Next Article in Journal
Seismic Performance of Recycled Aggregate Concrete-Filled Steel Tube Column–Composite Beam Frames with Column-End Stirrup Confinement
Previous Article in Journal
Analysis of the Impact of Fabric Surface Profiles on the Electrical Conductivity of Woven Fabrics
Previous Article in Special Issue
Understanding the Effect of Waiting for the Dissolution of Sodium Hydroxide in Geopolymer Concrete Mixes
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Unveiling the Influence and Mechanisms of Enhancing Ferrite-Phase Composition on the Properties of Calcium Sulfoaluminate Cement

1
School of Civil Engineering, NingboTech University, Ningbo 315100, China
2
School of Civil Engineering and Architecture, Zhejiang Sci-Tech University, Hangzhou 310018, China
3
College of Architectural and Engineering, Anqing Vocational & Technical College, Anqing 246003, China
4
Ningbo Langda Technology Co., Ltd., Ningbo 315100, China
*
Author to whom correspondence should be addressed.
Materials 2025, 18(11), 2457; https://doi.org/10.3390/ma18112457
Submission received: 30 March 2025 / Revised: 16 May 2025 / Accepted: 19 May 2025 / Published: 23 May 2025

Abstract

:
Calcium sulfoaluminate (CSA) cement has emerged as a low-carbon alternative to ordinary Portland cement (OPC), offering reduced CO2 emissions and rapid strength development. However, the role of the ferrite phase in CSA systems remains underexplored. This study investigates the influence of ferrite-phase composition on CSA cement properties through targeted clinker design, hydration analysis, and macro–micro performance testing. Nine clinker formulations were synthesized by systematically increasing the ferrite content (10–30%) while adjusting belite (C2S) proportions, using limestone, bauxite, and supplementary Fe2O3/SiO2. Results reveal that the ferrite phase enhances the formation and stabilization of ye’elimite (C4A3Š) during clinkering and reduces low-activity transitional phase products. Increasing the iron-phase content appropriately improves early strength by promoting ettringite (AFt) formation and refines pore structures to enhance later strength development. The maximum strength improvement is achieved when the target ferrite-phase content is set to 15%, showing a 25.1% increase in 1 d strength and an 11.5% increase in 28 d strength. While ferrite phases and C2S ensure long-term strength gains, excessive ferrite content reduces C4A3Š availability, limiting early AFt formation and compromising initial strength. These findings highlight the dual role of the ferrite phase in optimizing CSA cement performance and sustainability, providing a foundation for designing ferrite-rich, low-carbon binders.

1. Introduction

The global construction industry is currently facing unprecedented challenges driven by the urgent need for sustainable development and carbon emission reduction. Ordinary Portland Cement (OPC), the most widely used binder material in modern construction, is responsible for a significant portion of anthropogenic CO2 emissions, estimated to be around 5–8% of the global total [1,2]. Consequently, the search for alternative, low-carbon cementitious materials has become a paramount research focus worldwide [3,4]. Among the promising alternatives to OPC, Calcium Sulfoaluminate (CSA) cement has garnered significant attention due to its distinct environmental and performance advantages [5,6]. The production of CSA clinker requires lower calcination temperatures (typically 1250–1350 °C) compared to OPC (1450 °C) and utilizes raw materials with a lower calcium carbonate content, resulting in a potential reduction of CO2 emissions by up to 30–40% per ton of cement produced [7,8]. Furthermore, CSA cement exhibits unique properties highly desirable for various applications, including rapid setting and hardening, high early strength development, low drying shrinkage or even micro-expansion, excellent durability particularly in sulfate-rich environments, and good performance at low temperatures [9,10,11,12].
The properties of CSA cement are primarily governed by its main mineral phases, which typically include ye’elimite (C4A3Š) and belite (C2S) [13,14]. C4A3Š is the principal hydraulic phase responsible for the rapid setting and early strength gain through its reaction with calcium sulfates and water to form ettringite (AFt) and aluminum hydroxide (AH3) [15,16]. C2S contributes to the later-age strength development, similar to its role in OPC [17]. Besides these major phases, CSA clinkers invariably contain ferrite phases, commonly referred to as calcium aluminoferrite (CxAyFz) [18]. In most conventional CSA clinkers produced using bauxite and limestone, this phase exists as a solid solution, predominantly brownmillerite (C4AF) [19]. The ferrite phase primarily acts as a fluxing agent during the clinkering process, facilitating the formation of the liquid phase at lower temperatures, which promotes the combination of raw materials and the formation of C4A3Š [20]. C4AF can also form iron gels (Fe(OH)3) and iron-containing hydrates (Calcium Alumino-Ferrite hydrate, C-A-F-H), which could refine pore structures, thereby improving freeze-thaw resistance and chloride impermeability [21,22]. Studies have shown that due to the presence of ferrite phase minerals, CSA cement has better resistance to chloride ion corrosion than OPC [23].
Moreover, iron-rich industrial byproducts can replace costly raw materials, aligning with green construction demands under the “dual-carbon” strategy [24,25]. Zhang and Shi et al. prepared CSA clinker using solid waste red mud as the raw material, and explored the hydration and properties of the resulting cement clinker. Results showed that compressive strength could reach 40.0 MPa and 57.9 MPa at 1 d and 28 d [26,27]. Iacobescu et al. investigated the use of electric arc furnace steel slag as a raw material in the production of calcium ferroaluminate belite cement clinker (firing at 1320 °C) to save natural resources (i.e., limestone and clays) [28].
However, the role and potential optimization of the ferrite phase in CSA cement systems have received relatively less attention compared to the extensive research focused on ye’elimite hydration and the influence of calcium sulfates. The composition of the ferrite phase can vary significantly depending on the selection of raw materials [29,30]. This variability can potentially lead to inconsistencies in cement performance [31,32]. Wu et al. found that Fe-bearing minerals play a critical role in the preparation and performance of ferrite-rich sulfoaluminate cement [33]. Recently, there is a growing recognition that simply considering the ferrite phase as an inert filler or solely a fluxing agent might overlook its potential impact on the overall performance and durability of CSA-based materials [34]. Therefore, a critical question arises: Can the performance of CSA cement be further enhanced by strategically modifying the composition and reactivity of its ferrite phase?
This research aims to systematically investigate the effect of improving the ferrite phase mineral composition on the properties of CSA cement and to elucidate the underlying mechanisms governing these effects. This study seeks to provide a fundamental understanding of the role and optimization potential of the ferrite phase in modern CSA cement technology. The findings are expected to offer valuable insights for designing advanced CSA cements with tailored properties.

2. Materials and Methods

2.1. Materials

The primary raw materials used in this study for synthesizing cement clinker were bulk industrial commodities, including limestone, bauxite, and gypsum. Their chemical compositions, determined by X-ray fluorescence (XRF) using a Malvern Panalytical Zetium instrument (Malvern, UK) on powder samples, are summarized in Table 1 and Table 2. To achieve precise adjustment of the chemical composition, the analytical-grade reagents iron oxide (Fe2O3) and silicon dioxide (SiO2) were employed as fine-tuning additives, ensuring stoichiometric control over the ferrite and silicate phases during clinker formation.

2.2. Clinker Design Methodology

CSA cement primarily comprises key mineral phases such as C4A3Š, C2S, and ferrite phase. In this study, the clinker composition was modified by enhancing the proportions of ferrite phase and C2S, based on conventional CSA cement formulations. The clinker design methodology is outlined below.
(a)
Target Composition Design
Table 3 summarizes the predefined target mineralogical compositions for the cement clinker, including C4A3Š, C2S, ferrite phase and anhydrite (CaSO4, CŠ). These compositions were specifically designed to systematically investigate the influence of key phases, primarily focusing on varying the ferrite phase content. Recognizing C4AF as a representative ferrite-phase mineral, this study targeted a range of C4AF contents, from 10% up to 30%, to demonstrate how progressively higher ferrite contents influence the cement’s performance and properties. Furthermore, varying target C2S contents were also included in the experimental design to explore the coupled influence of ferrite and C2S variations on cement properties.
  • (b) Stoichiometric Batching Calculation
The required chemical composition of the raw mix was determined from the target clinker design values using the following governing equations (Equation (1a–e)) [35,36]. These equations are derived from the principle of mass conservation and define the total required mass of each major oxide (like CaO, SiO2, Al2O3, Fe2O3, SO3) in the raw meal as the sum of its mass contributions from the targeted clinker mineral phases. In all these equations, ω represents the mass of the corresponding substance.
ω(CaO) = 0.6512ω(C2S) + 0.3672ω(C4A3Š) + 0.4616ω(C4AF)
ω(SiO2) = 0.3488ω(C2S)
ω(Al2O3) = 0.5016ω(C4A3Š) + 0.2098ω(C4AF)
ω(Fe2O3) = 0.3300ω(C4AF)
ω(SO3) = 0.1311ω(C4A3Š) + 0.5882ω(CŠ)
  • (c) Raw Meal Proportioning
The raw material ratios (Table 4) were determined by correlating the chemical compositions of raw materials (Table 1) with the reaction-derived chemical requirements.
  • (d) Theoretical Clinker Yield and Basicity Coefficient Validation
According to the raw material ratio, we calculated the theoretical amount of cement clinker produced and the alkalinity coefficient (Equation (2)) [36], ensuring that the theoretical amount of cement clinker produced meets expectations and that the alkalinity coefficient was maintained at ≤1, guaranteeing optimal CaO content to fulfill the stoichiometric demands of target minerals while suppressing free lime (f-CaO) formation.
A l k a l i n i t y   c o e f f i c i e n t = ω C a O 0.7 ω T i O 2 0.73 ω A l 2 O 3 0.64 ω F e 2 O 3 + 1.40 ω F e 2 O 3 + 1.87 ω S i O 2

2.3. CSA Cement Production

The cement production process is shown in Figure 1. Raw materials were mixed and homogenized according to a predetermined ratio. The raw meal was then combined with 10 wt% water and compacted into cylindrical cakes (φ30 mm × h30 mm) under a pressure of 25 MPa. The cakes were dried at 105 °C to eliminate retained water, followed by sintering at 1300 °C in a resistance furnace for 40 min. AFter that, the sintered material was rapidly cooled using an electric fan to prevent mineral phase decomposition, obtaining CSA cement clinker. The cement clinker was subsequently mixed with 10% gypsum and ball-milled until the powder achieved a specific surface area of 350 (±10) m2/kg, yielding CSA cement.

2.4. Cement Hydration Heat Testing

The hydration heat of cement was determined using isothermal calorimetry, following the procedures outlined in ASTM C1702 [37]. Cement samples were mixed with deionized water at a water–cement ratio of 0.45 to form a homogeneous paste. This paste was then transferred into a sealed sample cell and placed within a TAM Air isothermal calorimeter maintained at a constant temperature of 20 ± 0.1 °C. Heat flow and cumulative heat release were continuously monitored for 24 h.

2.5. Hardened Cement Performance Testing

Cement paste specimens were prepared at a water–cement ratio of 0.45 using standardized steel cube molds (20 mm × 20 mm × 20 mm). Cement was added to the water, followed by rapid mixing for 3 min before the paste was cast into molds. Demolding was performed 24 h after casting, followed by curing in a controlled environment chamber (relative humidity ≥ 95%, temperature 20 ± 2 °C) until designated testing ages.
(a)
Compressive Strength
Specimens cured for 1, 3, 7, and 28 days were subjected to compressive strength testing using a servo-controlled hydraulic testing machine (UTM-5000 series). Cubic specimens were axially loaded at a constant displacement rate of 0.6 MPa/s until failure. Triplicate samples were tested at each curing stage, with results reported as mean values ± standard deviation.
  • (b) X-Ray Diffraction (XRD)
Samples cured for 1 day were dried in a constant-temperature oven at 60 °C for 72 h, then pulverized and sieved through a 200 mesh (75 μm) screen. Mineralogical phase analysis was conducted using a Bruker D8 Advance X-ray diffractometer (Billerica, MA, USA) equipped with Cu-Kα radiation (λ = 1.5406 Å). Continuous scans were performed over a 2θ range of 5–90° with a step size of 0.01° and scan rate of 2°/min.
  • (c) Mercury Intrusion Porosimetry (MIP)
Specimens cured for 1 day were dried in a 60 °C oven for 72 h, then broken into small pieces with approximate dimensions of 5 mm3. A Micromeritics AutoPore IV 9600 mercury intrusion porosimeter (Micromeritics, Norcross, GA, USA) was used to analyze the porous microstructure of the fractured samples, with a pressure range of 0.1 to 60,000 psia.
  • (d) Scanning Electron Microscopy (SEM)
Specimens cured for 1 day were dried in a 60 °C oven for 72 h, then fractured into thin flakes with an approximate area of 5 mm × 5 mm. These flakes were mounted on aluminum stubs and sputter-coated with a thin layer of gold. The surface morphology of the samples was observed using a high-resolution scanning electron microscope (Zeiss Sigma 300, Oberkochen, Germany).

3. Results and Discussion

3.1. Clinker Composition

XRD analysis was conducted on cement clinkers prepared under different compositional targets, including varying ferrite-phase contents and varying C2S contents (Figure 2 and Figure 3). Across all samples, the primary mineral phases consistently identified were C4A3Š, C2S, and the ferrite phase, including C4AF and dicalcium ferrite (C2F, Ca2Fe2O5). Additionally, the metastable intermediate phase gehlenite (C2AS, Ca2Al2SiO7), a low-reactivity transitional product, was observed in certain samples. Comparative analysis of diffraction peak intensities confirmed that the experimental mineral assemblages generally aligned with the designed targets. To compare the variations in mineral phases among the groups, quantitative analysis was performed using TOPAS-Academic (Bruker, Ettlingen, Germany). The fitting index (Rwp) for all refinements was controlled to be below 10%. Analysis patterns are shown in Figure 4.
Based on the quantitative analysis patterns shown in Figure 4, the proportion of each mineral was statistically analyzed, and the results are presented in Figure 5 and Figure 6. Figure 5 shows the mineral composition of cement clinkers with varying target ferrite-phase contents. Specifically, it was observed that at lower target ferrite-phase contents, the C4A3Š content was consistently lower than the target values. As the target ferrite-phase content increased, the measured C4A3Š content progressively approached the target design value. This trend suggests that elevated ferrite-phase content enhances the formation and development of C4A3Š. Notably, when the target ferrite-phase content exceeded 20%, the determined C4A3Š content was slightly higher than the target value. This could potentially be attributed to the formation of a C4A3−xFxŠ solid solution during clinker burning, involving the substitution of aluminum by iron atoms within the C4A3Š structure [38,39,40]. Simultaneously, analysis of the C4AF content across the different groups revealed that the experimentally determined values were consistently lower than their target values. This discrepancy may be primarily due to two factors: firstly, the formation of other iron-bearing mineral phases such as C2F, whose content increased with increasing target ferrite phase content; and secondly, iron entering the C4A3Š phase, as mentioned previously. Furthermore, at lower ferrite-phase contents, the C2S content was lower than the target value, and the content of the C2AS was relatively high. Conversely, as the target ferrite-phase content increased, the C2S content approached the target value, while the C2AS content progressively decreased. This observation indicates that the presence of the ferrite phase promotes the formation and stabilization of C2S. Mechanistically, during clinkering, the ferrite phase acts as a flux, lowering the eutectic temperature of the raw mix and facilitating the formation of the crystalline structure [41]. In summary, ferrite phases in CSA cement clinker primarily exist as C4AF and C2F. The increase in target ferrite-phase content is beneficial for the formation and stability of both C4A3Š and C2S. This trend underscores the critical role of ferrite-phase content in modulating competitive phase equilibria and suppressing potentially deleterious intermediate phases like C2AS, providing actionable insights for optimizing raw mix design in industrial cement production.
Figure 6 shows mineral composition of cement clinkers under fixed target ferrite-phase content but varying C2S contents. With the target ferrite-phase content fixed, an increase in the target C2S content leads to a significant decrease in the actual amount of C4AF formed in the synthesized clinker, gradually deviating from the initially set target value. Concurrently, this is accompanied by an increased formation of low-activity C2F. This phenomenon suggests that simply increasing the target C2S content can interfere with the normal formation of C4AF, resulting in the formation of the less reactive C2F instead of the more reactive C4AF from the raw materials. Given the hydration activity, an increase in C2F content negatively impacts clinker performance. Therefore, it is crucial to carefully consider the influence of C2S content adjustments on the ferrite-phase composition and to precisely control the target value of C2S during the synthesis process.

3.2. Hydration Characteristics

The hydration heat release process of cement samples B, F1, and F2 with different ferrite-phase contents was tested. Figure 7 and Figure 8 show the hydration heat flow curves and cumulative heat release curves of the cement with different target iron phases. From Figure 8, it can be seen that the total heat release of the three groups of samples in this study is relatively close, all around 240 J/g after 1 day.
As shown in Figure 7a, the heat flow curve of the samples has three heat release peaks. The first heat release peak is mainly due to the heat released from the dissolution of clinker particles, accompanied by the rapid hydration of a small amount of sulfoaluminate phase in the clinker with gypsum, marking the induction period of cement hydration [42,43]. Comparing the first heat release peaks of different target ferrite contents, it can be observed that as the target ferrite content increases, the first heat release peak decreases. This is because the iron solid solution and iron-alumina phase in the clinker minerals dissolve more slowly compared to the sulfoaluminate phase, resulting in a lower dissolution peak. The induction period for the three samples is similar, all ending within 1 h.
According to Figure 7b, the samples exhibit a second and a third heat release peak, corresponding to two acceleration/decay periods of the cement. The second heat release peak occurs around 4 h, primarily due to the reaction with gypsum to form AFt, accompanied by the hydration of some ferrite phase minerals [44,45]. Around 6 h, the third heat release peak appears, mainly due to the further hydration of C4A3Š and ferrite phase minerals. Comparing the heat release rates of different samples, it can be found that as the target ferrite content increases, the heat release rate decreases, and the duration of the second heat release peak increases. This may be because the increase in ferrite-phase content is accompanied by a decrease in the target design value of C4A3Š, thereby resulting in a reduction in heat flow during the first acceleration phase and an increase in the duration of the second acceleration phase.

3.3. Cement Strength Development

Figure 9 illustrates the compressive strength evolution of cements with varying target ferrite-phase contents at 1 d, 3 d, 7 d, and 28 d. All five groups exhibit excellent early and long-term strength performance, characterized by high early-age strength: 1 d compressive strength exceeds 24.0 MPa (maximum 30.0 MPa). This is attributed to rapid hydration of C4A3Š or ferrite-phase minerals and gypsum, promoting swift ettringite (AFt) formation that reinforces the hardened paste. Long-term strength progressively increases, reaching >50.0 MPa at 28 d, driven by sustained hydration of ferrite phases and C2S.
Comparing the strength of samples with different target ferrite-phase contents, it can be observed that as the target ferrite-phase content increases, the overall strength shows a trend of first increasing and then decreasing. This is because, when the ferrite-phase content is within an appropriate range, the presence of the ferrite phase can ensure the development and stability of C4A3Š and C2S during clinkering, maintaining the content of active minerals. The maximum strength improvement is achieved when the target ferrite-phase content is set to 15%, showing a 25.1% increase in 1 d strength and an 11.5% increase in 28 d strength. However, when the ferrite-phase content is too high, the increase in low-activity C2F may negatively affect the strength development of the samples. This study suggests that the reasonable target ferrite-phase range is between 15% and 20%.
Additionally, it can be observed that the growth of compressive strength from 1 day to 3 days is relatively gentle, with a low growth rate, while the strength growth from 3 days to 28 days is significant, and the growth rate of strength at 28 days shows an increasing trend with the increase in ferrite-phase content. This indicates that the strength from 1 day to 3 days mainly depends on the content of early-strength minerals; after 3 days, the ferrite-phase minerals and C2S gradually participate in the reaction, and the development of strength at 28 days should primarily depend on the hydration of C4AF and C2S.
Figure 10 shows the compressive strength of cement with varying C2S contents at 1 day, 3 days, 7 days, and 28 days. As can be seen from the figure, increasing C2S content leads to a decrease in early strength (in the first 7 days), which is due to the reduced content of C4A3Š in the cement, resulting in a lower amount of AFt formation that provides early strength. However, the later strength development rate is relatively fast, indicating that the high content of C2S has a significant effect on later strength.

3.4. Microstructural Analysis

Hardened cement specimens cured for 1 day were subjected to microstructural characterization, including hydration product composition, microporous structure, and microscopic morphology.

3.4.1. Hydration Product Composition

Based on the composition of high-ferrite CSA, C4A3Š and C4AF can react with gypsum (CaSO4·2H2O, CŠH2) respectively to form ettringite (AFt), aluminum gel (Al(OH)3, AH3), and iron gel (Fe(OH)3, FH3). The hydration reactions are proposed as follows (Equations (3a,b)) [21,45,46,47]:
C 4 A 3 Š + C Š H 2 + H A f t + A H 3 ( g e l )
C 4 A F + C Š H 2 + H A f t + F H 3 ( g e l )
XRD patterns of hydration products at 1 day (Figure 11 and Figure 12) confirm that AFt is the dominant crystalline phase across all samples, consistent with theoretical predictions. Meanwhile, a prominent amorphous halo is consistently observed in the XRD patterns of all samples, indicating the presence of a considerable quantity of non-crystalline or poorly crystalline material. Considering the well-established tendency of Al(OH)3 and Fe(OH)3 to form as amorphous gels during hydration [48], their presence likely contributes significantly to this observed diffuse scattering signal. Additionally, unhydrated clinker phases—such as C4A3Š, C2S, C4AF, C2F and C2AS—were identified, reflecting incomplete hydration at this early stage. Comparative analysis of clinker and hydration product XRD patterns reveals a significant reduction in C4A3Š content, whereas C2AS remains largely unchanged due to its low reactivity. Notably, the AFt content exhibits a non-linear dependence on ferrite content: it initially increases with moderate ferrite elevation (≤20%) but declines at higher levels (>20%). This trend correlates with the reduced C4A3Š content in high-ferrite clinkers, thereby limiting the sulfate–aluminate reaction essential for AFt formation.
Figure 12 presents the XRD patterns of hydration products at 1 day for samples with a fixed target ferrite-phase content but varying C2S contents. As shown in the figure, increasing the target C2S content appears to have minimal influence on the types and proportions of the hydration products at this early age. This observation is likely attributable to the relatively slow hydration rate of C2S, as indicated by the persistently high diffraction peaks of unreacted C2S visible in the patterns. Furthermore, with increasing target C2S content, the hydration of the C4A3Š phase becomes progressively more complete. Notably, in the F3S2 sample, the diffraction peaks of C4A3Š are almost undetectable. This trend highlights that the early strength development of these CSA-based systems is predominantly driven by the hydration products of C4A3Š, primarily AFt. Conversely, C2S is likely to contribute more significantly to the later-age strength of the material.

3.4.2. Microporous Structure

MIP tests were conducted to quantify the porosity, average pore diameter, and pore structure of samples at 1 day hydration (Figure 13 and Figure 14). Results reveal total porosity and average pore diameter initially decrease with increasing target ferrite content but rebound at higher levels (>15%). Notably, the sample with 15% target ferrite content (Group F1) achieves optimal pore refinement, exhibiting the lowest porosity (24.1%) and smallest average pore diameter (29.4 nm). This trend is attributed to the dual role of ferrite phases: (1) moderate target ferrite content (≤15%) enhances micro-aggregate filling effects, refining pore size distribution and reducing connectivity via dense packing of nano-scale C4AF particles; (2) excessive target ferrite content (>15%) impedes early hydration reactions, inducing localized porous structures due to incomplete dissolution of Fe-rich phases and interfacial debonding at boundaries. Concurrently, the proportion of pores >100 nm increases slightly with ferrite elevation, reflecting compromised microstructure homogeneity under high-ferrite conditions.

3.4.3. Microstructural Morphology

Figure 15 illustrates the SEM microstructural characteristics of samples after 1 day hydration. In experimental groups B, F1, and F3, abundant needle-like or rod-shaped ettringite (AFt) crystals with smooth surfaces, sharp boundaries, and uniform geometric dimensions (length: 1–2 µm; diameter: 0.1–0.3 µm) are clearly observed. These AFt crystals exhibit typical radial or clustered growth patterns, forming an interlocked structure with amorphous or fibrillar calcium silicate hydrate (C-S-H) gel. Specifically, the AFt crystalline framework is embedded within the flocculated C-S-H matrix, collectively constructing a dense early-stage hydration network that contributes to superior initial mechanical strength [49,50]. Notably, the AFt crystals in groups F1 and F3 demonstrate significantly larger dimensions (up to 2.5 µm in length), higher spatial density, and more pronounced clustering compared to group B, suggesting that optimized iron content enhances AFt crystal growth and stabilization.
In contrast, AFt crystal abundance is drastically reduced and spatially dispersed, while the C-S-H gel transitions from dense agglomerates to a loose network in groups F1S1, F3S1, and F3S2. Additionally, irregular smooth-surfaced particles with sharp edges (average size: 1.5–3 µm) are distributed throughout the matrix, identified as unreacted ferrite (C4AF) and C2S particles from the clinker. This microstructural evolution indicates that excessive ferrite and C2S content reduces early (1 d) hydration kinetics, delays reaction progress, and retards hydration product formation—a conclusion consistent with the mechanical performance data. These findings further validate the pivotal role of C4AF and C2S in modulating early hydration behavior, highlighting the need for balanced stoichiometric control in cement formulation.

4. Conclusions

This study demonstrates the critical impact of enhancing ferrite-phase composition on the properties of CSA cement, with key findings as follows:
  • The ferrite phase plays a critical role in regulating the mineralogical evolution of CSA clinker. Higher ferrite-phase content helps C4A3Š and C2S align more closely with their corresponding target design values, demonstrating that the ferrite phase promotes their stabilization during clinkering while reducing low-activity transitional products like C2AS.
  • The hydration characteristics of CSA cements are modulated by ferrite-phase content as evidenced by three distinct heat release peaks. Increasing ferrite phase suppresses the initial dissolution peak and prolongs the secondary reaction stage (4–6 h) by reducing AFt formation rates as ferrite phases partially replace sulfoaluminate components.
  • Moderate ferrite-phase content (15–20%) optimizes the strength development of calcium sulfoaluminate (CSA) cement: Early-stage strength (1–3 days) improves due to the ferrite phase (C4AF) promoting rapid nucleation of ettringite (AFt), while later-stage strength (28 days) benefits from pore structure refinement through secondary reaction products of the ferrite phase, achieving a balance between early hydration activity and long-term microstructural optimization.
  • Excessive ferrite content (>25%) causes adverse effects in the strength development of CSA: During clinkering, an elevated Fe2O3/Al2O3 ratio reduces C4A3Š formation and limits early AFt production, while increased proportions of low-reactivity C2F further degrade performance.

Author Contributions

Validation, J.M.; Formal analysis, C.W.; Investigation, K.H. and Y.B.; Data curation, Y.S., K.H. and A.Z.; Writing—original draft, S.L.; Writing—review & editing, Y.B.; Visualization, A.Z.; Supervision, G.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by Ningbo Public Welfare Science and Technology Plan Project (Grant No. 2023S056), Zhejiang Provincial Natural Science Foundation of China under Grant No.LQN25E080009, and the Higher Education Science Research Project of Anhui Province (No.2022AH052607).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

Author Guogang Ying was employed by the company Ningbo Langda Technology Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Andrew, R.M. Global CO2 emissions from cement production. Earth Syst. Sci. Data 2018, 10, 195–217. [Google Scholar] [CrossRef]
  2. Habert, G.; Miller, S.A.; John, V.M.; Provis, J.L.; Favier, A.; Horvath, A.; Scrivener, K.L. Environmental impacts and decarbonization strategies in the cement and concrete industries. Nat. Rev. Earth Environ. 2020, 1, 559–573. [Google Scholar] [CrossRef]
  3. Juenger, M.C.G.; Winnefeld, F.; Provis, J.L.; Ideker, J.H. Advances in alternative cementitious binders. Cem. Concr. Res. 2011, 41, 1232–1243. [Google Scholar] [CrossRef]
  4. Scrivener, K.L.; John, V.M. Gartner Eco-efficient cements: Potential economically viable solutions for a low-CO2 cement-based materials industry. Cem. Concr. Res. 2018, 114, 2–26. [Google Scholar] [CrossRef]
  5. Glasser, F.P.; Zhang, L. High-performance cement matrices based on calcium sulfoaluminate–Belite compositions. Cem. Concr. Res. 2001, 31, 1881–1886. [Google Scholar] [CrossRef]
  6. Péra, J.; Ambroise, J. New applications of calcium sulfoaluminate cement. Cem. Concr. Res. 2004, 34, 671–676. [Google Scholar] [CrossRef]
  7. Hargis, C.W.; Telesca, A.; Monteiro, P.J. Calcium sulfoaluminate (Ye’elimite) hydration in the presence of gypsum, calcite, and vaterite. Cem. Concr. Res. 2014, 65, 15–20. [Google Scholar] [CrossRef]
  8. Canbek, O.; Erdoğan, S.T. Influence of production parameters on calcium sulfoaluminate cements. Constr. Build. Mater. 2020, 239, 117866. [Google Scholar] [CrossRef]
  9. Tang, X.; Zhan, S.; Xu, Q.; He, K. Mechanical performance and chloride penetration of calcium sulfoaluminate concrete in marine tidal zone. Materials 2023, 16, 2905. [Google Scholar] [CrossRef]
  10. Wang, L.; Zhou, H.; Lian, S.; Tang, X. Drying–Wetting Correlation Analysis of Chloride Transport Behavior and Mechanism in Calcium Sulphoaluminate Cement Concrete. Materials 2024, 17, 4600. [Google Scholar] [CrossRef]
  11. Tan, B.; Okoronkwo, M.U.; Kumar, A.; Ma, H. Durability of calcium sulfoaluminate cement concrete. J. Zhejiang Univ. Sci. A 2020, 21, 118–128. [Google Scholar] [CrossRef]
  12. Tang, J.; Zhang, D.; Ma, G.; Ji, X.; Zhou, W. Early Hydration of Calcium Sulfoaluminate Cement at Elevated Temperatures. ACS Sustain. Chem. 2024, 12, 13654–13668. [Google Scholar] [CrossRef]
  13. Andac, Ö.; Glasser, F.P. Microstructure and microchemistry of calcium sulfoaluminate cement. MRS Online Proc. Libr. (OPL) 1994, 370, 143. [Google Scholar] [CrossRef]
  14. Park, S.; Jeong, Y.; Moon, J.; Lee, N. Hydration characteristics of calcium sulfoaluminate (CSA) cement/portland cement blended pastes. J. Build. Eng. 2021, 34, 101880. [Google Scholar] [CrossRef]
  15. Winnefeld, F.; Lothenbach, B. Hydration of calcium sulfoaluminate cements—Experimental findings and thermodynamic modelling. Cem. Concr. Res. 2010, 40, 1239–1247. [Google Scholar] [CrossRef]
  16. Sánchez-Herrero, M.J.; Fernández-Jiménez, A.; Palomo, A. C4A3Š hydration in different alkaline media. Cem. Concr. Res. 2013, 46, 41–49. [Google Scholar] [CrossRef]
  17. Telesca, A.; Marroccoli, M.; Pace, M.L.; Tomasulo, M.; Valenti, G.L.; Monteiro, P.J.M. A hydration study of various calcium sulfoaluminate cements. Cem. Concr. Compos. 2014, 53, 224–232. [Google Scholar] [CrossRef]
  18. Ye, S.; Feng, P.; Liu, J. Dissolution and early hydration of tetracalcium aluminoferrite (C4AF) in water and in aqueous sulfate solutions. Cem. Concr. Res. 2024, 186, 107676. [Google Scholar] [CrossRef]
  19. Mrak, M.; Winnefeld, F.; Lothenbach, B.; Dolenec, S. The influence of calcium sulfate content on the hydration of belite-calcium sulfoaluminate cements with different clinker phase compositions. Mater. Struct. 2021, 54, 1–17. [Google Scholar] [CrossRef]
  20. Seo, J.; Nawaz, A.; Jang, J.G.; Lee, H.K. Modifications in hydration kinetics and characteristics of calcium aluminate cement upon blending with calcium sulfoaluminate cement. Constr. Build. Mater. 2022, 342, 127958. [Google Scholar] [CrossRef]
  21. Cheng, Z.; Zhao, J.; Cui, L. Exploration of hydration and durability properties of ferroaluminate cement with compare to Portland cement. Constr. Build. Mater. 2022, 319, 126138. [Google Scholar] [CrossRef]
  22. Shao, Y.; Lu, X.; Li, Q.; Dong, Y.; Zhang, L.; Jiang, C.; Cheng, X. Study on the preparation and sulfate resistance of Portland cement clinker with the high Fe/Al ratio of ferrite phase. Cem. Concr. Compos. 2022, 134, 104699. [Google Scholar] [CrossRef]
  23. Zhang, P.; Qi, D.; Hao, L.; Wang, Z.; Liu, H.; Zhang, D.; Xie, Y.; Zhao, E. Effect of w/b ratio and supplemental cementitious material on the chloride penetration and corrosion resistance of ferroaluminate cement concrete. Constr. Build. Mater. 2024, 431, 136481. [Google Scholar] [CrossRef]
  24. Zhu, H.; Zhao, J.; Li, Z. Investigations on the hydration characteristics of blended ferroaluminate cement containing granulated blast furnace slag. Constr. Build. Mater. 2024, 417, 135243. [Google Scholar] [CrossRef]
  25. Xue, J.; Li, S.; Zhang, Z.; Liu, S.; Li, G.; Guan, X. Hydration, mechanical properties, and corrosion resistance of ferroaluminate cement in the presence of FA and GGBS. J. Build. Eng. 2025, 102, 111974. [Google Scholar] [CrossRef]
  26. Zhang, X.; Lu, X.L.; Feng, J.R.; Zheng, G.F.; Yang, Q.C.; Du, P.; Zhu, J.; Cheng, X. Calcium ferroaluminate cements made with red mud: Synthetic issues and mechanical properties. Ceram. Silikáty 2024, 68, 195–204. [Google Scholar] [CrossRef]
  27. Shi, N.; Ma, Y.; Zhang, X.; Li, J.; Lu, X.; Zhang, L.; Cheng, X. The Effect of Calcium Sulfate on the Hydration and Properties of Red Mud-Based Calcium Ferroaluminate Cement Clinker. Materials 2024, 17, 5064. [Google Scholar] [CrossRef]
  28. Iacobescu, R.I.; Pontikes, Y.; Koumpouri, D.; Angelopoulos, G.N. Synthesis, characterization and properties of calcium ferroaluminate belite cements produced with electric arc furnace steel slag as raw material. Cem. Concr. Compos. 2013, 44, 1–8. [Google Scholar] [CrossRef]
  29. Wu, S.; Yao, X.; Ren, C.; Yao, Y.; Zhang, C.; Wu, C.; Wang, W. Effect of iron on the preparation of iron-rich calcium sulfoatablluminate cement using gypsum as the sole calcium oxide source and its incorporation into mineral phases. Constr. Build. Mater. 2021, 290, 123214. [Google Scholar] [CrossRef]
  30. Yao, X.; Yang, S.; Huang, Y.; Wu, S.; Yao, Y.; Wang, W. Effect of CaSO4 batching in raw material on the iron-bearing mineral transition of ferric-rich sulfoaluminate cement. Constr. Build. Mater. 2020, 250, 118783. [Google Scholar] [CrossRef]
  31. Zheng, M.; Huang, J.; Yang, M.; Song, B.; Yang, L.; Wang, F. A composite low-carbon cement strategy: High ferrite cement with addition of ferroaluminate cement. Constr. Build. Mater. 2024, 456, 139250. [Google Scholar] [CrossRef]
  32. Liao, Y.; Cai, Z.; Deng, F.; Ye, J.; Wang, K.; Tang, S. Hydration behavior and thermodynamic modelling of ferroaluminate cement blended with steel slag. J. Build. Eng. 2024, 97, 110833. [Google Scholar] [CrossRef]
  33. Wu, S.; Cui, Y.; Yao, X.; Ren, C.; Yao, Y.; Wang, W. Preparation of iron-rich sulfoaluminate cement by regulating Fe-bearing minerals. Ceram. Int. 2025, in press. [CrossRef]
  34. Meng, F.; Lu, D.; Wang, G.; Wang, S.; Zhou, X.; Du, X. Experimental study on pore structures and mechanical properties of ferroaluminate cement under sulfate attack. J. Build. Eng. 2024, 97, 110905. [Google Scholar] [CrossRef]
  35. Bogue, R.H. Calculation of the compounds in Portland cement. Ind. Chem. Anal. Ed. 1929, 1, 192–197. [Google Scholar] [CrossRef]
  36. Chen, I.A.; Juenger, M.C. Incorporation of coal combustion residuals into calcium sulfoaluminate-belite cement clinkers. Cem. Concr. Compos. 2012, 34, 893–902. [Google Scholar] [CrossRef]
  37. ASTM C1702; Standard Test Method for Measurement of Heat of Hydration of Hydraulic Cementitious Materials Using Isothermal Conduction Calorimetry. ASTM: West Conshohocken, PA, USA, 2017.
  38. Abir, F.Z.; Mesnaoui, M.; Abouliatim, Y.; Nibou, L.; Labbilta, T.; El Hafiane, Y.; Smith, A. Effect of the addition of iron oxide on the microstructure of ye’elimite. Cem. Concr. Res. 2022, 151, 106625. [Google Scholar] [CrossRef]
  39. Ndzila, J.S.; Liu, S.; Jing, G.; Wang, S.; Ye, Z. The effect of Fe3+ ion substitution on the crystal structure of ye’elimite. Ceram. Silik 2020, 64, 18–28. [Google Scholar] [CrossRef]
  40. Irico, S.; Gastaldi, D.; Canonico, F.; Magnacca, G. Investigation of the microstructural evolution of calcium sulfoaluminate cements by thermoporometry. Cem. Concr. Res. 2013, 53, 239–247. [Google Scholar] [CrossRef]
  41. Tao, Y.; Wan, D.; Zhang, W.; Wang, F.; Hu, S. Intrinsic reactivity and dissolution characteristics of tetracalcium aluminoferrite. Cem. Concr. Res. 2021, 146, 106485. [Google Scholar] [CrossRef]
  42. Zhang, K.; Shen, P.; Yang, L.; Rao, M.; Wang, F. Improvement of the hydration kinetics of high ferrite cement: Synergic effect of gypsum and C3S–C4AF systems. ACS Sustain. Chem. 2021, 9, 15127–15137. [Google Scholar] [CrossRef]
  43. Lu, X.; Ye, Z.; Wang, S.; Du, P.; Li, C.; Cheng, X. Study on the preparation and properties of belite-ye’elimite-alite cement. Constr. Build. Mater. 2018, 182, 399–405. [Google Scholar] [CrossRef]
  44. Bullerjahn, F.; Zajac, M.; Haha, M.B.; Scrivener, K.L. Factors influencing the hydration kinetics of ye’elimite; effect of mayenite. Cem. Concr. Res. 2019, 116, 113–119. [Google Scholar] [CrossRef]
  45. Winnefeld, F.; Martin, L.H.; Müller, C.J.; Lothenbach, B. Using gypsum to control hydration kinetics of CSA cements. Constr. Build. Mater. 2017, 155, 154–163. [Google Scholar] [CrossRef]
  46. Hargis, C.W.; Kirchheim, A.P.; Monteiro, P.J.; Gartner, E.M. Early age hydration of calcium sulfoaluminate (synthetic ye’elimite, C4A3S) in the presence of gypsum and varying amounts of calcium hydroxide. Cem. Concr. Res. 2013, 48, 105–115. [Google Scholar] [CrossRef]
  47. Winnefeld, F.; Barlag, S. Calorimetric and thermogravimetric study on the influence of calcium sulfate on the hydration of ye’elimite. J. Therm. Anal. Calorim. 2010, 101, 949–957. [Google Scholar] [CrossRef]
  48. Cuesta, A.; Ichikawa, R.U.; Londono-Zuluaga, D.; De la Torre, A.G.; Santacruz, I.; Turrillas, X.; Aranda, M.A. Aluminum hydroxide gel characterization within a calcium aluminate cement paste by combined Pair Distribution Function and Rietveld analyses. Cem. Concr. Res. 2017, 96, 1–12. [Google Scholar] [CrossRef]
  49. Tang, X.; Xu, Q.; Qian, K.; Ruan, S.; Lian, S.; Zhan, S. Effects of cyclic seawater exposure on the mechanical performance and chloride penetration of calcium sulfoaluminate concrete. Constr. Build. Mater. 2021, 303, 124139. [Google Scholar] [CrossRef]
  50. Londono-Zuluaga, D.; Tobón, J.I.; Aranda, M.A.G.; Santacruz, I.; De la Torre, A.G. Clinkering and hydration of belite-alite-yeīelimite cement. Cem. Concr. Compos. 2017, 80, 333–341. [Google Scholar] [CrossRef]
Figure 1. Cement production process.
Figure 1. Cement production process.
Materials 18 02457 g001
Figure 2. XRD patterns of cement clinkers with varying target ferrite-phase contents.
Figure 2. XRD patterns of cement clinkers with varying target ferrite-phase contents.
Materials 18 02457 g002
Figure 3. XRD patterns of cement clinkers under fixed target ferrite-phase content but varying C2S contents: (a) Target ferrite phase of 15%; (b) Target ferrite phase of 25%.
Figure 3. XRD patterns of cement clinkers under fixed target ferrite-phase content but varying C2S contents: (a) Target ferrite phase of 15%; (b) Target ferrite phase of 25%.
Materials 18 02457 g003
Figure 4. Quantitative phase analysis patterns of samples.
Figure 4. Quantitative phase analysis patterns of samples.
Materials 18 02457 g004
Figure 5. Mineral composition of cement clinkers with varying target ferrite-phase contents.
Figure 5. Mineral composition of cement clinkers with varying target ferrite-phase contents.
Materials 18 02457 g005
Figure 6. Mineral composition of cement clinkers under fixed target ferrite-phase content but varying C2S contents.
Figure 6. Mineral composition of cement clinkers under fixed target ferrite-phase content but varying C2S contents.
Materials 18 02457 g006
Figure 7. Hydration heat flow of cement with different target ferrite phases: (a) induction period; (b) acceleration/decay period.
Figure 7. Hydration heat flow of cement with different target ferrite phases: (a) induction period; (b) acceleration/decay period.
Materials 18 02457 g007
Figure 8. Cumulative hydration heat of cement with different target ferrite phases.
Figure 8. Cumulative hydration heat of cement with different target ferrite phases.
Materials 18 02457 g008
Figure 9. Compressive strength development of cements with varying target ferrite-phase contents.
Figure 9. Compressive strength development of cements with varying target ferrite-phase contents.
Materials 18 02457 g009
Figure 10. Compressive strength development of cements with fixed target ferrite-phase content but varying C2S contents: (a) target ferrite phase of 15%; (b) target ferrite phase of 25%.
Figure 10. Compressive strength development of cements with fixed target ferrite-phase content but varying C2S contents: (a) target ferrite phase of 15%; (b) target ferrite phase of 25%.
Materials 18 02457 g010
Figure 11. XRD patterns of hydration products at 1 day with varying target ferrite-phase contents.
Figure 11. XRD patterns of hydration products at 1 day with varying target ferrite-phase contents.
Materials 18 02457 g011
Figure 12. XRD patterns of hydration products at 1 day with fixed target ferrite-phase content but varying C2S contents: (a) target ferrite phase of 15%; (b) target ferrite phase of 25%.
Figure 12. XRD patterns of hydration products at 1 day with fixed target ferrite-phase content but varying C2S contents: (a) target ferrite phase of 15%; (b) target ferrite phase of 25%.
Materials 18 02457 g012
Figure 13. Porosity and average pore size of samples at 1 day hydration.
Figure 13. Porosity and average pore size of samples at 1 day hydration.
Materials 18 02457 g013
Figure 14. Pore structure of samples at 1 day hydration.
Figure 14. Pore structure of samples at 1 day hydration.
Materials 18 02457 g014
Figure 15. SEM images of samples after 1 day hydration.
Figure 15. SEM images of samples after 1 day hydration.
Materials 18 02457 g015
Table 1. Principal chemical compositions of raw materials (wt%).
Table 1. Principal chemical compositions of raw materials (wt%).
CaOSiO2Al2O3Fe2O3MgOTiO2SO3Loss
Limestone51.162.260.740.414.16-0.1140.55
Bauxite0.8130.8946.516.120.172.230.1112.13
Gypsum28.711.930.900.290.730.0343.9822.30
Table 2. Trace element composition of raw materials (wt%).
Table 2. Trace element composition of raw materials (wt%).
P2O5ClCr2O3MnOCuOSrOZrO2
Limestone0.05530.0499-0.0196-0.0125-
Bauxite0.14410.02020.02900.01140.00530.02020.0457
Gypsum0.02020.0855---0.0171-
Table 3. Target mineralogical compositions for the cement clinker (%).
Table 3. Target mineralogical compositions for the cement clinker (%).
SamplesC4A3ŠC2SC4AF
B4445101
F13945151
F23445201
F32945251
F42445301
F1S13450151
F1S22955151
F3S12450251
F3S21955251
Table 4. Raw material ratios for experimental samples (%).
Table 4. Raw material ratios for experimental samples (%).
SamplesLimestoneBauxiteSiO2Fe2O3Gypsum
B57.4833.27009.25
F158.7131.320.391.268.32
F259.8629.321.022.447.36
F361.0127.321.643.626.41
F462.1725.312.264.815.45
F1S160.8527.782.571.477.34
F1S262.9724.264.741.676.36
F3S163.1423.783.823.825.43
F3S265.2620.275.984.024.47
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Lian, S.; Shao, Y.; Wang, C.; Bi, Y.; Ma, J.; Han, K.; Zhu, A.; Ying, G. Unveiling the Influence and Mechanisms of Enhancing Ferrite-Phase Composition on the Properties of Calcium Sulfoaluminate Cement. Materials 2025, 18, 2457. https://doi.org/10.3390/ma18112457

AMA Style

Lian S, Shao Y, Wang C, Bi Y, Ma J, Han K, Zhu A, Ying G. Unveiling the Influence and Mechanisms of Enhancing Ferrite-Phase Composition on the Properties of Calcium Sulfoaluminate Cement. Materials. 2025; 18(11):2457. https://doi.org/10.3390/ma18112457

Chicago/Turabian Style

Lian, Songsong, Yu Shao, Chenyu Wang, Yutian Bi, Jiaxing Ma, Kangzhan Han, Anzhe Zhu, and Guogang Ying. 2025. "Unveiling the Influence and Mechanisms of Enhancing Ferrite-Phase Composition on the Properties of Calcium Sulfoaluminate Cement" Materials 18, no. 11: 2457. https://doi.org/10.3390/ma18112457

APA Style

Lian, S., Shao, Y., Wang, C., Bi, Y., Ma, J., Han, K., Zhu, A., & Ying, G. (2025). Unveiling the Influence and Mechanisms of Enhancing Ferrite-Phase Composition on the Properties of Calcium Sulfoaluminate Cement. Materials, 18(11), 2457. https://doi.org/10.3390/ma18112457

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics