv and 3solv materials with a lower specific surface area and micropore volume and relatively larger nanocrystallites (Table 2). Note that these textural and morphological characteristics are rather similar for the three mentioned samples.
In addition, the importance of the small HKUST-1 crystallite size for a good adsorption capacity is illustrated by an example of 1mw material with the highest specific surface area and porosity, but a very large crystal size, around 25 µm. This sample has a decreased adsorption capacity compared with the 5mw sample with lower specific surface area and porosity but a small nanocrystallite size (Table 2 and Table 3).
The selectivity tendency follows some trends other than the adsorption capacity. To the best of our knowledge, the IAST and ideal selectivity values for the ethane/methane pair in a wide pressure range were reported for the HKUST-1 material for the first time (Figure 5).
The best ideal selectivity ratio for C2H6:CH4 was obtained on the 1solv sample (Table 4). It should be noted that currently, there are no available literature data on the ideal selectivity of adsorption of methane and ethane on HKUST-1. Thus, we have calculated the ideal selectivity for the ethane/methane pair based on the data from works [15,16]. At 1 bar and 298 K, the calculated value of the ideal selectivity for C2H6/CH4 was 4.375. It should be noted that this value can serve for comparison purposes only because it was obtained on two different samples and from different experiments. Nevertheless, the ideal selectivity value obtained for the 1solv material is 7.76 at 1 atm, which is noticeably higher than that reported in [15,16].
In the case of the 2solv material, the entrapped IL not only reduces the adsorption values but also has a remarkable impact on selectivity. Therefore, this sample shows similar adsorption values of methane and ethane at pressures of around 20 atm (Table 3).
In IAST calculations, the value for y(CH4) = 0.9 was selected because ethane is the minor component of natural gas, with concentrations usually within 5–15%. Note that the dependencies of the ideal selectivity exhibit a similar shape, asymptotically decreasing to unity at higher pressures. The IAST method, provides different dependencies. As shown in Figure 5, all HKUST-1 samples synthesized by various methods show a clear maximum in the pressure range from 3 to 5 atm. The maximum value of the IAST selectivity for the 1solv material is around 16.5 for the ethane/methane pair.
The correlation of the obtained ideal selectivity with textural characteristics of the synthesized samples reveals that the ideal selectivity almost linearly increases with a gain in the SBET value (R2 = 0.85) (Figure 6a), while the correlation of the selectivity with the Vmicro/Vmeso ratio was less clear (R2 = 0.62) (Figure 6b). It can be suggested that an “ideal” sample of HKUST-1 designed for methane and ethane separation should have as high as possible SBET and a maximum fraction of micropores. Moreover, the average particle size has almost no impact on selectivity, which makes it very promising for industrial application because the use of adsorbents with larger particle sizes in certain cases should be more convenient from the practical point of view.

4. Conclusions

A series of HKUST-1 materials were synthesized in an IL medium under solvothermal conditions and under MW activation. Using this kind of solvent system allows one to reduce the HKUST-1 crystallite size efficiently as compared to HKUST-1 materials synthesized both under solvothermal and MW conditions. It was found that synthesis variables, such as reaction time and IL content in the reaction mixture, dramatically influence the phase purity, crystallinity, crystallite size and textural properties of resulting HKUST-1 samples. Moreover, the used ILs appear to be stable under microwave conditions and may be separated and reused in the following experiments.
In particular, the HKUST-1 material prepared in ILs by the MW activation technique under optimized synthesis conditions features an enhanced adsorption capacity for ethane and methane. The achieved methane adsorption value for this material is comparable with the best adsorption capacities demonstrated by the best MOF adsorbents, e.g., DUT-76 MOF.
To the best of our knowledge, the IAST and ideal selectivity values for the ethane/methane pair were reported for the HKUST-1 material for the first time in a wide pressure range. The correlation between the ideal selectivities of the synthesized HKUST-1 materials and their specific surface area (BET) and the ratio of micro:meso pore volumes was found. The adsorbent prepared in the DMF–water system under solvothermal conditions shows the best ideal selectivity (experimental and calculated by IAST).
The HKUST-1 samples synthesized in common solvent systems and ILs under solvothermal conditions and MW fields may serve as models for investigations of the factors influencing the adsorption behavior of the MOF materials. Therefore, the results of this work may contribute to the design of the adsorbents for ethane and methane based on HKUST-1 material as well as new MOFs.

Supplementary Materials

The following data are available online at https://www.mdpi.com/article/10.3390/cryst12020279/s1, Figure S1: Heating rates of [BMIM] OTf and water : DMF = 1 : 1 solvent systems in MW fields; Figure S2: Dependence of the yield of the HKUST-1 material on the reaction time under conditions of the MW-assisted synthesis; Figure S3: 1H NMR spectra of the neat IL OMIM OTf and of the same IL recycled after synthesis; Figure S4: A comparison of experimental XRD patterns of HKUST-1DMF-MW synthesized by the MW technique in DMF as single solvent and 1mw material; Figure S5: The experimental and calculated after the Pawley fitting XRD patterns of the 3solv sample; Figure S6: The experimental and calculated after the Pawley fitting XRD patterns of the sample 3solv-after-rinsing; Figure S7: The experimental and calculated after the Pawley fitting XRD patterns of the sample 2solv-after-rinsing; Figure S8: Experimental XRD pattern of HKUST-1 sample produced using tenfold quantities of the reagents; Figure S9: XRD patterns of 1mw, 8solv, 5mw and 7mw materials soaked in MeOH; Figure S10: XRD patterns of 1mw, 8solv, 5mw and 7mw materials soaked in H2O; Figure S11: SEM images of the 1mw and 1solv samples; Figure S12: SEM images of the 8solv, 2solv-after-rinsing and 3solv-after-rinsing samples; Figure S13: SEM images of the 6mw and 7mw samples; Figure S14: TG Curves of the 1mw, 8solv, 5mw and 7mw materials; Figure S15: DRIFT spectra of the 5mw sample and ionic liquid OMIM OTf in a wide range and 1800–750 cm−1 region; Figure S16: DRIFT spectra of the 7mw sample and ionic liquid EMIM Tf2N in a wide range and 1800–750 cm−1 region; Figure S17: DRIFT spectra of 5mw (black), 7mw (red) and 8solv (green) samples; Figure S18: DRIFT spectra of 5mw, 7mw and 8solv samples in the frequency range of 3800–2400 cm−1. Figure S19: DRIFT spectra of 5m, 7mw and 8solv samples in the frequency range of 1800–750 cm−1. Figure S20: The schematic diagram of the adsorption setup; Figure S21: Methane adsorption isotherms for all obtained samples at 298 K; Figure S22: Ethane adsorption isotherms for all obtained samples at 298 K. Table S1: Elemental analysis data for the synthesized HKUST-1 materials.

Author Contributions

Conceptualization, G.S.D., L.M.G. and V.I.I.; methodology, V.V.V., D.A.A., G.S.D. and L.M.G.; software, V.V.C.; validation, L.M.G., G.S.D. and V.V.C.; formal analysis, G.I.K., O.P.T., V.D.N. and V.V.C.; investigation, V.V.V., D.A.A., G.S.D., L.M.G., G.I.K., O.P.T., V.D.N. and V.V.C.; resources, L.M.K.; data curation, V.I.I., G.S.D. and L.M.G.; writing—original draft preparation, G.S.D., L.M.G. and V.I.I.; writing—review and editing, L.M.K. and V.I.I.; visualization, V.V.C. and G.I.K.; supervision, L.M.K.; project administration, V.I.I. and L.M.K.; funding acquisition, L.M.K. and V.I.I. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by RFBR, grant number 20-33-90102 in the material synthesis part and grant number 19-03-00930 in the adsorption and characterization parts.

Data Availability Statement

Samples of the compounds HKUST-1 are available from the authors.

Acknowledgments

Electron microscopy characterization was performed in the Department of Structural Studies of Zelinsky Institute of Organic Chemistry, Moscow.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Li, Y.; Weser, G. Methane and Natural Gas Utilization. Energy Technol. 2020, 8, 2000460. [Google Scholar] [CrossRef]
  2. Mokhatab, S.; Poe, W.A.; Mak, J.Y. Chapter 13—Unconventional Gas Processing. In Handbook of Natural Gas Transmission and Processing, 4th ed.; Gulf Professional Publishing: Houston, TX, USA, 2018; pp. 409–431. [Google Scholar]
  3. Kumar, S.; Kwon, H.-T.; Choi, K.-H.; Lim, W.; Cho, J.; Tak, K.; Moon, I. LNG: An eco-friendly cryogenic fuel for sustainable development. Appl. Energy 2011, 88, 4264–4273. [Google Scholar] [CrossRef]
  4. Li, X.; Chen, J. Adsorption of natural gas and its whole components on adsorbents. Adsorption 2011, 17, 949–954. [Google Scholar] [CrossRef]
  5. Guecueyener, C.; van den Bergh, J.; Gascon, J.; Kapteijn, F. Ethane/Ethene Separation Turned on Its Head: Selective Ethane Adsorption on the Metal-Organic Framework ZIF-7 through a Gate-Opening Mechanism. J. Am. Chem. Soc. 2010, 132, 17704. [Google Scholar] [CrossRef]
  6. Long, J.R.; Yaghi, O.M. The pervasive chemistry of metal-organic frameworks. Chem. Soc. Rev. 2009, 38, 1213–1214. [Google Scholar] [CrossRef]
  7. Férey, G. Hybrid porous solids: Past, present, future. Chem. Soc. Rev. 2008, 37, 191–214. [Google Scholar] [CrossRef]
  8. Joshi, J.N.; Zhu, G.; Lee, J.J.; Carter, E.A.; Jones, C.W.; Lively, R.P.; Walton, K.S. Probing Metal-Organic Framework Design for Adsorptive Natural Gas Purification. Langmuir 2018, 34, 8443–8450. [Google Scholar] [CrossRef]
  9. Tsivadze, A.; Aksyutin, O.; Ishkov, A.; Fomkin, A.; Men’shchikov, I.; Pribylov, A.; Isaeva, V.; Kustov, L.; Shkolin, A.; Strizhenov, E. Adsorption of methane on an MOF-199 organometallic framework structure at high pressures in the range of supercritical temperatures. Prot. Met. Phys. Chem. Surf. 2016, 52, 24–29. [Google Scholar] [CrossRef]
  10. Senkovksa, I.; Kaskel, S. High pressure methane adsorption in the metal-organic frameworks Cu3(btc)2, Zn2(bdc)2dabco, and Cr3F(H2O)2O(bdc)3. Microporous Mesoporous Mater. 2008, 112, 108–115. [Google Scholar] [CrossRef]
  11. Plonka, A.; Chen, X.; Wang, H.; Krishna, R.; Dong, X.; Banerjee, D.; Woerner, W.; Han, Y.; Li, J.; Parise, J. Light Hydrocarbon Adsorption Mechanisms in Two Calcium-Based Microporous Metal Organic Framework. Chem. Mater. 2016, 28, 1636–1646. [Google Scholar] [CrossRef] [Green Version]
  12. Stoeck, U.; Senkovska, I.; Bon, V.; Krause, S.; Kaskel, S. Assembly of metal-organic polyhedra into highly porous frameworks for ethene delivery. Chem. Commun. 2015, 51, 1046–1049. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  13. Peng, Y.; Krungleviciute, V.; Eryazici, I.; Hupp, J.T.; Farha, O.K.; Yildirim, T. Methane Storage in Metal–Organic Frameworks: Current Records, Surprise Findings, and Challenges. J. Am. Chem. Soc. 2013, 135, 11887–11894. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  14. Isaeva, V.I.; Chernyshev, V.V.; Fomkin, A.A.; Shkolin, A.V.; Veselovsky, V.V.; Kapustin, G.I.; Sokolova, N.A.; Kustov, L.M. Preparation of novel hybrid catalyst with an hierarchical micro-/mesoporous structure by direct growth of the HKUST-1 nanoparticles inside Mesoporous Silica Matrix (MMS). Microporous Mesoporous Mater. 2020, 300, 110136. [Google Scholar] [CrossRef]
  15. Hamon, L.; Jolimaitre, E.; Pirngruber, G.D. CO2 and CH4 Separation by Adsorption Using Cu-BTC Metal-Organic Framework. Ind. Eng. Chem. Res. 2010, 49, 7497–7503. [Google Scholar] [CrossRef]
  16. Chuah, C.Y.; Samarasinghe, S.A.S.C.; Li, W.; Goh, K.; Bae, T.-H. Leveraging Nanocrystal HKUST-1 in Mixed-Matrix Membranes for Ethylene/Ethane Separation. Membranes 2020, 10, 74. [Google Scholar] [CrossRef]
  17. He, Y.; Zhou, W.; Qian, G.; Chen, B. Methane storage in metal-organic frameworks. Chem. Soc. Rev. 2014, 43, 5657–5678. [Google Scholar] [CrossRef]
  18. Isaeva, V.I.; Chernyshev, V.V.; Sokolova, N.A.; Kapustin, G.I. Modifying the Hydrophobic Properties of Metal-Organic Framework HKUST-1. Russ. J. Phys. Chem. A 2018, 92, 2391–2395. [Google Scholar] [CrossRef]
  19. Qiu, S.; Du, J.; Xiao, Y.; Zhao, Q.; He, G. Hierarchical porous HKUST-1 fabricated by microwave-assisted synthesis with CTAB for enhanced adsorptive removal of benzothiophene from fuel. Sep. Purif. Technol. 2021, 271, 118868. [Google Scholar] [CrossRef]
  20. Han, S.; Ciufo, R.; Meyerson, M.; Keitz, B.; Mullins, C. Solvent-free vacuum growth of oriented HKUST-1 thin films. J. Mater. Chem. A 2019, 7, 19396–19406. [Google Scholar] [CrossRef]
  21. Glowniak, S.; Szczęśniak, B.; Choma, J.; Jaroniec, M. Mechanochemistry: Toward green synthesis of metal-organic frameworks. Mater. Today 2021, 46, 109–124. [Google Scholar] [CrossRef]
  22. Usman, K.A.S.; Maina, J.W.; Seyedin, S.; Conato, M.T.; Payawan, L.M., Jr.; Dumée, L.F.; Razal, J.M. Downsizing metal-organic frameworks by bottom-up and top-down methods. NPG Asia Mater. 2020, 12, 58. [Google Scholar] [CrossRef]
  23. Isaeva, V.I.; Eliseev, O.L.; Kazantsev, R.V.; Chernyshev, V.V.; Tarasov, A.L.; Davydov, P.E.; Lapidus, A.L.; Kustov, L.M. Effect of the support morphology on the performance of Co nanoparticles deposited on metal-organic framework MIL-53(Al) in Fischer-Tropsch synthesis. Polyhedron 2019, 157, 389–395. [Google Scholar] [CrossRef]
  24. Isaeva, V.I.; Tarasov, A.L.; Chernyshev, V.V.; Kustov, L.M. Control of Morphology and Size of Microporous Framework MIL-53(Al) Crystals by Synthesis Procedure. Mendeleev Commun. 2015, 25, 466–470. [Google Scholar] [CrossRef]
  25. Kinik, F.P.; Uzun, A.; Keskin, S. Ionic Liquid/Metal-Organic Framework Composites: From Synthesis to Applications. ChemSusChem 2017, 10, 2842–2863. [Google Scholar] [CrossRef] [PubMed]
  26. Ermer, M.; Mehler, J.; Kriesten, M.; Avadhut, Y.; Schulz, P.; Hartmann, M. Synthesis of the novel MOF hcp UiO-66 employing ionic liquids as a linker precursor. Dalton Trans. 2018, 47, 14426–14430. [Google Scholar] [CrossRef]
  27. Guo, X.; Geng, S.; Zhuo, M.; Chen, Y.; Zaworotko, M.J.; Cheng, P.; Zhang, Z. The Utility of the Template Effect in Metal-Organic Frameworks. Coord. Chem. Rev. 2019, 391, 44–68. [Google Scholar] [CrossRef]
  28. Shang, W.; Kang, X.; Ning, H.; Zhang, J.; Zhang, X.; Wu, Z.; Mo, G.; Xing, X.; Han, B. Shape and Size Controlled Synthesis of MOF Nanocrystals with the Assistance of Ionic Liquid Microemulsions. Langmuir 2013, 29, 13168–13174. [Google Scholar] [CrossRef]
  29. Deiko, G.S.; Isaeva, V.I.; Kustov, L.M. New Molecular Sieve Materials: Composites Based on Metal–Organic Frameworks and Ionic Liquids. Pet. Chem. 2019, 59, 770–787. [Google Scholar] [CrossRef]
  30. Liu, C.; Zhang, B.; Zhang, J.; Peng, L.; Kang, X.; Han, B.; Wu, T.; Sang, X.; Ma, X. Gas promotes the crystallization of nano-sized metal-organic frameworks in ionic liquid. Chem. Commun. 2015, 51, 11445–11448. [Google Scholar] [CrossRef]
  31. Blanita, G.; Borodi, G.; Lazar, M.D.; Biris, A.-R.; Barbu-Tudoran, L.; Coldea, I.; Lupu, D. Microwave assisted non-solvothermal synthesis of metal-organic frameworks. RSC Adv. 2016, 6, 25967–25974. [Google Scholar] [CrossRef]
  32. Isaeva, V.I.; Saifutdinov, B.R.; Chernyshev, V.V.; Vergun, V.V.; Kapustin, G.I.; Kurnysheva, Y.P.; Ilyin, M.M.; Kustov, L.M. Impact of the Preparation Procedure on the Performance of the Microporous HKUST-1 Metal-Organic Framework in the Liquid-Phase Separation of Aromatic Compounds. Molecules 2020, 25, 2648. [Google Scholar] [CrossRef] [PubMed]
  33. Aguiar, L.W.; Otto, G.P.; Kupfer, V.L.; Fávaro, S.L.; Silva, C.T.P.; Moisés, M.P.; de Almeida, L.; Guilherme, M.R.; Radovanovic, E.; Girotto, E.M.; et al. Simple, fast, and low-cost synthesis of MIL-100 and MIL-88B in a modified domestic microwave oven. Mater. Lett. 2020, 276, 128127. [Google Scholar] [CrossRef]
  34. Vaid, T.P.; Kelleya, S.P.; Rogers, R.D. Structure-directing effects of ionic liquids in the ionothermal synthesis of metal-organic frameworks. IUCrJ 2017, 4, 380–392. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  35. Yang, L.; Lu, H. Microwave-assisted Ionothermal Synthesis and Characterization of Zeolitic Imidazolate Framework-8. Chin. J. Chem. 2012, 30, 1040–1044. [Google Scholar] [CrossRef]
  36. Silva, C.; Safadi, B.; Moises, M.; Meneguin, J.; Arroyo, P.; Favaro, S.; Girotto, E.; Radovanovic, E.; Rinaldi, A. Synthesis of Zn-BTC metal-organic framework assisted by a home microwave oven and their unusual morphologies. Mater. Lett. 2016, 182, 231–234. [Google Scholar] [CrossRef]
  37. Bonhôte, P.; Dias, A.P.; Papageorgiou, N.; Kalyanasundaram, K.; Grätzel, M. Hydrophobic, highly conductive ambient-temperature molten salts. Inorg. Chem. 1996, 35, 1168–1178. [Google Scholar] [CrossRef]
  38. Kashin, A.S.; Ananikov, V.P. A SEM study of nanosized metal films and metal nanoparticles obtained by magnetron sputtering. Russ. Chem. Bull. 2011, 60, 2602–2607. [Google Scholar] [CrossRef]
  39. Blach, T.P.; Gray, E. Sieverts apparatus and methodology for accurate determination of hydrogen uptake by light-atom hosts. J. Alloys Compd. 2007, 31, 446–447. [Google Scholar] [CrossRef]
  40. Sychev, V.V.; Wasserman, A.A.; Zagoruchenko, V.A.; Kozlov, A.D.; Spiridonov, G.A.; Tsymarnyi, V.A. Thermodynamic Properties of Ethane; Izdatel’stvo Standartov: Moscow, Russia, 1982; 305p. (In Russian) [Google Scholar]
  41. Sychev, V.V.; Wasserman, A.A.; Zagoruchenko, V.A.; Kozlov, A.D.; Spiridonov, G.A.; Tsymarnyi, V.A. Thermodynamic Properties of Methane; Izdatel’stvo Standartov: Moscow, Russia, 1979; 351p. (In Russian) [Google Scholar]
  42. Pawley, G.S. Unit-cell refinement from powder diffraction scans. J. Appl. Crystallogr. 1981, 14, 357–361. [Google Scholar] [CrossRef]
  43. Zlokazov, V.B.; Chernyshev, V.V. MRIA—A program for a full profile analysis of powder multiphase neutron-diffraction time-of-flight (direct and Fourier) spectra. J. Appl. Crystallogr. 1992, 25, 447–451. [Google Scholar] [CrossRef] [Green Version]
  44. Smirnova, N.A.; Safonova, E.A. Ionic liquids as surfactants. Russ. J. Phys. Chem. 2010, 84, 1695–1704. [Google Scholar] [CrossRef]
  45. Funasako, Y.; Nosho, M.; Mochida, T. Ionic liquids from copper(II) complexes with alkylimidazole-containing tripodal ligands. Dalton Trans. 2013, 42, 10138–10143. [Google Scholar] [CrossRef] [PubMed] [Green Version]
Figure 1. The combined presentation of the XRD patterns of the 5mw (red), 7mw (blue) and 8solv (green) samples. The vertical black bars show the calculated peak positions of the cubic HKUST-1 phase.
Figure 1. The combined presentation of the XRD patterns of the 5mw (red), 7mw (blue) and 8solv (green) samples. The vertical black bars show the calculated peak positions of the cubic HKUST-1 phase.
Crystals 12 00279 g001
Figure 2. TEM images of 5mw (a) and 4mw (b) materials.
Figure 2. TEM images of 5mw (a) and 4mw (b) materials.
Crystals 12 00279 g002
Figure 3. Adsorption isotherms for the 5mw (■), 1mw (●) and 1solv (▲) materials at 298 K. Hollow symbols—methane adsorption, solid symbols—ethane adsorption.
Figure 3. Adsorption isotherms for the 5mw (■), 1mw (●) and 1solv (▲) materials at 298 K. Hollow symbols—methane adsorption, solid symbols—ethane adsorption.
Crystals 12 00279 g003
Figure 4. Adsorption isotherms for the samples ▼—2solv, ▲—3solv, ●—2solv-after-rinsing and ■—3solv-after-rinsing at 298 K. Hollow symbols—methane adsorption, solid symbols—ethane adsorption.
Figure 4. Adsorption isotherms for the samples ▼—2solv, ▲—3solv, ●—2solv-after-rinsing and ■—3solv-after-rinsing at 298 K. Hollow symbols—methane adsorption, solid symbols—ethane adsorption.
Crystals 12 00279 g004
Figure 5. The pressure dependencies of C2H6/CH4 ideal and IAST selectivities at 298 K for the 1solv, 5mw and 8solv samples.
Figure 5. The pressure dependencies of C2H6/CH4 ideal and IAST selectivities at 298 K for the 1solv, 5mw and 8solv samples.
Crystals 12 00279 g005
Figure 6. The correlation of the ideal selectivity of the synthesized HKUST-1 adsorbents for a C2H6/CH4 mixture with (a) SBET and (b) Vmicro/Vmeso.
Figure 6. The correlation of the ideal selectivity of the synthesized HKUST-1 adsorbents for a C2H6/CH4 mixture with (a) SBET and (b) Vmicro/Vmeso.
Crystals 12 00279 g006
Table 1. Synthesis of the HKUST-1 samples.
Table 1. Synthesis of the HKUST-1 samples.
MaterialConditionsReaction Mixture CompositionYield
Cu2+ Source H3btcSolvent
1solv [32]Solvothermal, 10 h, 100 °CCu(NO3)2∙3H2O, 2 g, 8.58 mmol1 g, 4.7 mmolDMF : H2O
: EtOH =
1:1:1, total volume - 45 mL
1.187 g, 83%
2solvSolvothermal, 24 h, 130 °CCu(NO3)2∙3H2O, 1 g, 3 g, 15 mmol1.5 g, 7 mmolEMIM Tf2N,
5 mL
0.86 g, 40%
3solvSolvothermal, 24 h, 130 °CCu(NO3)2∙3H2O, 1 g, 3 g, 15 mmol1.5 g, 7 mmolOMIM OTf,
5 mL
1.17 g, 54%
8solvSolvothermal, 24 h, 130 °CCu(NO3)2∙3H2O, 1.2 g, 4.9 mmol0.6 g, 2.8 mmolBMIM OTF,
10 mL
0.86 g, 99%
1mw [32]MW, 30 minCu(NO3)2∙3H2O, 2 g, 8.58 mmol1 g, 4.7 mmolDMF : H2O
1 : 1, total volume - 40 mL
1.121 g, 79% [Molecules, 2020]
4mwMW, 2 minCu(NO3)2∙3H2O, 1 g, 4 mmol0.5 g, 2.3 mmolBMIM OTF,
5 mL
0.26 g, 70%
5mwMW, 3 minCu(NO3)2∙3H2O, 1.2 g, 4.9 mmol0.6 g, 2.8 mmolOMIM OTF, 10 mL0.75 g, 90%
6mwMW, 7 minCu(NO3)2∙3H2O, 3.6 g, 18 mmol1.68 g, 8 mmolBMIM OTF,
5 mL
2.1 g, 87%
7mwMW, 5 minCu(NO3)2∙3H2O, 3.63 g, 15 mmol2.1 g, 10 mmolEMIM Tf2N,
5 mL
2.1 g, 70%
Table 2. Textural properties and particle size of the synthesized HKUST-1 materials.
Table 2. Textural properties and particle size of the synthesized HKUST-1 materials.
MaterialILHeating MethodABET(ISO), *
m2/g
Vtotal, a
cm3/g
Vmicro, c
cm3/g
Vmeso, b
cm3/g
Pore Width, nmParticle Size
1solv [32]-Solv16480.8160.7140.1020.6–0.98 µm
2solvEMIM Tf2NSolv4970.2740.2300.0440.6–0.9340 nm
3solvOMIM OTfSolv5300.2850.2470.0380.6–0.9~1 µm
2solv-after-rinsingEMIM Tf2NSolv11580.5600.4240.1360.6–1.0720 nm
3solv-after-rinsingOMIM OTfSolv12460.5740.4580.1160.65–1.0870 nm
8solvBMIM OTfSolv17010.7530.6370.1160.6–0.9350 nm
1mw [32]-MW20500.8360.7770.0590.4–0.825 µm
4mwBMIM OTfMW14300.6760.5280.1480.6–0.9200 nm
5mwOMIM OTfMW17820.7590.6800.0790.6–0.9290 nm
6mwBMIM OTfMW8180.4160.3300.0860.6–0.9790 nm
7mwEMIM Tf2NMW17720.7660.6800.0640.6–0.9250–400 nm
* ISO 9277. a Vtotal was estimated from the adsorption value at p/p0 = 0.99; b Vμ = VΣVmeso. c The cumulative mesopore volume was calculated at 2 nm from the desorption branch of the isotherm by the BJH method and the standard thickness of the adsorption film.
Table 3. Adsorption capacities of synthesized HKUST-1 materials towards methane and ethane.
Table 3. Adsorption capacities of synthesized HKUST-1 materials towards methane and ethane.
Sample Codea(C2H6, 1 atm), mmol/ga(CH4, 1 atm), mmol/ga(C2H6, 5 atm), mmol/ga(CH4, 5 atm), mmol/ga(C2H6, 20 atm), mmol/ga(CH4, 20 atm), mmol/g
1solv5.740.748.12.759.127
1mw6.10.828.53.489.47.93
2solv2.320.523.371.273.893.31
3solv2.10.513.061.253.63.2
2solv-after-rinsing3.720.85.182.606.025.54
3solv-after-rinsing3.770.775.482.696.465.80
4mw4.30.925.742.796.425.28
5mw7.181.0310.3411.49.37
6mw3.580.625.262.196.024.89
7mw5.970.898.73.339.988
8solv5.810.988.713.74108.49
HKUST-1 lit. data3.5 [16]0.8 [15]-2.9 [15]-7.0 [15]
Table 4. Ideal selectivity for methane and ethane for obtained samples of HKUST-1.
Table 4. Ideal selectivity for methane and ethane for obtained samples of HKUST-1.
Sample CodeIdeal Selectivity *IAST Selectivity at y(CH4) = 0.9
C2H6:CH4 at P = 1 atmC2H6:CH4 at P = 5 atmC2H6:CH4 at P = 20 atmC2H6:CH4 at P = 1 atmC2H6:CH4 at P = 5 atmC2H6:CH4 at P = 20 atm
1solv7.762.951.3016.1316.0513.40
1mw7.442.441.1912.2812.5110.64
2solv3.562.101.157.718.677.36
3solv3.752.091.184.847.296.90
2solv-after-rinsing4.882.011.085.907.766.40
3solv-after-rinsing5.392.031.095.457.836.69
4mw4.672.061.226.498.978.71
5mw6.972.581.2211.011.8910.51
6mw5.772.401.239.6110.138.30
7mw6.712.611.259.8211.019.6
8solv5.932.331.189.3010.058.51
* Ideal selectivity was calculated as the ratio of adsorption values of methane and ethane at equal pressures (1, 5, 20 atm).
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Deyko, G.S.; Glukhov, L.M.; Isaeva, V.I.; Chernyshev, V.V.; Vergun, V.V.; Archipov, D.A.; Kapustin, G.I.; Tkachenko, O.P.; Nissenbaum, V.D.; Kustov, L.M. Modifying HKUST-1 Crystals for Selective Ethane Adsorption Using Ionic Liquids as Synthesis Media. Crystals 2022, 12, 279. https://doi.org/10.3390/cryst12020279

AMA Style

Deyko GS, Glukhov LM, Isaeva VI, Chernyshev VV, Vergun VV, Archipov DA, Kapustin GI, Tkachenko OP, Nissenbaum VD, Kustov LM. Modifying HKUST-1 Crystals for Selective Ethane Adsorption Using Ionic Liquids as Synthesis Media. Crystals. 2022; 12(2):279. https://doi.org/10.3390/cryst12020279

Chicago/Turabian Style

Deyko, Gregory S., Lev M. Glukhov, Vera I. Isaeva, Vladimir V. Chernyshev, Vadim V. Vergun, Danil A. Archipov, Gennady I. Kapustin, Olga P. Tkachenko, Vera D. Nissenbaum, and Leonid M. Kustov. 2022. "Modifying HKUST-1 Crystals for Selective Ethane Adsorption Using Ionic Liquids as Synthesis Media" Crystals 12, no. 2: 279. https://doi.org/10.3390/cryst12020279

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics