Design-Informed Evaluation and Fretting Damage Mapping of Additive-Manufactured Ti-6Al-4V Components

by
Ahmad Sadeghian
1 and
Saeed Adibnazari
2,*
1
School of Science and Engineering, Sharif University of Technology, International Campus, Kish Island 79417-76655, Iran
2
Department of Aerospace Engineering, Sharif University of Technology, Tehran 1458889694, Iran
*
Author to whom correspondence should be addressed.
Designs 2025, 9(5), 100; https://doi.org/10.3390/designs9050100
Submission received: 21 July 2025 / Revised: 10 August 2025 / Accepted: 18 August 2025 / Published: 25 August 2025
(This article belongs to the Section Mechanical Engineering Design)

Abstract

This paper experimentally investigates the fretting fatigue behavior of metal additive-manufactured Ti-6Al-4V alloy specimens fabricated using the selective laser melting (SLM) method, focusing on damage characterization and fatigue life assessment. Based on the ASTM E466 standard, the test components were manufactured using metal 3D printing technology. Fretting fatigue tests were conducted under varying axial stress levels and contact loads, followed by microscopic examinations using scanning electron microscopy (SEM) to analyze damage mechanisms. A fretting map was developed based on SEM observations, providing insights into damage evolution under different loading conditions. These findings contribute to a better understanding of the relationship between fretting fatigue parameters and failure mechanisms. The developed fretting map and experimental observations provide a foundation for further studies aimed at enhancing the fretting fatigue life assessment of standard specimens for different test parameters. Finally, this paper includes design-oriented evaluation frameworks that can guide engineers in integrating AM components into safety-critical systems under fretting fatigue conditions.

1. Introduction

Fretting is a failure mode that occurs at the contact surfaces of two components subjected to low-amplitude oscillatory relative motions and fatigue loading. Fretting, combined with fatigue, can significantly reduce the lifespan of various mechanical components, including bearings, screw-type joints, bolted or dovetail joints, press-fitted shafts, couplings, and others. In gas turbine engines, fretting fatigue is especially prominent, occurring at the contact interfaces of the turbine blade roots, compressors dovetail joints, or fir-tree root joints in power turbines. Also, metal 3D printing has recently emerged as a transformative manufacturing technology. It offers significant advantages, such as eliminating the need for mold fabrication and enabling the production of geometrically complex components [1]. The metal additive manufacturing technique provides remarkable versatility, enabling the cost-effective production of metal components that may otherwise be prohibitively expensive or infeasible to produce using conventional techniques [2].
Given the critical importance of turbine components for reliable engine performance, this research aims to integrate material testing with design validation by evaluating the fretting fatigue life and damage characteristics of standard Ti-6Al-4V alloy specimens fabricated using additive manufacturing. By employing selective laser melting (SLM), a powder bed fusion technique, this study not only investigates fatigue performance under representative loading conditions but also derives design-relevant insights. These insights contribute to a more informed approach to the structural design of AM components in fatigue-critical applications. Furthermore, this study introduces a novel integration of experimental fretting fatigue results into a design-supportive fretting damage map, aiming to assist engineers in determining operational safety margins and optimizing design parameters for AM components under fretting-prone conditions. The following section reviews prior research, highlighting the need for experimentally grounded tools to guide design decisions in the context of fretting fatigue.

2. Literature Review

Farsha Abbasi et al. [3] provided a comprehensive review of the effects of variable cyclic contact loading on the fretting fatigue behavior of various engineering components. Iyer and Mall [4] conducted fretting fatigue tests for two types of contact surface geometries, including flat and cylindrical titanium alloy Ti-6Al-4V surfaces, under constant and two-level block remote bulk stresses. Under two-level block loading, the stress amplitude and high-cyclic fatigue (HCF) frequency of the applied load influenced the fretting fatigue life. Also, fracture topographies were drawn for the different test conditions. Furthermore, the impact of fretting pad geometry on crack initiation in Ti-6Al-4V was investigated in [5], detailing crack location and orientation along the contact surface. In the study, finite element modeling (FEM) was utilized to simulate and compare fretting fatigue behavior in both low- and high-cycle fatigue regimes with experimental results. In [6] a fracture mechanics approach was employed to develop a nonlinear integrated model for surface contacts, enabling the prediction of conditions under which small fretting-induced fatigue cracks are arrested. Studies on nickel- and titanium-based alloys, conducted using a specialized multiaxial fretting test machine, further advanced the understanding of fretting behavior [7]. This research also developed a finite element contact model for multiaxial shakedown fatigue analysis, specifically applied to highly loaded blade–disk connections.
The influence of manufacturing techniques on fatigue life was investigated by Chan et al. [8]. This study used scanning electron microscopy (SEM) to identify crack initiation sites of regular Ti-6Al-4V compared to that produced using other manufacturing techniques. Another study [9] has further elucidated the fretting performance of Ti-6Al-4V produced via additive manufacturing (AM), particularly selective laser melting (SLM) or laser powder bed fusion (LPBF), in direct comparison with conventionally manufactured counterparts. Their results showed no statistically significant differences in wear track depth or fretting current between AM and traditional Ti-6Al-4V materials. Glodek et al. [10] conducted the first dedicated fretting fatigue tests on LPBF-fabricated Ti-6Al-4V dovetail specimens, employing a purpose-built test apparatus and validated finite element model to replicate stick–slip conditions. Their findings revealed that while AM-Ti-6Al-4V exhibited enhanced crack propagation resistance relative to wrought material, it was more prone to fretting damage initiation. Together, these studies underscore the nuanced trade-offs between AM and conventional Ti-6Al-4V in fretting-related applications, emphasizing the need for design and life prediction frameworks that explicitly account for AM-induced microstructural features and degradation mechanisms.
In a different context, focusing on the influence of loading conditions rather than manufacturing routes, Huayang Zhang et al. [11] investigated the impact of applied tangential force on the fretting fatigue life of tested specimens. The study examined crack initiation life, crack growth life, and total fatigue life using an extended finite element method (XFEM) combined with a cyclic cohesive damage model. Mario Lavella [12] conducted fretting fatigue experiments of additively manufactured blades of the intermetallic alloy TiAl. The tests were performed at a specific loading frequency and high temperature to replicate real aircraft turbine operating conditions. Both analytical approaches and two-dimensional finite element (FE) analyses were employed to evaluate the stress distribution at the contact surfaces of the components. In [13], several 3D contact geometries, including cylinder-on-plane and punch-on-plane configurations, were examined under different slip regimes to perform finite element numerical analysis. Moreover, this study investigated the fatigue damage of the Ti-6Al-4V alloy in the presence of fretting wear. Numerical simulations were conducted to analyze the effects of fatigue fretting, focusing on wear or fatigue crack initiation.
Resende Pereira et al. [14] presented a finite element model of fretting fatigue for cylindrical contact interfaces and discussed aspects of fretting fatigue crack initiation, including crack location, orientation, and length. The study also provided experimental results and analytical solutions for the cylindrical contact model of fretting fatigue. Furthermore, additional aspects of fretting fatigue, including out-of-phase loading, cohesive zone modeling, wear effects, heterogeneity, and crystal orientation, were briefly reviewed. To complement simulation-based approaches, Egan [15] reviewed recent innovations in design for additive manufacturing (DfAM), with particular emphasis on the integration of topology optimization and fatigue-informed simulation frameworks for the development of high-performance, material-efficient components. These strategies align well with contemporary modeling efforts that aim to connect microstructural characteristics with macro-scale mechanical constraints in fretting fatigue and contact interface applications. In [16], a fretting fatigue crack initiation life model was developed based on slip amplitude as a macroscopic feature of the contact interfaces. A damage parameter combined with a damage severity factor was used to predict crack initiation life. Additionally, a series of fretting fatigue tests were conducted to evaluate the accuracy of the proposed prediction model. Furthermore, a plastic fretting fatigue life prediction model was established in [17] based on standard structural contact theory. This model was evaluated by comparing cyclic load maximum stress values obtained through experimental studies and FEM simulation.
Lingfeng Wang et al. [18] explored the application of additive manufacturing (AM) in the production and repair of aero-engine titanium alloy blades. Additionally, the study summarized key factors influencing the fatigue performance of AM titanium alloys and discussed the fatigue mechanism, research methods, and process optimizations of AM manufactured components. In [19], the fatigue life of two-layered Ti-6Al-4V alloys, composed of an additively manufactured layer and a conventional wrought layer, was investigated under constant amplitude loading to evaluate the effect of post-heat treatment on fatigue life. Grzegorz Glodek et al. [20] performed a tribo-mechanical fretting fatigue analysis of additively manufactured Ti-6Al-4V under cyclic loading to model the dovetail joint connection between a turbine blade and disk. A dedicated test apparatus was used to assess the performance of the 3D-printed material in comparison to its wrought counterpart. In addition, a finite element model was employed to analyze stress distribution at the contact surfaces.
The aim of the present study is to investigate the fretting fatigue behavior of Ti-6Al-4V alloy fabricated by selective laser melting (SLM), with a particular focus on the influence of axial stress and contact load on fatigue life and damage mechanisms. Standard axial fatigue tests, aligned with ASTM E466, were conducted under varying loading conditions, followed by post mortem damage analysis using scanning electron microscopy (SEM) to identify dominant damage modes. The novelty of this work lies in its integration of experimental findings and damage characterization into a design-supportive framework. Unlike previous studies that primarily emphasized material-level responses, the current research develops a fretting damage map that classifies safe and critical operational zones based on observed transitions in damage morphology. This map serves as a practical tool to guide design constraints, component qualification, and material selection for AM-based components exposed to fretting-induced fatigue, particularly in safety-critical applications such as aerospace turbine interfaces.

3. Experimental Method Characteristics

To conduct the fretting fatigue tests, four different types of standard specimens (A, B, C, and D) are specified by the ASTM E466 standard committee [21]. In addition, this standard defines specific limits on the dimensions and configurations of the test specimens. In this study, the recognized specimen type A was used for the tests based on this standard, as illustrated in Figure 1. Table 1 presents dimensional specifications for specimen type A based on the ASTM E466 standard. According to the ASTM E466 standard, the geometrical dimensional values of the specimens and fretting pads used in this study are shown in Figure 2.

3.1. Manufacturing of Test Components with Metal 3D Printing Technology

The test components, including fretting pads, were specifically designed for the experiments in this study. To fabricate the components, selective laser melting (SLM) technology was employed, and its manufacturing process specifications are presented in Table 2. The specimens were produced on a powder bed fusion system (Model: M100P; Manufacturer: Noura; City: Isfehan; Country: Iran), with the following process parameters: laser power, scanning speed, layer thickness, and hatch spacing, as listed in Table 2. The fretting pads and fatigue test specimens are shown on a manufacturing stand in Figure 3.
Figure 4 depicts the 3D model of the deposition technique along the Z direction (component height) used in the metal additive manufacturing process for producing the fatigue specimens and fretting pads.

3.2. Preparation of Test Specimens for Fretting Fatigue Experiment and Microscopic Examination

To improve surface quality, the test specimens were mirror-polished, as shown in Figure 5.
According to the ASTM E466 standard, the fretting fatigue tests were conducted using a bridge-type configuration (Figure 6). In this method, a vertical force is applied to the test specimen via the fretting pads in the gauge section, eliminating the need for external frames connected to the testing machine. In this setup, the frame used to apply the axial oscillating (dynamic) force was directly connected to the standard test specimen.
The proving ring used in this study was equipped with a strain gauge attached to its outer surface, facilitating the measurement of the force exerted on the screws of the ring (see Figure 7).
The strain gauge was initially calibrated to establish the correlation between strain values measured by the data acquisition (DAQ) system connected to a computer and the values of axial force exerted on the screws. Figure 8 presents the calibration results of this calibration to adjust the normal force of fretting pads versus the measured strain by the strain gauge attached to the proving ring. The relationship between the measured strain and the compressive force exerted by the fretting pads is given by F = 2 × ϵ , where F represents the contact load in N and ϵ denotes the strain in μm.
The normal force was measured precisely by first calibrating the proving ring using a DAQ card connected to a computer. Before applying any force to the screws, the strain reading was set to zero (Figure 9). Following calibration, the fretting pads were attached to the specimen by tightening the screws, and the normal force was adjusted to the desired level.

3.3. Test Setup and Design Rationale

The fatigue testing machine used to conduct the experiments is shown in Figure 10. The test setup was developed in accordance with ASTM E466 recommendations, utilizing a bridge-type abrasive configuration to apply controlled fretting contact forces. The selected specimen geometry (type A) and loading configuration were chosen to replicate loading conditions typical of high-performance components, such as dovetail joints in turbine engines, where fretting fatigue is a critical concern. This configuration allows the test results to be extrapolated more reliably to real-world applications and provides a design-oriented framework for understanding fatigue behavior in metal additive-manufactured parts. By capturing the combined influence of axial stress and contact load in a controlled environment, the test setup contributes not only to accurate material characterization but also to the validation of design assumptions in AM-based engineering systems.

4. Experimental Results and Discussions

The test specifications and results are shown in Table 3. Based on the obtained results, Figure 11 graphically illustrates the relationship between the maximum axial stress and fretting fatigue life ( N ) of the test specimens under different applied contact loads P_contact. As expected, at an axial stress of 300 MPa and a frequency of 30 Hz, increasing the contact load on the fretting pads leads to a reduction in fatigue life ( N ) . Furthermore, a comparison of experimental results for test cases 1, 3, 4, 6, and 7 shows that increasing the maximum oscillating axial stress significantly reduces fretting fatigue life. Interrupted tests were conducted on specimen # 2 and specimen # 5 to study the fretting damage and obtain a fretting map for the additive-manufactured Ti-6Al-4V alloy. The following section elaborates on the microscopic examination of test cases 1_7.

4.1. Microscopic Examination of the Fretted and Fracture Surfaces

After each fretting fatigue test, a microscopic examination was conducted on the fretted and fractured surfaces using a scanning electron microscope (SEM). The SEM images and corresponding analyses below provide insights into the characterization of fretting fatigue damage in metal additive-manufactured Ti-6Al-4V alloy specimens, contributing to the development of a fretting map. Figure 12 shows a low-magnification SEM image of the fretted surface of specimen # 2 , where the test was interrupted to characterize fretting damage.
As observed in Figure 12, the fretting damage characteristics near the contacting edges differ significantly from those observed closer to the center of the contact surfaces. At the contacting edges, the dominant damage modes are slip, stick, or a combination of both. In contrast, delamination-type damage is primarily observed near the central contact zone. Figure 13 shows a higher magnification of the fretting damage on the contact surfaces of tested specimen # 5 , which was taken from a specimen subjected to interrupted fretting fatigue. Closer observation of the fretted region revealed various types of fretting wear, including stick, slip, and delamination, but no cracks were observed in this area.
Further SEM images of the surfaces exhibiting signs of fretting damage for test case # 1 are presented in Figure 14. Figure 14a shows the presence of secondary cracks in the fretted zone of the specimen. Figure 14b–d illustrate spalling and delamination damage, which are characteristic features of fretting fatigue. The SEM image in Figure 14e presents potential pitting or cavity formation caused by fretting between two surfaces, which is a particularly intriguing observation. Conspicuously, this SEM image reveals distinct damage characteristics compared to those typically observed in titanium-based alloys subjected to fretting. The SEM images of the fracture surface of specimen # 3 are presented in Figure 15. Figure 15a,b illustrate fretting damage, specifically pits, on the fracture surface at different magnifications. Figure 15c,d illustrate the fracture surface characteristics of specimen # 3 .
Figure 16 shows images at higher magnifications of the damage on the fretted region of specimens # 2 and # 5 . Figure 16a exhibits stick–slip-like damage resulting from the fretting fatigue test on specimen # 2 . Figure 16b presents a rare view of three types of damage, stick, slip, and delamination, on the fretted surface of specimen # 5 .
From a design engineering perspective, the coexistence of stick, slip, and delamination modes on the same contact surface highlights the complexity of fretting-induced damage in AM components. The observed damage diversity underscores the need for tailored design strategies, such as surface treatments, localized geometry modifications, or stress-relief heat treatments to mitigate damage progression. These insights provide crucial input for developing more resilient interface designs in turbine blades, orthopedic implants, and similar fretting-sensitive structures fabricated by metal additive manufacturing.

4.2. Fretting Map Extraction Using SEM Examination

Based on SEM observations, a fretting map was developed for the additively manufactured Ti-6Al-4V alloy. In Figure 17, the transition between fretting and fretting fatigue zones is shown using a linear fit, providing a preliminary boundary representation. The displacement amplitude on the x-axis refers to the measured relative slip amplitude between contact surfaces using SEM observations, which represents the cyclic relative motion during fretting. Figure 17 clearly illustrates that below the linear curve-fitted line connecting the points, fretting damage has no significant effect on the fatigue life of metal additive-manufactured Ti-6Al-4V alloy specimens fabricated using the SLM method under a specific oscillating axial fatigue loading condition and frequency.
Regarding the design applicability, while the current map is based on a simplified specimen geometry, it provides a design aid that can inform safe operating zones and guide preliminary design screening for AM titanium components under fretting conditions. This fretting map offers a visual design aid by delineating safe operational regimes where fretting-induced fatigue cracking is minimized. It serves as a basis for determining allowable combinations of displacement amplitude and contact load in component design and may be incorporated into future computational design optimization workflows.

5. Conclusions

This study experimentally investigated the fretting fatigue behavior of additively manufactured Ti-6Al-4V alloy specimens, fabricated using the selective laser melting (SLM) method, in accordance with ASTM E466 specifications. Through systematic and standardized testing procedures combined with detailed microscopic examinations, key insights were obtained into the damage mechanisms and failure characteristics of AM Ti-6Al-4V under fretting fatigue conditions.
Scanning electron microscopy (SEM) analyses revealed secondary cracks within the fretting damage zone, along with characteristic spalling, delamination, and slip-and-stick damage patterns. Based on these observations, a fretting map was developed, providing valuable insights into the damage characteristics and crack initiation conditions under fretting and fretting fatigue situations. Importantly, the findings were translated into a design-relevant framework, where the extracted fretting damage map can serve as a tool for informing design verification and optimization processes. By identifying critical fretting damage modes that influence the fatigue performance of AM components, this work contributes to the development of fretting fatigue-aware design strategies for high-performance applications. Furthermore, this integration of experimental insights into a visual and data-driven fretting map offers a practical design-oriented tool that can support early-stage crack nucleation, material selection, and lifecycle reliability assessment of AM components subjected to fretting fatigue.
Future work should focus on expanding the number of test specimens and broadening the range of experimental conditions to develop a more comprehensive and robust fretting map. This will enable the integration of such data into computational design environments, ultimately supporting early-stage design evaluation, digital twin development, and lifecycle-based design decisions for metal additive-manufactured components.

Author Contributions

Conceptualization, A.S. and S.A.; methodology, A.S. and S.A.; software, A.S. and S.A.; validation, A.S. and S.A.; formal analysis, A.S. and S.A.; investigation, A.S. and S.A.; resources, A.S. and S.A.; data curation, A.S. and S.A.; writing—original draft preparation, A.S. and S.A.; writing—review and editing, A.S. and S.A.; visualization, A.S. and S.A.; supervision, A.S. and S.A.; project administration, A.S. and S.A.; funding acquisition, A.S. and S.A. Both authors contributed equally to all parts of the work. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The results of the experiments conducted in this study are presented within the article.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Vanaei, S.; Zirak, N. Diverse application of 3D printing process. In Industrial Strategies and Solutions for 3D Printing: Applications and Optimization; Wiley: Hoboken, NJ, USA, 2024; pp. 59–80. [Google Scholar]
  2. Ibhadode, O.; Zhang, Z.; Sixt, J.; Nsiempba, K.M.; Orakwe, J.; Martinez-Marchese, A.; Ero, O.; Imani Shahabad, S.; Bonakdar, A.; Toyserkani, E. Topology optimization for metal additive manufacturing: Current trends, challenges, and future outlook. Virtual Phys. Prototyp. 2023, 18, 181–192. [Google Scholar] [CrossRef]
  3. Abbasi, F.; Majzoobi, G.H.; Mendiguren, J. A review of the effects of cyclic contact loading on fretting fatigue behavior. Adv. Mech. Eng. 2020, 12, 1–17. [Google Scholar] [CrossRef]
  4. Iyer, M. Effects of cyclic frequency and contact pressure on fretting fatigue under two-level block loading. Fatigue Fract. Eng. Mater. Struct. 2000, 23, 335–346. [Google Scholar] [CrossRef]
  5. Lykins, C.D.; Mall, S.; Jain, V.K. A shear stress-based parameter for fretting fatigue crack initiation. Fatigue Fract. Eng. Mater. Struct. 2001, 24, 461–473. [Google Scholar] [CrossRef]
  6. Attia, M.H. Prediction of fretting fatigue behavior of metals using a fracture mechanics approach with special consideration to the contact problem. J. Tribol. 2005, 127, 685–693. [Google Scholar] [CrossRef]
  7. Wackers, P.; Arrieta, V.; Alquezar-Getan, M.; Constantinescu, A.; Maitournam, H. A Modeling approach to predict fretting fatigue on highly loaded blade roots. J. Eng. Gas Turbines Power 2010, 132, 082101. [Google Scholar] [CrossRef]
  8. Chan, K.S.; Koike, M.; Mason, R.L.; Okabe, T. Fatigue life of titanium alloys fabricated by additive layer manufacturing techniques for dental implants. Metall. Mater. Trans. A 2013, 44, 1010–1022. [Google Scholar] [CrossRef]
  9. Mace, A.O.; Kurtz, M.A.; Gilbert, J.L. Fretting and Fretting Corrosion Behavior of Additively Manufactured Ti-6Al-4V and Ti-Nb-Zr Alloys in Air and Physiological Solutions. J. Funct. Biomater. 2024, 15, 38. [Google Scholar] [CrossRef] [PubMed]
  10. Glodek, G.; Gothivarekar, S.; Van Hooreweder, B.; Talemi, R. Investigating fretting fatigue response of additively manufactured Ti-6Al-4V in dovetail joint connections. Int. J. Fatigue 2025, 199, 109024. [Google Scholar] [CrossRef]
  11. Zhang, H.; Liu, J.; Zuo, Z. Investigation into the effects of tangential force on fretting fatigue based on XFEM. Tribol. Int. 2016, 99, 23–28. [Google Scholar] [CrossRef]
  12. Lavella, M.; Botto, D. Fretting fatigue analysis of additively manufactured blade root made of intermetallic Ti-48Al-2Cr-2Nb alloy at high temperature. Materials 2018, 11, 1052. [Google Scholar] [CrossRef] [PubMed]
  13. Basseville, S.; Missoum-Benziane, D.; Cailletaud, G. 3D finite element study of the fatigue damage of Ti-6Al-4V in presence of fretting wear. Comput. Mech. 2019, 64, 663–683. [Google Scholar] [CrossRef]
  14. Pereira, K.; Vanegas-Useche, L.V.; Abdel Wahab, M. Aspects of Fretting Fatigue Finite Element Modelling. Comput. Mater. Contin. 2020, 64, 97–144. [Google Scholar] [CrossRef]
  15. Egan, P.F. Design for Additive Manufacturing: Recent Innovations and Future Directions. Designs 2023, 7, 83. [Google Scholar] [CrossRef]
  16. Badrikouhi, E.; Adibnazari, S. A new model for predicting fretting fatigue crack initiation life based on effective slip amplitude. Sci. Iran. 2023, 30, 1255–1264. [Google Scholar] [CrossRef]
  17. Zhou, J.; Yang, B.; Li, S.; Huo, J. Fretting fatigue life prediction of dovetail structure based on plastic effect and sensitivity analysis of influencing factors. Materials 2023, 16, 3521. [Google Scholar] [CrossRef] [PubMed]
  18. Wang, L.; Li, Y.; Zhou, L.; Lou, Y.; Liu, S.; Zheng, D.; Yi, M. Progress in additive manufacturing, additive repair and fatigue evaluation of aviation titanium alloy blades. Mater. Res. Lett. 2023, 11, 973–1012. [Google Scholar] [CrossRef]
  19. Nagalingam, A.P.; Gopasett, S.K.; Wang, J.; Yuvaraj, H.K.; Gopinath, A.; Yeo, S.H. Comparative fatigue analysis of wrought and laser powder bed fused Ti-6Al-4V for aerospace repairs: Academic and industrial insights. Int. J. Fatigue 2023, 176, 107879. [Google Scholar] [CrossRef]
  20. Glodek, G.; Gothivarekar, S.; Van Hooreweder, B.; Talemia, R. Tribo-mechanical fracture analysis of additively manufactured Ti-6Al-4V under cyclic loading. Procedia Struct. Integr. 2024, 66, 331–336. [Google Scholar] [CrossRef]
  21. ASTM E466; Standard Practice for Conducting Force Controlled Constant Amplitude Axial Fatigue Tests of Metallic Materials. ASTM: West Conshohocken, PA, USA, 2015.
Figure 1. Typical sketch of standard specimen type A designated by the ASTM E466 standard committee utilized in this study.
Figure 1. Typical sketch of standard specimen type A designated by the ASTM E466 standard committee utilized in this study.
Designs 09 00100 g001
Figure 2. Geometrical dimensions of the components utilized in the fretting fatigue tests.
Figure 2. Geometrical dimensions of the components utilized in the fretting fatigue tests.
Designs 09 00100 g002
Figure 3. Fretting pads and fatigue test specimen on a manufacturing stand.
Figure 3. Fretting pads and fatigue test specimen on a manufacturing stand.
Designs 09 00100 g003
Figure 4. Three-dimensional modeling of deposition technique in Z direction through additive manufacturing process. (a) Fatigue test specimen. (b) Fretting pad.
Figure 4. Three-dimensional modeling of deposition technique in Z direction through additive manufacturing process. (a) Fatigue test specimen. (b) Fretting pad.
Designs 09 00100 g004
Figure 5. Test specimens before and after polishing.
Figure 5. Test specimens before and after polishing.
Designs 09 00100 g005
Figure 6. Schematic view of bridge-type abrasive fatigue test recognized by the ASTM E466 standard [21].
Figure 6. Schematic view of bridge-type abrasive fatigue test recognized by the ASTM E466 standard [21].
Designs 09 00100 g006
Figure 7. Installation of strain gauge on proving ring.
Figure 7. Installation of strain gauge on proving ring.
Designs 09 00100 g007
Figure 8. Variation in the normal force exerted by the fretting pads versus measured strain by the strain gauge attached to the proving ring.
Figure 8. Variation in the normal force exerted by the fretting pads versus measured strain by the strain gauge attached to the proving ring.
Designs 09 00100 g008
Figure 9. Calibration of the strain gauge on a standard specimen connected to a DAQ system to regulate the normal force exerted on the fretting pads.
Figure 9. Calibration of the strain gauge on a standard specimen connected to a DAQ system to regulate the normal force exerted on the fretting pads.
Designs 09 00100 g009
Figure 10. Fatigue testing machine used in this study.
Figure 10. Fatigue testing machine used in this study.
Designs 09 00100 g010
Figure 11. Maximum axial stress Vs. fretting fatigue life ( N ) for different applied contact loads P_contact on the fretting pads, R = 0.1.
Figure 11. Maximum axial stress Vs. fretting fatigue life ( N ) for different applied contact loads P_contact on the fretting pads, R = 0.1.
Designs 09 00100 g011
Figure 12. Contact surface damages induced by fretting fatigue in specimen # 2 , 50×.
Figure 12. Contact surface damages induced by fretting fatigue in specimen # 2 , 50×.
Designs 09 00100 g012
Figure 13. Contact surface damages induced by fretting fatigue in specimen # 5 , 500×.
Figure 13. Contact surface damages induced by fretting fatigue in specimen # 5 , 500×.
Designs 09 00100 g013
Figure 14. (a) Observation of a crack on the surface of the specimen within the fretting damage area, (bd) evidence of fretting damage, including spalling and delamination, (e) pitting observed on the fretted surface of the specimen, (f) potential presence of third-body particles generated as a result of the fretting between two contact surfaces.
Figure 14. (a) Observation of a crack on the surface of the specimen within the fretting damage area, (bd) evidence of fretting damage, including spalling and delamination, (e) pitting observed on the fretted surface of the specimen, (f) potential presence of third-body particles generated as a result of the fretting between two contact surfaces.
Designs 09 00100 g014
Figure 15. (a) Observation of fretting damage on the fracture surface, (b) fretting pit observed on the fracture surface, (c) fracture surface characteristics a distance away from the fretting area.
Figure 15. (a) Observation of fretting damage on the fracture surface, (b) fretting pit observed on the fracture surface, (c) fracture surface characteristics a distance away from the fretting area.
Designs 09 00100 g015
Figure 16. (a) Fretting damage induced by interrupted fretting fatigue in test specimen # 2 , 500× and (b) fretting damage induced by interrupted fretting fatigue test in specimen # 5 , 3000×.
Figure 16. (a) Fretting damage induced by interrupted fretting fatigue in test specimen # 2 , 500× and (b) fretting damage induced by interrupted fretting fatigue test in specimen # 5 , 3000×.
Designs 09 00100 g016
Figure 17. Relationship between displacement (μm) and normal force ( N ) .
Figure 17. Relationship between displacement (μm) and normal force ( N ) .
Designs 09 00100 g017
Table 1. ASTM E466 standard dimensional specifications suggested for fretting fatigue test specimens utilized in this study.
Table 1. ASTM E466 standard dimensional specifications suggested for fretting fatigue test specimens utilized in this study.
RelationDescriptionApplied (×)/Not Applied (−)
W / W = 1.5 The ratio of the claimed region width to test zone width (suggested value; other values are allowed)×
R 8 W To minimize the stress concentration factor×
2 W / T 6 The specimen width-to-thickness ratio must be in the range of 2–6×
19.4 W T 645 Cross-sectional area of reduction area (mm2)×
2 W L 3 W Test zone length must be 2 to 3 times the specimen width (W)×
Table 2. Metal additive manufacturing (AM) specifications for standard fatigue specimens and fretting pads.
Table 2. Metal additive manufacturing (AM) specifications for standard fatigue specimens and fretting pads.
Process CharacteristicsStandard SpecimenPad
Mass of powder consumption285 g52 g
Method of manufacturingSLM
Powder materialTi6Al4V
Layer thickness30 μm
Energy density70 j/mm3
Maximum laser power of machine300 W
Powder characteristicsAtomized gas less than 65 μm
Build plate dimensionsD (diameter) = 124 mm, h (height) = 150 mm
Table 3. Specifications of conducted experiments and obtained results.
Table 3. Specifications of conducted experiments and obtained results.
Test Case No.Maximum Axial Stress (MPa)Stress Ratio, RVertical Force Applied on Fretting Pads (N)Loading Frequency (Hz)No. of Cycles (×1000)Description/Comments
13000.175030139Fretting Fatigue
23000.17503035 (interrupted test)Interrupted test
35000.17503036Fretting Fatigue
45000.17503017Fretting Fatigue
53000.15003050 (interrupted test)Interrupted test
63000.130030176Fretting Fatigue
73000.1125030109Fretting Fatigue
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Sadeghian, A.; Adibnazari, S. Design-Informed Evaluation and Fretting Damage Mapping of Additive-Manufactured Ti-6Al-4V Components. Designs 2025, 9, 100. https://doi.org/10.3390/designs9050100

AMA Style

Sadeghian A, Adibnazari S. Design-Informed Evaluation and Fretting Damage Mapping of Additive-Manufactured Ti-6Al-4V Components. Designs. 2025; 9(5):100. https://doi.org/10.3390/designs9050100

Chicago/Turabian Style

Sadeghian, Ahmad, and Saeed Adibnazari. 2025. "Design-Informed Evaluation and Fretting Damage Mapping of Additive-Manufactured Ti-6Al-4V Components" Designs 9, no. 5: 100. https://doi.org/10.3390/designs9050100

APA Style

Sadeghian, A., & Adibnazari, S. (2025). Design-Informed Evaluation and Fretting Damage Mapping of Additive-Manufactured Ti-6Al-4V Components. Designs, 9(5), 100. https://doi.org/10.3390/designs9050100