Article

Phase Evolution and Synthesis of Be12 Nb Intermetallic Compound in the 800–1300 °C Temperature Range

by
Sergey Udartsev
1,2,
Inesh E. Kenzhina
1,
Timur Kulsartov
1,3,
Kuanysh Samarkhanov
1,3,*,
Zhanna Zaurbekova
1,
Yuriy Ponkratov
1,3,
Alexandr Yelishenkov
1,
Meiram Begentayev
1,
Saulet Askerbekov
1,
Aktolkyn Tolenova
1,
Manarbek Kylyshkanov
2,
Mikhail Podoinikov
2,
Ainur Kaynazarova
2 and
Oleg Obgolts
2
1
Department of General Physics, Satbayev University, Almaty 050032, Kazakhstan
2
Ulba Metallurgical Plant JSC, Ust-Kamenogorsk 070005, Kazakhstan
3
Materials Testing Department, Institute of Atomic Energy Branch of National Nuclear Center of the Republic of Kazakhstan, Kurchatov 071100, Kazakhstan
*
Author to whom correspondence should be addressed.
Materials 2025, 18(12), 2915; https://doi.org/10.3390/ma18122915
Submission received: 10 May 2025 / Revised: 15 June 2025 / Accepted: 16 June 2025 / Published: 19 June 2025
(This article belongs to the Section Advanced Materials Characterization)

Abstract

Beryllium-based intermetallic compounds, such as Be12Nb, are attracting growing interest for their high thermal stability and potential to replace pure beryllium as neutron reflectors and multipliers in both fission and future fusion reactors, with additional applications in metallurgy, aerospace, and hydrogen technology. The paper presents the results of an investigation of the thermal treatment and phase formation of the intermetallic compound Be12Nb from a mixture of niobium and beryllium powders in the temperature range of 800–1300 °C. The phase evolution was assessed as a function of sintering temperature and time. A nearly single-phase Be12Nb composition was achieved at 1100 °C, while decomposition into lower-order beryllides such as Be17Nb2 occurred at temperatures ≥1200 °C, indicating thermal instability of Be12Nb under vacuum. Careful handling of sintering in low vacuum minimized oxidation, though signs of possible BeO formation were noted. The findings complement and extend earlier reports on Be12Nb synthesis via plasma sintering, mechanical alloying, and other powder metallurgy routes, providing broader insight into phase formation and synthesis. These results provide a foundation for optimizing the manufacturing parameters required to produce homogeneous Be12Nb-based components and billets at an industrial scale. Additionally, they help define the operational temperature limits necessary to preserve the material’s phase integrity during application.

1. Introduction

Beryllium-based intermetallic compounds [1,2], particularly those of the Be12M type (where M = Ti, Cr, V, Zr, etc.), have attracted increasing interest due to their high thermal stability, low swelling, and favorable neutron breeding properties, making them promising candidates for use as neutron multipliers in future fusion facilities such as ITER and DEMO [3,4,5,6,7]. DEMO-type reactors are projected to operate under more extreme conditions than ITER, including higher neutron flux [8,9,10] and sustained high temperatures, requiring structural and functional materials with enhanced oxidation resistance [11,12], high melting points, and low tritium retention [13,14].
The intermetallic compound Be12Nb has been proposed as a potential alternative to pure beryllium for high-temperature applications in both nuclear [15] and aerospace systems [16,17] due to its theoretically high thermal stability [18], corrosion resistance, etc. Additional interest has emerged around its potential use in hydrogen-related technologies, such as solid-state hydrogen storage [19]. However, it must be noted that Be12Nb has not yet seen practical implementation due to challenges in synthesis, phase stability, and limited mechanical property data.
The phase diagram of the beryllium–niobium (Be–Nb) system at atmospheric pressure is given in [20] and shown in Figure 1.
Six intermetallic compounds are formed in the Be–Nb system: Be12Nb, Be17Nb2, Be5Nb, Be3Nb, Be2Nb, and Be2Nb3.
The compound Be12Nb is formed via a peritectic reaction at 1672 °C from the liquid phase and the compound Be17Nb2. According to the diagram, the intermetallic Be17Nb2 melts congruently at 1800 °C. At 1415 °C, it decomposes to form Be12Nb and Be5Nb. The compound Be5Nb is presumably formed via a peritectoid reaction at 1485 °C from two intermetallics: Be17Nb2 and Be3Nb. The intermetallic compound Be3Nb has the highest melting point in the system, equal to 1980 °C. It melts congruently and does not undergo further transformations down to room temperature. The beryllide Be2Nb is also formed via a peritectic reaction from the liquid phase and the intermetallic Be3Nb. Finally, the intermetallic Be2Nb3 is formed via a peritectic reaction from the solid solution of niobium in beryllium and the liquid phase at 1590 °C. There are also two eutectic reactions in the system: Be17Nb2 + Be3Nb and Be2Nb + Be2Nb3, with eutectic temperatures of 1620 and 1440 °C, respectively.
The synthesis of Be12Nb is complicated by several intrinsic material factors: its high melting point (1672 °C) [20], the large disparity between the melting points of its constituent elements (Be: 1283 °C; Nb: 2468 °C), the volatility and chemical reactivity of beryllium, and the tendency for melt contamination or crucible interaction under high-temperature conditions. These difficulties make conventional melting methods impractical, thereby driving interest in solid-state sintering routes, such as powder metallurgy, to synthesize Be12Nb.
Obtaining large-sized billets or workpieces from beryllium intermetallics using conventional alloying methods faces several clear challenges. The main drawback is the inability to achieve a single-phase Be12Nb structure. Due to the relatively high melting point of Be12Nb (1672 °C) and the significant difference in the melting points of beryllium (1285 °C) and niobium (2468 °C), a key challenge is identifying a reliable melting method that also suppresses the evaporation of beryllium, which has a high vapor pressure during the melting process. The high reactivity of beryllium necessitates melting in crucibles made of beryllium oxide; otherwise, the melt becomes contaminated with impurities from the crucible material. Additionally, the high melting temperatures of the final product require overheating the melt to prevent early crystallization when it comes into contact with the mold or necessitate preheating the mold. The low casting characteristics of beryllium intermetallics lead to significant shrinkage cavities, porosity, and cracks. For this reason, the manufacturing of large-sized billets and components from beryllides is usually produced using vacuum pressure solid-state sintering methods.
Several approaches have been explored to synthesize Be12Nb. In [21] used plasma sintering at 900–1000 °C was used, and observed that increased Be12Nb phase formation occurred with extended sintering durations. In a follow-up study, [22] compared sinterability and thermal stability of Nb- and V-based beryllides, confirming that prolonged sintering times enhanced the Be12Nb fraction but did not achieve phase-pure material [19]. Similarly, [23] demonstrated Be12Nb formation via mechanical alloying and annealing, although notable contamination from tungsten carbide milling media was observed. Sputter deposition methods have also been used to investigate phase stability and composition ranges of Be12Nb thin films [24,25,26,27], revealing a stoichiometric window and potential for metastable phase formation. Hot isostatic pressing (HIP) has shown success in synthesizing dense Be12Nb samples, though later studies have indicated potential for embrittlement and grain boundary degradation [28,29].
In previous work, the authors of the present study investigated the synthesis of Be3Nb, identifying a sequence of intermediate beryllide phases and optimal conditions for single-phase formation at 1300 °C [30]. Building on that, the current study focuses on the synthesis of Be12Nb applied to a stoichiometric mixture of pre-compacted beryllium and niobium powders within the temperature range of 800 °C and 1300 °C. The aim is to determine the optimal conditions for forming a single-phase Be12Nb compound as a function of sintering temperature and time. The research findings can be applied in the development of vacuum hot pressing or plasma sintering processes for producing single-phase Be12Nb billets.

2. Materials and Methods

High-purity PTB-56 grade beryllium powder and NbP-3b grade niobium powder, both produced by UMP JSC (Ust-Kamenogorsk, Kazakhstan), were used in this study. These industrially manufactured powders are known for their high chemical purity and were selected based on characteristics similar to those reported in [30].
For the research, PTB-56 grade beryllium powder and NbP-36 grade niobium powder [31] were used, both produced by JSC “Ulba Metallurgical Plant,” Ust-Kamenogorsk, Kazakhstan. The chemical compositions of the beryllium and niobium powders are provided in Table 1 and Table 2.
Particle size analysis was performed using an Analysette 22 NanoTec (Fritsch GmbH, Markt Einersheim, Germany) laser particle sizer. The particle size distribution curve of Nb and Be powders is given in Figure 2.
Figure 2a shows that the particle sizes of niobium powder range from 10 to 70 µm, with an average effective particle size of 31.27 µm. Figure 2b demonstrates that the particle size distribution of beryllium powder exhibits two distinct regions. Approximately 4.0% by mass of the beryllium powder particles have sizes ranging from 1.5 to 6 µm, with an average size of about 1.8 µm in this range, referred to as the fine fraction. The remaining particles range in size from 6 to 60 µm. Overall, the average effective particle size of the beryllium powder is 23.67 µm.
SEM images of the powder particles obtained using an electron microscope at ×1000 magnification are shown in Figure 3.
As seen, the beryllium powder particles predominantly have a round, flaky shape without internal voids, while the niobium powder particles exhibit an angular shape with sharp edges and flat faces, also without internal voids.
To synthesize Be12Nb, beryllium and niobium powders were mixed in a stoichiometric ratio corresponding to 53.79 wt.% Be and 46.21 wt.% Nb. Mixing was carried out for at least 1 h using a Turbula C 2.0 turbulent mixer, Willy A. Bachofen AG, Basel, Switzerland. The mixed powder was then compacted using a P-10 hydraulic press, Carver, Inc., Wabash, IN, USA with a maximum load of 100 kN, producing cylindrical briquettes with diameters of 14 mm and heights of approximately 20 mm. A schematic representation of the overall experimental procedure is provided in Figure 4.
Sintering was conducted in a vacuum furnace in the temperature range of 800 °C to 1300 °C, in 100 °C increments. For each temperature, holding durations of 1, 2, and 3 h were used. The heating rate was maintained at 15–20 °C/min, and vacuum pressure during sintering did not exceed 2 × 10−3 Torr. No external pressure was applied during sintering, and the samples were left to cool naturally in the furnace after the holding period. A total of 22 samples were synthesized under varying time-temperature conditions.
After sintering, each sample was manually ground to a powder with an average particle size of 10–20 μm for structural and phase analysis. X-ray diffraction (XRD) analysis was performed using a Bruker D8 Advance Eco diffractometer, Bruker, Billerica, MA, USA. Scanning parameters were consistent with those used in [30]. The quantitative phase analysis was performed using the Rietveld method [32] with the TOPAS 6.0 software [33,34] and crystal structure data from the *.cif files of niobium beryllides.
Microstructural characterization was conducted using a JEOL JSM-5610 scanning electron microscope, JEOL, Tokyo, Japan. Both the backscattered electron (BSE) mode, for compositional contrast, and the secondary electron (SE) mode, for surface topography, were used. Representative results showing the pressed briquette and SEM images at different magnifications are presented in Figure 5. The images confirm that beryllium (darker regions) and niobium (lighter regions) powders were in tight mechanical contact before sintering.

3. Results

Sintering of pressed briquettes composed of niobium and beryllium powders led to a visible increase in volume and a loosening of structural integrity as the reaction progressed. Figure 6 illustrates briquettes sintered at different temperatures: (a) and (b) after 2 h and 3 h at 800 °C, respectively, and (c) and (d) after 2 h and 6 h at 1300 °C. At higher sintering temperatures, more pronounced expansion was observed. In contrast, samples sintered at 800 °C exhibited no substantial morphological changes.
The volumetric expansion of the briquettes can be attributed to two main factors. First, increased internal pressure due to residual gases trapped in the porous matrix may cause mechanical expansion upon heating. Second, and more significantly, the formation of intermetallic compounds during sintering leads to substantial lattice volume increases. As shown in Table A1, intermetallic phases such as Be12Nb (231.3 Å3) possess unit cell volumes far exceeding those of the starting elements—niobium (36.15 Å3) and beryllium (16.22 Å3). This transformation, caused by the rearrangement of the crystal structure from elemental powders to larger-volume beryllide structures, underpins the observed macroscopic swelling. Furthermore, as the powders react and form new phases, the initial compacted structure becomes disrupted, resulting in visible loosening of the briquettes.
The results of X-ray phase analysis and quantification of niobium beryllide phases formed in each temperature–time range are presented in the following subsections.

3.1. Synthesis at 800 °C

XRD results after sintering at 800 °C for 1, 2, and 3 h are shown in Figure 7.
At the initial stage of synthesis at 800 °C, the diffraction patterns are dominated by peaks corresponding to the unreacted beryllium and niobium. The intensity of peaks associated with intermetallic compounds (Be12Nb, Be17Nb2, Be3Nb, Be2Nb, Be2Nb3) remains significantly lower, indicating limited phase formation. The samples predominantly consist of beryllium (~80 wt.%) and niobium (~12 wt.%), as shown in the quantitative analysis using TOPAS 6.0 software (Figure 8).
The low intensity of beryllide peaks suggests that either the activation energy at this temperature is insufficient to drive significant reaction, or the reaction kinetics are too slow to form appreciable amounts of intermetallics within the 1–3 h range. Only slight synthesis of beryllides with Be/Nb atom ratios < 3 or =3 was observed. Nb3Be2 content remained under 4 wt.%, while Be2Nb and Be3Nb did not exceed 2 wt.% each.
SEM images of powders of niobium beryllides synthesized at 800 °C for 2 h, taken in SE and BSE modes at various (×500 and ×1000) magnifications, are shown in Figure A1.
SEM images of powders sintered at 800 °C for 2 h confirm the limited reaction progress. Particles of the original powders remain distinct, with little to no evidence of morphological transformation. This further supports the conclusion that at 800 °C, diffusion is insufficient to promote extensive phase development.

3.2. Synthesis at 900 °C

The results of X-ray diffraction analysis after sintering at 900 °C for 1, 2, and 3 h are presented in Figure 9.
The formation of several intermetallic phases is evident at this temperature. Figure 10 shows the evolution of phase composition with time. After 1 h, the contents of unreacted beryllium and niobium decrease significantly (44.6 wt.% and 22.27 wt.%, respectively), and Be2Nb3 begins to form (~20 wt.%). After 2 h, virtually no free niobium remains (~0.71 wt.%), and all five beryllide phases (Be12Nb, Be17Nb2, Be3Nb, Be2Nb, and Be2Nb3) are detected, each with roughly similar fractions (~4.6 wt.% average). By 3 h, the content of Be3Nb peaks at ~30 wt.%, with most elemental niobium and beryllium depleted. Some beryllium may remain either dissolved within the intermetallics or present as atomic-scale residue at phase boundaries.
SEM analysis of powders sintered for 2 h at 900 °C (Figure A2) shows morphological changes consistent with early-stage intermetallic formation.
The niobium particles appear more rounded with smoother surfaces, suggesting the onset of diffusion-driven phase development. However, a considerable fraction of the original powders remains unreacted, indicating an incomplete transformation at this stage.

3.3. Synthesis at 1000 °C

The results of X-ray phase analysis after sintering at 1000 °C for 1, 2, and 3 h are shown in Figure 11.
A marked shift in phase distribution is observed at this temperature. The diffraction intensity of unreacted Nb and Be significantly decreases, and a substantial rise in the intensity of Be12Nb and Be17Nb2 peaks is noted. Figure 12 shows the compositional dynamics of the powder mixture.
After 1 h, Be12Nb and Be17Nb2 each constitute approximately 40 wt.% of the mixture, while the residual elemental content drops below 1 wt.%. By 2 and 3 h, the Be12Nb phase continues to grow, reaching 55 wt.% and 72 wt.%, respectively, as other intermediate beryllides reduce.

3.4. Synthesis at 1100 °C

The X-ray diffraction patterns of powders sintered at 1100 °C for 1, 2, and 3 h are presented in Figure 13.
At this temperature, the phase composition becomes largely monophasic. From the first hour of sintering, Be12Nb is the predominant phase (~95 wt.%), with minor traces of Be17Nb2 (~4 wt.%). This trend remains consistent for extended sintering durations (2 and 3 h), indicating that 1100 °C is optimal for achieving a nearly single-phase Be12Nb compound. The calculated post-annealing content of the mixture components for these sintering conditions is shown in Figure 14.
SEM images of powders sintered at 1100 °C for 2 h are shown in Figure A3. The microstructure becomes more uniform compared to lower temperatures. Beryllium particles are no longer visible, and the Be12Nb particles appear rounded and slightly swollen, consistent with full transformation and densification.

3.5. Synthesis at 1200 °C

The X-ray diffraction patterns of powders sintered at 1200 °C for 1, 2, and 3 h are presented in Figure 15.
Figure 16 shows the evolution of phase composition with time. After 1 and 2 h, the mixture is predominantly monophasic with ~94 wt.% and ~92 wt.% Be12Nb, respectively. However, after 3 h, the Be12Nb content declines, and Be17Nb2 (~8 wt.%), along with other beryllides with Be/Nb < 3, begin to reappear, totaling ~5 wt.%.
The surface features sintered at 1200 °C are largely consistent with those observed at 1100 °C. While the morphology of Be12Nb is generally preserved, the XRD peaks are slightly weaker in intensity compared to the 1100 °C samples, possibly indicating the onset of partial decomposition or phase redistribution.
The decomposition of the niobium beryllide Be12Nb at temperatures of 1200 °C and above can likely be explained by the following reasons.
First, at temperatures of 1200 °C and higher under vacuum conditions, Be12Nb begins to dissociate due to the breaking of certain bonds within the compound, followed by the evaporation of beryllium into the free volume of the vacuum furnace.
Second, as the temperature approaches the α-Be to β-Be phase transformation, a rearrangement of the electronic structure occurs, which likely also leads to a restructuring of the crystal lattice at this temperature, resulting in the formation of weaker chemical bonds. This causes some beryllium atoms to detach and evaporate into the free volume of the furnace.

3.6. Synthesis at 1300 °C

The X-ray diffraction patterns after sintering at 1300 °C for 1, 2, and 3 h are shown in Figure 17.
The corresponding phase composition of the synthesized powders is shown in Figure 18. At 1 h, the phase Be12Nb dominates (~87 wt.%), accompanied by minor amounts of Be17 Nb2 and residual beryllium (~8 wt.%). As sintering progresses to 2 h, the proportion of Be12Nb slightly decreases to 86 wt.%, while Be17Nb2 increases to ~10 wt.%. After 3 h, a more complex multiphase mixture emerges. Be12Nb content decreases substantially (~67 wt.%), and low-order beryllides and free beryllium appear more prominently, suggesting either decomposition of Be12Nb or incomplete transformation.
SEM analysis of powders sintered at 1300 °C for 2 h is shown in Figure A4. The microstructure is similar to that at 1200 °C, with Be12Nb particles still present but displaying signs of instability. Compared to the samples sintered at 1100 °C, the features are less defined, and localized degradation is more evident. This suggests a possible onset of thermal instability in the Be12Nb phase under vacuum conditions at this temperature.

3.7. Additional Synthesis at 1300 °C

Due to the increasing formation of other intermetallic phases at 1300 °C with prolonged sintering, further experiments were conducted to elucidate the underlying mechanisms. Two hypotheses were considered: (1) partial evaporation of beryllium under vacuum due to its high volatility above its melting point (1283 °C), and (2) thermal instability of Be12Nb itself at elevated temperatures, leading to its decomposition into lower-order beryllides.
To test these possibilities, fresh powder mixtures were compacted and sintered at 1300 °C for 3 and 6 h. XRD results (Figure 19) showed a significant decrease in Be12Nb content, particularly after 6 h. For 3 h of sintering, Be12Nb was still the dominant phase (83 wt.%), but after 6 h, Be17Nb2 became predominant (57 wt.%), while Be12Nb dropped to 17 wt.%.
SEM images of the powder sintered for 6 h at 1300 °C are presented in Figure A5, revealing structural degradation consistent with phase transformation and beryllium loss.
A two-step sintering process was also performed to separate thermal effects from beryllium volatilization. The sample was held at 1100 °C for 1 h and subsequently sintered at 1300 °C for 2 h. XRD analysis (Figure 20) expressed in logarithmic units confirmed a heterogeneous phase composition, with 59 wt.% Be12Nb, 34 wt.% Be17Nb2, and minor fractions of Be3Nb and Be2Nb.
The phase distribution for this two-step process is illustrated in Figure 21.
These findings suggest that Be12Nb becomes thermally unstable at or above 1300 °C under vacuum, leading to its dissociation into lower-order beryllides.

4. Discussion

Figure 22 summarizes the outcomes of the synthesis experiments, illustrating the evolution of various intermetallic phases, including the target compound Be12Nb, as a function of sintering temperature and time. At the initial stage (800 °C), the XRD patterns and quantitative analysis show that the samples primarily consist of unreacted niobium and beryllium powders. The synthesis of intermetallic phases is minimal and limited to low levels of Be2Nb3, indicating that the activation energy required for significant diffusion and reaction is not achieved at this temperature.
By 900 °C, the onset of intermetallic compound formation becomes evident, starting with the Be2Nb3 phase via the reaction pathway 3Nb + 2Be → Be2Nb3. This reaction occurs well below the melting points of either constituent, suggesting a solid-state diffusion mechanism. The small atomic radius and higher mobility of beryllium facilitate its penetration into the niobium lattice, leading to progressive intermetallic formation from the particle surfaces inward. The formation front likely begins at the beryllium–niobium interface and progresses through successive reactions, forming intermediate compounds such as Be2Nb and Be3Nb. These phases represent different local Be/Nb ratios depending on beryllium availability at the reaction interface. The formation of these intermediate phases continues as the system evolves towards equilibrium.
At 1000 °C, the Be12Nb phase becomes more prominent, but full conversion is not achieved within the studied time frames. Residual Be17Nb2 and trace beryllium suggest incomplete transformation or possible precursor–product relationships between Be12Nb and other phases. It has been proposed in earlier work [35] that Be17Nb2 may result from the decomposition or transformation of Be12Nb under certain thermal conditions, possibly explaining their co-existence.
The most favorable condition for the formation of a nearly single-phase Be12Nb material was achieved at 1100 °C. At this temperature, Be12Nb accounts for more than 95 wt.% of the sample, indicating optimal kinetics for diffusion and reaction. The formation mechanism likely involves sequential incorporation of beryllium into niobium-rich phases until the stoichiometric 12:1 ratio is satisfied.
At 1200 °C, however, the system begins to show early signs of instability. Although Be12Nb is still the predominant phase after 1–2 h, longer exposure leads to the emergence of Be17Nb2 and other lower-order beryllides. This suggests that elevated temperatures may induce phase dissociation, particularly under low vacuum conditions where beryllium volatility increases.
At 1300 °C, the thermal stability of Be12Nb further degrades. As demonstrated by both standard and extended sintering trials, prolonged exposure results in a significant decline of Be12Nb content, replaced by Be17Nb2 and other low-order phases. This behavior may result from the evaporation of beryllium and/or the thermal decomposition of Be12Nb.
The stepwise sintering experiment (1100 °C for 1 h followed by 1300 °C for 2 h) reinforces this hypothesis. Despite the initial formation of Be12Nb at 1100 °C, subsequent exposure to 1300 °C resulted in its partial degradation and the formation of Be17Nb2, Be3Nb, and Be2Nb.
Comparison with prior studies confirms these findings. Nakamichi et al. [21] and Kim J.-H. et al. [22] reported that while sintering at 900–1000 °C enables Be12Nb formation, extended times are required, and complete phase purity is not achieved. Our results demonstrate that sintering at 1100 °C is more effective, allowing for higher phase purity in shorter durations. Furthermore, our study reveals the critical limitation of Be12Nb at elevated temperatures, a detail not emphasized in prior reports.
In summary, the findings from this study clarify the phase formation pathway of Be12Nb and identify 1100 °C as the optimal sintering temperature for achieving a nearly single-phase material. Beyond this temperature, thermal instability under vacuum leads to degradation, limiting the processing window for potential applications.

5. Conclusions

This study provides a comprehensive analysis of the phase evolution during the synthesis of the Be12Nb intermetallic compound from a mixture of pre-compacted beryllium and niobium powders across the temperature range of 800–1300 °C. The experimental findings confirm that:
  • Intermetallic phase formation initiates at 900 °C, beginning with Be2Nb3, and proceeds through intermediate phases as beryllium diffuses into the niobium matrix.
  • The optimal synthesis temperature for nearly single-phase Be12Nb formation is 1100 °C, where over 95 wt.% Be12Nb was achieved after 1–3 h of sintering.
  • Temperatures above 1200 °C lead to the decomposition of Be12Nb and the formation of lower-order beryllides such as Be17Nb2, likely due to thermal instability and beryllium volatility under vacuum.
  • Two-stage and prolonged sintering experiments confirm the metastable nature of Be12Nb at elevated temperatures, emphasizing the importance of thermal control during processing.
This information will help substantiate the optimal processing parameters for producing Be12Nb-based billets and guide the technological considerations necessary for fabricating components with stable phase composition via optimized sintering conditions.

Author Contributions

Conceptualization, S.U. and M.K.; methodology, S.U.; software, A.K.; validation, O.O., Y.P., and Z.Z.; formal analysis, T.K.; I.E.K., and M.B.; investigation, S.U.; K.S., and M.P.; resources, M.K.; data curation, A.Y., S.A. and A.T.; writing—original draft preparation, K.S.; writing—review and editing, K.S. and Z.Z.; visualization, O.O.; supervision, I.E.K.; project administration, M.B.; funding acquisition, I.E.K. All authors have read and agreed to the published version of the manuscript.

Funding

This research has been funded by the Committee of Science of the Ministry of Science and Higher Education of the Republic of Kazakhstan, grant number BR21882237.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

Authors Sergey Udartsev, Manarbek Kylyshkanov, Mikhail Podoinikov, Ainur Kaynazarova and Oleg Obgolts were employed by the company Ulba Metallurgical Plant JSC. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
ITERInternational Thermonuclear Experimental Reactor
DEMODemonstration power plant
XRDX-ray powder diffraction
SEMScanning electron microscope
SESecondary electrons
BSEBackscattered electrons

Appendix A

Table A1. Crystal structures of Be-Nb intermetallic compounds at 20 °C.
Table A1. Crystal structures of Be-Nb intermetallic compounds at 20 °C.
CompoundProportion of Be in the CompoundPearson Symbol, Space GroupCrystal Lattice ParametersICDD PDF2 Card Numbers
Be100% wt.Hexagonal, hP2, P63/mmca = b = 2.2858, c = 3.5843 α = β = 90°, γ = 120°
Vcr. lat. = 16.22
01-071-0257
Nb0% wt.Cubic, cI2, Im-3ma = b = c = 3.3066, α = β = γ = 90°
Vcr. lat. = 36.15
00-035-0789
Be2Nb36.07% wt.Tetragonal, tP10, P4/mbma = b = 6.490, c = 3.350, α = β = γ = 90°
Vcr. lat. = 141.10
03-065-1657
Be2Nb16.25% wt. Cubic ,   cF 24 ,   Fd 3 m a = b = c = 6.535, α = β = γ = 90°
V cr. lat. = 279.09
03-065-1723
Be3Nb22.54% wt.Rhombohedral, hR12, R-3ma = b = 4.561, c = 21.050
α = β = γ = 90°
V cr. lat. = 379.23
03-065-2134
Be17Nb245.19% wt. Rhombohedral ,   hR 19 ,   R 3 m a = b = 7.409, c = 10.840
α = β = 90°, γ = 120°
V cr. lat. = 515.32
01-072-5522
Be12Nb53.79% wt.Tetragonal, tI26, I4/mmma = b = 7.3272, c = 3.350
α = β= γ = 90°
V cr. lat. = 231.30
03-065-2771

Appendix B

Figure A1. SEM images of niobium beryllide powders synthesized at 800 °C for 2 h: (a) BSE mode; (b) SE mode.
Figure A1. SEM images of niobium beryllide powders synthesized at 800 °C for 2 h: (a) BSE mode; (b) SE mode.
Materials 18 02915 g0a1
Figure A2. SEM images of niobium beryllide powders sintered at 900 °C for 2 h: (a) ×200 magnification in BSE mode; (b) ×1000 magnification in BSE mode; (c) ×1000 magnification in SE mode.
Figure A2. SEM images of niobium beryllide powders sintered at 900 °C for 2 h: (a) ×200 magnification in BSE mode; (b) ×1000 magnification in BSE mode; (c) ×1000 magnification in SE mode.
Materials 18 02915 g0a2
Figure A3. SEM images of the powder surface after sintering for 2 h at 1100 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in SE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Figure A3. SEM images of the powder surface after sintering for 2 h at 1100 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in SE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Materials 18 02915 g0a3
Figure A4. SEM images of the powder surface after sintering for 2 h at 1300 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in BSE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Figure A4. SEM images of the powder surface after sintering for 2 h at 1300 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in BSE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Materials 18 02915 g0a4
Figure A5. SEM images of the powder surface after sintering for 6 h at 1300 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in BSE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Figure A5. SEM images of the powder surface after sintering for 6 h at 1300 °C: (a) ×200 magnification in BSE mode; (b) ×500 magnification in BSE mode; (c) ×2000 magnification in SE mode; (d) ×5000 magnification in SE mode.
Materials 18 02915 g0a5

References

  1. Jacobson, L.A.; Hanrahan, J.R., Jr.; Smith, J.L. Beryllides. In Intermetallic Compounds—Principles and Practice: Progress; Westbrook, J.H., Fleischer, R.L., Eds.; Wiley: Chichester, UK, 2002; Volume 3. [Google Scholar] [CrossRef]
  2. Walsh, K.A.; Vidal, E.E.; Goldberg, A.; Dalder, E.N.C.; Olson, D.L.; Mishra, B. ASM Handbook—Beryllium and Beryllium Alloys; ASM International: Novelty, OH, USA, 2009. [Google Scholar]
  3. Bachurin, D.V.; Vladimirov, P.V. Ab initio study of Be and Be12Ti for fusion applications. Intermetallics 2018, 100, 163–170. [Google Scholar] [CrossRef]
  4. Gaisin, R.; Frants, Y.; Kolmakov, M.; Zorin, B.; Kylyshkanov, M.; Podoinikov, M.; Udartsev, S.; Vechkutov, A.; Chakin, V.; Vladimirov, P. Beryllium intermetallics: Industrial experience on development and manufacture. Nucl. Mater. Energy 2023, 35, 10144. [Google Scholar] [CrossRef]
  5. Kawamura, H.; Takahashi, H.; Yoshida, N.; Shestakov, V.; Ito, Y.; Uchida, M.; Yamada, H.; Nakamichi, M.; Ishitsuka, E. Application of beryllium intermetallic compounds to neutron multiplier of fusion blanket. Fusion Eng. Des. 2002, 61–62, 391–397. [Google Scholar] [CrossRef]
  6. Nishitani, T.; Tanigawa, H.; Jitsukawa, S.; Nozawa, T.; Hayashi, K.; Yamanishi, T.; Tsuchiya, K.; Möslang, A.; Baluc, N.; Pizzuto, A.; et al. Fusion materials development program in the broader approach activities. J. Nucl. Mater. 2009, 386–388, 405–410. [Google Scholar] [CrossRef]
  7. Federici, G.; Boccaccini, L.; Cismondi, F.; Gasparotto, M.; Poitevin, Y.; Ricapito, I. An overview of the EU breeding blanket design strategy as an integral part of the DEMO design effort. Fusion Eng. Des. 2019, 141, 30–42. [Google Scholar] [CrossRef]
  8. Chakin, V.; Fedorov, A.; Gaisin, R.; Zmitko, M. Swelling of Highly Neutron Irradiated Beryllium and Titanium Beryllide. J. Nucl. Eng. 2022, 3, 398–408. [Google Scholar] [CrossRef]
  9. Zdorovets, M.V.; Shlimas, D.I.; Kozlovskiy, A.L.; Borgekov, D.B. Study of the Application Efficiency of Irradiation with Heavy Ions to Increase the Helium Swelling Resistance of BeO Ceramics. Metals 2022, 12, 307. [Google Scholar] [CrossRef]
  10. Zdorovets, M.V.; Shlimas, D.I.; Kozlovskiy, A.L.; Borgekov, D.B. Effect of Irradiation with Low-Energy He2+ Ions on Degradation of Structural, Strength and Heat-Conducting Properties of BeO Ceramics. Crystals 2022, 12, 69. [Google Scholar] [CrossRef]
  11. Paine, R.M.; Stonehouse, A.J.; Beaver, W.W. High temperature oxidation resistance of the beryllides. Corrosion 1964, 20, 307t–313t. [Google Scholar] [CrossRef]
  12. Kulsartov, T.; Samarkhanov, K.; Bochkov, V.; Kenzhin, Y.; Ponkratov, Y.; Kenzhina, I.; Zaurbekova, Z.; Sapatayev, Y.; Askerbekov, S.; Yelishenkov, A.; et al. High-temperature corrosion testing of titanium beryllides in the presence of water vapor and oxygen. J. Nucl. Mater. 2024, 600, 155294. [Google Scholar] [CrossRef]
  13. Kim, J.-H.; Miyamoto, M.; Hujii, Y.; Nakamichi, M. Reactivity and deuterium retention properties of titanium–beryllium intermetallic compounds. Intermetallics 2017, 82, 20–25. [Google Scholar] [CrossRef]
  14. Kenzhin, E.A.; Kenzhina, I.E.; Kulsartov, T.V.; Ponkratov, Y.V.; Gordienko, Y.N.; Bochkov, V.S.; Samarkhanov, K.K.; Shaimerdenov, A.A.; Askerbekov, S.K.; Udartsev, S. Study of interaction of hydrogen isotopes with titanium beryllide (Be12Ti). Fusion Eng. Des. 2023, 191, 113738. [Google Scholar] [CrossRef]
  15. Rubel, M.J.; Bailescu, V.; Coad, J.P.; Hirai, T.; Likonen, J.; Linke, J.; Lungu, C.P.; Matthews, G.F.; Pedrick, L.; Riccardo, V.; et al. Beryllium Plasma-Facing Components for the ITER-Like Wall Project at JET. J. Phys. Conf. Ser. 2008, 100, 062028. [Google Scholar] [CrossRef]
  16. Snead, L.L.; Zinkle, S.J. Use of Beryllium and Beryllium Oxide in Space Reactors. AIP Conf. Proc. 2005, 746, 768–775. [Google Scholar] [CrossRef]
  17. Satya Prasad, V.V.; Baligidad, R.G.; Gokhale, A.A. Niobium and Other High Temperature Refractory Metals for Aerospace Applications. In Aerospace Materials and Material Technologies; Prasad, N., Wanhill, R., Eds.; Springer: Singapore, 2017. [Google Scholar] [CrossRef]
  18. Samsonov, G.V. The chemistry of the beryllides. Russ. Chem. Rev. 1966, 35, 339. [Google Scholar] [CrossRef]
  19. Sandrock, G. State-of-the-Art Review of Hydrogen Storage in Reversible Metal Hydrides for Military Fuel Cell Applications; SunaTech, Inc.: Ringwood, NJ, USA, 1997. [Google Scholar]
  20. Okamoto, H. Be–Nb (Beryllium–Niobium). J. Phase Equilibria 1993, 14, 532–534. [Google Scholar] [CrossRef]
  21. Nakamichi, M.; Yonehara, K.; Wakai, D. Trial fabrication of beryllides as advanced neutron multiplier. Fusion Eng. Des. 2011, 86, 2262–2264. [Google Scholar] [CrossRef]
  22. Kim, J.-H.; Nakamichi, M. Comparative study of sinterability and thermal stability in plasma-sintered niobium and vanadium beryllides. J. Alloys Compd. 2015, 638, 277–281. [Google Scholar] [CrossRef]
  23. Chou, T.C.; Nieh, T.G.; Wadswarth, J. Structural evolution in niobium beryllides during mechanical alloying. Scr. Metall. Mater. 1992, 27, 881–886. [Google Scholar] [CrossRef]
  24. Brimhall, J.L.; Charlot, L.A.; Bruemmer, S.M. Metastable Phase Formation in Be–Nb Intermetallic Compounds. MRS Proc. 1990, 213, 175. [Google Scholar] [CrossRef]
  25. Brimhall, J.L.; Charlot, L.A.; Bruemmer, S.M. Phase stability and compositional range of sputter deposited Be12Nb. Scr. Metall. Mater. 1991, 25, 553–558. [Google Scholar] [CrossRef]
  26. Brimhall, J.L.; Charlot, L.A.; Bruemmer, S.M. Phase stability in Be–Nb and Be–Nb–Zr intermetallics. Mater. Sci. Eng. A 1992, 152, 76–80. [Google Scholar] [CrossRef]
  27. Brimhall, J.L.; Charlot, L.A.; Bruemmer, S.M. Phase formation and stability in sputter deposited Be–Nb compounds. J. Mater. Res. 1992, 7, 89–99. [Google Scholar] [CrossRef]
  28. Bruemmer, S.M.; Charlot, L.A.; Brimhall, J.L.; Henager, C.H.; Hirth, J.P. Dislocation structures in Be12Nb after high-temperature deformation. Philos. Mag. A 1992, 65, 1083–1094. [Google Scholar] [CrossRef]
  29. Henager, C.H.; Jacobson, R.E.; Bruemmer, S.M. Elevated temperature mechanical properties of Be12Nb. Mater. Sci. Eng. A 1992, 153, 416–421. [Google Scholar] [CrossRef]
  30. Kulsartov, T.; Udartsev, S.; Samarkhanov, K.; Gordienko, Y.N.; Ponkratov, Y.V.; Baklanova, Y.Y.; Zaurbekova, Z.A.; Kaynazarova, A.E.; Podoinikov, M.A.; Kylyshkanov, M.K.; et al. The temperature-time dependence of the amount and type of niobium beryllides formed during the synthesis of the binary intermetallic compound NbBe3. Intermetallics 2023, 163, 108065. [Google Scholar] [CrossRef]
  31. GOST 26252-84; Niobium Powder. Specifications. Standards Publishing House: Moscow, Russia, 1984.
  32. Coelho, A.A. TOPAS & TOPAS-Academic: An optimization program integrating computer algebra and crystallographic objects written in C++. J. Appl. Cryst. 2018, 51, 210–218. [Google Scholar] [CrossRef]
  33. Bruker. TOPAS, Version 6.0, Bruker AXS: Karlsruhe, Germany, 2017.
  34. Rietveld, H.M. A profile refinement method for nuclear and magnetic structures. J. Appl. Cryst. 1969, 2, 65–71. [Google Scholar] [CrossRef]
  35. Gillam, E.; Rooksby, H.P.; Brownlee, L.D. Structural relationships in beryllium–titanium alloys. Acta Crystallogr. 1964, 17, 762–763. [Google Scholar] [CrossRef]
Figure 1. Be-Nb phase diagram.
Figure 1. Be-Nb phase diagram.
Materials 18 02915 g001
Figure 2. Fractional composition of powders: (a) NbP-3b niobium; (b) PTB-56 beryllium.
Figure 2. Fractional composition of powders: (a) NbP-3b niobium; (b) PTB-56 beryllium.
Materials 18 02915 g002
Figure 3. SEM images of powder particles: (a) beryllium; (b) niobium.
Figure 3. SEM images of powder particles: (a) beryllium; (b) niobium.
Materials 18 02915 g003
Figure 4. Schematic representation of the experimental workflow for the synthesis of the Be12Nb binary intermetallic compound.
Figure 4. Schematic representation of the experimental workflow for the synthesis of the Be12Nb binary intermetallic compound.
Materials 18 02915 g004
Figure 5. Appearance and microstructure of the Be–Nb powder compact prior to sintering: (a) Densely pressed cylindrical briquette; (b) SEM image in backscattered electron (BSE) mode; (c) SEM image in secondary electron (SE) mode.
Figure 5. Appearance and microstructure of the Be–Nb powder compact prior to sintering: (a) Densely pressed cylindrical briquette; (b) SEM image in backscattered electron (BSE) mode; (c) SEM image in secondary electron (SE) mode.
Materials 18 02915 g005
Figure 6. Appearance of briquettes after sintering: (a) 2 h at 800 °C; (b) 3 h at 800 °C; (c) 2 h at 1300 °C; (d) 6 h at 1300 °C.
Figure 6. Appearance of briquettes after sintering: (a) 2 h at 800 °C; (b) 3 h at 800 °C; (c) 2 h at 1300 °C; (d) 6 h at 1300 °C.
Materials 18 02915 g006
Figure 7. X-ray diffraction patterns after sintering at 800 °C.
Figure 7. X-ray diffraction patterns after sintering at 800 °C.
Materials 18 02915 g007
Figure 8. Phase composition of powders after sintering at 800 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 8. Phase composition of powders after sintering at 800 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g008
Figure 9. X-ray diffraction patterns after sintering at 900 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 9. X-ray diffraction patterns after sintering at 900 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g009
Figure 10. Phase composition of powders after sintering at 900 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 10. Phase composition of powders after sintering at 900 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g010
Figure 11. X-ray diffraction patterns after sintering at 1000 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 11. X-ray diffraction patterns after sintering at 1000 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g011
Figure 12. Phase composition of powders after sintering at 1000 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 12. Phase composition of powders after sintering at 1000 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g012
Figure 13. X-ray diffraction patterns after sintering at 1100 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 13. X-ray diffraction patterns after sintering at 1100 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g013
Figure 14. Phase composition of powders after sintering at 1100 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 14. Phase composition of powders after sintering at 1100 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g014
Figure 15. X-ray diffraction patterns after sintering at 1200 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 15. X-ray diffraction patterns after sintering at 1200 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g015
Figure 16. Phase composition of powders after sintering at 1200 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 16. Phase composition of powders after sintering at 1200 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g016
Figure 17. X-ray diffraction patterns after sintering at 1300 °C for 1 h (light blue), 2 h (red), and 3 h (dark blue).
Figure 17. X-ray diffraction patterns after sintering at 1300 °C for 1 h (light blue), 2 h (red), and 3 h (dark blue).
Materials 18 02915 g017
Figure 18. Phase composition of powders after sintering at 1300 °C for 1 h (blue), 2 h (red), and 3 h (green).
Figure 18. Phase composition of powders after sintering at 1300 °C for 1 h (blue), 2 h (red), and 3 h (green).
Materials 18 02915 g018
Figure 19. X-ray diffraction patterns after sintering at 1300 °C for 3 h (light blue) and 6 h (dark blue).
Figure 19. X-ray diffraction patterns after sintering at 1300 °C for 3 h (light blue) and 6 h (dark blue).
Materials 18 02915 g019
Figure 20. XRD patterns after stepwise sintering at 1100 °C for 1 h, followed by 1300 °C for 2 h.
Figure 20. XRD patterns after stepwise sintering at 1100 °C for 1 h, followed by 1300 °C for 2 h.
Materials 18 02915 g020
Figure 21. Phase composition of niobium beryllide powders after stepwise sintering.
Figure 21. Phase composition of niobium beryllide powders after stepwise sintering.
Materials 18 02915 g021
Figure 22. Summarized outcomes of the Be12Nb synthesis: (a) Temperature–time dependence during the synthesis of niobium beryllide Be12Nb from beryllium and niobium powders; (b) dynamic evolution of Be–Nb intermetallic phases synthesized in the 800–1300 °C range.
Figure 22. Summarized outcomes of the Be12Nb synthesis: (a) Temperature–time dependence during the synthesis of niobium beryllide Be12Nb from beryllium and niobium powders; (b) dynamic evolution of Be–Nb intermetallic phases synthesized in the 800–1300 °C range.
Materials 18 02915 g022
Table 1. Chemical composition of PTB-56 grade beryllium powder.
Table 1. Chemical composition of PTB-56 grade beryllium powder.
ElementBeCrMgSiTiFeNiPbAlCuCOMn
Content (%, wt.)99.107 0.0230.0140.0240.0140.1560.0170.010.0180.0030.040.560.014
Table 2. Chemical composition of NbP-3b grade niobium powder.
Table 2. Chemical composition of NbP-3b grade niobium powder.
ElementNbTaTiSiFeWMoNCOHNiAlMgCuZr
Content (%, wt.)99.706 0.090.001 0.0020.0020.0030.0040.0120.0070.130.0080.0010.0010.0010.0010.001
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Udartsev, S.; Kenzhina, I.E.; Kulsartov, T.; Samarkhanov, K.; Zaurbekova, Z.; Ponkratov, Y.; Yelishenkov, A.; Begentayev, M.; Askerbekov, S.; Tolenova, A.; et al. Phase Evolution and Synthesis of Be12 Nb Intermetallic Compound in the 800–1300 °C Temperature Range. Materials 2025, 18, 2915. https://doi.org/10.3390/ma18122915

AMA Style

Udartsev S, Kenzhina IE, Kulsartov T, Samarkhanov K, Zaurbekova Z, Ponkratov Y, Yelishenkov A, Begentayev M, Askerbekov S, Tolenova A, et al. Phase Evolution and Synthesis of Be12 Nb Intermetallic Compound in the 800–1300 °C Temperature Range. Materials. 2025; 18(12):2915. https://doi.org/10.3390/ma18122915

Chicago/Turabian Style

Udartsev, Sergey, Inesh E. Kenzhina, Timur Kulsartov, Kuanysh Samarkhanov, Zhanna Zaurbekova, Yuriy Ponkratov, Alexandr Yelishenkov, Meiram Begentayev, Saulet Askerbekov, Aktolkyn Tolenova, and et al. 2025. "Phase Evolution and Synthesis of Be12 Nb Intermetallic Compound in the 800–1300 °C Temperature Range" Materials 18, no. 12: 2915. https://doi.org/10.3390/ma18122915

APA Style

Udartsev, S., Kenzhina, I. E., Kulsartov, T., Samarkhanov, K., Zaurbekova, Z., Ponkratov, Y., Yelishenkov, A., Begentayev, M., Askerbekov, S., Tolenova, A., Kylyshkanov, M., Podoinikov, M., Kaynazarova, A., & Obgolts, O. (2025). Phase Evolution and Synthesis of Be12 Nb Intermetallic Compound in the 800–1300 °C Temperature Range. Materials, 18(12), 2915. https://doi.org/10.3390/ma18122915

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop