Next Article in Journal
Growth and Characterization of Organic 2-Chloro 5-Nitroaniline Crystal Using the Vertical Bridgman Technique
Previous Article in Journal
Analysis of the Effect of Simultaneous Melt Shearing and Cooling on Grain Formation and Rheology of A356 Aluminum Alloy
Previous Article in Special Issue
Towards Closed-Loop Recycling of Ceramic Particle-Reinforced Aluminium Alloys: Comparative Study of Resistance-Heating Sintered Primary and Solid-State Recycled Secondary SiCp/AlSi7Mg Composites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Investigation of Hardness and Microanalysis of Sintered Aluminum-Based Supplemented Metal Matrix Machined Composites

1
Department of Electrical and Computer Engineering, University of UTAH Asia Campus, Incheon 21985, Republic of Korea
2
Department of Mechanical Engineering & Technology, Government College University, Faisalabad 37000, Pakistan
3
NUST Business School, National University of Sciences and Technology (NUST), Islamabad 44000, Pakistan
4
Department of Materials Science and Engineering, Pak-Austria Fachhochschule Institute of Applied Sciences and Technology, Haripur 22620, Pakistan
5
School of Mechanical Engineering, Pusan National University, Busan 46241, Republic of Korea
6
Department of Mechanical Engineering, Institute of Space Technology, Islamabad 44000, Pakistan
*
Authors to whom correspondence should be addressed.
These authors contributed equally to this work.
Crystals 2023, 13(9), 1347; https://doi.org/10.3390/cryst13091347
Submission received: 28 July 2023 / Revised: 21 August 2023 / Accepted: 22 August 2023 / Published: 4 September 2023
(This article belongs to the Special Issue Current Status and Recent Progress on Advanced Aluminum Alloys)

Abstract

:
Aluminum metal matrix composites (AMMCs) have become increasingly ubiquitous in the fields of aerospace and automobile businesses due to their lightweight properties. Their machining is a challenging task because of the presence of supplemented particles, also called reinforcements. As the wt% of the supplemented particles changes, the morphological and machining behaviors of the AMMCs change. The present work is focused on exploring the thermo-mechanical properties of AMMCs which would help in AMMC applications in the aerospace industry with a new collection of composites containing silicon carbide (SiC) and zircon/zirconium silicate (ZrSiO4) as supplements in wt% of 5%, 20%, 30%, and 40%. Uniform binary and hybrid sample pallets are prepared by powder metallurgy (PM). The said samples are sintered and then machined using wire electric discharge machining (WEDM) employing brass wire with a feed rate of 2 to 3 mm/min. Also, analysis of porosity and recast layer formation is performed via the microstructure, scanning electron microscopy (SEM), and energy dispersive spectroscopy (EDS). Some interesting and useful findings are obtained which can extend the applications of AMMCs in automobiles and the aerospace industry. The results reveal that temperature and wt% are playing their significant roles in the changes in the thermo-mechanical properties of AMMCs. Mathematical equations via regression analysis using Minitab 17 and Excel are developed for the congruence of experimental data. Analysis of Variance (ANOVA) is also performed. Hence, the most optimized relationships for the best machining output are established and presented in this proposed study.

1. Introduction

Aluminum has a significant and pervasive use in both industrial and consumer applications due to its advantageous properties as a lightweight, nonmagnetic, malleable, and ductile element [1]. In recent applications, aluminum is used in combination metals, ceramics, or organic components by making them as aluminum metal matrix composites (AMMCs) to improve the physical and mechanical properties of the base metal, like hardness, quality, resistance to wear, conductivity, stiffness, etc., in order to trigger attention towards their most advanced applications in the aerospace and automobile industries [2].
Composite materials reinforced with materials imparting good mechanical properties have taken a wider place in industry for their high material efficiencies. The methods of preparation for such composites are also very important, as they contribute towards the thermo-mechanical properties of the composites [3,4]. The reinforcements must be non-reactive and stable enough at working temperatures and also possess superior mechanical properties [5]. Among many supplemented materials like carbides and nitrides, silicon carbide (SiC) has an added advantage over others due to its low density, better heat conductivity, and high elastic modulus, along with its easy availability. It is also inexpensive when compared to the others [6]. AMMCs with varying wt% of SiC also revealed that hardness and tensile strength increases, along with the reduction in percentage elongation, when increasing the wt% of SiC up to 25% [7]. It was also observed that AMMCs with 10% SiC were more favorable for applications in industries like aerospace, automobile, and military parts due to their supercilious mechanical properties. Few properties are directly affected by the addition of supplementary materials, like hardness, roughness, and wear, especially [4,5].
Hardness, tensile strengths, and impact strengths of AMMCs supplemented with SiC increase when increasing the wt% of reinforcement [8,9,10]. In the preparations of AMMCs with SiC as supplements, micro hardness, clustered regions, and porosities increase as the wt% of supplements increase along with the reduction in the particle size of the reinforcement [11]. As far as their machining is concerned, non-traditional or advanced mechanisms are required for the accurate machining of AMMCs, e.g., laser beam machining (LBM) and water jet machining (WJM). But these machining methods are limited to linear machining only [3].
Despite other non-traditional machining methods, the electrical discharge machining (EDM) process was found to be the most promising one for the removal of material from AMMCs. EDM removes the material by erosion through melting and vaporizing in the presence of dielectric fluid [12,13,14]. Spark erosion occurs between the tool and the workpiece gap [15]. The machinability of MMCs is dependent upon the processes of machining being adopted, along with the proper selection of the process material and operating parameters, irrespective of the natures of the AMMCs [16]. Furthermore, formation of a recast layer during machining must be removed without distorting the surface integrity, as it imparts tensile residual stresses, resulting in cracking and low fatigue strength in the material being machined [17].
Machining explorations of properties, such as elemental analysis, micro hardness, porosity, surface roughness, etc., can be performed by using X-Ray diffraction (XRD), scanning electron microscopy (SEM), electron probe microscopic analysis (EPMA), and differential thermal analysis (DTA). The characterization results offer important, new information about the composite powder’s microstructure and phase distribution [18]. The uniform distribution of supplemented particles results in greater strength and imparts high hardness, which eventually leads to high resistance to wear [19,20]. Moreover, in EDM, brass electrode wire is found to be more reliable when compared to others because of its higher material removal rate (MRR); non-electric parameters of EDM, like flushing pressure, also contribute towards MRR.
Therefore, it is concluded that the machining and modeling of machined profiles of AMMCs are yet to be explored in many aspects [21]. Hybrid aluminum metal matrix composites (HAMMCs) are the foremost engineering materials due to their outstanding characteristics and applications. The machining of HAMMCs paved a new path to explore machining behaviors and their effects on the applications of these modern materials in the industry [22,23]. It was also found that the cutting processes of AMMCs are not completely explored [24]. The machining of AMMCs is quite difficult due to the presence of hard supplementary particles. They have higher levels of hardness compared to tools made up of carbide and high-speed steel (HSS) [25]. Out of advanced non-conventional machining processes, EDM is found to be the more reliable thermal process, in which the material is removed precisely by small spark erosion [26]. However, the EDM is established enough in many sophisticated industries like aerospace, automotive, and surgical instruments [27]. The machining behaviors of SiC-supplemented AMMCs have not been completely explored until now in the literature. Therefore, in the current study, aluminum is selected as a matrix material supplemented by SiC and ZrSiO4 particles to produce composites by the PM route. Varying wt% of SiC and ZrSiO4 are added and then machined. The machine profile is investigated for microstructure investigation along with hardness of the machined surface.

2. Methodology

2.1. Sample Preparation

The pure aluminum powder is used for the preparation of MMCs. The average particle size (APS) range was 43–45 μm. Silicon carbide micro particles (SiC) with APS were 37–45 μm. The APS of zircon was <50 nm. Particle type and discontinuous reinforcements were used. All powders were 99% pure. The hardness of AMMCs was be increased with the increase in wt% of ZrSiO4 and SiC-reinforced MMCs [28]. The challenging task lay in the preparation of the samples due to low wettability of the supplementary material phase. Therefore, the preparation of AMMCs could not be possible by traditional casting methods [29]. A few properties of SiC powder and ZrSiO4 are mentioned in Table 1.
The first step of preparation of samples was to weigh the powder as required. For this purpose, powders were weighted using a digital weight balance of least 0.1 mg. The measured weights of powders were ball-milled for one hour with the help of 35 balls of steel (molybdenum each of size 5 mm) to further grind the mixture. A 10:1 ball-to-powder ratio (BPR) was used during the mixing of powders in order to achieve homogeneous mixing. Powders were mixed at 150 rpm for 60 min, respectively. After mixing, powders were fed into the uniaxial hydraulic press with the help of a die as shown in Figure 1 with a diameter of 20 mm, generating a pallet of the sample as shown on the left side of Figure 2.
The mixture was compacted with the help of a hydraulic press for 2 min under a pressure of 196 Mpa. After 2 min, the press was released and the sample was removed from the circular die.
After compaction of binary and hybrid AMMCs, the samples were fed to sintering furnace to heat them at different temperatures ranging from 500 °C to 1100 °C. Sintered samples, as shown on the left side of Figure 1, were subjected to machining, and then the porosity, chemical composition, and mechanical properties were examined, as well as the hardness of the machined surface. The hardness of the machined samples was measured with the Vickers hardness tester. The hardness was measured from the size of an impression generated under load by a pyramid-shaped diamond indenter. Here, the load of 980.7 mN was taken for 10 s. Furthermore, the SEM analysis was conducted to study the microstructure examination using FESEM [30] as shown in Figure 3.
For the validation of experimental results, mathematical equations were estimated for each input parameter using regression analysis. Fabricated sample (20 mm diameter and 4 mm thickness) compositions and sintering conditions are mentioned in the published work of part of this research before machining [9]. The plan of the experiment mentioning the designed ratio of reinforcements along with the selected sintering temperature and sintering time in sintering furnace is shown in Table S1 of the attached Supplementary File.

2.2. Machining of Samples

Machining of AMMCs is a challenging task because of the abrasive nature of supplemented particles. Traditional machining processes such as turning, milling, or drilling are adopted for machining MMCs. But low surface integrity and accuracy of the machined samples hindered the adoption of conventional machining for MMCs [31].
In the current study, the WEDM with a brass wire 0.25 mm in diameter was used, keeping the pulse on/off time at constant values during the operation. The wire feed rate was 2 to 3 mm/min. WEDM is a non-conventional thermal machining process in which a wire made up of copper, brass or molybdenum can be used as an electrode [32]. It is pertinent to know that the conductivity of the electrode and work-piece is mandatory for the material removal as series of successive sparks are the source for cutting [33,34,35]. Electric sparks produce heat at a temperature of 8000–12,000 °C, causing melting and vaporization of the work-piece in the local surface layers. During the WEDM process, dielectric fluid is consistently flushed in and out to carry the eroded material away [36]. The surface of the work-piece is cooled side by side and solidified at a very high rate due to the high thermal conductivity of water. This solidification of the top surface of the work-piece results in the formation of a recast layer [37]. There are certain electrical and nonelectrical parameters of WEDM which are needed to be selected at appropriate levels before the start of machining [38]. Table 2 shows the machining conditions of WEDM. The samples are cut in a transverse direction across the diameter.

3. Results and Discussions

Estimation of elements in AMMC reinforced with SiC and ZrSiO4 with varying wt% was performed by EDS analysis using SEM. The images obtained showed that porosity, high pressure and close compaction of powder generates dense microstructure which improves the heat conduction capacity and strength of AMMCs. The irregular and random shapes of particles in the composite were observed. It was also observed that as the wt% of the supplements increases, consolidation of samples from solid state to liquid state occurs in the case of all twelve samples. Moreover, the recast layer was assumed to increase the surface hardness of machined samples.

3.1. EDS Analysis of Samples

Optical microscopic examination of the composite reveals the presence of reinforcement particles in the form of clusters as shown in Figure 4 of hybrid AMMCs. Machining of such samples is not obvious as well.
EDS analysis of the samples containing 40% by weight of SiC confirms that SiC particles are present in the synthesized composites as shown in Figure 5, whereas Table 3 presents the wt% of each constituent element.
It is important to note that oxides were also formed during the machining of AMMCs. Similarly, the case of hybrid composite with SiC and ZrSiO4 is shown in Figure 6 and wt% is presented in Table 4.

3.2. Porosity

Agglomerations or clustering of the reinforcements of varying size and shape are observed in Figure 7; they result in particulate-rich and particulate-depleted regions.
Porosity and depleted zones were seen in the images obtained via SEM because of the difference between the melting points of base metal and supplementary materials (composition); however, one profound aspect which can be a next-level investigation is the compaction pressure selected in this research since compaction pressure is inversely proportional to porosity. It is also observed in the previous studies that a small increase in wt% of reinforcements causes drastic porosity due to the clustering and agglomeration at high concentrations of supplements [39]. Hence, it can be concluded that supplementary particles act as a barrier between rearrangement and diffusion of reinforcements resulting in higher porosity, irrespective of the sintering temperature.

3.3. Hardness of Machined Samples

The hardness of machined samples may be enormously affected due to the heating and machining of samples. For this reason, investigation of hardness was performed with the Vicker hardness tester. Hardness of the samples was tested by a micro indenter with a diamond probe using a force of 980.7 mN for 10 s with a high-voltage harness tester at room temperature. It was observed that the Al-SiC binary composite matrix contains a wt% of 5 and 20, whereas the hybrid composite of Al-SiC 5%–ZrSiO4 40% has approximately the same hardness. It is important to note that the SiC wt% was at its lowest value in the above cases. As the wt% of SiC increases, the hardness of AMMCs increases. Meanwhile, the smallest value of hardness, i.e., 13.83 HV, was observed for the composite with 40% of ZrSiO4. The observed trend in this study shows that as the wt% of ZrSiO4 increases, the hardness decreases. However, the maximum hardness out of all twelve samples is observed, i.e., 104.06 HV, for AMMC with 20 wt% of ZrSiO4. It is important to note that as the sintering temperature increases, the hardness of the machined samples increases. However, in the case of AMMCs supplemented with ZrSiO4, hardness decreases with the increase in temperature beyond 700 °C. Sintering time does not impart much to the change in hardness of machined samples. Table 5 shows the values measured for hardness along with the standard deviation against each measurement.
The change in composition of AMMCs affects their hardness [40]. In the case of Al-SiC, hardness increases with the increase in wt% of SiC as shown in Figure 8, whereas the reverse was observed in the case of Al-ZrSiO4 (Figure 9). Moreover, for hybrid AMMCs, i.e., Al-SiC-ZrSiO4, wt% of SiC enhanced the hardness, whereas ZrSiO4 tried to pull it down as presented in Figure 10. Therefore, minimum levels of hardness of machined profiles were achieved at 40% of ZrSiO4 in the case of both hybrid and binary AMMCs. All the results above showed that the hardness of machined samples is greatly influenced by the sintering temperature and the concentration of supplements. It is evident from the below plots that predicted and actual hardness correspond to one another in the case of Al-ZrSiO4 binary composites and Al-SiC-ZrSiO4 hybrid composites. In the case of Al-SiC, the trend of actual and predicted results is the same, but the composites did not correspond exactly to one another. ANOVA and regression equations were generated for the compliance of the experimental results. In the case of binary AMMCs of Al-ZrSiO4, ANOVA showed that the sintering temperature and wt% produce significant values.

3.4. Regression Analysis for Hardness of Machined Samples

The experimental values were then validated and tested against the predicted values by using regression analysis and ANOVA. Few observations had a substantial impact on the model prediction according to the study of the main effect plot, with some data having a stronger influence on the anticipated values than other. To pinpoint the reasons of these data, by improving the experimental design, we could increase the precision of the model predictions. In general, the plots are a useful tool for locating significant observations and enhancing the prediction model’s precision [30,41]. Equation (1) shows the relation between the hardness of machined samples of Al-SiC-ZrSiO4 against input parameters, respectively.
Hardness (HV) = 634.92 + 24.835 ZrSiO4 wt% − 1.4673 Sintering T (°C).
The regression equation presented the same behavior as that which the experimental results showed. However, there was no significant factor (p > 0.05) found in the case of the hardness of machined AMMCs supplemented with SiC and the hybrid of SiC and ZrSiO4. In the case of Al- ZrSiO4, Equation (1) completely satisfied the statistical requirements observed in ANOVA, as sintering temperature and composition show significant values (p < 0.05).
However, the comparison graphs of predicted and experimental values for hardness at different levels of temperature and compositions showed a similar trend in the case of Al-SiC AMMCs, and they are exactly lying over one another in the case of Al-ZrSiO4 and hybrid AMMCs as shown in Figure 11.

3.5. Recast Layer

The recast layer is fine-grained, hard, brittle, and different from its parent material structure. The formation of these layers is the result of process parameters of machining and work-piece compositions [42]. The major reason for the presence of a recast layer is the improper flushing of eroded material during pulse-off time and higher current and nature of supplements added into MMCs [43]. In the current study, recast layers were also observed, which increased the hardness of AMMCs. The white layer known as the recast layer appeared on the machined surface with cracks and micro voids, which can be seen via SEM (Figure 12).
Here, it is also important to note that SiC particles are hard in nature, which can distort the recast layer and result in cracks, voids, and phase transformations. This can cause drastic changes in the surface properties of the machined profile. The current study can be extended by investigating the surface properties of these AMMCs. Proper selection of wt% of reinforcements and peak current are the two most significant factors affecting the quality and thickness of the recast layer [44]. In the present study, WEDM parameters were kept constant on specific machining conditions, but by varying the machining conditions, significant results can be found which may contribute a lot to the available research regarding surface studies of AMMCs. In the future, this study can be extended for the optimization of machining parameters for such composites and cover the currently needed area to explore. Parametric analysis for the change in thickness of the recast layer would also contribute to the new findings.

4. Conclusions

The conclusions drawn from the findings and discussions are listed below.
EDS examination confirms the presence of SiC and ZrSiO4 in the aluminum matrix machined samples, where the distribution of reinforcements is inferred from elemental analysis.
The current investigation found that the machinability of each sample varies with wt%, the hardness of machined AMMCs is significantly affected by wt% of supplements, both individually and collectively. Since the strength of AMMCs must be improved [45], the high wt% of brittle SiC and ZrSiO4 was added to the matrix alloy; optimal machining conditions are required. The machined profile becomes harder as the SiC weight percentage rises.
The morphology of the AMMCs changes as a result of the addition of different reinforcements to the metal matrix.
Particulate-rich and particulate-depleted zones are formed by the aggregation or clustering of the supplements of various shapes and sizes. This is a result of liquid phase sintering occurring at higher temperatures, specifically 1100 °C, which causes heterogeneous distribution and, ultimately, agglomeration and segregation [46].
During sintering, supplements mix with molten matrix material at high temperatures in the liquid phase to create detrimental phases. Because SiC (3.21 g/cm3) and ZrSiO4 (4.56 g/cm3) have different densities, aggregation occurs as the reinforcement particles slide on the molten metal. This can be prevented by using a two-stage addition of reinforcement particles [47], as opposed to the single-stage addition used here.
As there is no significant relationship between sintering time and compaction pressure, sintering time for both machined and sintered samples does not significantly affect the hardness of either [48].
The regression equations of HAMMC Al-SiC-ZrSiO4 and machined Al-ZrSiO4 satisfy the statistical criteria for ANOVA tables.
From the microstructure, it can be shown that samples are sintered by liquid-state sintering rather than solid-state sintering as temperature and the proportion of reinforcements increase.
Additionally, when the weight percentage of ZrSiO4 raises, dendritic gaps and porosity are seen in the microstructure, resulting in a brittle structure. This is may be due to slow cooling.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/cryst13091347/s1.

Author Contributions

Conceptualization, M.R.B. and F.G.; methodology, T.Z.; software, U.G.; validation, S.B. and M.R.B.; formal analysis, F.G.; investigation, T.Z.; resources, U.G.; data curation, S.B.; writing—original draft preparation, M.R.B. and F.G.; writing—review and editing, U.G. and S.B; visualization, T.Z.; supervision, S.B.; funding acquisition, U.G. and M.R.B. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the National Research Foundation (NRF) of Korea through the Auspices of the Ministry of Science and ICT, Republic of Korea, under Grant NRF-2020R1G1A1012741.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data used to make the manuscript can be made available from the corresponding author(s) on reasonable request.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Kawahara, M.; Kato-Negishi, M. Link between Aluminum and the Pathogenesis of Alzheimer’s Disease: The Integration of the Aluminum and Amyloid Cascade Hypotheses. Int. J. Alzheimer’s Dis. 2011, 2011, e276393. [Google Scholar] [CrossRef]
  2. Manish, S.; Dhakad, S.K.; Agarwal, P.; Pradhan, M.K. Review on Various Aluminum Based Metal Matrix Composite. Int. J. Eng. Res. 2018, 6, 2. [Google Scholar] [CrossRef]
  3. Rajak, D.K.; Pagar, D.D.; Kumar, R.; Pruncu, C.I. Recent progress of reinforcement materials: A comprehensive overview of composite materials. J. Mater. Res. Technol. 2019, 8, 6354–6374. [Google Scholar] [CrossRef]
  4. Kim, D.-Y.; Choi, H.-J. Recent Developments towards Commercialization of Metal Matrix Composites. Materials 2020, 13, 2828. [Google Scholar] [CrossRef]
  5. Dubey, A.K.; Yadava, V. Laser Beam Machining—A Review. Int. J. Mach. Tools Manuf. 2008, 48, 609–628. [Google Scholar]
  6. Yigezu, B.S.; Jha, P.K.; Mahapatra, M.M. The Key Attributes of Synthesizing Ceramic Particulate Reinforced Al-Based Matrix Composites through Stir Casting Process: A Review. Mater. Manuf. Process. 2013, 28, 969–979. [Google Scholar]
  7. Pal, M.K.; Vikram, A.; Bajaj, V. Enhanced microstructure and mechanical properties of sic particle reinforced Aluminium alloy composite materials. Acta Met. Slovaca 2019, 25, 253–258. [Google Scholar] [CrossRef]
  8. Ashkani, O.; Tavighi, M.R.; Karamimoghadam, M.; Moradi, M.; Bodaghi, M.; Rezayat, M. Influence of Aluminum and Copper on Mechanical Properties of Biocompatible Ti-Mo Alloys: A Simulation-Based Investigation. Micromachines 2023, 14, 1081. [Google Scholar] [CrossRef]
  9. Gillani, F.; Khan, M.Z.; Shah, O.R. Sensitivity Analysis of Reinforced Aluminum Based Metal Matrix Composites. Materials 2022, 15, 4225. [Google Scholar] [CrossRef]
  10. Meena, K.L.; Manna, A.; Banwait, S.S. An Analysis of Mechanical Properties of the Developed Al/SiC-MMC’s. Am. J. Mech. Eng. 2013, 1, 14–19. [Google Scholar]
  11. Das, D.; Mishra, P.C.; Chaubey, A.K.; Samal, C. Characterization of the developed aluminium matrix composites-an experimental analysis. Mater. Today Proc. 2018, 5, 3243–3249. [Google Scholar] [CrossRef]
  12. Rizwee, M.; Minz, S.S.; Orooj, M.; Hassnain, M.Z.; Khan, M.J. Electric Discharge Machining Method for Various Metal Matrix Composite Materials. Int. J. Innov. Technol. Explor. Eng. (IJTEE) 2019, 8, 1796–1807. [Google Scholar] [CrossRef]
  13. Choudhary, S.K.; Jadoun, R.S. Current Advanced Research Development of Electric Discharge Machining (EDM): A Review. Int. J. Res. Advent Technol. 2014, 2, 273–297. [Google Scholar]
  14. Li, J.; Chen, W.; Zhu, Y. Study on Generating Machining Performance of Two-Dimensional Ultrasonic Vibration-Composited Electrolysis/Electro-Discharge Technology for MMCs. Materials 2022, 15, 617. [Google Scholar] [CrossRef]
  15. Gillani, F.; Zahid, T.; Bibi, S.; Khan, R.S.U.; Bhutta, M.R.; Ghafoor, U. Parametric Optimization for Quality of Electric Discharge Machined Profile by Using Multi-Shape Electrode. Materials 2022, 15, 2205. [Google Scholar] [CrossRef] [PubMed]
  16. Abu Qudeiri, J.E.; Saleh, A.; Ziout, A.; Mourad, A.-H.I.; Abidi, M.H.; Elkaseer, A. Advanced Electric Discharge Machining of Stainless Steels: Assessment of the State of the Art, Gaps and Future Prospect. Materials 2019, 12, 907. [Google Scholar] [CrossRef]
  17. Rajkumar, K.; Poovazhagan, L.; Selvakumar, G.; Muthukumar, B. Wire Electrical Discharge Machining Integrity Studies on the Aluminium Nanocomposite. In Advances in Manufacturing Processes; Springer: Berlin/Heidelberg, Germany, 2019; pp. 543–554. [Google Scholar] [CrossRef]
  18. Rezayat, M.; Karamimoghadam, M.; Ashkani, O.; Bodaghi, M. Characterization and Optimization of Cu-Al2O3 Nanocomposites Synthesized via High Energy Planetary Milling: A Morphological and Structural Study. J. Compos. Sci. 2023, 7, 300. [Google Scholar] [CrossRef]
  19. Hashim, J.; Looney, L.; Hashmi, M.S.J. Particle distribution in cast metal matrix composites—Part I. J. Mater. Process. Technol. 2002, 123, 251–257. [Google Scholar] [CrossRef]
  20. Levashov, E.; Kurbatkina, V.; Alexandr, Z. Improved Mechanical and Tribological Properties of Metal-Matrix Composites Dispersion-Strengthened by Nanoparticles. Materials 2010, 3, 97–109. [Google Scholar] [CrossRef]
  21. Dhupal, D.; Naik, S.; Das, S.R. Modelling and Optimization of Al–SiC MMC through EDM Process Using Copper and Brass Electrodes. Mater. Today Proc. 2018, 5, 11295–11303. [Google Scholar] [CrossRef]
  22. Gavisiddesha, P.; Thotappa, C.; Algur, V.; Suresh Reddy, B. Optimization of Wire Cut Electric Discharge Machining Characteristics of Hybrid Aluminium Composites (Al6061/Gr/SiCp) Using Taguchi Method. In Sustainable Machining Strategies for Better Performance; Springer: Berlin/Heidelberg, Germany, 2022; pp. 49–60. [Google Scholar]
  23. Feldshtein, E.E.; Dyachkova, L.N.; Patalas-Maliszewska, J. On Investigating the Microstructural, Mechanical, and Tribological Properties of Hybrid FeGr1/SiC/Gr Metal Matrix Composites. Materials 2021, 14, 174. [Google Scholar] [CrossRef]
  24. Karabulut, Ş.; Karakoç, H.; Çitak, R. Effect of the B4C Reinforcement Ratio on Surface Roughness of A16061 Based Metal Matrix Composite in Wire-EDM Machining. In Proceedings of the 2017 8th International Conference on Mechanical and Aerospace Engineering (ICMAE), Prague, Czech Republic, 22–25 July 2017; IEEE: Piscataway, NJ, USA, 2017; pp. 812–815. [Google Scholar]
  25. Bains, P.S.; Sidhu, S.S.; Payal, H.S. Fabrication and Machining of Metal Matrix Composites: A Review. Mater. Manuf. Process. 2016, 31, 553–573. [Google Scholar] [CrossRef]
  26. Abbas, N.M.; Solomon, D.G.; Bahari, M.F. A review on current research trends in electrical discharge machining (EDM). Int. J. Mach. Tools Manuf. 2007, 47, 1214–1228. [Google Scholar] [CrossRef]
  27. Ramasawmy, H.; Blunt, L. Effect of EDM process parameters on 3D surface topography. J. Mater. Process. Technol. 2004, 148, 155–164. [Google Scholar] [CrossRef]
  28. Kannan, V.S.; Lenin, K.; Srinivasan, D.; Kumar, D.R. Investigation on Laser Square Hole Drilling of AA7475/SiC/ZrSiO4 Composites. Silicon 2022, 14, 4557–4574. [Google Scholar] [CrossRef]
  29. Krishna, S.M.; Shridhar, T.N.; Krishnamurthy, L. Research Significance, Applications and Fabrication of Hybrid Metal Matrix Composites. Int. J. Innov. Sci. Eng. Technol. 2015, 2, 227–237. [Google Scholar]
  30. Rezayat, M.; Karamimoghadam, M.; Yazdi, M.S.; Moradi, M.; Bodaghi, M. Statistical analysis of experimental factors for synthesis of copper oxide and tin oxide for antibacterial applications. Int. J. Adv. Manuf. Technol. 2023, 127, 3017–3030. [Google Scholar] [CrossRef]
  31. Gururaja, S.; Ramulu, M.; Pedersen, W. Machining of MMCS: A Review. Mach. Sci. Technol. 2013, 17, 41–73. [Google Scholar] [CrossRef]
  32. Pramanik, A.; Basak, A.; Prakash, C. Understanding the wire electrical discharge machining of Ti6Al4V alloy. Heliyon 2019, 5, e01473. [Google Scholar] [CrossRef]
  33. Pramanik, A.; Basak, A.K.; Dixit, A.R.; Chattopadhyaya, S. Processing of duplex stainless steel by WEDM. Mater. Manuf. Process. 2018, 33, 1559–1567. [Google Scholar] [CrossRef]
  34. Mussada, E.K.; Hua, C.C.; Rao, A.K.P. Surface hardenability studies of the die steel machined by WEDM. Mater. Manuf. Process. 2018, 33, 1745–1750. [Google Scholar] [CrossRef]
  35. Kar, S.; Patowari, P.K. Electrode wear phenomenon and its compensation in micro electrical discharge milling: A review. Mater. Manuf. Process. 2018, 33, 1491–1517. [Google Scholar] [CrossRef]
  36. Gostimirovic, M.; Kovac, P.; Sekulic, M.; Skoric, B. Influence of discharge energy on machining characteristics in EDM. J. Mech. Sci. Technol. 2012, 26, 173–179. [Google Scholar] [CrossRef]
  37. Arikatla, S.P.; Mannan, K.T.; Krishnaiah, A. Parametric Optimization in Wire Electrical Discharge Machining of Titanium Alloy Using Response Surface Methodology. Mater. Today Proc. 2017, 4, 1434–1441. [Google Scholar] [CrossRef]
  38. Muthuramalingam, T.; Mohan, B. A review on influence of electrical process parameters in EDM process. Arch. Civ. Mech. Eng. 2015, 15, 87–94. [Google Scholar] [CrossRef]
  39. El-Kady, O.; Fathy, A. Effect of SiC particle size on the physical and mechanical properties of extruded Al matrix nanocomposites. Mater. Des. 2014, 54, 348–353. [Google Scholar] [CrossRef]
  40. Srivastava, A.K.; Dixit, A.R.; Tiwari, S. A review on the intensification of metal matrix composites and its nonconventional machining. Sci. Eng. Compos. Mater. 2018, 25, 213–228. [Google Scholar] [CrossRef]
  41. Moradi, M.; Karamimoghadam, M.; Meiabadi, S.; Casalino, G.; Ghaleeh, M.; Baby, B.; Ganapathi, H.; Jose, J.; Abdulla, M.S.; Tallon, P.; et al. Mathematical Modelling of Fused Deposition Modeling (FDM) 3D Printing of Poly Vinyl Alcohol Parts through Statistical Design of Experiments Approach. Mathematics 2023, 11, 3022. [Google Scholar] [CrossRef]
  42. Paswan, K.; Chattopadhyaya, S.; Pramanik, A. A Review Paper on Machining of Metal Matrix Composite and Optimizing Methods used in Electrical Discharge Machining. Mater. Today Proc. 2018, 5, 24428–24438. [Google Scholar] [CrossRef]
  43. Vignesh, S.; Mohan, B.; Muthuramalingam, T.; Karthikeyan, S. Evaluation of Recast Layer Thickness of Electrical Discharge Machined AISI 202 Stainless Steel with Various Pulse Generators. In Proceedings of the Applied Mechanics and Materials; Trans Tech Publications: Bach, Switzerland, 2015; Volume 766, pp. 518–522. [Google Scholar]
  44. Singh Sidhu, S.; Singh Bains, P. Study of the Recast Layer of Particulate Reinforced Metal Matrix Composites machined by EDM. Mater. Today Proc. 2017, 4, 3243–3251. [Google Scholar] [CrossRef]
  45. Kaviyarasan, K.; Kumar, J.P.; Anandh, S.K.; Sivavishnu, M.; Gokul, S. Comparison of mechanical properties of Al6063 alloy with ceramic particles. Mater. Today Proc. 2020, 22, 3067–3074. [Google Scholar] [CrossRef]
  46. Haanappel, S.; Thije, R.T.; Sachs, U.; Rietman, B.; Akkerman, R. Formability analyses of uni-directional and textile reinforced thermoplastics. Compos. Part A: Appl. Sci. Manuf. 2014, 56, 80–92. [Google Scholar] [CrossRef]
  47. Olakanmi, E.O.T.; Cochrane, R.F.; Dalgarno, K.W. A review on selective laser sintering/melting (SLS/SLM) of aluminium alloy powders: Processing, microstructure, and properties. Prog. Mater. Sci. 2015, 74, 401–477. [Google Scholar] [CrossRef]
  48. Kumar, G.V.; Rao, C.P.; Selvaraj, N. Mechanical and Tribological Behavior of Particulate Reinforced Aluminum Metal Matrix Composites—A review. J. Miner. Mater. Charact. Eng. 2011, 10, 59–91. [Google Scholar] [CrossRef]
Figure 1. Die assembly used for making compact samples with the help of hydraulic press. The diameter of samples to be prepared is 20 mm and the thickness is 4 mm.
Figure 1. Die assembly used for making compact samples with the help of hydraulic press. The diameter of samples to be prepared is 20 mm and the thickness is 4 mm.
Crystals 13 01347 g001
Figure 2. The left side of the figure shows fabricated AMMC while the right side shows a machined sample.
Figure 2. The left side of the figure shows fabricated AMMC while the right side shows a machined sample.
Crystals 13 01347 g002
Figure 3. Field emission scanning electron microscope (FESEM) used for EDS analysis and microstructure images.
Figure 3. Field emission scanning electron microscope (FESEM) used for EDS analysis and microstructure images.
Crystals 13 01347 g003
Figure 4. Clustering zone observed in hybrid AMMCs.
Figure 4. Clustering zone observed in hybrid AMMCs.
Crystals 13 01347 g004
Figure 5. EDS analysis of AMMC with 40% SiC as a supplement. Left side shows microstructure image and right side presents the graphical presentations of elements included in composite showing their wt%.
Figure 5. EDS analysis of AMMC with 40% SiC as a supplement. Left side shows microstructure image and right side presents the graphical presentations of elements included in composite showing their wt%.
Crystals 13 01347 g005
Figure 6. EDS analysis of AMMC with 20% SiC and 30% ZrSiO4 as a supplement. Left side shows microstructure image and right side presents the graphical presentations of elements included in composite showing their wt%.
Figure 6. EDS analysis of AMMC with 20% SiC and 30% ZrSiO4 as a supplement. Left side shows microstructure image and right side presents the graphical presentations of elements included in composite showing their wt%.
Crystals 13 01347 g006
Figure 7. Porosity is shown in machined AMMC with 40% SiC.
Figure 7. Porosity is shown in machined AMMC with 40% SiC.
Crystals 13 01347 g007
Figure 8. Main effect plot for machined Al-SiC.
Figure 8. Main effect plot for machined Al-SiC.
Crystals 13 01347 g008
Figure 9. Main effect plot for machined Al-ZrSiO4.
Figure 9. Main effect plot for machined Al-ZrSiO4.
Crystals 13 01347 g009
Figure 10. Main effect plot for Hybrid AMMCs.
Figure 10. Main effect plot for Hybrid AMMCs.
Crystals 13 01347 g010
Figure 11. Comparison of experimental and predicted hardness values.
Figure 11. Comparison of experimental and predicted hardness values.
Crystals 13 01347 g011
Figure 12. SEM image of Al-SiC sample showing white recast layer.
Figure 12. SEM image of Al-SiC sample showing white recast layer.
Crystals 13 01347 g012
Table 1. Property table for reinforcements [25].
Table 1. Property table for reinforcements [25].
Elastic ModulusSiCZrSiO4
Elastic Modulus410 GPa275 GPa
Thermal Conductivity30–40 W/mK3.5 W/Mk (at 600 k)
Table 2. Machining conditions of WEDM.
Table 2. Machining conditions of WEDM.
Machining ConditionsSymbolUnitValues
Gap voltageVpmV50
Pulse-on timeTONµs12
Pulse-off-timeTOFFµs14
Wire feed rateWFSmm/min2–3
Wire diameterWDMm0.25
Table 3. List of elements found as a result of EDS using SEM in the Al + 40% SiC supplemented composites.
Table 3. List of elements found as a result of EDS using SEM in the Al + 40% SiC supplemented composites.
ElementsWeight%Atomic%
Al44.9832.44
Si1.711.18
C3.776.11
O49.5460.26
Table 4. List of elements found as a result of EDS using SEM in the Al + 30% SiC + 20% ZrSiO4 supplemented composites.
Table 4. List of elements found as a result of EDS using SEM in the Al + 30% SiC + 20% ZrSiO4 supplemented composites.
ElementsWeight%Atomic%
Al44.5537.34
Si13.5910.95
C10.8320.39
O20.2828.66
Zr10.752.67
Table 5. Hardness values for machined samples.
Table 5. Hardness values for machined samples.
SampleTypeSampleMean Hardness
(HV) ± STD
Al-SiCBinaryS130.8 ± 2.4
S236.0 ± 2.2
S359.4 ± 2.4
S467.7 ± 3.1
Al-ZrSiO4BinaryS525.4 ± 2.2
S6104.0 ± 2.4
S760.2 ± 3.1
S813.8 ± 1.8
Al-SiC-ZrSiO4HybridS929.8 ± 2.2
S1049.4 ± 2.6
S1150.6 ± 2.2
S1255.4 ± 2.9
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Bhutta, M.R.; Gillani, F.; Zahid, T.; Bibi, S.; Ghafoor, U. Investigation of Hardness and Microanalysis of Sintered Aluminum-Based Supplemented Metal Matrix Machined Composites. Crystals 2023, 13, 1347. https://doi.org/10.3390/cryst13091347

AMA Style

Bhutta MR, Gillani F, Zahid T, Bibi S, Ghafoor U. Investigation of Hardness and Microanalysis of Sintered Aluminum-Based Supplemented Metal Matrix Machined Composites. Crystals. 2023; 13(9):1347. https://doi.org/10.3390/cryst13091347

Chicago/Turabian Style

Bhutta, Muhammad Raheel, Fouzia Gillani, Taiba Zahid, Saira Bibi, and Usman Ghafoor. 2023. "Investigation of Hardness and Microanalysis of Sintered Aluminum-Based Supplemented Metal Matrix Machined Composites" Crystals 13, no. 9: 1347. https://doi.org/10.3390/cryst13091347

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop