Article

Study of Texture Analysis on Asymmetric Cryorolled and Annealed CoCrNi Medium Entropy Alloy

1
State Key Laboratory of High Performance Complex Manufacturing, Central South University, Changsha 410083, China
2
Light Alloys Research Institute, Central South University, Changsha 410083, China
3
College of Mechanical and Electrical Engineering, Central South University, Changsha 410083, China
4
Mark Wainwright Analytical Centre, University of New South Wales, Sydney, NSW 2052, Australia
*
Author to whom correspondence should be addressed.
Crystals 2020, 10(12), 1154; https://doi.org/10.3390/cryst10121154
Submission received: 11 November 2020 / Revised: 9 December 2020 / Accepted: 15 December 2020 / Published: 18 December 2020
(This article belongs to the Section Inorganic Crystalline Materials)

Abstract

:
CoCrNi equiatomic medium entropy alloy sheets were prepared by asymmetric rolling, cryorolling, and asymmetric cryorolling. The asymmetric cryorolled samples exhibited a noteworthy ultra-fine-grain heterogeneous lamella structure. The microstructure and corresponding hardness obtained by different rolling processes and subsequent annealing are compared. It can be seen from the results that the cryogenic deformation temperature had a stronger effect on the mechanical properties of the medium entropy alloys (MEA), compared with the shear strain caused by the asymmetric cryorolling. The effect of annealing temperature on texture components and volume fractions of the specially rolled samples was also analyzed. The result revealed that the recrystallized MEA exhibited similar texture components and the corresponding volume fraction, which indicated that the rolling process had limited influence on the formation of annealing texture. The recrystallized texture after annealing retained the deformation texture and twin related orientations appeared. Asymmetric rolled MEA showed strong random composition than symmetric rolled MEA regardless of rolling temperature. The recrystallized textures of the species obtained by the three rolling processes did not exhibit a significant dependence on the annealing temperature.

1. Introduction

High entropy alloys (HEAs) are a popular direction for the current development of material science, which have many unique structures and characteristics due to their special composition. The HEAs have been found to have many excellent properties that exceed traditional alloys, such as high hardness [1], high strength [2,3,4,5,6], high plasticity, high toughness [7,8], high fatigue resistance [9], strong corrosion resistance [10], strong radiation resistance [11], and ultra-high tensile properties and plasticity at cryogenic temperatures [12]. They have great potential to replace and upgrade current industrial alloys and are the development direction of future materials. Medium entropy alloys (MEAs) are based on the concept of high entropy alloys, a new type of multi-component alloy with three or four principal elements as the characteristics and mixing entropy of 1R or 1.5R [13]. While having the distinguished properties of high entropy alloys (the lattice distortion effect; sluggish diffusion [14,15]), medium entropy alloys also perform excellent even better mechanical properties. In the comparison of the properties of the equiatomic medium entropy alloys and the high entropy alloys, the ternary equiatomic middle entropy alloy CoCrNi was found to have the highest strength. Interestingly, it also has the highest plasticity, and it stably exhibits such advantageous performance in a wide range of test temperatures [16]. Likewise, Laplanche et al. [17] found that there were more nano twins in the deformation process of equiatomic CoCrNi MEA compared with the classical equiatomic high entropy alloy CoCrNiFeMn. The existence of deformation twins in an extended strain range imparted a good strength–ductility synergy [17]. The equiatomic medium entropy CoCrNi alloy has become a new interest in the research of medium entropy alloys because of its simple, stable crystal structure and excellent mechanical properties. However, the current research mainly focuses on the evolution of the recrystallized structure of MEA after plastic deformation [18,19] and the influence of nano twins on the properties of alloy [17,20,21,22,23,24]. Nevertheless, considering the actual investment in industrial production applications, it is necessary to further study the changes in the microstructure and texture of the alloy during plastic deformation and recrystallization during mechanical processing.
As an interesting thermo-mechanical processing (TMP) route, cryorolling can bring obvious grain refinement and improve materials properties by inhibiting the dynamic recovery and improving the twinning activity during the deformation process. Asymmetric cryorolling can introduce more shear strain to bring better thinning effect [25,26]. These researches mainly focus on some traditional alloys [27,28,29,30,31], and there are few studies on HEAs or MEAs. It is meaningful to combine the two process to study whether there will be more interesting coupling reactions. In the previous work [32,33], we found that the rolling speed ratio (1.2, 1.4, and 1.6) and cryogenic temperature (−190 °C) could have an obvious impact on the performance of the equiatomic medium entropy alloy CoCrNi, especially when the rolling speed ratio is 1.4, compared with the ordinary rolling process, the MEA obtained by asymmetric cryorolling had an obvious performance improvement effect, and the strength and plasticity are improved at the same time. These results show that asymmetric cryorolling is very suitable for producing higher-performance MEAs, and it is also meaningful to analyze the crystal texture of the material obtained by this TMP route. Therefore, we chose the asymmetric cryorolling with the rolling speed ratio of 1.4 and compared it with cryorolling and asymmetric rolling. The reason for choosing 1.4 here is because it is more typical compared to rolling speed ratio of 1.2 (relatively low) or 1.6 (relatively high) and can better representing the deformation features of asymmetric rolling. At the same time, it showed excellent mechanical properties when the rolling speed ratio is 1.4, and it is more valuable to study it. In the paper, we studied the evolution of texture components, strength, volume fractions and corresponding microstructure with the different temperatures annealing. It was aimed to further understand the MEAs produced by these special processes and to fill the gaps in texture research of the asymmetric cryorolled CoCrNi MEAs.

2. Experimental

The experimental equiatomic CrCoNi alloy ingots were prepared by vacuum arc melting and the test specimens for rolling were prepared by wire cutting. The initial thickness of the specimen was 1 mm. These sheets were asymmetrically rolled (room temperature, rolling speed ratio of 1.4), cryorolled (−196 °C), and asymmetric cryorolled (−196 °C, rolling speed ratio of 1.4) to a final thickness of 0.2 mm in 9 passes. To maintain cryogenic temperatures during the cryorolling and asymmetric cryorolling, the samples were immersed in liquid nitrogen for more than 10 min before each rolling pass. These rolled samples were then isochronally annealed at 600 °C, 700 °C, and 800 °C for 30 min.
The microstructure and texture were characterized by using an electron backscatter diffraction (EBSD) system (Oxford Instruments, Nordlys, Abingdon, Oxfordshire, UK) at Institute of Metal Research (China Academy of Sciences, Shenyang, Liaoning, China). The samples for EBSD observations were mechanically polished and then were ion-etched using a Leica RES101 ion-etcher (Leica Microsystems, Ernst-Leitz-Strasse, Wetzlar, Germany). The step size for the EBSD measurements was 0.0754 μm. The EBSD tests were taken from the ND–RD plane close to the center of the deformed specimens to reveal the microstructure. The orientation distribution function (ODF) in this paper illustrated the TD-RD section of the samples processed at different rolling conditions and annealing temperatures. The acquired EBSD results were analyzed using the HKL Channel 5 Software. The texture volume fractions were calculated by the texture component function, the volume fraction of individual texture components was calculated using a spread of 10° from their ideal orientation.
Micro-hardness tests were performed on the HXD-2000TMC/LCD (Taiming, Shanghai, China) digital micro-hardness tester with a load of 4.903 N and a retention time of 10 s. Five evenly distributed locations were selected on each sample for measurement to ensure accurate experimental results. The variance of each group of data was calculated to obtain the final hardness value.

3. Results and Discussion

Figure 1 shows the coincidence site lattice (CSL) grain boundary (GB) diagrams of the asymmetric rolled, cryorolled, and asymmetric cryorolled equiatomic medium entropy CoCrNi alloy. Figure 1a,c,e depicts the CSL grain boundary after annealing at 600 °C, and Figure 1b,d,f represents the CSL grain boundary after annealing at 800 °C. Red, green, purple, yellow, and pink lines correspond to ∑3, ∑5, ∑9, ∑11, and ∑27 boundaries, respectively. It is evident from Figure 1 that a high proportion of ∑3 boundaries, while few ∑9, ∑27, ∑5, ∑11 boundaries and other special grain boundaries were observed in all the samples. It could be seen that asymmetric rolled CoCrNi MEA samples have obvious coarse-grained and fine-grained layer structures, and cryorolled CoCrNi MEA samples have a finer microstructure. The stacking fault energy of CoCrNi medium entropy alloy is very low, even lower than that of CrMnFeCoNi high entropy alloy, which promotes a high tendency to produce ∑3 twin boundaries [17,34,35]. Correspondingly, a large number of red ∑3 grain boundaries were observed in Figure 1. Meanwhile, it is worth mentioning that most of the ∑3 grain boundaries in the CoCrNi MEA annealed at 600 °C were curved. While in the CoCrNi MEA annealing at 800 °C, the degree of recrystallization was further increased, at this time, the ∑3 grain boundaries were generally straight, which is consistent with the change after annealing of CoCrFeNiMn high entropy alloy observed by Tang et al. [36]. Furthermore, the research of Thomson et al. [37] revealed that as the annealing progress, the degree of recrystallization increases, and the curved incoherent ∑3 grain boundaries would be transformed into straight coherent ∑3 grain boundaries through fine tuning. The curved ∑3 twin boundary is a mobile incoherent grain boundary, and would react with other grain boundaries during this process. The ∑9 grain boundaries could be formed by the twinning reaction of the incoherent ∑3 grain boundaries when impinged with each other, as a result, a relatively large number of ∑9 boundaries were observed in the 600 °C CoCrNi MEA, as illustrated in Figure 1a,c,e. According to the theory of ‘∑3 regeneration model’, the impingement of ∑3 and ∑9 is more inclined to generate ∑3 grain boundaries rather than ∑27 grain boundaries for CoCrNi medium entropy alloys with low stacking fault energy and greater mobility. Consequently, a large number of ∑3 grain boundaries were still observed in the samples annealed at 800 °C [38]. At the same time, this also explain the phenomenon of less ∑9 ratio observed in Figure 1b,d,f after annealing at higher temperature, which is also consistent with the phenomenon observed by Dan Sathiaraj et al. [39].
Figure 2 depicts the corresponding grain size distribution of the equiatomic CoCrNi MEA after asymmetric rolling, cryorolling, and asymmetric cryorolling followed by annealing. It could be seen that the majority of the grain sizes are sub-micron level, mainly distribute in the range of 0–0.25 μm. The grain size distribution after annealing at 600 °C is mainly in the range of 0–6.25 μm (Figure 2a,c,e) compared to that of 0–9.75 μm after annealing at 800 °C (Figure 2b,d,f) which exhibits obvious grain coarsening. It is evident from Figure 2 that the overall average grain size is in the micron range and has an ultra-fine grain structure. This result may be attributed to the sluggish diffusion characteristics of the high entropy alloys [40] and the fine microstructure in the rolled CoCrNi MEA before annealing. As shown in Figure 2a,b, large-scale grains of 5.75–6.25 μm and 9.25–9.75 μm appeared in the room temperature asymmetrically rolling MEAs annealed at 600 °C and 800 °C, respectively. This result indicates that asymmetric rolling is feasible for producing heterogeneous lamellar structure. As shown in Figure 2c,d, the upper limit of grain distribution of the cryogenic symmetrically rolled CoCrNi MEA annealed at 600 °C and 800 °C (4.75 μm, 5.75 μm) was significantly smaller than that of asymmetrically rolled at room temperature (6.25 μm, 9.75 μm). Meanwhile, the proportion of ultra-fine grain size (0–0.25 μm) of the two was nearly the same, and the overall average grain size of the cryogenic symmetrically rolled and annealed CoCrNi MEA was less, which verified the better effect of cryogenic rolling on grain refinement. As shown in Figure 2e,f, the CoCrNi MEA of asymmetric cryorolling had the smallest upper limit of grain size distribution at 600 °C, large-scale grains of 8.75–9.25 μm were observed after annealing at 800 °C. As shown in Figure 1b,f, the large-scale grains of asymmetric cryorolling was smaller than of asymmetric rolling. In addition, it can be obviously observed that the size of the small-grain of the asymmetric cryorolled CoCrNi MEA annealed at 800 °C was finer, compared with the MEAs obtained by other two processes (Figure 1b,d,f). This indicated that that the asymmetric cryorolling process could bring obvious grain refinement, while still maintaining the obvious difference in coarse and fine grains of the asymmetric rolling.
Figure 3 depicts the orientation distribution function (ODF) sections of the CoCrNi MEA after asymmetric rolling, cryorolling, asymmetric cryorolling followed by subsequent annealing, displaying important recrystallization texture components and α-fiber observed in the CoCrNi MEA. Their corresponding Euler angles and Miller indices are given in Table 1. The ODF in Figure 4 illustrates the TD-RD section of the samples processed at different rolling conditions and annealing temperatures. The ϕ 2 = 0 ° ODF sections of the CoCrNi MEA after annealing at 600 °C (Figure 4a,c,e) exhibited the development of a weak and discontinuous α-{110}fiber extending from the {110}<001>Goss to the {110}<110>Rotated Goss through the {110}<115>G/B, {110}<112>Brass, and{110}<111>A orientations. The A component is the first order twin related to G/B [39]. α-{110} fiber texture was also observed in the samples annealed at 800 °C and showed the maximum intensity located near {110}<115>G/B and {110}<111>A. Obvious retention of deformation texture was observed. A number of previous studies on the five-element CoCrFeNiMn high entropy alloy and the quaternary CrFeCoNi medium entropy alloy also displayed the existence of deformation texture in the recrystallization texture [41,42,43,44]. The retention of deformation texture usually occurs in case of prolonged recovery or primary or discontinuous recrystallization without any preferential orientation selection. Based on the softening mechanism of HEAs [42], the extended recovery is ruled out, so this phenomenon was explained by the discontinuous recrystallization mechanics without preferential orientation selection [43]. A similar trend of retention of deformation texture after annealing was observed in twinning-induced-plasticity (TWIP) steels. The micro shear bands in the deformed materials of both had no significant contribution to the preferential nucleation analysis [41,43]. The presence of the relatively strong {110}<111>A component corresponded to the large number of ∑3 twin boundaries in Figure 1. Furthermore, the low stacking fault energy (SFE) of CoCrNi MEA could lead to numerous annealing twins, which in turn enhances the formation of the {110}<111>A component [43,45]. The BS orientation was weak due to the slower recrystallization kinetics of the BS orientation region. During the recrystallization process, the region near BS orientation was gradually replaced by adjacent recrystallized grains due to the slower recrystallization rate [43]. The {142}<211>K component was observed in the ϕ 2 = 15 ° ODF sections and the corresponding strength of K component increased with increasing annealing temperature from 600 °C to 800 °C. The typical brass recrystallization (BR) {236}<385>BR component was observed in the ϕ 2 = 35 ° sections. In low SFE alloys such as brass, there is often a strong BR component after annealing due to the nucleation at shear bands and subsequent preferential growth [46]. However, at ϕ 1 , ϕ , ϕ 2 = 80 ° , 31 ° , 35 ° sections, no obviously strong BR component was observed. The BR component was relatively weak, there is less tendency to preferential nucleation in HEAs, which corresponds to the retention of the deformation texture in the ϕ 2 = 0 ° sections. This phenomenon is similar to that observed in other annealed HEAs and MEAs [39,42,43,47]. In the ϕ 2 = 45 ° sections, strong {113}<332>D component was observed nearby ϕ 1 , ϕ , ϕ 2 = 90 ° , 25 ° , 45 ° . The α-fiber twin related texture components were observed. While D and K components have first order twin relation with G [32]. {123}<634>S component and strong {13 6 25}<20 15 14>M component were visible in the ϕ 2 = 65 ° sections. The parameters of the ideal texture components referred above are derived from [39,41,42]. The texture composition of the asymmetric rolled, cryorolled, and asymmetric cryorolled CoCrNi MEAs followed by subsequent annealing did not show significant change with annealing temperature. Similar behavior was also observed in the studies of symmetric rolling in previous reports of HEAs and MEAs. It might could attribute to the effect of sluggish diffusion of the HEAs, which could also lead to higher fraction of random components in HEAs [39,41,42,43,44,48].
Previous studies on texture have reported that process parameters such as imposed strain, strain path, annealing temperature have a relatively great impact on the recrystallization texture of FCC metals [49]. However, in the present study, although the rolling process enhanced the microstructure and mechanical properties of CoCrNi medium entropy alloy significantly, the CoCrNi MEA that underwent annealing and recrystallization formed a similar texture composition. This should be due to the absence of obvious preferential nucleation and preferential growth during annealing. Similar situations have been reported in other HEA studies. When the mechanical properties and structure of the equiatomic CoCrFeMnNi high entropy alloy after rolling with different strains were different, the recrystallization texture of the alloys showed similar recrystallization texture [42].
The change in texture composition of the equiatomic CoCrNi alloy after asymmetric rolling, cryorolling, and asymmetric cryorolling followed by annealing at different temperatures is displayed in Figure 5a–c. The asymmetric rolled and annealed samples showed stronger random components compared to symmetric rolled and annealed CoCrNi MEA. In Figure 5, the random component was expressed as R (sum of volume fraction of components other than those shown in Table 1). The total volume fraction of the α-fiber (the sum of the volume fractions of the components along the α-fiber, namely G, G/B, BS, G/B(T) and Rt-G, in Figure 5, the α-fiber was expressed as α) did not exhibit significant changes and each texture component showed only a slight change with the annealing temperature. It is consistent with the results from the ODF sections in Figure 4. Haase et al. [50] reported that the main influence mechanism of texture randomization was the formation of twins during annealing, and the retention of deformation texture components in the recrystallization texture was mainly due to the nucleation of new grains at the grain boundary closed to the parent grains. Figure 5d depicts the change in texture index (characterizing texture intensity) with the annealing temperature. It can be seen in Figure 5d that in the CoCrNi MEA under any rolling process, the texture index increases with an increase in annealing temperature, corresponding to the ODF sections of Figure 4, it was also observed that the MEA annealed at 800 °C had stronger texture components. It is in agreement with the research results of the cold-rolled and annealed CoCrFeMnNi high entropy alloy [41].
Figure 6 shows the microhardness variation with the rolling and annealing conditions, plotting the hardness as a function of rolling process methods. It evident that the hardness obtained after cryorolling is higher than that after asymmetric rolling, while the hardness of the MEA obtained by asymmetric cryorolling is higher than the both. The difference between the hardness obtained after cryorolling and asymmetric cryorolling is relatively small, and they are significantly higher than the hardness obtained after asymmetric rolling. This is also consistent with the previous analysis of the grain size distribution about Figure 2. The overall average grain size of the cryorolling material is significantly smaller. These results suggest that deformation temperature has a larger contribution to the mechanical strength improvement of our studied MEA, compared to the shear strain introduced by asymmetric rolling. According to previous studies [51,52,53,54], it has been proven that dislocation density and deformed microstructure is greatly affected by the deformation temperature for various metallic materials. The suppression of dynamic recovery by cryogenic deformation temperature leads to high defect density, which brings more potential nucleation sites during annealing and leads to finer grains [26]. The similar phenomenon has also been obtained in the current study. Moreover, the difference in hardness caused by different rolling process methods are almost kept even when annealing temperature is less than 700 °C. When annealing temperature reaches 800 °C, the hardness of asymmetric cryorolling deformed MEA is obviously higher than the other two. Corresponding to Figure 1, it can be seen that the large-scale grains of asymmetric cryorolling was smaller than of asymmetric rolling. Meanwhile, the size of the small-grain of the asymmetric cryorolled CoCrNi MEA was obviously finer, compared with the MEAs obtained by other two processes. This showed that the asymmetric cryorolled deformed MEA after high temperature annealing had better thermal stability. This similar phenomenon has also been observed in previous studies on cryorolling, asymmetric rolling and asymmetric cryorolling [29], and this issue will be further studied in the future.

4. Conclusions

The evolution of the texture and microstructure of the equiatomic medium entropy CoCrNi alloy after cryorolling, asymmetric rolling, and asymmetric cryorolling followed by subsequent annealing was investigated in the present work. Based on the research results, the following conclusions are drawn:
(1)
As the annealing temperature increases, the ∑3 grain boundaries gradually becomes straight from curve. The grain sizes of the annealed samples were mostly in the sub-micron. After high temperature annealing, the ultra-fine grain structure with an average size in the micron level were still maintained. The CoCrNi MEA after cryorolling and subsequent annealing had a high proportion of ultra-fine (0–0.25 μm) grain size distribution and the upper limit of grain size was lower, compared with other rolled sample. Meanwhile, the asymmetrically rolled and annealed samples had an obvious two-stage grain size distribution. Asymmetrically cryorolled samples still remained heterogeneous grain size characteristics after high temperature annealing with finer small-grain and lower large-scale grain size.
(2)
Annealed and recrystallized samples formed similar texture components and texture strength increased with increasing annealing temperature. After annealing, the α-fiber textures such as G, G/B, Bs, A, and S textures were retained. A few orientations generated by annealing twinning were also observed. The asymmetric rolled and annealed samples exhibited stronger random components than symmetric rolled and annealed samples. The annealing temperature had little effect on the volume fraction of different texture components.
(3)
The hardness obtained after cryorolling and asymmetric cryorolling are similar, which are relatively higher than the hardness obtained after asymmetric rolling. It is mainly attributed to that deformation temperature has more significant effect on improving the mechanical properties, compared to the shear strain introduced by asymmetric rolling.

Author Contributions

Y.W.: Experiments, Investigation, Writing—original draft, review & editing. J.L.: Investigation, Writing—review. L.B.: Investigation, Writing—review. C.K.: Experiments, Investigation, Writing—review & editing. H.Y.: Conceptualization, Writing—review & editing, Supervision. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by National Key Research and Development Program (Grant No. 2019YFB2006500), the National Natural Science Foundation of China (Grant number: 51674303), Innovation Driven Program of Central South University (Grant number: 2019CX006), and the Research Fund of the Key Laboratory of High Performance Complex Manufacturing at Central South University.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Yeh, J.W.; Chen, S.K.; Lin, S.J.; Gan, J.Y.; Chin, T.S.; Shun, T.T.; Tsau, C.H.; Chang, S.Y. Nanostructured high-entropy alloys with multiple principal elements: Novel alloy design concepts and outcomes. Adv. Eng. Mater. 2004, 6, 299–303. [Google Scholar] [CrossRef]
  2. Liang, Y.J.; Wang, L.; Wen, Y.; Cheng, B.; Wu, Q.; Cao, T.; Xiao, Q.; Xue, Y.; Sha, G.; Wang, Y.; et al. High-content ductile coherent nanoprecipitates achieve ultrastrong high-entropy alloys. Nat. Commun. 2018, 9, 4063. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  3. Huang, H.; Wang, J.; Yang, H.; Ji, S.; Yu, H.; Liu, Z. Strengthening CoCrNi medium-entropy alloy by tuning lattice defects. Scr. Mater. 2020, 188, 216–221. [Google Scholar] [CrossRef]
  4. Du, X.H.; Li, W.P.; Chang, H.T.; Yang, T.; Duan, G.S.; Wu, B.L.; Huang, J.C.; Chen, F.R.; Liu, C.T.; Chuang, W.S.; et al. Dual heterogeneous structures lead to ultrahigh strength and uniform ductility in a Co-Cr-Ni medium-entropy alloy. Nat. Commun. 2020, 11, 2390. [Google Scholar] [CrossRef]
  5. Wen, R.; You, C.; Zeng, L.; Wang, H.; Zhang, X. Achieving a unique combination of strength and ductility in CrCoNi medium-entropy alloy via heterogeneous gradient structure. J. Mater. Sci. 2020, 55, 12544–12553. [Google Scholar] [CrossRef]
  6. Feng, X.; Yang, H.; Fan, R.; Zhang, W.; Meng, F.; Gan, B.; Lu, Y. Heavily twinned CoCrNi medium-entropy alloy with superior strength and crack resistance. Mater. Sci. Eng. A 2020, 788, 139591. [Google Scholar] [CrossRef]
  7. Gludovatz, B.; Hohenwarter, A.; Catoor, D.; Chang, E.H.; George, E.P.; Ritchie, R.O. A fracture-resistant high-entropy alloy for cryogenic applications. Science 2014, 345, 1153–1158. [Google Scholar] [CrossRef] [Green Version]
  8. Qian, C.; Li, K.; Guo, X.Y.; Liu, B.; Long, Z.Y.; Liu, Y. Effect of WC grain size on mechanical properties and microstructures of cemented carbide with medium entropy alloy Co-Ni-Fe binder. J. Cent. South Univ. 2020, 27, 1146–1157. [Google Scholar] [CrossRef]
  9. Tang, Z.; Yuan, T.; Tsai, C.W.; Yeh, J.W.; Lundin, C.D.; Liaw, P.K. Fatigue behavior of a wrought Al0.5CoCrCuFeNi two-phase high-entropy alloy. Acta Mater. 2015, 99, 247–258. [Google Scholar] [CrossRef]
  10. Chen, Y.Y.; Duval, T.; Hung, U.D.; Yeh, J.W.; Shih, H.C. Microstructure and electrochemical properties of high entropy alloys—A comparison with type-304 stainless steel. Corros. Sci. 2005, 47, 2257–2279. [Google Scholar] [CrossRef]
  11. Xia, S.; Gao, M.C.; Yang, T.; Liaw, P.K.; Zhang, Y. Phase stability and microstructures of high entropy alloys ion irradiated to high doses. J. Nucl. Mater. 2016, 480, 100–108. [Google Scholar] [CrossRef] [Green Version]
  12. Liu, J.P.; Chen, J.X.; Liu, T.W.; Li, C.; Chen, Y.; Dai, L.H. Superior strength-ductility CoCrNi medium-entropy alloy wire. Scr. Mater. 2020, 181, 19–24. [Google Scholar] [CrossRef]
  13. Yeh, J.W. Alloy design strategies and future trends in high-entropy alloys. JOM 2013, 65, 1759–1771. [Google Scholar] [CrossRef]
  14. Jian, W.R.; Xie, Z.; Xu, S.; Su, Y.; Yao, X.; Beyerlein, I.J. Effects of lattice distortion and chemical short-range order on the mechanisms of deformation in medium entropy alloy CoCrNi. Acta Mater. 2020, 199, 352–369. [Google Scholar] [CrossRef]
  15. Kucza, W.; Dąbrowa, J.; Cieślak, G.; Berent, K.; Kulik, T.; Danielewski, M. Studies of “sluggish diffusion” effect in Co-Cr-Fe-Mn-Ni, Co-Cr-Fe-Ni and Co-Fe-Mn-Ni high entropy alloys; determination of tracer diffusivities by combinatorial approach. J. Alloy. Compd. 2018, 731, 920–928. [Google Scholar] [CrossRef]
  16. Wu, Z.; Bei, H.; Pharr, G.M.; George, E.P. Temperature dependence of the mechanical properties of equiatomic solid solution alloys with face-centered cubic crystal structures. Acta Mater. 2014, 81, 428–441. [Google Scholar] [CrossRef]
  17. Laplanche, G.; Kostka, A.; Reinhart, C.; Hunfeld, J.; Eggeler, G.; George, E.P. Reasons for the superior mechanical properties of medium-entropy CrCoNi compared to high-entropy CrMnFeCoNi. Acta Mater. 2017, 128, 292–303. [Google Scholar] [CrossRef]
  18. Sathiyamoorthi, P.; Bae, J.W.; Asghari-Rad, P.; Park, J.M.; Kim, J.G.; Kim, H.S. Effect of annealing on microstructure and tensile behavior of CoCrNi medium entropy alloy processed by high-pressure torsion. Entropy 2018, 20, 849. [Google Scholar] [CrossRef] [Green Version]
  19. Ma, Y.; Yuan, F.; Yang, M.; Jiang, P.; Ma, E.; Wu, X. Dynamic shear deformation of a CrCoNi medium-entropy alloy with heterogeneous grain structures. Acta Mater. 2018, 148, 407–418. [Google Scholar] [CrossRef] [Green Version]
  20. Yang, M.; Yan, D.; Yuan, F.; Jiang, P.; Ma, E.; Wu, X. Dynamically reinforced heterogeneous grain structure prolongs ductility in a medium-entropy alloy with gigapascal yield strength. Proc. Natl. Acad. Sci. USA 2018, 115, 7224–7229. [Google Scholar] [CrossRef] [Green Version]
  21. Huang, H.; Li, X.; Dong, Z.; Li, W.; Huang, S.; Meng, D.; Lai, X.; Liu, T.; Zhu, S.; Vitos, L. Critical stress for twinning nucleation in CrCoNi-based medium and high entropy alloys. Acta Mater. 2018, 149, 388–396. [Google Scholar] [CrossRef]
  22. Jo, Y.H.; Jung, S.; Choi, W.M.; Sohn, S.S.; Kim, H.S.; Lee, B.J.; Kim, N.J.; Lee, S. Cryogenic strength improvement by utilizing room-temperature deformation twinning in a partially recrystallized VCrMnFeCoNi high-entropy alloy. Nat. Commun. 2017, 8, 15719. [Google Scholar] [CrossRef] [PubMed]
  23. Slone, C.E.; Chakraborty, S.; Miao, J.; George, E.P.; Mills, M.J.; Niezgoda, S.R. Influence of deformation induced nanoscale twinning and FCC-HCP transformation on hardening and texture development in medium-entropy CrCoNi alloy. Acta Mater. 2018, 158, 38–52. [Google Scholar] [CrossRef]
  24. Wu, Z.; Parish, C.M.; Bei, H. Nano-twin mediated plasticity in carbon-containing FeNiCoCrMn high entropy alloys. J. Alloy. Compd. 2015, 647, 815–822. [Google Scholar] [CrossRef] [Green Version]
  25. Won, J.W.; Lee, S.; Park, S.H.; Kang, M.; Lim, K.R.; Park, C.H.; Na, Y.S. Ultrafine-grained CoCrFeMnNi high-entropy alloy produced by cryogenic multi-pass caliber rolling. J. Alloy Compd. 2018, 742, 290–295. [Google Scholar] [CrossRef]
  26. Yu, H.; Lu, C.; Tieu, A.K.; Li, H.J.; Godbole, A.; Zhang, S. Special rolling techniques for improvement of mechanical properties of ultrafine-grained metal sheets: A review. Adv. Eng. Mater. 2016, 18, 754–769. [Google Scholar] [CrossRef] [Green Version]
  27. Shi, J.T.; Hou, L.G.; Ma, C.Q.; Zuo, J.R.; Cui, H.; Zhuang, L.Z.; Zhang, J.S. Mechanical properties and microstructures of 5052 Al alloy processed by asymmetric cryorolling. Mater. Sci. Forum 2016, 850, 823–828. [Google Scholar] [CrossRef]
  28. Yu, H.; Tieu, K.; Lu, C.; Lou, Y.; Liu, X.; Godbole, A.; Kong, C. Tensile fracture of ultrafine grained aluminum 6061 sheets by asymmetric cryorolling for microforming. Int. J. Damage Mech. 2014, 23, 1077–1095. [Google Scholar] [CrossRef] [Green Version]
  29. Yu, H.; Wang, L.; Chai, L.; Li, J.; Lu, C.; Godbole, A.; Wang, H.; Kong, C. High thermal stability and excellent mechanical properties of ultrafine-grained high-purity copper sheets subjected to asymmetric cryorolling. Mater. Charact. 2019, 153, 34–45. [Google Scholar] [CrossRef]
  30. Yu, H.; Du, Q.; Godbole, A.; Lu, C.; Kong, C. Improvement in strength and ductility of asymmetric-cryorolled copper sheets under low-temperature annealing. Metall. Mater. Trans. A 2018, 49, 4398–4403. [Google Scholar] [CrossRef]
  31. Yu, H.; Lu, C.; Tieu, A.K.; Li, H.; Godbole, A.; Kong, C.; Zhao, X. Simultaneous grain growth and grain refinement in bulk ultrafine-grained copper under tensile deformation at room temperature. Metall. Mater. Trans. A 2016, 47, 3785–3789. [Google Scholar] [CrossRef] [Green Version]
  32. Zhang, Z.; Wu, Y.; Bhatta, L.; Li, C.; Gan, B.; Kong, C.; Wang, Y.; Yu, H. Mechanical properties and microstructure evolution of a CrCoNi medium entropy alloy subjected to asymmetric cryorolling and subsequent annealing. Mater. Today Commun. 2020. [Google Scholar] [CrossRef]
  33. Wu, Y.; Zhang, Z.; Liu, J.; Kong, C.; Wang, Y.; Tandon, P.; Pesin, A.; Zhilyaev, A.P.; Yu, H. Superior strengthening effect on heterogeneous lamellar structure in medium entropy alloy CrCoNi processed by asymmetric cryorolling. Under reviewing.
  34. Okamoto, N.L.; Fujimoto, S.; Kambara, Y.; Kawamura, M.; Chen, Z.M.T.; Matsunoshita, H.; Tanaka, K.; Inui, H.; George, E.P. Size effect, critical resolved shear stress, stacking fault energy, and solid solution strengthening in the CrMnFeCoNi high-entropy alloy. Sci. Rep. 2016, 6, 35863. [Google Scholar] [CrossRef] [PubMed]
  35. Zhao, Y.L.; Yang, T.; Tong, Y.; Wang, J.; Luan, J.H.; Jiao, Z.B.; Chen, D.; Yang, Y.; Hu, A.; Liu, C.T.; et al. Heterogeneous precipitation behavior and stacking-fault-mediated deformation in a CoCrNi-based medium-entropy alloy. Acta Mater. 2017, 138, 72–82. [Google Scholar] [CrossRef]
  36. Tang, Q.; Cai, X.; Dai, P. Grain boundary character distribution in CoCrFeMnNi high-entropy alloy after cold rolling and subsequent annealing. Heat Treat. Met. 2016, 41, 217–221. [Google Scholar]
  37. Thomson, C.B.; Randle, V. “Fine tuning” at Σ3n boundaries in nickel. Acta Mater. 1997, 45, 4909–4916. [Google Scholar] [CrossRef]
  38. Randle, V. Mechanism of twinning-induced grain boundary engineering in low stacking-fault energy materials. Acta Mater. 1999, 47, 4187–4196. [Google Scholar] [CrossRef]
  39. Dan Sathiaraj, G.; Skrotzki, W.; Pukenas, A.; Schaarschuch, R.; Jose Immanuel, R.; Panigrahi, S.K.; Arout Chelvane, J.; Satheesh Kumar, S.S. Effect of annealing on the microstructure and texture of cold rolled CrCoNi medium-entropy alloy. Intermetallics 2018, 101, 87–98. [Google Scholar] [CrossRef]
  40. Beke, D.L.; Erdélyi, G. On the diffusion in high-entropy alloys. Mater. Lett. 2016, 164, 111–113. [Google Scholar] [CrossRef]
  41. Sathiaraj, G.D.; Bhattacharjee, P.P.; Tsai, C.W.; Yeh, J.W. Effect of heavy cryo-rolling on the evolution of microstructure and texture during annealing of equiatomic CoCrFeMnNi high entropy alloy. Intermetallics 2016, 69, 1–9. [Google Scholar] [CrossRef]
  42. Sathiaraj, G.D.; Bhattacharjee, P.P. Effect of cold-rolling strain on the evolution of annealing texture of equiatomic CoCrFeMnNi high entropy alloy. Mater. Charact. 2015, 109, 189–197. [Google Scholar] [CrossRef]
  43. Bhattacharjee, P.P.; Sathiaraj, G.D.; Zaid, M.; Gatti, J.R.; Lee, C.; Tsai, C.W.; Yeh, J.W. Microstructure and texture evolution during annealing of equiatomic CoCrFeMnNi high-entropy alloy. J. Alloy. Compd. 2014, 587, 544–552. [Google Scholar] [CrossRef]
  44. Sathiaraj, G.D.; Ahmed, M.Z.; Bhattacharjee, P.P. Microstructure and texture of heavily cold-rolled and annealed fcc equiatomic medium to high entropy alloys. J. Alloy. Compd. 2016, 664, 109–119. [Google Scholar] [CrossRef]
  45. Sathiaraj, G.D.; Lee, C.; Tsai, C.W.; Yeh, J.W.; Bhattacharjee, P.P. Evolution of microstructure and crystallographic texture in severely cold rolled high entropy equiatomic CoCrFeMnNi alloy during annealing. IOP Conf. Ser. Mater. Sci. Eng. 2015, 82, 012068. [Google Scholar] [CrossRef]
  46. Jia, N.; Eisenlohr, P.; Roters, F.; Raabe, D.; Zhao, X. Orientation dependence of shear banding in face-centered-cubic single crystals. Acta Mater. 2012, 60, 3415–3434. [Google Scholar] [CrossRef]
  47. Sathiaraj, G.D.; Bhattacharjee, P.P. Effect of starting grain size on the evolution of microstructure and texture during thermo-mechanical processing of CoCrFeMnNi high entropy alloy. J. Alloy. Compd. 2015, 647, 82–96. [Google Scholar] [CrossRef]
  48. Tsai, K.Y.; Tsai, M.H.; Yeh, J.W. Sluggish diffusion in Co–Cr–Fe–Mn–Ni high-entropy alloys. Acta Mater. 2013, 61, 4887–4897. [Google Scholar] [CrossRef]
  49. Sathiaraj, G.D.; Pukenas, A.; Skrotzki, W. Texture formation in face-centered cubic high-entropy alloys. J. Alloy. Compd. 2020, 826, 154183. [Google Scholar] [CrossRef]
  50. Haase, C.; Barrales-Mora, L.A. Influence of deformation and annealing twinning on the microstructure and texture evolution of face-centered cubic high-entropy alloys. Acta Mater. 2018, 150, 88–103. [Google Scholar] [CrossRef] [Green Version]
  51. Shi, Y.; Li, M.; Guo, D.; Ma, T.; Zhang, Z.; Li, X.; Zhang, G.; Zhang, X. Extraordinary toughening by cryorolling in Zr. Adv. Eng. Mater. 2014, 16, 167–170. [Google Scholar] [CrossRef]
  52. D’yakonov, G.S.; Zherebtsov, S.V.; Klimova, M.V.; Salishchev, G.A. Microstructure evolution of commercial-purity titanium during cryorolling. Phys. Met. Metall. 2015, 116, 182–188. [Google Scholar] [CrossRef]
  53. Yu, H.; Yan, M.; Li, J.; Godbole, A.; Lu, C.; Tieu, K.; Li, H.; Kong, C. Mechanical properties and microstructure of a Ti-6Al-4V alloy subjected to cold rolling, asymmetric rolling and asymmetric cryorolling. Mater. Sci. Eng. A 2018, 710, 10–16. [Google Scholar] [CrossRef] [Green Version]
  54. Liu, J.; Wu, Y.; Wang, L.; Wang, H.; Kong, C.; Pesin, A.; Zhilyaev, A.P.; Yu, H. Fabrication and Characterization of High-Bonding-Strength Al/Ti/Al-Laminated Composites via Cryorolling. Acta Metall. Sin. Engl. Lett. 2020, 33, 871–880. [Google Scholar] [CrossRef]
Figure 1. Coincidence site lattice (CSL) GB maps of (a) asymmetrically rolled medium entropy alloys (MEA) CrCoNi with annealing at 600 °C, (b) asymmetrically rolled MEA CrCoNi with annealing at 800 °C, (c) cryorolled MEA CrCoNi with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled MEA CrCoNi with annealing at 600 °C, and (f) asymmetric cryorolled MEA CrCoNi with annealing at 800 °C.
Figure 1. Coincidence site lattice (CSL) GB maps of (a) asymmetrically rolled medium entropy alloys (MEA) CrCoNi with annealing at 600 °C, (b) asymmetrically rolled MEA CrCoNi with annealing at 800 °C, (c) cryorolled MEA CrCoNi with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled MEA CrCoNi with annealing at 600 °C, and (f) asymmetric cryorolled MEA CrCoNi with annealing at 800 °C.
Crystals 10 01154 g001
Figure 2. Grain size distribution of (a) asymmetrically rolled MEA CrCoNi with annealing at 600 °C, (b) asymmetrically rolled MEA CrCoNi with annealing at 800 °C, (c) cryorolled MEA CrCoNi with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled MEA CrCoNi with annealing at 600 °C, and (f) asymmetric cryorolled MEA CrCoNi with annealing at 800 °C.
Figure 2. Grain size distribution of (a) asymmetrically rolled MEA CrCoNi with annealing at 600 °C, (b) asymmetrically rolled MEA CrCoNi with annealing at 800 °C, (c) cryorolled MEA CrCoNi with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled MEA CrCoNi with annealing at 600 °C, and (f) asymmetric cryorolled MEA CrCoNi with annealing at 800 °C.
Crystals 10 01154 g002
Figure 3. Schematic representation of important recrystallization texture components and α-fiber observed in the CoCrNi MEA, orientation distribution function (ODF) sections at ϕ 2 = 0°, 15°, 35°, 45°, and 65°.
Figure 3. Schematic representation of important recrystallization texture components and α-fiber observed in the CoCrNi MEA, orientation distribution function (ODF) sections at ϕ 2 = 0°, 15°, 35°, 45°, and 65°.
Crystals 10 01154 g003
Figure 4. ODFs ( ϕ 2 = 0°, 15°, 35°, 45°, and 65° sections) sections of (a) asymmetrically rolled CoCrNi MEA with annealing at 600 °C, (b) asymmetrically rolled CoCrNi MEA with annealing at 800 °C, (c) cryorolled CoCrNi MEA with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled CoCrNi MEA with annealing at 600 °C, and (f) asymmetric cryorolled CoCrNi MEA with annealing at 800 °C.
Figure 4. ODFs ( ϕ 2 = 0°, 15°, 35°, 45°, and 65° sections) sections of (a) asymmetrically rolled CoCrNi MEA with annealing at 600 °C, (b) asymmetrically rolled CoCrNi MEA with annealing at 800 °C, (c) cryorolled CoCrNi MEA with annealing at 600 °C, (d) cryorolled MEA CrCoNi with annealing at 800 °C, (e) asymmetric cryorolled CoCrNi MEA with annealing at 600 °C, and (f) asymmetric cryorolled CoCrNi MEA with annealing at 800 °C.
Crystals 10 01154 g004
Figure 5. Variation of texture components with annealing temperature in (a) asymmetrically rolled CoCrNi MEA, (b) cryorolled CoCrNi MEA (c) asymmetric cryorolled CoCrNi MEA; (d) comparison of the variation of texture index with annealing temperature between asymmetrically rolled, cryorolled and asymmetric cryorolled CoCrNi MEA.
Figure 5. Variation of texture components with annealing temperature in (a) asymmetrically rolled CoCrNi MEA, (b) cryorolled CoCrNi MEA (c) asymmetric cryorolled CoCrNi MEA; (d) comparison of the variation of texture index with annealing temperature between asymmetrically rolled, cryorolled and asymmetric cryorolled CoCrNi MEA.
Crystals 10 01154 g005
Figure 6. The hardness change diagram of the CoCrNi MEA (a) after asymmetric rolling, cryorolling, asymmetric cryorolling, and subsequent annealing at (b) 600 °C, (c) 700 °C, (d) 800 °C.
Figure 6. The hardness change diagram of the CoCrNi MEA (a) after asymmetric rolling, cryorolling, asymmetric cryorolling, and subsequent annealing at (b) 600 °C, (c) 700 °C, (d) 800 °C.
Crystals 10 01154 g006
Table 1. Important recrystallization texture components in the CoCrNi MEA.
Table 1. Important recrystallization texture components in the CoCrNi MEA.
Texture ComponentSymbolEuler AngleMiller Indices
Cube(C) Crystals 10 01154 i0010, 0, 0{001}<100>
Copper(Cu) Crystals 10 01154 i00290, 35, 45{112}<111>
Goss(G) Crystals 10 01154 i0030, 45, 0{110}<001>
Brass(Bs) Crystals 10 01154 i00435, 45, 0{110}<112>
S Crystals 10 01154 i00559, 37, 63{123}<634>
G/B Crystals 10 01154 i00617, 45, 0{110}<115>
A Crystals 10 01154 i00755, 45, 0{110}<111>
Rotated Goss(Rt-G) Crystals 10 01154 i00890, 45, 0{110}<110>
BR Crystals 10 01154 i00980, 31, 35{236}<385>
M Crystals 10 01154 i01080, 30, 65{13 6 25}<20 15 14>
D Crystals 10 01154 i01190, 25, 45{113}<332>
K Crystals 10 01154 i01227, 64, 14{142}<211>
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Wu, Y.; Liu, J.; Bhatta, L.; Kong, C.; Yu, H. Study of Texture Analysis on Asymmetric Cryorolled and Annealed CoCrNi Medium Entropy Alloy. Crystals 2020, 10, 1154. https://doi.org/10.3390/cryst10121154

AMA Style

Wu Y, Liu J, Bhatta L, Kong C, Yu H. Study of Texture Analysis on Asymmetric Cryorolled and Annealed CoCrNi Medium Entropy Alloy. Crystals. 2020; 10(12):1154. https://doi.org/10.3390/cryst10121154

Chicago/Turabian Style

Wu, Yuze, Juan Liu, Laxman Bhatta, Charlie Kong, and Hailiang Yu. 2020. "Study of Texture Analysis on Asymmetric Cryorolled and Annealed CoCrNi Medium Entropy Alloy" Crystals 10, no. 12: 1154. https://doi.org/10.3390/cryst10121154

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop