Next Article in Journal
Atmospheric and Marine Corrosion of PEO and Composite Coatings Obtained on Al-Cu-Mg Aluminum Alloy
Next Article in Special Issue
Additive Manufacturing of Ti-48Al-2Cr-2Nb Alloy Using Gas Atomized and Mechanically Alloyed Plasma Spheroidized Powders
Previous Article in Journal
Micro- and Nanoparticulate Hydroxyapatite Powders as Fillers in Polyacrylate Bone Cement—A Comparative Study
Previous Article in Special Issue
Erratum: Polozov, I., et al. Fabrication of Silicon Carbide Fiber-Reinforced Silicon Carbide Matrix Composites Using Binder Jetting Additive Manufacturing from Irregularly-Shaped and Spherical Powders. Materials 2020, 13, 1766
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Heat Treatment of Corrosion Resistant Steel for Water Propellers Fabricated by Direct Laser Deposition

by
Ruslan Mendagaliev
1,2,
Olga Klimova-Korsmik
1,2,3,
Vladimir Promakhov
3,*,
Nikita Schulz
3,
Alexander Zhukov
3,
Viktor Klimenko
3 and
Andrey Olisov
3
1
Institute of Laser and Welding Technologies, St. Petersburg State Marine Technical University, St. Petersburg 190121, Russia
2
Institute of Metallurgy, Mechanical Engineering and Transport, Peter the Great St. Petersburg Polytechnic University, St. Petersburg 195251, Russia
3
SEC Siberian Center for Industrial Design and Prototyping, National Research Tomsk State University, Tomsk Oblast 634050, Russia
*
Author to whom correspondence should be addressed.
Materials 2020, 13(12), 2738; https://doi.org/10.3390/ma13122738
Submission received: 16 May 2020 / Revised: 10 June 2020 / Accepted: 15 June 2020 / Published: 17 June 2020
(This article belongs to the Special Issue Materials, Design and Process Development for Additive Manufacturing)

Abstract

:
The urgency of heat treatment of samples of maraging steel obtained by direct laser deposition from steel powder 06Cr15Ni4CuMo is considered. The structural features and properties of 06Cr15Ni4CuMo steel samples after direct laser deposition and heat treatment are studied. The work is devoted to research into the influence of thermal processing on the formation of structure and the mechanical properties of deposit samples. Features of formation of microstructural components by means of optical microscopy are investigated. Tests for tension and impact toughness are conducted. As a result, it was established that the material obtained by the direct laser deposition method in its initial state significantly exceeds the strength characteristics of heat treatment castings of similar chemical composition, but is inferior to it in terms of impact toughness and relative elongation. The increase in relative elongation and impact toughness up to the level of cast material in the deposit samples is achieved at the subsequent heat treatment, which leads to the formation of the structure of tempered martensite and reduction in its content at two-stage tempering in the structure of the metal. The strength of the material is also reduced to the level of cast metal.

1. Introduction

Currently, to increase the competitiveness of shipyards for the manufacture of parts of marine engineering, new high-tech technologies are used. Additive manufacturing methods are increasingly being used, including direct laser deposition technology (DLD). In the DLD process it is possible to obtain parts, including from shipbuilding steels used in the Arctic. Iron and its modified alloys are the most important class of metallic materials used in shipbuilding. Different grades of stainless steels can be treated as a part of traditional manufacturing techniques such as casting, machining, powder metallurgy and welding, including any combination of those. [1,2].
As a result of the research on estimation of material characteristics in 1980, this has been developed and mastered in the industry of martensitic–austenitic stainless steel (CA6NM—06Cr15Ni4CuMo) for manufacturing compressors [3], propeller blade [4,5,6,7], castings of blades, components of chemical and oil industry and other cast details of responsible purpose, and now for the manufacture of large castings for a propeller blade of blades and hub steel of 06Cr15Ni4CuMo. Currently, it is relevant to obtain parts and blanks for industrial production of this steel by the DLD method.
With the development of modern production technologies, it has become possible to manufacture parts from virtually any metal powder using additive technologies (AM). AM is characterized by quick fabrication and economical spending of expensive materials. Direct laser deposition (DLD) methods are of special interest when large workpieces need to be made using AM. The DLD technology makes it possible to fabricate large parts from stainless and cold-resistant steels [8,9,10,11,12]. The features of the DLD process include high temperature gradients, and repeated fast heating and fast cooling that cause residual strains and form heterogeneities in the microstructure. Microstructural features, such as grain size and morphology (as well as phase transitions), are very sensitive to the dynamic thermal history and they directly influence the microhardness, tear strength and modulus of resilience [13,14,15,16,17,18].
The mechanical properties of alloys obtained using DLD depend on their structure-phase states. For steels, an important role is played by the content of laminar low-carbon martensite (α′) microstructure and the presence of other phases, such as delta ferrite (δ), austenite (γ) and chromium carbides. It is known that the austenite phase is preserved in the tempering process and/or it is restored as a result of the treatment of quenched material. The secondary phase of ferrite in the alloy is δ-ferrite, which forms at very high temperatures during hardening in the course of casting or the DLD process [19].
To achieve high mechanical characteristics for martensite stainless steel, heat treatment (HT) is normally used. However, the microstructure of alloys obtained using DLD is close to a cast structure and is anisotropic. Such materials are characterized by low plasticity and modulus of resilience [20,21,22]. Here, the material’s inner structure is particularly influenced by cyclic heating during DLD due to layer-by-layer metal deposition [23,24,25]. During the fabrication process, the work piece is tempered. While classical casting and welding envisages a full HT cycle (quenching and tempering), parts fabricated by deposition require the development of ad-hoc HT that is different from the classical one [26,27]. The influence of these effects on the structural characteristics and mechanical properties needs research, specifically the presence of residual austenite γ, non-quenched martensite α′, and delta ferrite δ. These factors govern the final properties of the manufactured parts.
The goal of the research work was to grow a plate of 06Cr15Ni4CuMo steel and further reveal the patterns of microstructure formation and mechanical properties after high tempering and determine the maintenance regime providing the required level of ductility of steel not inferior to casting.

2. Materials and Methods

2.1. Materials

We have chosen 06Cr15Ni4CuMo (an analog of CA6NM) for the material. The starting material is 06Cr15Ni4CuMo fraction 45–160 µm Figure 1 is the producer of the “Polema” powder. The chemical composition of the steel is provided in Table 1.
The impact bending tests of the 06Cr15Ni4CuMo steel were conducted on an RKP 450 (Zwick/Roell, Ulm, Germany) unit at −10 °С, with impact energy 150 J and tensile tests were performed on a Z100 (Zwick/Roell, Ulm, Germany) unit at room temperature. Samples made under mechanical tensile testing GOST 1497-84 (RU) and impact testing GOST 6996-66 (RU).
To show the structure, we used chemical etching with Kalling’s reagent in a solution (33 mL HCl + 33 mL of ethanol + 33 mL of H2O + 1.5 g of CuCl2) over 30–60 s.
The deposited cladding layers were visually examined and instrumentally measured; then, they were investigated by optical microscopy on the DMI 500 Leica (Leica Microsystems, Wetzlar, Germany) microscopes using Thixomet (Thixomet, St.-Petersburg, Russia).

2.2. Fabrication of Samples Using DLD and Their Heat Treatment

We used the following equipment: a robotic complex based on an LRM-200iD_7L (Fanuc, Oshino, Japan) industrial robot; fiber laser based on a LS-3 Yb (IRE Polus Ltd., Fryazino, Moscow Region, Russia) unit; an FLW D30 (IPG Photonics, Oxford, UK) laser deposition head with a detachable SO12 (Fraunhofer IWS, Aachen, Germany) deposition nozzle and a Twin 10C (Sulzer Metco Inc., New York, NY, USA) powder feeder. A shielding gas atmosphere was used for deposition: an air-proof chamber filled with argon at an excess pressure of 2–3 MPa. In the argon-filled chamber the content of oxygen was not more than 300 ppm. Manufacturing of samples by DLD method was carried out at power P = 2300 W, speed V = 25 mm/s and cross section of depositing bead 2 × 0.8 mm2 powder flow rate G = 35 g/min, displacement along the Δx = 1.6 mm, and Δz = 0.7 mm. Five blocks (1 in the initial state and 4 per HT) with LxWxH dimensions 130 × 80 × 16 mm in Figure 2 were deposit simultaneously: a layer was applied alternately to each of the samples, after that the transition to the next layer took place.
DLD was carried out in a shielding chamber with controllable atmosphere. High purity argon was used as a transport and protective gas. Overpressure of 2–3 Mbar was maintained in the deposition chamber. The residual oxygen content in the working atmosphere did not exceed 300 ppm. The porosity in the grown plates did not exceed 2% of the total volume of the deposit sample.
The heat treatment was performed in a SNOL 30/1300 muffle furnace without, shielding gas. The heating rate was 200 °С per hour with subsequent exposure and cooling as shown in Figure 3. Cooling rate of samples after high-temperature tempering was 50 °C per hour and then air cooling was 150 °C.

3. Results

In the course of parts fabrication from martensite grade steels using DLD, forced process thermal cycling is taking place due to extensive heat deposition. Heat deposition then impacts the presence of retained austenite and δ-ferrite [28] in the structure of the samples fabricated by DLD. Residual austenite can have a negative effect on hardness and toughness.
In the course of tempering during subsequent cooling, metal plasticity deteriorates, and this is due to the formation of secondary martensite as a result of conversion of residual austenite. That is why it makes sense to conduct a second tempering of secondary martensite. This promotes an increase in the metal’s relative elongation, creating a finer structure as a result of the decomposition of secondary martensite and the formation of quenched martensite.
Cast metal needs HT for quenching and dual subsequent tempering. During DLD, however, forced thermal cycling is taking place. This strengthens the samples, so we only need to conduct dual tempering to achieve the desired results. Based on the mentioned data from the literature and the results of experimental studies of the steel’s characteristics, we have found HT modes for the samples. These modes envisaged high-temperature tempering that would provide the best combination of mechanical properties: high strength, elongation, and impact strength [27].
After DLD the steel has high strength characteristics and low plasticity. To achieve the required mechanical properties for the steel, we have selected several HT modes, as shown in Table 2.
Different δ-morphologies were clearly revealed after etching the fabricated sample, Figure 4a. These morphologies are created by the incomplete growth of Widmanstetten γ-grains during the solid-state δ→γ phase transformation, Figure 4b. Here, incomplete growth results in residual δ stringer inclusions being left at the borders [4]. These inclusions outline the growth front that resembles the initial orientation of the ex- Widmanstett patterns in the final microstructure. During further cooling, γ-austenite converts into α′-martensite, but some amount of δ-delta-ferrite remains in the final microstructure, as shown in Figure 4a. Afterwards, the fabrication δ-delta-ferrite was discovered in the samples, and its content did not exceed 5%.
At such high temperatures, δ-grains are growing rapidly during heating. Then, during the cooling process, they convert into a γ-phase with subsequent transition into a α′ structure. In Figure 4b, after a single iteration of high-temperature tempering, some amount of γ-austenite (as well as M7C3 chromium carbides) is still observed.
Figure 4c,d shows some amount of non-converted α′-martensite that is an unstable microstructure in the α matrix. It promotes the formation of carbides, interlayer boundaries at large angles and a γ-phase.
Figure 4e,f includes a structure after high-temperature tempering that is represented by quenched lath α′-martensite with fine particles of residual austenite. The particles are located between martensite laths and at the boundaries of martensite batches with large inclusions of δ-ferrite in the matrix basis.
The best mechanical properties were achieved at dual tempering at Т = 620 °С, t = 2 h/x2 the cycle is repeated twice Figure 4. This mode complies with the technical specifications for this steel grade while having slightly lower plasticity characteristics.
Figure 5 shows the distribution of microhardness single weld bed and their arrangement for different HT modes and a thermokinetic diagram for Fe-Cr-Ni.
The average microhardness in the fabricated sample tempered at 750 °С, Figure 5b, was 355 HV. Tempering at 750 °С was chosen because of the phase transition into the γ-austenity area that preceded the dissolution of existing chromium carbides in the fabricated sample (i.e., M23C6/M7C3). Thus, it increased the concentration of carbon in the martensite matrix at room temperature.
With temperature reduction to 650 °С it was possible to decrease the hardness to 280 HV with an exposure time of 2 h, and an exposure time of 4 h was required to decrease it to 301 HV. At high-temperature tempering at Т = 620 °С with an exposure time of 2 h, the microhardness was 260 HV, and it was 273 HV after the second tempering.

4. Discussion

It is established that the DLD process is the fastest and most convenient for creating parts. After the process, it is necessary to produce high tempering to achieve all the necessary mechanical properties. Samples obtained by the DLD method are not inferior in characteristics to casting, and in some cases are most in demand.
Thus, we can conclude that the propeller with an optimized structure has reliability characteristics close to the original solid version. We showed the manufacturing of hub and blades via DLD and built-up propeller before and after CNC-machining and manual polishing. After all producing stages, the propeller was weighted. The weight test showed that the mass is finished product is 105 kg. This is 20% less than the original cast design. A more detailed description of design analysis, optimization procedure and production process is presented in [30].

5. Conclusions

The DLD process of 06Cr15Ni4CuMo steel achieves a high strength due to the forced thermal cycling process at low impact toughness and relative elongation. In order to eliminate the imbalance of the complex of mechanical properties, HT is proposed.
According to the results of a comparison of mechanical properties, it was established that the lowest structural matrices are tempered by fine martensite with a low level of residual austenite and δ-ferrite. Based on the analysis of the relationship between HT, mechanical properties and 06Cr15Ni4CuMo steel structure, the most suitable heat treatment mode for deposit samples was established, consisting of a double HT at Т = 620 °С, t = 2 h/x2; the cycle is repeated twice, in which a finely dispersed structure of tempered rack martensite is formed, providing a set of properties equal to the material obtained by casting.

Author Contributions

Conceptualization, R.M. and V.P.; methodology, V.P., V.K. and O.K.-K.; validation, A.Z. and N.S.; resources, V.K. and V.P.; writing—original draft preparation, R.M., A.O., O.K.-K., and V.P.; writing—review and editing, N.S. and R.M.; visualization, A.Z.; supervision, R.M. and A.O. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by RFBR and Tomsk Region, project number 19-48-703019, was supported by The Tomsk State University competitiveness improvement program (grant No. 8.2.04.2020), grant SP-724.2019.1.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Khodabakhshi, F.; Farshidianfar, M.; Gerlich, A.; Nosko, M.; Trembošová, V.; Khajepour, A. Microstructure, strain-rate sensitivity, work hardening, and fracture behavior of laser additive manufactured austenitic and martensitic stainless steel structures. Mater. Sci. Eng. A 2019, 756, 545. [Google Scholar] [CrossRef]
  2. Promakhov, V.; Zhukov, A.; Ziatdinov, M.; Zhukov, I.; Schulz, N.; Kovalchuk, S.; Dubkova, Y.; Korsmik, R.; Klimova-Korsmik, O.; Turichin, G.; et al. Inconel 625/TiB2 Metal Matrix Composites by Direct Laser Deposition. Metals 2019, 9, 141. [Google Scholar] [CrossRef] [Green Version]
  3. Winck, L.B.; Ferreira, J.; Araújo, J.; Manfrinato, M.D.; Silva, C. Surface nitriding influence on the fatigue life behavior of ASTM A743 steel type CA6NM. Surf. Coat. Technol. 2013, 232, 844. [Google Scholar] [CrossRef]
  4. Wen, P.; Cai, Z.; Feng, Z.; Wang, G. Microstructure and mechanical properties of hot wire laser clad layers for repairing precipitation hardening martensitic stainless steel. Opt. Laser Technol. 2015, 75, 207. [Google Scholar] [CrossRef]
  5. Promakhov, V.; Khmeleva, M.; Zhukov, I.A.; Platov, V.V.; Khrustalyov, A.; Vorozhtsov, A.B. Influence of Vibration Treatment and Modification of A356 Aluminum Alloy on Its Structure and Mechanical Properties. Metals 2019, 9, 87. [Google Scholar] [CrossRef] [Green Version]
  6. Mirakhorli, F.; Cao, X.; Pham, X.-T.; Wanjara, P.; Fihey, J. Phase structures and morphologies of tempered CA6NM stainless steel welded by hybrid laser-arc process. Mater. Charact. 2017, 123, 264. [Google Scholar] [CrossRef]
  7. Zhukov, I.A.; Kozulin, A.A.; Khrustalyov, A.; Matveev, A.E.; Platov, V.V.; Vorozhtsov, A.B.; Zhukova, T.V.; Promakhov, V. The Impact of Particle Reinforcement with Al2O3, TiB2, and TiC and Severe Plastic Deformation Treatment on the Combination of Strength and Electrical Conductivity of Pure Aluminum. Metals 2019, 9, 65. [Google Scholar] [CrossRef] [Green Version]
  8. Turichin, G.; Zemlyakov, E.; Babkin, K.; Ivanov, S.; Vildanov, A. Analysis of distortion during laser metal deposition of large parts. Procedia CIRP 2017, 74, 154. [Google Scholar] [CrossRef]
  9. Turichin, G.; Zemlyakov, E.; Kuznetsov, M.; Babkin, K.; Kurakin, A.; Vildanov, A. Direct laser deposition with transversal oscillating of laser radiation. In Proceedings of the International Conference Laser Optics, St. Petersburg, Russia, 4–8 June 2018; p. 124. [Google Scholar] [CrossRef]
  10. Turichin, G.; Kuznetsov, M.; Tsibulskiy, I.; Firsova, A. Hybrid Laser-Arc Welding of the High-Strength Shipbuilding Steels: Equipment and Technology. Phys. Procedia 2017, 89, 156. [Google Scholar] [CrossRef]
  11. Rahman, N.U.; Capuano, L.; Cabeza, S.; Feinaeugle, M.; Garcia-Junceda, A.; De Rooij, M.; Matthews, D.; Walmag, G.; Gibson, I.; Römer, G. Directed energy deposition and characterization of high-carbon high speed steels. Addit. Manuf. 2019, 30. [Google Scholar] [CrossRef]
  12. Zhao, X.; Dong, S.; Yan, S.; Liu, X.; Liu, Y.; Xia, D.; Lv, Y.; He, P.; Xu, B.; Han, H. The effect of different scanning strategies on microstructural evolution to 24CrNiMo alloy steel during direct laser deposition. Mater. Sci. Eng. A 2019. [Google Scholar] [CrossRef]
  13. Turichin, G.; Klimova, O.; Zemlyakov, E.; Babkin, K.; Kolodyazhnyy, D.; Shamray, F.; Travyanov, A.; Petrovskiy, P. Technological aspects of high speed direct laser deposition based on heterophase powder metallurgy. Phys. Procedia 2015, 78, 397. [Google Scholar] [CrossRef] [Green Version]
  14. Turichin, G.A.; Zemlyakov, E.V.; Klimova, O.G.; Babkin, K.D. Hydrodynamic instability in high-speed direct laser deposition for additive manufacturing. Phys. Procedia 2016, 83, 674. [Google Scholar] [CrossRef] [Green Version]
  15. Glukhov, V.; Turichin, G.; Klimova-Korsmik, O.; Zemlyakov, E.; Babkin, K. Quality Management of Metal Products Prepared by High-Speed Direct Laser Deposition Technology. Key Eng. Mater. 2016, 684, 461. [Google Scholar] [CrossRef]
  16. Turichin, G.; Kuznetsov, M.; Pozdnyakov, A.; Gook, S.; Gumenyuk, A.; Rethmeier, M. Influence of heat input and preheating on the cooling rate, microstructure and mechanical properties at the hybrid laser-arc welding of API 5L X80 steel. Procedia CIRP 2018, 74, 748. [Google Scholar] [CrossRef]
  17. Turichin, G.; Zemlyakov, E.; Babkin, K.; Ivanov, S.; Vildanov, A. Laser metal deposition of Ti-6Al-4V alloy with beam oscillation. Procedia CIRP 2018, 74, 184. [Google Scholar] [CrossRef]
  18. Klimova-Korsmik, O.; Turichin, G.; Zemlyakov, E.; Babkin, K.; Petrovsky, P.; Travyanov, A. Structure formation in Ni superalloys during high-speed direct laser deposition. Mater. Sci. Forum 2017, 879, 978. [Google Scholar] [CrossRef]
  19. Trudel, A.; Lévesque, M.; Brochu, M. Microstructural effects on the fatigue crack growth resistance of a stainless steel CA6NM weld. Eng. Fract. Mech. 2014, 115, 60. [Google Scholar] [CrossRef]
  20. Fang, J.; Dong, S.; Li, S.; Wang, Y.; Xu, B.; Li, J.; Liu, B.; Jiang, Y. Direct laser deposition as repair technology for a low transformation temperature alloy: Microstructure, residual stress, and properties. Mater. Sci. Eng. A 2019, 748, 119. [Google Scholar] [CrossRef]
  21. Guan, T.; Chen, S.; Chen, X.; Liang, J.; Liu, C.; Wang, M. Effect of laser incident energy on microstructures and mechanical properties of 12CrNi2Y alloy steel by direct laser deposition. J. Mater. Sci. Technol. 2019, 35, 395. [Google Scholar] [CrossRef]
  22. Wei, S.; Wang, G.; Yu, J.; Rong, Y. Competitive failure analysis on tensile fracture of laser-deposited material for martensitic stainless steel. Mater. Des. 2017, 118, 1. [Google Scholar] [CrossRef]
  23. Sarafan, S.; Wanjara, P.; Champliaud, H.; Thibault, D. Characteristics of an autogenous single pass electron beam weld in thick gage CA6NM steel. Int. J. Adv. Manuf. Technol. 2015, 78, 1523. [Google Scholar] [CrossRef]
  24. Barros, R.; Silva, F.J.G.; Gouveia, R.M.; Saboori, A.; Marchese, G.; Biamino, S.; Salmi, A.; Atzeni, E. Laser Powder Bed Fusion of Inconel 718: Residual Stress Analysis Before and After Heat Treatment. Materials 2020, 13, 2248. [Google Scholar] [CrossRef] [Green Version]
  25. Liu, Y.; Li, A.; Cheng, X.; Zhang, S.; Wang, H. Effects of heat treatment on microstructure and tensile properties of laser melting deposited AISI 431 martensitic stainless steel. Mater. Sci. Eng. A 2016, 666, 27. [Google Scholar] [CrossRef]
  26. Gouveia, R.M.; Silva, F.J.G.; Atzeni, E.; Sormaz, D.; Alves, J.L.; Pereira, A.B. Effect of Scan Strategies and Use of Support Structures on Surface Quality and Hardness of L-PBF AlSi10Mg Parts. Materials 2020, 13, 2248. [Google Scholar] [CrossRef]
  27. Rashid, R.A.R.; Nazari, K.; Barr, C.; Palanisamy, S.; Orchowski, N.; Matthews, N.; Dargusch, M. Effect of laser reheat post-treatment on the microstructural characteristics of laser-cladded ultra-high strength steel. Surf. Coat. Technol. 2019, 372, 93. [Google Scholar] [CrossRef]
  28. Tsukanov, V.V.; Tsyganko, L.K.; Petrov, S.N.; Shandyba, G.A.; Ziza, A.I. Structural transformations during heat treatment of cast corrosion-resistant martensitic steel. Metallobrabotka 2016, 3, 42. [Google Scholar]
  29. Folkhard, E.; Rabensteiner, G.; Perteneder, E. Welding Metallurgy of Stainless Steels; Springer: Vienna, Austria, 1988; p. 98. [Google Scholar]
  30. Korsmik, R.; Rodionov, A.; Korshunov, V.; Ponomarev, D.; Prosychev, I.; Promakhov, V. Topological optimization and manufacturing of vessel propeller via LMD-method. Mater. Today Proc. 2020. [Google Scholar] [CrossRef]
Figure 1. Surface of powder particles 06Cr15Ni4CuMo.
Figure 1. Surface of powder particles 06Cr15Ni4CuMo.
Materials 13 02738 g001
Figure 2. The scheme of cutting samples for mechanical testing.
Figure 2. The scheme of cutting samples for mechanical testing.
Materials 13 02738 g002
Figure 3. The heat treatment of the samples fabricated by deposition.
Figure 3. The heat treatment of the samples fabricated by deposition.
Materials 13 02738 g003
Figure 4. The microstructure of 06Cr15Ni4CuMo (a) DLD; (b) mode 1 (Т = 750 °С, t = 2 h); (c) mode 2 (Т = 650 °С, t = 2 h); (d) mode 3 (Т = 650 °С, t = 4 h); (e) mode 4 (Т = 620 °С, t = 2 h); (f) mode 5 (Т = 620 °С, t = 2 h/x2).
Figure 4. The microstructure of 06Cr15Ni4CuMo (a) DLD; (b) mode 1 (Т = 750 °С, t = 2 h); (c) mode 2 (Т = 650 °С, t = 2 h); (d) mode 3 (Т = 650 °С, t = 4 h); (e) mode 4 (Т = 620 °С, t = 2 h); (f) mode 5 (Т = 620 °С, t = 2 h/x2).
Materials 13 02738 g004aMaterials 13 02738 g004b
Figure 5. (a) microhardness; (b) the Fe–Cr–Ni equilibrium phase diagram [29].
Figure 5. (a) microhardness; (b) the Fe–Cr–Ni equilibrium phase diagram [29].
Materials 13 02738 g005
Table 1. The chemical composition of the steel.
Table 1. The chemical composition of the steel.
Material GradeElements Mass Ratio, %
CSiMnCrNiMoSPFeCu
06Cr15Ni4CuMo≤0.060.400.60–0.9014.0–15.54.0–4.40.11–0.280.0150.015Bal.1.0–1.5
Table 2. Mechanical properties for heat treatment (HT) modes.
Table 2. Mechanical properties for heat treatment (HT) modes.
P (W)V (mm/s)Yield Strength,
σв, (MPa)
Ultimate Strength, σ0.2, (MPa)Relative Elongation,
δs, (%)
Impact Toughness,
KV−10, (J)
Technical specificationsN/AN/A≥790≥620≥19≥40
DLD2300251088792817
b/Т = 750 °С, t = 2 h
Mode 118402011147987.516
c/Т = 650 °С, t = 2 h
Mode 21840208635301539
d/Т = 650 °С, t = 4 h
Mode 3230025891.7587.21229
e/Т = 620 °С, t = 2 h
Mode 4230020816.4698.31642
f/Т = 620 °С, t = 2 h/x2 the cycle is repeated twice
Mode 5230020804.4666.81942

Share and Cite

MDPI and ACS Style

Mendagaliev, R.; Klimova-Korsmik, O.; Promakhov, V.; Schulz, N.; Zhukov, A.; Klimenko, V.; Olisov, A. Heat Treatment of Corrosion Resistant Steel for Water Propellers Fabricated by Direct Laser Deposition. Materials 2020, 13, 2738. https://doi.org/10.3390/ma13122738

AMA Style

Mendagaliev R, Klimova-Korsmik O, Promakhov V, Schulz N, Zhukov A, Klimenko V, Olisov A. Heat Treatment of Corrosion Resistant Steel for Water Propellers Fabricated by Direct Laser Deposition. Materials. 2020; 13(12):2738. https://doi.org/10.3390/ma13122738

Chicago/Turabian Style

Mendagaliev, Ruslan, Olga Klimova-Korsmik, Vladimir Promakhov, Nikita Schulz, Alexander Zhukov, Viktor Klimenko, and Andrey Olisov. 2020. "Heat Treatment of Corrosion Resistant Steel for Water Propellers Fabricated by Direct Laser Deposition" Materials 13, no. 12: 2738. https://doi.org/10.3390/ma13122738

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop