Next Article in Journal
Improved Thermal and Electrical Properties of P-I-N-Structured Perovskite Solar Cells Using ZnO-Added PCBM as Electron Transport Layer
Previous Article in Journal
Mesoporous Carbons and Highly Cross-Linking Polymers for Removal of Cationic Dyes from Aqueous Solutions—Studies on Adsorption Equilibrium and Kinetics
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Influence of Tempering Temperature on Mechanical and Rotational Bending Fatigue Properties of 40CrNi2MoE Steel

1
Institute of Special Steels, Central Iron and Steel Research Institute Co., Ltd., Beijing 100081, China
2
Tianjin Heavy Industries Research & Development Co., Ltd., Tianjin 300457, China
*
Author to whom correspondence should be addressed.
Materials 2024, 17(6), 1377; https://doi.org/10.3390/ma17061377
Submission received: 10 January 2024 / Revised: 19 February 2024 / Accepted: 24 February 2024 / Published: 17 March 2024
(This article belongs to the Section Metals and Alloys)

Abstract

:
In order to examine the mechanical properties and rotational bending fatigue performance of 40CrNi2MoE steel subsequent to tempering at varying temperatures, the steel specimen was subjected to tempering within the range of 400~460 °C. SEM, EBSD, and TEM were used to analyze the microstructure as well as precipitates. The strain hardening law was studied using the modified Crussard–Jaoult method. Investigations were undertaken to reveal the rotational bending fatigue life with respect to the tempering temperature. The findings indicate that the strength and fatigue life of the examined steels exhibit a decline as the tempering temperature increases, with the primary factor affecting this trend being the alteration in dislocation density. No notable impact on the fatigue fracture morphology exerted by tempering temperature was found within the range of the experiment. The C–J model analysis reveals that the work-hardening behavior of the trial steels is influenced by dislocations and the second phase.

1. Introduction

40CrNi2MoE steel, belonging to the nickel–chromium–molybdenum series of low-alloy ultra-high-strength steels, epitomizes exemplary material characteristics, including notable strength, toughness, and favorable hardenability. As a result, its usage spans a wide range of applications, prominently in the manufacture of vital components like aircraft landing gears [1,2].
Extensive investigations have been devoted to exploring the influence of various heat treatment protocols, specifically austenitizing temperature, tempering temperature, and cryogenic treatment, on the metallurgical structure and mechanical properties of 40CrNi2MoE steel. Manokaran [3] has studied the influence of different melting routes (vacuum degassing, electro-slag remelting, and vacuum arc remelting) on toughness behavior, which suggests that the homogeneously distributed fragmented carbides in ESR may cause its lesser embrittlement.
It has been demonstrated that there is an enhanced fracture toughness of 40CrNi2MoE steel through augmented residual austenite content while eliminating twinned martensite [4,5,6,7]. Conversely, elevating tempering temperature prompts the decomposition of lath martensite and the coarsening of carbides, thereby detrimentally influencing the strength of the material [8,9,10]. With the increase in tempering temperature, the type of precipitated carbides in steel will be transformed. Low-temperature tempering below 300 °C produces transition carbides η, and when tempered above 325 °C, η carbides are gradually transformed into cementite and the elemental redistribution of cementite occurs. However, when the tempering temperature is increased to above 575 °C, the coarsened cementite reduces the fracture properties of the steel [11].
Various strength–toughness 40CrNi2MoE steels obtained by adjusting tempering temperature have different crack propagations, which is determined by the competitive relationship between stress and strain around the crack tip. As toughness increases, the crack extension mechanism changes from stress-controlled to strain-controlled, and the fracture morphology transitions from a cleavage plane to dimples [12].
To preserve the steel’s strength while simultaneously bolstering its toughness, the literature posits the adoption of an isothermal quenching process to achieve a dual-phase microstructure comprising bainite and martensite, which has more enhanced mechanical performance [13,14,15]. The inclusion of bainite exhibits crack arrest capabilities, while the presence of bainite at the crack front induces stress relaxation effects, culminating in a substantial enhancement in fracture toughness. By applying these refined modifications, a thorough examination of 40CrNi2MoE steel affords a comprehensive analysis of the impact that varying tempering temperatures exert on microstructural attributes, mechanical properties, and the ensuing rotating bending fatigue performance. In addition, toughness can be improved by short-time tempering as well, which may be connected to the reduction in retained austenite decomposition to inter-lath cementite [16].
The constituents employed in aerospace shafts may be exposed to cyclic bending fatigue loads during operational deployment, potentially culminating in fatigue failure. Investigations [17,18,19] have unveiled that, under conditions of elevated cyclic bending loads, fatigue failures primarily emanate from non-metallic inclusions or procedural defects intrinsic to the steel matrix.
This research aims to establish a theoretical framework supported by empirical evidence, thereby facilitating further advancements in augmenting the rotating bending fatigue life of 40CrNi2MoE steel, ultimately contributing to the progression of steel science and engineering.

2. Materials and Methods

The present study utilized 40CrNi2MoE steel as its experimental material, which underwent a fabrication process involving vacuum induction melting coupled with vacuum consumable electrode remelting. The detailed chemical composition of the material is presented in Table 1.
The tested steel was subsequently made into initial blanks, which were then subjected to an oil-quenching procedure at 840 °C for 1 h. Following this, a tempering process ensued, lasting 4 h at 400 °C, 420 °C, 440 °C, or 460 °C. The schematic diagram of the heat treatment process is shown in Figure 1.
To comprehensively evaluate the material’s characteristics, a battery of assessments was undertaken, encompassing both mechanical properties and microstructural attributes. Tensile and impact tests that were undertaken adhered to GB/T 228.1-2021 [20] and GB/T 229-2020 [21]. The microstructure of trial steels was observed by the high-resolution Thermo Fisher Scientific Quanta FEG 650 scanning electron microscope (SEM) and Thermo Scientific Apreo 2C equipped with an EDAX Velocity Super EBSD detector (Waltham, MA, USA). Furthermore, nano-precipitates were scrutinized through a transmission electron microscopy (TEM) analysis. This investigation utilized the FEI Tecnal G2 F20 (Hillsboro, OR, USA) field emission transmission electron microscope, incorporating an energy-dispersive spectroscopy system (EDS) to study the nano-precipitation and dislocations in the trial steels. Dislocation density and austenite content were meticulously ascertained through the X-ray diffraction (XRD) method. Furthermore, the initial blanks underwent precision machining, yielding rotating bending fatigue specimens tailored to accommodate tests.
The rotating bending fatigue test adhered to the standards outlined in GB/T 4337-2015 [22] and was conducted on the QBWP-6000 machine (QianBang, Changchun, China), operating at ambient temperature. The test employed a four-point force methodology with a frequency of 80 Hz, a stress concentration factor (Kt) of 1, and a stress ratio (R) of −1, and the loading waveform adopted was a sinusoidal wave. Upon the completion of the fatigue tests, the fracture surfaces underwent immersion in acetone to undergo thorough ultrasonic cleaning. Subsequently, the fracture morphology was meticulously observed and analyzed utilizing the Quanta FEG 650 SEM (Hillsboro, OR, USA), which was equipped with an X-ray energy dispersive spectrometer.

3. Results and Discussion

3.1. Microstructure

The microstructural characteristics of 40CrNi2MoE steel subsequent to tempering at discrete temperatures of 400, 420, 440, and 460 °C are elucidated by Figure 2. Evidently discernible in the depiction is the dominance of a microstructure comprised of tempered martensite, characterized by lath martensite and precipitated carbides. Analytical findings from XRD underscore austenite content within the specimens post-tempering at varying temperatures, all falling within the narrow spectrum of 0.30% to 0.36%. This result implies that the tempering temperature exerts a modest influence on the austenite content.
To investigate the nanostructure of the trial steels, TEM investigation was acquired, as illustrated in Figure 3. The TEM bright-field (BF) and dark-field (DF) image reveals the presence of abundant needle-like precipitates intricately embedded along both the boundaries and the interior of the martensitic lath. Simultaneously, a nearly spherical secondary phase within these laths comes into view. Through selected area electron diffraction (SAED), these needle-like precipitates are discerned to be cementite (Fe3C). Concurrently, the nearly spherical secondary phase, conspicuous for its Cr enrichment, is found to correspond to M23C6 carbides. A discernible metamorphosis transpires as the tempering temperature ascends, wherein the needle-like cementite morphology gradually transmutes into rod-like configurations.

3.2. Mechanical Properties

Tensile and impact mechanical property tests were conducted on 40CrNi2MoE steel subjected to various tempering temperatures. The variation in the mechanical properties of the tested steel concerning the tempering temperature is illustrated in Figure 4. Within the temperature spectrum, both ultimate strength (σul) and yield strength (σy) of the tested steel ebb concomitant to the ascendant tempering temperature. Discernibly, the ultimate strength of the tested steel consistently transcends the 1400 MPa threshold, with the yield ratio (σyul) concurring within the 0.90–0.92 ambit, thus manifesting comprehensive mechanical properties. An observation is the affirmative correlation of tempering temperature with both the resilience against impact absorbed energy (KU2) and the yield ratio. And the reduction in area (RA) is slightly influenced by tempering temperature. Upon conjoining the mechanical performance curve with the minutiae gleaned from microscopic scrutiny of the microstructure, an observation ensues: following tempering at 400 °C, the microstructure shows a lath configuration of relative finesse, a concurrence that corresponds with the acme in tensile and yield strengths.
The deformation characteristics of 40CrNi2MoE steel under uniaxial tension at different tempering temperatures were investigated. The Crussard–Jaoult (C–J) analysis [23], renowned for its sensitivity in capturing variations in strain hardening mechanisms at low strains, proved to be a valuable tool for assessing the influence of processing and microstructural factors on the deformation behavior of steels. By employing the modified C–J analytical method to fit the true stress–strain curve, it was possible to discern the strain-hardening properties exhibited by 40CrNi2MoE steel at different stages of development. The modified C–J analytical method is an outgrowth of the Swift equation [24,25,26], which is expressed as ε = ε 0 + k · σ n . A transformation is achieved by logarithmically processing both facets of this equation, thereby engendering Equation (1):
ln d σ d ε = 1 n ln σ + ln kn
In Equation (1), k is a material constant, while n denotes the exponent characterizing strain hardening. The construction of the ln d σ d ε l n σ curve is synonymous with the generation of the modified Crussard–Jaoult (C–J) analysis plot [27,28]. The real strains at distinctive junctures within this plot are denominated as transition strains, εt.
Figure 5a delineates the trend in the strain-hardening exponent, as inferred from the derivative of the true stress–strain curve post-yield point, fitted with a polynomial function. This tendency unfurls in two discernible phases: an initial precipitous descent succeeded by a gradual abatement until the specimen reaches a state of instability. In proximity to a strain of 0.03, an almost linear plateau manifests, signifying a relative constancy in the strain-hardening exponent at this juncture. Preceding the plateau zone, with escalating tempering temperatures, there is a gradual diminution in the strain-hardening exponent. Conversely, under elevated strains, specimens subject to tempering at heightened temperatures evince an augmented strain-hardening exponent.
In accordance with dislocation theory, when subjected to lower levels of strain, dislocation motion predominantly manifests through the slip mechanism. As the tempering temperature escalates, there is a heightened prevalence of interactions and the subsequent redistribution of high-density dislocation structures. Furthermore, the pinning effect exerted by precipitate particles upon dislocations undergoes augmentation, thereby bestowing increased stability upon dislocation entities and, concurrently, engendering a noteworthy reduction in the population density of mobile dislocations [29].
Consequently, during the initial phase of the strain-hardening curve, there is a conspicuous decrement in the strain-hardening exponent concomitant with the progressive elevation in tempering temperature. This trend aligns harmoniously with the corresponding alterations in dislocation density as ascertained via X-ray diffraction (XRD). Nonetheless, once dislocations commence their motion, the interactions between dislocations and precipitate particles experience attenuation, resulting in a partial augmentation in the population density of mobile dislocations. This, in turn, serves to decelerate the otherwise declining tendency of the strain-hardening exponent.
Furthermore, as a consequence of the spherization process observed in precipitate particles subsequent to tempering at higher temperatures, the interplay with dislocations experiences a further diminishment. The spherization and the interplay will be discussed in Section 3.6. Consequently, following tempering at 460 °C, the amplitude of the upsurge in the mobile dislocation density surpasses that which follows tempering at 400 °C. This phenomenon contributes substantially to the mitigation of the reduction in the strain-hardening exponent. As a result, there is a discernible augmentation in the strain-hardening exponent subsequent to the plateau zone, coinciding with the progressive elevation in the tempering temperature.
Figure 5b elucidates the post-yield evolution of the modified C–J model curve. This curve unfolds across three distinct phases: an initial gradual decline, a precipitous descent, and an intermediate transitional phase. The values of n characterizing each phase, alongside their respective turning point strain ε t , find their summation in Table 2 and Table 3. The n parameter’s magnitude mirrors the robustness of the strain-hardening phenomenon. In the inaugural phase, the efficacy of strain hardening experiences attenuation concomitant with the escalation in tempering temperature. Furthermore, with increasing strain levels, the strain-hardening capacity of specimens subjected to varying tempering temperatures exhibits diminution. The elevation in tempering temperature induces a concurrent decline in the mobile dislocation density inherent to these specimens. Consequently, the work-hardening rate during deformation registers a gradual deceleration, harmonizing with the constriction of the strain range characterizing the initial half of the adapted C–J model curve.

3.3. Fatigue Life

To investigate the influence of diverse tempering temperatures on the rotating bending fatigue life of 40CrNi2MoE steel, rotational fatigue examinations were executed on smooth experimental specimens subjected to tempering procedures at varying temperatures. The test parameters have been given at the front, and the maximum stress is 800 MPa. The outcomes are delineated in Figure 6, which illustrates the fatigue life’s dependence on tempering temperature in the examination of the trial steels. Notably, within the experimental temperature spectrum, specimens undergoing tempering at 400 °C manifested the most elevated fatigue life, attaining 313,763 cycles. Additionally, with escalating tempering temperatures, a conspicuous decrement in fatigue life ensues, comporting harmoniously with the concurrent trend in strength variation. This concordance illustrates that the factors governing fatigue life are consonant with the determinants of strength.

3.4. Fatigue Limit and S-N Curve

In pursuit of ensuring the steel’s impact toughness without compromising its high strength, a tempering temperature of 440 °C was selected for ascertaining the conditional fatigue limit and constructing the S-N curve. The appraisal of the conditional fatigue limit for 40CrNi2MoE steel, subjected to rotational bending, was executed employing the staircase method, and the resultant staircase plot is showcased in Figure 7a. The initial stress was set at 710 MPa, accompanied by a stress gradient of 30 MPa. A cohort of 12 specimens was enlisted for this endeavor, and the targeted cycle count was set at 107. Computed in accordance with Equation (2), the fatigue limit for 40CrNi2MoE steel is at a commendable 695 MPa. Considering that the yield strength after tempering at 440 °C is 1288 MPa, the ratio of fatigue strength to yield strength is 0.54.
σ RN = 1 m i = 1 n V i σ i
In Equation (2), m signifies the number of qualified specimens and n conveys the enumeration of stress-level tiers, while Vi and σi delineate, in a distinct manner, the quantification of samples and the magnitudes of stress, correspondingly, for the i-th level of stress.
The S-N curve of 40CrNi2MoE steel under rotational bending fatigue assessment was determined through a grouped methodology. Three distinct stress levels were selected and five specimens for fatigue evaluation at each tier were subjects. Within the domain of fatigue design and performance assessment, three usual S-N curve models [30,31] are conventionally employed, namely, the exponential function model, the power function model, and the three-parameter model. Notably, comprehensive empirical findings unequivocally support the precision and predictive efficacy of the three-parameter model [32,33]. In the context of the S-N curve, which takes into consideration the fatigue strength denoted as Si, the equation for accommodating the three-parameter model can be expressed as Equation (3) [18]:
S = S i 1 + C N b
Within this equation, b denotes the negative gradient of the S-N curve, while C signifies a material constant. As S converges toward the threshold Si, N asymptotically tends toward infinity. The data points were fitted to the three-parameter model using Origin 2021 software, as depicted by the red curve in Figure 7b, culminating in the formulation of the equation as follows:
S = 695 1 + 4217.12 N 0.916 ,   R 2 = 0.854
It can be seen that the model is fitted better and can reflect the relationship between the fatigue life of 40CrNi2MoE steel and the amount of stress it is subjected to under the test conditions.
Owing to the inherent dispersion in fatigue test data, a one-to-one correspondence between fatigue stress and life is regrettably absent. In actuality, the S-N curve embodies the fatigue life profile for a survival probability of P = 50%. To articulate fatigue life profiles for varying survival probabilities, the formulation of P-S-N curves becomes indispensable. Calculations were meticulously conducted for standard normal deviations and probabilistic fatigue life at survival probabilities of 50%, 99%, and 99.9%, subsequently followed by a linear regression analysis. The resultant P-S-N curve is thoughtfully presented in Figure 7b. From the P-S-N curves, it can be noticed that the fitted line with P = 99.9% is slightly conservative, and all of its predicted fatigue life is shorter than the measured values.
In a scholarly pursuit, Zhang et al. [33] undertook an investigation of SAE 4340 steel subjected to tempering at varying temperatures, yielding an array of mechanical strengths. Their inquiry encompassed the assimilation of fatigue data gleaned from an assortment of high-strength steel alloys, as well as aluminum and copper alloys. Within this ambit, they systematically elucidated the intricate nexus between fatigue strength and tensile strength. The findings unveiled a quadratic correlation between these two pivotal parameters, from which sprang forth a comprehensive fatigue strength formula of import:
σ w = σ b C P · σ b
Within the confines of this formula, fatigue strength is symbolized and denoted as σ w , while σ b represents tensile strength, and C and P are both constants. The enduring fatigue characteristics of 40CrNi2MoE steel, gleaned from this empirical endeavor, were harnessed for the fitting of a nuanced three-parameter model curve, thereby yielding insights into the fatigue performance at divergent tempering temperatures. The application of the aforementioned equation, Equation (5), to this fitting procedure bestowed upon them the ensuing mathematical representation:
σ w = σ b 1.349 5.709 × 10 4 · σ b
Notably, this model demonstrated a commendable goodness of fit, quantified by a coefficient of R2 = 0.892.

3.5. Fracture Surface

The fatigue fracture surfaces resulting from rotational bending fatigue present a wealth of valuable information regarding the fracture process. Characteristically, these fatigue fracture surfaces manifest three discernible morphological domains: the fatigue crack origin region, the crack propagation region, and the fatigue final rupture region. Conventionally, the final rupture region is positioned diametrically opposite the origin region. However, due to the accelerated advancement in fatigue cracks in the reverse rotational direction, the location of the rupture region deviates at a certain angular offset in the reverse rotation direction, as elucidated by previous research [34]. The intermediate plane strain region exhibits a radial pattern, as illustrated in Figure 8a. Upon an examination of the fatigue fracture surfaces exhibited by 40CrNi2MoE steel subjected to rotational bending fatigue, a notable revelation emerged: all fatigue cracks originated exclusively from the specimen’s surface. This phenomenon can be ascribed to the persistent oscillation of tensile and compressive stresses, which act upon multiple points of the specimen’s surface in a sinusoidal fashion, thereby culminating in the highest stress amplitude at the surface. Furthermore, the primary origins of crack initiation are traced back to the presence of inclusions, specifically, slag inclusions, and processing defects. These inclusions encompass a blend of Al2O3, CaO, and MgO, in composite arrangements of two or more constituents, as distinctly delineated in Figure 8b. It is noteworthy that no cracks were initiated solely as a consequence of one kind of inclusion during the fatigue tests. The level of control of inclusions in the steelmaking process needs to be improved.
Within the propagation region, as delineated in Figure 8c, the emergence of a profusion of secondary cracks is discernible. The genesis of these secondary cracks serves the purpose of mitigating stress concentration at the major crack, thus decelerating the advancement velocity of the major crack. In the context of rotational-bending-fatigue-induced fracture surfaces of 40CrNi2MoE steel, the presence of extensive fatigue striations does not manifest within the propagation region. Rather, such fatigue striations, with lengths spanning from 10 to 20 μm, are restricted to isolated diminutive planes. These striations signify the distance traversed by fatigue cracks during each sinusoidal loading cycle, rendering them instrumental for appraising variations in fracture propagation rates through an evaluation of the inter-striation spacing. Figure 8d serves to elucidate the morphological attributes of the final rupture region. Upon scrutiny of the fatigue surfaces, it becomes patently apparent that there exist no noteworthy disparities in the morphology of fractures or the sources of crack initiation across varying tempering temperature conditions. The examination of the fatigue fracture surfaces elucidates that the chosen tempering temperature range in the experimental paradigm is comparatively narrow, thereby falling short in eliciting pronounced distinctions in the morphological attributes of fractures and the origins of initiation.

3.6. Dislocation Density

For this section, an investigation was performed on 40CrNi2MoE steel using XRD to measure the alteration in dislocation density with varying tempering temperatures. This study also utilized TEM to examine the presence of dislocations within the martensite laths. The samples were treated by quenching, and tempering for different times.
The XRD result is shown as depicted in Figure 9a. As tempering temperature rose, there was a gradual reduction in dislocation density within the 40CrNi2MoE steel. This phenomenon can be attributed to the release of residual stresses during the tempering process. By alleviating the resistance to dislocation movement, this stress release facilitated increased dislocation annihilation and subsequently caused a decline in dislocation density [35]. Concurrently, as the tempering temperature rises, a marginal portion of the martensitic phase undergoes an inverse transformation, giving rise to the formation of reverse-transformed austenite. The higher cubic symmetry and atomic packing density of the austenite lattice structure made it more susceptible to dislocation slip, resulting in a further decrease in dislocation density.
Furthermore, it can be seen that the increase in tempering temperature reduces the entangled dislocations within the martensitic slats of the test steel in the TEM BF images (Figure 9b,d). TEM images revealed that a transformation occurred in the precipitated carbides within the laths as the tempering temperature increased. This transformation changed their elongated needle-like shapes into shorter rod-like forms, leading to reduced hindrance to dislocation motion [36]. Consequently, this transformation promoted dislocation annihilation and caused a decrease in dislocation density.
Upon comparing the effects of tempering temperature on dislocation density, tensile strength, and fatigue life, it was observed that the sample tempered at 400 °C exhibited the highest dislocation density and the highest strength, as well as the longest fatigue life. Nevertheless, as the tempering temperature continued to rise, a concurrent decrease was observed in both dislocation density and the parameters of strength and fatigue life. Consequently, it can be inferred that the deterioration of tensile strength and fatigue life resulting from elevated tempering temperature predominantly stems from the diminishment in dislocation density. And the reduction in dislocation density can be attributed to the attenuated interplay between dislocations and precipitates, as well as the alleviation of residual stresses and the genesis of reverse-transformed austenite through the tempering process.

4. Conclusions

This study scrutinizes the impact of tempering temperature on the mechanical characteristics, work hardening phenomena, and rotating bending fatigue of 40CrNi2MoE ultra-high-strength steel, and a succinct examination of the contributory role of dislocation density is presented. The following conclusions can be drawn:
  • The present study was undertaken to scrutinize the impact of tempering temperature upon the mechanical attributes of 40CrNi2MoE steel. Notably, subsequent to tempering at 400 °C, the tensile strength of 40CrNi2MoE steel attains its zenith, registering at Rm = 1530 MPa. With the incremental elevation in the tempering temperature, both the strength and yield ratio manifest a discernible decrement, predominantly ascribed to the diminishment in dislocation density. Moreover, it is noteworthy that toughness evinces a correlation with the tempering temperature.
  • A modified C–J analysis illuminates that, concomitant with the escalation in tempering temperature, the strain-hardening capacity experiences a gradual attenuation. Dislocations, together with precipitations, along with their interplay, constitute the chief determinants governing the strain-hardening demeanor of the examined steel.
  • Under the purview of experimental conditions, the fatigue life of 40CrNi2MoE steel attains its apogee, nearing 320,000 cycles, following tempering at 400 °C. As the tempering temperature ascends, the fatigue life precipitously plummets, in tandem with the trend in the fluctuation of strength. This phenomenon predominantly hinges on the density of dislocations. Additionally, the three-parameter model presents a congruence with the S-N curve.
  • The predominant origins of fatigue initiation in the context of rotational bending were inclusions, such as Al2O3, CaO, and MgO. Remarkably, the tempering temperature exerts no significant sway upon either the fount of initiation or the fracture morphology.

Author Contributions

Conceptualization, Y.L.; methodology, S.H. and X.-Y.L.; validation, Z.-W.Z. and C.-D.Y.; formal analysis, Z.-W.Z. and Y.L.; data curation, C.-D.Y.; writing—original draft preparation, C.-D.Y.; writing—review and editing, Y.L. and X.-Y.L.; visualization, C.-D.Y.; supervision, Y.L.; project administration, S.H.; funding acquisition, X.-Y.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Heilongjiang Province's key technology project: ‘Leading the Charge with Open Competition’ of Science and Technology Department, Heilongjiang Province (grant number 2023ZXJ04A02), and National Key Research and Development Program of China (grant number 2022YFB3705200).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All the data that support the findings of this study are available upon reasonable request.

Acknowledgments

This work has been fully supported by Science and Technology Department of Heilongjiang Province and National Key Research and Development Program of China. The authors would like to thank them for the funding received.

Conflicts of Interest

Author Zhi-Wei Zang was employed by the company Tianjin Heavy Industries Research & Development Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Wagri, N.K.; Jain, N.K.; Petare, A.; Das, S.R.; Tharwan, M.Y.; Alansari, A.; Alqahtani, B.; Fattouh, M.; Elsheikh, A. Investigation on the Performance of Coated Carbide Tool during Dry Turning of AISI 4340 Alloy Steel. Materials 2023, 16, 668. [Google Scholar] [CrossRef]
  2. Bakhshi, S.; Asadi Asadabad, M.; Bakhshi, S. Influence of the heat treatment on the quantitative features of the fracture surfaces and the mechanical properties of AISI 4340 steel sheets. Ironmak. Steelmak. 2023, 50, 295–309. [Google Scholar] [CrossRef]
  3. Manokaran, M.; Kashinath, A.S.; Jha, J.S.; Toppo, S.P.; Singh, R.P. Influence of Tempering in Different Melting Routes on Toughness Behavior of AISI 4340 Steel. J. Mater. Eng. Perf. 2015, 29, 6748–6760. [Google Scholar] [CrossRef]
  4. Lai, G.Y.; Wood, W.E.; Clark, R.A.; Zackay, V.F.; Parker, E.R. The effect of austenitizing temperature on the microstructure and mechanical properties of as-quenched 4340 steel. Metall. Mater. Trans. B 1974, 5, 1663–1670. [Google Scholar] [CrossRef]
  5. Bakhshi, S.; Mirak, A. Textural development, martensite lath formation and mechanical properties variation of a super strength AISI4340 steel due to austenitization and tempering temperature changes. Mater. Charact. 2022, 188, 111923. [Google Scholar] [CrossRef]
  6. Zhao, H.Z.; Lee, Y.; Liu, X.H.; Wang, G.D. On the martensite transformation kinetics of AISI 4340 steel. J. Northeast Univ. Nat. Sci. 2006, 27, 650–653. [Google Scholar]
  7. Zhirafar, S.; Rezaeian, A.; Pugh, M. Effect of cryogenic treatment on the mechanical properties of 4340 steel. J. Mater. Process. Technol. 2007, 186, 298–303. [Google Scholar] [CrossRef]
  8. Souza, M.F.; Serrão, L.F.; Pardal, J.M.; Tavares, S.S.M.; Fonseca, M.C. Tempering influence on residual stresses and mechanical properties of AISI 4340 steel. Int. J. Adv. Manuf. Technol. 2022, 120, 1123–1134. [Google Scholar] [CrossRef]
  9. Wang, C.L.; Wang, Y.P.; Niu, Z.Q.; Hu, G.J.; Zhou, W.L.; Chen, G.Q.; Fu, X.S. Effect of tempering temperature on mechanical properties and dry friction properties of 40CrNi2Mo steel. Trans. Mater. Heat Treat. 2020, 41, 75–82. [Google Scholar]
  10. Clarke, A.J.; Miller, M.K.; Field, R.D.; Coughlin, D.R.; Gibbs, P.J.; Clarke, K.D.; Alexander, D.J.; Powers, K.A.; Papin, P.A.; Krauss, G. Atomic and nanoscale chemical and structural changes in quenched and tempered 4340 steel. Acta Mater. 2014, 77, 17–27. [Google Scholar] [CrossRef]
  11. Clarke, A.J.; Klemm-Toole, J.; Clarke, K.D.; Coughlin, D.R.; Pierce, D.T.; Euser, V.K.; Poplawsky, J.D.; Clausen, B.; Brown, D.; Almer, J.; et al. Perspectives on Quenching and Tempering 4340 Steel. Metall. Mater. Trans. A 2020, 51, 4984–5005. [Google Scholar] [CrossRef]
  12. Li, H.F.; Wang, S.G.; Zhang, P.; Qu, R.T.; Zhang, Z.F. Crack propagation mechanisms of AISI 4340 steels with different strength and toughness. Mater. Sci. Eng. A 2018, 729, 130–140. [Google Scholar] [CrossRef]
  13. Bilal, M.M.; Yaqoob, K.; Zahid, M.H.; Haq, E.U.; Tanveer, W.H.; Wadood, A.; Ahmed, B. Effect of austempering conditions on the microstructure and mechanical properties of AISI 4340 and AISI 4140 steels. J. Mater. Res. Technol. 2019, 8, 5194–5200. [Google Scholar] [CrossRef]
  14. Che, X.J.; Yang, M.S.; Tang, H.Y.; Li, J.X.; Pang, X.D.; Sun, Y. Inclusion control and fatigue performance in high performance GCr15 bearing steel. Steel 2018, 53, 76–85+101. [Google Scholar]
  15. Bakhshi, S.; Mirak, A. The effect of low temperature transformation time on microstructural & textural evolution, mechanical properties and fracture behavior of a low alloy, medium carbon, super strength AISI 4340 steel. Mater. Sci. Eng. A 2022, 831, 142247. [Google Scholar]
  16. Euser, V.K.; Williamson, D.L.; Clarke, K.D.; Findley, K.O.; Speer, J.G.; Clarke, A.J. Effects of short-time tempering on impact toughness, strength, and phase evolution of 4340 steel within the tempered martensite embrittlement regime. Metall. Mater. Trans. B 2019, 50, 3654–3662. [Google Scholar] [CrossRef]
  17. Lu, L.T.; Li, W.; Zhang, J.W.; Shiozawa, K.; Zhang, W.H. Analysis of rotary bending gigacycle fatigue properties of bearing steel GCr15. Acta Metall. Sin. 2009, 45, 73–78. [Google Scholar]
  18. Guo, J.; Yang, M.S.; Lu, D.H.; Li, X.Y. Rotational bending fatigue life and fatigue crack initiation mechanism of Cr4Mo4V bearing steel. J. Mater. Eng. 2019, 47, 134–143. [Google Scholar]
  19. Lai, F.; Mao, K.; Cao, C.; Hu, A.; Tu, J.; Lin, Y. Rotating Bending Fatigue Behaviors of C17200 Beryllium Copper Alloy at High Temperatures. Materials 2023, 16, 815. [Google Scholar] [CrossRef]
  20. GB/T 228.1; Metallic Materials—Tensile Testing—Part 1: Method of Test at Room Temperature. State Administration for Market Regulation, and Standardization Administration of the P.R.C.: Beijing, China, 2021.
  21. GB/T 229; Metallic Materials—Charpy Pendulum Impact Test Method. State Administration for Market Regulation, and Standardization Administration of the P.R.C.: Beijing, China, 2020.
  22. GB/T 4337; Metallic Materials—Fatigue Testing—Rotating Bar Bending Method. General Administration of Quality Supervision, Inspection and Quarantine of the People’s Republic of China, and Standardization Administration of the P.R.C.: Beijing, China, 2015.
  23. Zhou, P.; Wang, L.; Cui, C.; Hu, Y.; Xu, K. Effect of Intercritical Temperature on the Microstructure and Mechanical Properties of 10CrMnMoSi Dual-phase Steel. J. Mater. Eng. Perf. 2023, 32, 8949–8960. [Google Scholar] [CrossRef]
  24. Ling, Y.; Hu, F.; Yan, H.; Zhou, W.; Zhang, Z.C.; Wu, K.M. Microstructural transformation and plasticity mechanism of 2GPa medium-carbon medium-manganese nano-bainitic steel. Iron Steel 2022, 57, 131–143. [Google Scholar]
  25. Yang, D.Z.; Xiong, Z.P.; Zhang, C.; Feng, G.Z.; Cheng, Z.F.; Cheng, X.W. Evolution of microstructures and mechanical prop-erties with tempering temperature of a pearlitic quenched and tempered steel. J. Iron Steel Res. Int. 2021, 29, 1393–1403. [Google Scholar] [CrossRef]
  26. Wang, Y.H.; Huang, X.M.; Zhang, L.; Guo, Y.B.; Chu, L.S.; Dai, G.Z. Characterization and simulation of strain-hardening behavior of a cold-rolled dual phase steel of 780 MPa grade by means of modified C-J method and RVE model. Chin. J. Mater. Res. 2017, 31, 801–808. [Google Scholar] [CrossRef]
  27. Soares, G.C.; Gonzalez, B.M.; Santos, L.A. Strain hardening behavior and microstructural evolution during plastic deformation of dual phase, non-grain oriented electrical and AISI 304 steels. Mater. Sci. Eng. A 2017, 684, 577–585. [Google Scholar] [CrossRef]
  28. Xie, B.; Cai, Q.; Yu, W.; Cao, J.M.; Yang, Y.F. Effect of tempering temperature on resistance to deformation behavior for low carbon bainitic YP960 steels. Mater. Sci. Eng. A 2014, 618, 586–595. [Google Scholar] [CrossRef]
  29. Zhang, J.W.; Lu, L.T.; Shen, X.L.; Yi, H.F.; Zhang, W.H. Evaluation method of fatigue damage under variable amplitude stress based on plastic strain. Acta Metall. Sin. 2009, 45, 1464–1465. [Google Scholar]
  30. Li, C.; Wu, S.; Zhang, J.; Xie, L.Y.; Zhang, Y.H. Determination of the fatigue PSN curves—A critical review and improved backward statistical inference method. Int. J. Fatigue 2020, 139, 105789. [Google Scholar] [CrossRef]
  31. Cai, W.; Li, W.; Xu, J. Study on the P-S-N Curve of Sucker Rod Based on Three-Parameter Weibull Distribution. Materials 2022, 15, 560. [Google Scholar] [CrossRef]
  32. Zhao, Y.X.; Gao, Q.; Wang, J.N. Unified approach for estimating the probabilistic design S-N curves of three commonly used fatigue stress-life models. Nucl. Power Eng. 2001, 22, 42–52. [Google Scholar]
  33. Pang, J.C.; Li, S.X.; Wang, Z.G.; Zhang, Z.F. General relation between tensile strength and fatigue strength of metallic materials. Mater. Sci. Eng. A 2013, 564, 331–341. [Google Scholar] [CrossRef]
  34. Han, S.; Li, Y.; Wang, C.X.; Liu, X.M.; Li, J.X. Behavior of rotating-bending fatigue failure of AF1410 steel. Iron Steel 2013, 48, 82–85. [Google Scholar]
  35. Roy, A.K.; Bandyopadhyay, S.; Suresh, S.B.; Maitra, D.; Kumar, P.; Wells, D.; Ma, L. Relationship of residual stress to dislocation density in cold-worked martensitic alloy. Mater. Sci. Eng. A 2006, 416, 134–138. [Google Scholar] [CrossRef]
  36. Hu, Z.F. Study on the Properties and Microstructure of High CoNi Alloy Steel. Ph.D. Thesis, University of Science and Technology Beijing, Beijing, China, 2001. [Google Scholar]
Figure 1. Heat treatment process schematic diagram.
Figure 1. Heat treatment process schematic diagram.
Materials 17 01377 g001
Figure 2. SEM (ad) and EBSD (eh) of 40CrNi2MoE steel after tempering at various temperatures.
Figure 2. SEM (ad) and EBSD (eh) of 40CrNi2MoE steel after tempering at various temperatures.
Materials 17 01377 g002
Figure 3. TEM of two carbides in 40CrNi2MoE steel after tempering at 440 °C: (a,b) BF and DF image of cementite at lath boundaries; (c,d) BF and DF image of cementite inside martensite lath; (e) BF and SAED of M23C6.
Figure 3. TEM of two carbides in 40CrNi2MoE steel after tempering at 440 °C: (a,b) BF and DF image of cementite at lath boundaries; (c,d) BF and DF image of cementite inside martensite lath; (e) BF and SAED of M23C6.
Materials 17 01377 g003
Figure 4. The effect of tempering temperature on mechanical properties of 40CrNi2MoE steel. (a) Trends of ultimate strength (σul), yield strength (σy), and yield ratio (σyul); (b) Trends of reduction in area (RA) and impact absorbed energy (KU2).
Figure 4. The effect of tempering temperature on mechanical properties of 40CrNi2MoE steel. (a) Trends of ultimate strength (σul), yield strength (σy), and yield ratio (σyul); (b) Trends of reduction in area (RA) and impact absorbed energy (KU2).
Materials 17 01377 g004
Figure 5. (a) Strain hardening rates vs. true strain curves; (b) ln(dσ/dε) vs. lnσ of tested steel after tempering at different temperatures.
Figure 5. (a) Strain hardening rates vs. true strain curves; (b) ln(dσ/dε) vs. lnσ of tested steel after tempering at different temperatures.
Materials 17 01377 g005
Figure 6. Nf vs. tempering temperature.
Figure 6. Nf vs. tempering temperature.
Materials 17 01377 g006
Figure 7. (a) Staircase plot; (b) P-S-N curves of 40CrNi2MoE steel and three-parameter model fitting curve.
Figure 7. (a) Staircase plot; (b) P-S-N curves of 40CrNi2MoE steel and three-parameter model fitting curve.
Materials 17 01377 g007
Figure 8. SEM morphology of rotational bending fatigue fracture. (a) Macrostructure morphology; (b) complex inclusion origin and its component; (c) crack propagation region; (d) final rupture region.
Figure 8. SEM morphology of rotational bending fatigue fracture. (a) Macrostructure morphology; (b) complex inclusion origin and its component; (c) crack propagation region; (d) final rupture region.
Materials 17 01377 g008
Figure 9. (a) Density of dislocation vs. tempering temperature; (b,c) BF and DF of dislocations and cementite inside lath after tempering at 400 °C, respectively; (d,e) BF and DF of dislocations and cementite inside lath after tempering at 460 °C, respectively.
Figure 9. (a) Density of dislocation vs. tempering temperature; (b,c) BF and DF of dislocations and cementite inside lath after tempering at 400 °C, respectively; (d,e) BF and DF of dislocations and cementite inside lath after tempering at 460 °C, respectively.
Materials 17 01377 g009
Table 1. Composition of 40CrNi2MoE (mass fraction, %).
Table 1. Composition of 40CrNi2MoE (mass fraction, %).
CSiMnCrNiMoFe
0.410.250.780.851.860.26Bal.
Table 2. Strain hardening rates and turning point strain of different stages.
Table 2. Strain hardening rates and turning point strain of different stages.
Tempering Temperature/°Cn
IIIIII
40021.0739.862132
42024.1736.931445
44023.4730.51580
46024.0341.001872
Table 3. Turning point strain of different stages.
Table 3. Turning point strain of different stages.
Tempering
Temperature/°C
ε t /%
I→IIII→III
4000.0640.130
4200.0700.100
4400.2200.245
4600.0730.011
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Yao, C.-D.; Li, Y.; Zang, Z.-W.; Li, X.-Y.; Han, S. Influence of Tempering Temperature on Mechanical and Rotational Bending Fatigue Properties of 40CrNi2MoE Steel. Materials 2024, 17, 1377. https://doi.org/10.3390/ma17061377

AMA Style

Yao C-D, Li Y, Zang Z-W, Li X-Y, Han S. Influence of Tempering Temperature on Mechanical and Rotational Bending Fatigue Properties of 40CrNi2MoE Steel. Materials. 2024; 17(6):1377. https://doi.org/10.3390/ma17061377

Chicago/Turabian Style

Yao, Chang-Da, Yong Li, Zhi-Wei Zang, Xin-Yang Li, and Shun Han. 2024. "Influence of Tempering Temperature on Mechanical and Rotational Bending Fatigue Properties of 40CrNi2MoE Steel" Materials 17, no. 6: 1377. https://doi.org/10.3390/ma17061377

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.