Next Article in Journal
A Review on Insights for Green Production of Unconventional Protein and Energy Sources Derived from the Larval Biomass of Black Soldier Fly
Next Article in Special Issue
Catalytic Performance of Lanthanum Promoted Ni/ZrO2 for Carbon Dioxide Reforming of Methane
Previous Article in Journal
Fabrication of Highly Filled Composites with an Innovative Miniaturized Spouted Bed
Previous Article in Special Issue
Hydrogen Production by Partial Oxidation Reforming of Methane over Ni Catalysts Supported on High and Low Surface Area Alumina and Zirconia
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Catalytic Performance of Metal Oxides Promoted Nickel Catalysts Supported on Mesoporous γ-Alumina in Dry Reforming of Methane

by
Anis H. Fakeeha
1,2,
Abdulaziz A. Bagabas
3,
Mahmud S. Lanre
1,
Ahmed I. Osman
4,*,
Samsudeen O. Kasim
1,
Ahmed A. Ibrahim
1,
Rasheed Arasheed
3,
Abdulmajeed Alkhalifa
3,
Ahmed Y. Elnour
1,
Ahmed E. Abasaeed
1 and
Ahmed S. Al-Fatesh
1,*
1
Chemical Engineering Department, College of Engineering, King Saud University, P.O. Box 800, Riyadh 11421, Saudi Arabia
2
King Abdullah City for Atomic and Renewable Energy, (K.A. CARE) Energy Research and Innovation Center at Riyadh, Riyadh 11421, Saudi Arabia
3
National Petrochemical Technology Center (NPTC), Materials Science Research Institute (MSRI), King Abdulaziz City for Science and Technology, P.O. Box 6086, Riyadh 11442, Saudi Arabia
4
School of Chemistry and Chemical Engineering, Queen’s University Belfast, Belfast BT9 5AG, Northern Ireland, UK
*
Authors to whom correspondence should be addressed.
Processes 2020, 8(5), 522; https://doi.org/10.3390/pr8050522
Submission received: 14 April 2020 / Accepted: 26 April 2020 / Published: 28 April 2020

Abstract

:
Dry reforming of CH4 was conducted over promoted Ni catalysts, supported on mesoporous gamma-alumina. The Ni catalysts were promoted by various metal oxides (CuO, ZnO, Ga2O3, or Gd2O3) and were synthesized by the incipient wetness impregnation method. The influence of the promoters on the catalyst stability, coke deposition, and H2/CO mole ratio was investigated. Stability tests were carried out for 460 min. The H2 yield was 87% over 5Ni+1Gd/Al, while the CH4 and CO2 conversions were found to decrease in the following order: 5Ni+1Gd/Al > 5Ni+1Ga/Al > 5Ni+1Zn/Al > 5Ni/Al > 5Ni+1Cu/Al. The high catalytic performance of 5Ni+1Gd/Al, 5Ni+1Ga/Al, and 5Ni+1Zn/Al was found to be closely related to their contents of NiO species, which interacted moderately and strongly with the support, whereas free NiO in 5Ni+1Cu/Al made it catalytically inactive, even than 5Ni/Al. The 5Ni+1Gd/Al catalyst showed the highest CH4 conversion of 83% with H2/CO mole ratio of ~1.0.

1. Introduction

The combustion of paraffin hydrocarbons such as methane (CH4) yields water and carbon dioxide, which is one of the main contributors to global warming. Efforts have been made for years for converting CH4 and CO2 into highly desired synthesis gas (syngas), composed of hydrogen and carbon monoxide H2/CO [1,2,3]. The reaction of CH4 with CO2 is also known as dry reforming of methane (DRM) [4,5], used along with other types of methane reforming such as steam and oxy-reforming reactions [6]. The usage of the DRM reaction to produce valuable chemicals helps to reduce the harmful impacts of CO2 and CH4 on the environment [7,8]. The CH4 has a much higher global warming potential than carbon dioxide [9]. However, DRM is hampered by rapid catalyst deactivation due to carbon deposition and sintering of both the support and the active metal of catalyst [9,10,11]. The produced hydrogen is widely employed in various industries such as the production of raw chemicals (e.g., methanol and ammonia), fuel cell applications, hydrogenation agent in oil refineries, and reducing gases for the steel industry [4]. DRM includes two main reactions, the reforming of methane (Equation (1)) and the reverse water gas shift (Equation (2)):
CO 2 + CH 4 2 CO + 2 H 2
CO 2 + H 2 CO + H 2 O
The conventional catalyst used in the DRM reaction is nickel supported on alumina (Ni/Al2O3) because of its low cost and relatively high catalytic activity [12,13]. Shen et al. [14] investigated Ni-based catalysts supported on different morphologies of alumina (nanosheet, nanofiber, and particle) in the dry reforming of methane. The catalyst with nanosheet morphology displayed superb catalytic activity due to the best docking of Ni nanoparticle on the (110) plane of alumina nanosheet. However, alumina with nanofiber morphology exhibited the best stability due to the confinement of Ni particles within the nest-like structure of alumina nanofiber. Their results indicated that the catalytic performance of DRM was dependent on the morphology of alumina support. However, the Ni/Al2O3 is known to deactivate due to the blockage of its active sites by carbon deposition, an issue widely reported in the literature [15,16]. To tackle this problem, coke resistant mesoporous materials are used as supports [8] because of their large surface areas and small or medium pores. Moreover, supports play an important role in the catalytic activity due to their probable chemical effect through their interaction with the active phase. Osman et al. [17] reported that using Al2O3 support led to better interaction and synergetic effect among the active metal species in the catalyst composition. Mesoporous Al2O3-supported nickel catalysts exhibited the highest activity, stability, and excellent coke-resistance ability for DRM among several oxide-supported Ni catalysts [18,19,20]. The strong interaction between Ni and mesoporous Al2O3 improved the dispersion of Ni, retarded its sintering, and improved the adsorption of CO2 because highly dispersed Ni was very active for the reforming reaction and was less active for carbon deposition via CH4 decomposition. Furthermore, mesoporous supported Ni catalysts were active for the direct activation of CH4 on the surface of supported materials [16]. Al-Fatesh [21] investigated the promotional influence of gadolinium (Gd) on Ni/Y2O3 catalyst, employed during the production of H2 from carbon dioxide and methane. It was observed that a small amount of the promoter (1.0 wt. %) could decrease carbon deposition by 35% in comparison to the unpromoted one. Carbon dioxide temperature-programmed desorption (CO2-TPD) results showed that Gd-promoted catalysts possessed higher basicity than non-promoted Ni/Y2O3 catalyst. In other work, Al-Fatesh et al. [22] investigated the effect of various loadings of gallium promoter of Ni supported on MCM-41 on the activity and stability for the production of syngas by DRM. The addition of gallium generated high surface areas, where 2.5 wt. % of Ga resulted in a surface area of 1036 m2/g, which was less than that of the unpromoted one (~1133 m2/g). The addition of Ga reduced both the density of basic sites and the amount of carbon deposition. Weight loss was not recorded for the 3.0 wt. % Ga + 5.0 wt. % Ni/MCM-41 sample. The 2.0 wt. % Ga sample displayed 88.2% conversion of methane and the best stability, while activity declined to only 1.6% after running the reaction for 400 min at 800 °C. The promoter increased the ratio of H2/CO mole ratio from 0.9 to 1.0. Alternatively, Al-Fatesh et al. [23] studied the influence of Gd promoter in Ni-supported on mesoporous silica (MCM-41) in DRM. The catalytic performance was attained to be significantly enhanced with approximately 0.1 wt. % Gd loading. Thus, Gd can act as a promoter for Ni-based catalysts in DRM reaction. This catalyst (i.e., 0.1 wt. % Gd + 5.0 wt. % Ni/MCM-41) resulted in >87% CH4 and >91% CO2 conversions and in the production of syngas with H2/CO mole ratio nearly equal to one. Mesoporous alumina supported catalyst was designed to allow for Ni dispersion [16]. The investigators decreased the carbon formation by promoting alumina with basic metal oxides. The Ni-based catalysts were able to retard the deactivation by promoting the catalyst supports. It was established that Ni/MCM-41 promoted by rhodium (Rh), prepared via the one-pot procedure, enhanced the stability and activity of the catalyst [24]. Copper (Cu) and cobalt (Co) addition to Ni/Al2O3-ZrO2 catalyst enhanced the surface area, as reflected by BET surface area, especially by cobalt addition, while the Cu addition made the support particles more compact, and, in general, Cu and Co addition improved the conversion, the yields of hydrogen and carbon monoxide, and syngas ratio. The comparison of promoters revealed that the activity of Co was better than Cu [25]. The addition of zinc (Zn) to a Co/ZrO2 catalyst, at a ratio up to 2.0 wt. %, had a positive effect on the catalyst activity and stability, whereas further addition above this limit had the opposite effect. The positive effect of zinc was due to the prevention of Co oxidation by the formation of a Co−Zn alloy [26].
The objective of this study was to determine the optimal promoter for Ni supported on mesoporous γ-alumina (meso-γ-Al2O3) catalyst to maintain great stability and activity, while minimizing the carbon deposition during the DRM process. The effect of promoters such as Gd, Ga, Zn, and Cu on the activity, stability, and coke formation of Ni/meso-γ-Al2O3 catalysts was examined. Various characterization techniques were employed to understand the catalytic performance.

2. Experimental Part

2.1. Materials

Nickel nitrate hexahydrate [Ni(NO3)2·6H2O,98%, Alfa Aesar], cupric nitrate trihydrate [Cu(NO3)2·3H2O, purum p.a.; 98.0–103% (RT), Fluka], zinc nitrate hexahydrate [Zn(NO3)2·6H2O, 98%, Alfa Aesar], gallium(III) nitrate hydrate [Ga(NO3)3·xH2O, 99.9% (metal basis), Alfa Aesar], gadolinium(III) nitrate hexahydrate [Gd(NO3)3·6H2O, 99.9%, Ventron, Alfa Produkte], and mesoporous γ-alumina (meso-γ-Al2O3,1/8" pellets, Alfa Aesar) were purchased and were used as received. Ultrapure water was used.

2.2. Synthesis of Nickel Oxide Supported on Mesoporous-γ-Al2O3 Doped with Metal Oxide

The catalysts were prepared by the incipient wetness impregnation method, also known as dry impregnation, and the procedure is described as follows. We used this method because when using nickel nitrate as a precursor for nickel, with high concentration, the solution pH is reduced, and the surface of alumina support is interrupted and is dissolved, which, in turn, creates docking sites for nickel and enables its efficient dispersion onto alumina [27]. On this basis, the required amounts of nickel nitrate hexahydrate to introduce nickel oxide with a weight percentage of 5.0 wt. %, of metal nitrate promoter source to introduce metal oxide promoter with a weight percentage of 1.0 wt. %, and of meso-γ-Al2O3 were mixed and were ground together mechanically. Ultrapure water drops were added to the mixture to form a paste, which was stirred mechanically until it was completely dry at room temperature. Drying (at room temperature) and the addition of ultrapure water processes were performed three times to ensure homogeneous distribution within each sample. The samples were then calcined at 600 °C for three hours under static air, where the temperature was ramped at a rate of 3.0 °C·min−1. Here and after, the catalysts will be referred as 5Ni/Al for non-promoted and 5Ni+1X/Al (X = Cu, Zn, Ga, or Gd) for promoted catalysts.

2.3. Catalytic Testing

DRM experiments were carried out under atmospheric pressure at a reaction temperature of 700 °C. A tubular stainless-steel reactor (i.d., 9.0 mm; length, 300 mm) was used. An amount of 0.1 g of the catalyst was placed between two quartz wool beds to perform the activity test. Temperature measurement, during the reaction, was measured by K-type thermocouple, which was placed axially at the center of the catalyst bed. Before the reaction, the catalysts were reduced at 600 °C with the flow of H2 for an hour at a flow rate of 30.0 mL/min. During the experiments, the mixture of methane, carbon dioxide and nitrogen in a 3:3:1 volume ratio was used as feed gas, having space velocity of 2990 h−1. The effluent gas was analyzed by an on-line GC (GC-2014 Shimadzu Corp., Kyoto, Japan), equipped with a thermal conductivity detector (TCD) and two columns: Porapak Q and Molecular Sieve 5A. This GC was connected in series/bypass connections in order to have a complete analysis of the reaction products. The methane conversion and hydrogen yield were calculated:
CH 4   conversion   ( % ) = CH 4 , in   CH 4 , out   CH 4 , in × 100
CO 2   conversion   ( % ) = CO 2 , in   CO 2 , out   CO 2 , in × 100
H 2   yield   ( % ) = H 2 , out   2 × CH 4 , in × 100
H 2   CO = mole   of   H 2   produced mole   of   CO   produced
Deactivation   Factor   ( % ) = Initial   CH 4 Conversion Final   CH 4 Conversion Initial   CH 4 Conversion × 100

2.4. Catalyst Characterization

2.4.1. N2 Physisorption

The Pore size distribution and the surface area of the catalysts were determined by physisorption of nitrogen at −196 °C by using a Micromeritics Tristar II 3020 surface area and porosity analyzer. The distribution of the pore size was calculated by Barrett, Joyner, and Halenda (BJH) method.

2.4.2. XRD

Rigaku (Miniflex) diffractometer, with a Cu Kα X-ray radiation working at 40 kV and 40 mA, was used to examine the structure of the catalysts before and after the reaction. A step of 0.02° and scanning 2θ range of 10–85° were used. X’Pert high score plus software was used to evaluate the data obtained from the instrument. Different phases were matched to the JCPDS data bank. The result of the XRD analysis (Figure S1) is discussed in the supplementary file.

2.4.3. TPR

A sample of 70 mg was put in the TPR cell of a Micromeritics Auto Chem II apparatus. Then the furnace temperature was increased from room temperature to 1000 °C with heating rate of 10 °C·min−1, under 40 mL·min−1 flow of 10 vol. % H2/Ar mixture. The H2 consumption was monitored by a TCD unit.

2.4.4. Temperature-Programmed Oxidation (TPO)

TPO is a useful technique for describing the type of carbon deposit over the surface of the catalyst. With respect to the literature, formed carbon, over the surface of catalysts in CO2 reforming of methane, occurs in various forms: graphitic, amorphous, and atomic [28]. Under oxidative medium and high temperature, deposited carbon can be oxidised to carbon dioxide. The carbon oxidation below 250 °C is called atomic carbon, while the carbon which oxidised in the range of 250–600 °C was categorized as amorphous, whereas graphitic carbon burned above 600 °C [28]. To this end, the TPO was performed under 10% O2/He atmosphere for identifying the form of deposited carbon on the surface of the catalyst by using a Micromeritics AutoChem II (Micromeritics, Atlanta, GA, USA). The analysis was performed in the temperature range of 50−800 °C, under a flow of 40 mL/min of 10% O2/He. The spent catalyst was pre-treated under argon atmosphere at 150 °C for half an hour and the temperature was then reduced to 25 °C.

2.4.5. Thermo-Gravimetric Analysis (TGA)

The TGA was carried out under air flow at 50 mL/min, using a TGA-15 SHIMADZU analyser, to determine the amount of carbon deposited on the catalyst surface after the reaction, where 10–15 mg of the spent catalyst was filled into a platinum pan of the thermo-balance. Then, the temperature was increased to 1000 °C at a heating rate of 20 °C·min−1, and the weight reduction was determined.

2.4.6. Laser Raman (NMR-4500) Spectrometer

Laser Raman (NMR-4500) Spectrometer (JASCO, Japan) was used to record Raman spectra of the spent catalyst samples. The wavelength of the excitation beam was set to 532 nm, and objective lens of 100× magnification was used for the measurement. The laser intensity was adjusted to 1.6 mW. Each spectrum was received by averaging 3 exposures on 10 seconds. Spectra were recorded in the range 1200–3000 cm−1 (Raman shift) and were processed by using Spectra Manager Ver.2 software (JASCO, Japan).

3. Results and Discussion

3.1. BET (Brunauer–Emmett–Teller) and the BJH (Barrett, Joyner, and Halenda) analyses

These analyses provided the specific surface areas (SBET), pore volume (VP), and average pore diameter (dp), depending on promoter identity. Table 1 displays the SBET, VP, and dp values for all the catalysts investigated in this work.
Promoter loading of 1.0 wt. % did not affect VP and Pd. The SBET parameter was not also affected by the promoter type except in the case of Gd promoter, which led to a slight increase in SBET in comparison with non-promoted catalyst. Nitrogen adsorption-desorption isotherms (Figure 1) showed that all prepared catalysts had a mesoporous structure. The catalysts displayed type IV isotherm with a hysteresis loop of the H3-type, resulting from capillary condensation and evaporation at high relative pressures. This structural feature indicated the mesoporous structure of the γ-Al2O3 support with hexagonal array. There was no significant change in the framework of the support due to the loading of the promoter. The isotherms of the catalysts had a strongly noticeable increase in the relative pressure region of 0.65–0.95 due to combination of N2 capillary condensation in the mesopore and the condensation of N2 in the interstitial cavities of the support.

3.2. Temperature-Programmed Reduction (TPR)

The H2-TPR was used to study the ease and extent of reducibility of the fresh catalysts. The reduction peaks as a function of temperature are shown in Figure 2. Reduction peaks were detected below 800 °C. The different reduction temperature regions were due to the interaction strength between NiO and supports. The meso-γ-Al2O3 support showed no reduction peaks in TPR measurement [29]. Three reduction peaks were detected for promoted catalysts, whereas two peaks were detected for the non-promoted catalyst. The first peak, in the temperature range of 200−300 °C, was quite close to the reduction temperature of bulk NiO, which indicated that this kind of NiO had no interaction with the support. The second peak, in the temperature range of 500−600 °C, indicated moderate interaction with the support, while the third peak, in the temperature range of 700−800 °C, showed strong interaction of NiO with the mesoporous γ-Al2O3, as NiAl2O4 was being formed [30]. This strong interaction improved the dispersion of Ni and hindered its sintering during the DRM. The broadening of the last peak could be attributed to the reduction of Ni ion situated at different layers in the pore wall [25], thus emphasizing the intense interaction between the NiO particles and the support. The non-promoted catalyst 5Ni/Al had reduction peaks for NiO that strongly interacted with support in the temperature range of 700–800 °C. The 5Ni+1Cu/Al catalyst had reduction peaks for free NiO additionally at 300 °C. The rest of the catalysts (i.e., 5Ni+1Zn/Al, 5Ni+1Ga/Al, and 5Ni+1Gd/Al) had reduction peaks for NiO moderately and strongly interacted with the support. The 5Ni+1Gd/Al catalyst had a higher intensity of both types of NiO than 5Ni+1Zn/Al and 5Ni+1Ga/Al catalysts. The 5Ni/Al showed the highest peak at 700–800 °C for all catalysts and no apparent peaks at low temperatures, justifying its requirement for high reduction temperature and low tendency to react with hydrogen. The negative peaks below 200 °C in the TPR profiles are due to the hydrogen spillover into the mesopores of the catalysts, as we reported in our previous publication [31].

3.3. Catalytic Activity

Figure 3A,B shows the conversions of CH4 and CO2 along the time-on-stream (TOS). The catalysts were highly stable at the reaction temperature of 700 °C during the reaction time of 460 min, as shown in Figure 3. The CH4 and CO2 conversions of the catalyst system were found in order of 5Ni+1Gd/Al > 5Ni+1Ga/Al > 5Ni+1Zn/Al > 5Ni/Al > 5Ni+1Cu/Al. The catalytic performances of the first three catalysts were found to correlate with the content of NiO, which interacted moderately and strongly with the support, as shown in the H2-TPR result above. The H2/CO mole ratio over these catalysts were also close to 1.0 (Table 2). It hinted towards suppression of reverse water gas shift reaction (CO2 + H2 → CO + H2O) over these catalyst systems. The 5Ni+1Gd/Al catalyst was found to be the most stable and resulted in the highest conversions of CH4 (~83%) and CO2 and (~89%) with the highest activity for producing syngas because of its higher oxygen storage capacity [23]. The calculated deactivation factors (DF) were shown in Table 2 below, with the lowest DF for the 5Ni+1Gd/Al catalyst. The H2/CO molar ratio versus TOS is shown in Figure 3C. The presence of free NiO (as shown in H2-TPR) in 5Ni+1Cu/Al caused less catalytic performance even than the non-promoted catalyst 5Ni/Al. Low H2/CO ratio for both catalysts may be due to the dominance of reverse water gas shift reaction.

3.4. Temperature Programmed Oxidation (TPO)

TPO is a useful characterization technique for the analysis of the kind of carbon deposits on the surface of spent catalysts. As mentioned before, carbon deposits on the spent catalysts could be graphitic, amorphous, or atomic in nature, depending on the temperature of oxidation. It has been reported that carbon that oxidizes below 250 °C is atomic in nature, while carbon that oxidizes between 250–600 °C falls under the category of amorphous. Lastly, graphitic carbon oxidizes at a temperature above 600 °C [28].
The TPO showed peaks that correspond to the kind of carbon formed on the catalyst surface. The TPO curves for all the spent catalysts had higher intensity peaks appearing below 250 °C (Figure 4), corresponding to less ordered (more reactive) atomic carbon [32,33,34]. The negative peaks that appeared at around 400 °C indicate oxidation of the metals. A small positive peak can be seen at around 400 °C for all the used catalysts except 5Ni+1Zn/Al. This is an indication of the presence of amorphous carbon on these catalysts. Moreover, there appeared to be very small deposits of graphitic carbon on the spent 5Ni+1Ga/Al and 5Ni+1Cu/Al, which can be ascribed to the peaks appearing at above 600 °C.

3.5. Thermogravimetric analysis (TGA) of Spent Catalyst

The profiles of the five spent catalysts showed weight losses of 3.0 wt. %, 5.0 wt. %, 4.0 wt. %, 4.0 wt. %, and 2.0 wt. % for 5Ni+1Cu/Al, 5Ni+1Gd/Al, 5Ni+1Zn/Al, and 5Ni/Al, respectively (Figure 5). All the spent catalysts were studied after catalytic cycle at 700 °C during 460 min on stream. The 5Ni+1Gd/Al had the highest carbon content due to high methane conversion into syngas and its decomposition into carbon. The catalyst probably did not do much in gasifying the carbon deposits, indicating its ability to accumulate carbon deposits compared to the other catalysts. On the other hand, 5Ni/Al showed the least carbon content.

3.6. Scanning Electron Microscope (SEM)

The SEM images of all samples are shown in Figure 6. The morphology of all the catalyst samples were more or less the same. All the catalysts showed agglomerated particles with undefined shapes, where the identity of the promoter had no effect on the morphology.

3.7. Raman Analysis

On the Raman spectra of all the spent catalysts (Figure 7), there are two bands with Raman shifts: 1474 ± 5 cm−1 and 1537 ± 10 cm−1, which correspond to the D and G band, respectively. The D band can be ascribed to carbon deposits with imperfect structures that are disordered (amorphous), while the G band is a characteristic of well-ordered carbon structure (graphitic) [35,36,37]. The ID/IG ratio showed that the spent 5Ni/Al had the highest disordered (amorphous) carbon on its surface after the reaction, while this ratio decreased for the promoted catalysts, indicating that the presence of promoters caused a good order of carbon deposits (graphitic). This conclusion about the deposited carbon on the surface of the spent catalysts from Raman spectra was in parallel with the results of their corresponding TPO analysis.

4. Conclusions

The N2 physisorption analysis confirmed the mesoporosity of the prepared catalysts. In the TPR analysis, an extra peak was observed owing to the promoting effects. In the XRD analysis, no peaks related to promoters were detected, and hence, they scattered well in the matrix of the catalyst. The TPO analysis depicted the presence of atomic carbon, some amorphous and graphitic carbon, as well as the oxidation of the metals. The TGA analysis indicated a similar amount of carbon deposition for all the spent catalyst. The SEM analysis displayed agglomerated particles with undefined shapes. Promoters with 1.0 wt. % loading (CuO, ZnO, Ga2O3, or Gd2O3) were used for enhancing the catalytic performance of 5Ni/Al in DRM. The CH4 and CO2 conversions increased in the order of 5Ni+1Cu/Al < 5Ni/Al < 5Ni+1Zn/Al < 5Ni+1Ga/Al < 5Ni+1Gd/Al. The catalytic performance of 5Ni+1Gd/Al, 5Ni+1Ga/Al, and 5Ni+1Zn/Al were found to correlate with the content of the NiO, which interacts moderately and strongly with support. Free NiO species in 5Ni+1Cu/Al made its catalytic performance even inferior to that of 5Ni/Al. 5Ni+1Gd/Al showed the highest conversions of CH4 (~83%) and CO2 (~89%) with H2/CO mole ratio of ~1.0.

Supplementary Materials

The following are available online at https://www.mdpi.com/2227-9717/8/5/522/s1, Figure S1: XRD patterns of non-promoted and promoted catalysts.

Author Contributions

Experiment, A.S.A.-F., M.S.L., and S.O.K., writing—original draft preparation, A.S.A.-F., A.A.B., A.A.I., A.H.F., M.S.L., A.Y.E., and S.O.K.; preparation of catalyst, A.A., A.A.B., and R.A., writing—review and editing, A.A.B., A.E.A., A.I.O., A.S.A.-F., and A.H.F. All authors have read and agreed to the published version of the manuscript.

Funding

Funding: The work is supported by the Deanship of Scientific Research programs of King Saud University via project No. RGP-1435-078.

Acknowledgments

The KSU authors would like to extend their sincere appreciation to the Deanship of Scientific Research at the King Saud University for funding this research group project # No. RGP-1435-078. The author would like to thank Charlie Farrell who assisted in the proof-reading of the manuscript.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Aghamohammadi, S.; Haghighi, M.; Karimipour, S. A Comparative Synthesis and Physicochemical Characterizations of Ni/Al2O3–MgO Nanocatalyst via Sequential Impregnation and Sol–Gel Methods Used for CO2 Reforming of Methane. J. Nanosci. Nanotechnol. 2013, 13, 4872–4882. [Google Scholar] [CrossRef]
  2. Fan, M.-S.; Abdullah, A.Z.; Bhatia, S. Hydrogen production from carbon dioxide reforming of methane over Ni–Co/MgO–ZrO2 catalyst: Process optimization. Int. J. Hydrog. Energy 2011, 36, 4875–4886. [Google Scholar] [CrossRef]
  3. Xu, L.; Song, H.; Chou, L. Mesoporous nanocrystalline ceria–zirconia solid solutions supported nickel based catalysts for CO2 reforming of CH4. Int. J. Hydrog. Energy 2012, 37, 18001–18020. [Google Scholar] [CrossRef]
  4. Batiot-Dupeyrat, C.; Valderrama, G.; Meneses, A.; Martinez, F.; Barrault, J.; Tatibouët, J.M. Pulse study of CO2 reforming of methane over LaNiO3. Appl. Catal. A Gen. 2003, 248, 143–151. [Google Scholar] [CrossRef]
  5. Gallego, G.S.; Batiot-Dupeyrat, C.; Barrault, J.; Florez, E.; Mondragón, F. Dry reforming of methane over LaNi1−yByO3±δ (B=Mg, Co) perovskites used as catalyst precursor. Appl. Catal. A Gen. 2008, 334, 251–258. [Google Scholar] [CrossRef]
  6. Osman, A.I. Catalytic Hydrogen Production from Methane Partial Oxidation: Mechanism and Kinetic Study. Chem. Eng. Technol. Accept. 2020. [CrossRef]
  7. Sutthiumporn, K. Development of Nickel Based Catalystssynthesized over Different Precursors for Dry CO2 Reforming of Methane to Syngas Production. Master’s Thesis, National University of Singapore, Singapore, 2011; pp. 7–10. Available online: https://core.ac.uk/download/pdf/48655900.pdf (accessed on 28 February 2020).
  8. Zhan, H.-J.; Shi, X.-Y.; Huang, X.; Zhao, N. Highly coke-resistant ordered mesoporous Ni/SiC with large surface areas in CO2 reforming of CH4. J. Fuel Chem. Technol. 2019, 47, 942–948. [Google Scholar] [CrossRef]
  9. Fakeeha, A.H.; Al-Fatesh, A.S.; Ibrahim, A.A.; Abasaeed, A.E. Effect of Calcium Promoter on Ni-Based Catalysts Supported on α-Al2O3 and TiO2-P25. Appl. Mech. Mater. 2012, 204–208, 3909–3913. [Google Scholar] [CrossRef]
  10. Al-Fatesh, A.S.A.; Ibrahim, A.A.; Fakeeha, A.H.; Abasaeed, A.E. Activity and Carbon Formation of a Low Ni-Loading Alumina-Supported Catalyst. J. Chem. Eng. Jpn. 2011, 44, 328–335. [Google Scholar] [CrossRef]
  11. Serrano-Lotina, A.; Daza, L. Influence of the operating parameters over dry reforming of methane to syngas. Int. J. Hydrog. Energy 2014, 39, 4089–4094. [Google Scholar] [CrossRef]
  12. Karam, L.; Reboul, J.; El Hassan, N.; Nelayah, J.; Massiani, P. Nanostructured Nickel Aluminate as a Key Intermediate for the Production of Highly Dispersed and Stable Nickel Nanoparticles Supported within Mesoporous Alumina for Dry Reforming of Methane. Molecules 2019, 24, 4107. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  13. Karam, L.; Reboul, J.; Casale, S.; Massiani, P.; El Hassan, N. Porous Nickel-Alumina Derived from Metal-Organic Framework (MIL-53): A New Approach to Achieve Active and Stable Catalysts in Methane Dry Reforming. ChemCatChem 2020, 12, 373–385. [Google Scholar] [CrossRef] [Green Version]
  14. Shen, D.; Huo, M.; Li, L.; Lyu, S.; Wang, J.; Wang, X.; Zhang, Y.; Li, J. Effects of alumina morphology on dry reforming of methane over Ni/Al2O3 catalysts. Catal. Sci. Technol. 2020, 10, 510–516. [Google Scholar] [CrossRef]
  15. Sajjadi, S.M.; Haghighi, M.; Rahmani, F. Dry reforming of greenhouse gases CH4/CO2 over MgO-promoted Ni–Co/Al2O3–ZrO2 nanocatalyst: Effect of MgO addition via sol–gel method on catalytic properties and hydrogen yield. J. Sol-Gel Sci. Technol. 2014, 70, 111–124. [Google Scholar] [CrossRef]
  16. Dias, J.A.C.; Assaf, J.M. Influence of calcium content in Ni/CaO/γ-Al2O3 catalysts for CO2-reforming of methane. Catal. Today 2003, 85, 59–68. [Google Scholar] [CrossRef]
  17. Osman, A.I.; Abu-Dahrieh, J.K.; Cherkasov, N.; Fernandez-Garcia, J.; Walker, D.; Walton, R.I.; Rooney, D.W.; Rebrov, E. A highly active and synergistic Pt/Mo2C/Al2O3 catalyst for water-gas shift reaction. Mol. Catal. 2018, 455, 38–47. [Google Scholar] [CrossRef] [Green Version]
  18. Hou, Z.; Yokota, O.; Tanaka, T.; Yashima, T. Investigation of CH4 Reforming with CO2 on Meso-Porous Al2O3-Supported Ni Catalyst. Catal. Lett. 2003, 89, 121–127. [Google Scholar] [CrossRef]
  19. Abbas, H.F.; Wan Daud, W.M.A. Hydrogen production by methane decomposition: A review. Int. J. Hydrog. Energy 2010, 35, 1160–1190. [Google Scholar] [CrossRef]
  20. Paksoy, A.I.; Caglayan, B.S.; Aksoylu, A.E. A study on characterization and methane dry reforming performance of Co–Ce/ZrO2 catalyst. Appl. Catal. B Environ. 2015, 168–169, 164–174. [Google Scholar] [CrossRef]
  21. Al-Fatesh, A.S. Promotional effect of Gd over Ni/Y2O3 catalyst used in dry reforming of CH4 for H2 production. Int. J. Hydrog. Energy 2017, 42, 18805–18816. [Google Scholar] [CrossRef]
  22. Al-Fatesh, A.S.; Ibrahim, A.A.; Abu-Dahrieh, J.K.; Al-Awadi, A.S.; El-Toni, A.M.; Fakeeha, A.H.; Abasaeed, A.E. Gallium-Promoted Ni Catalyst Supported on MCM-41 for Dry Reforming of Methane. Catalysts 2018, 8, 229. [Google Scholar] [CrossRef] [Green Version]
  23. Al-Fatesh, A.S.; Atia, H.; Ibrahim, A.A.; Fakeeha, A.H.; Singh, S.K.; Labhsetwar, N.K.; Shaikh, H.; Qasim, S.O. CO2 reforming of CH4: Effect of Gd as promoter for Ni supported over MCM-41 as catalyst. Renew. Energy 2019, 140, 658–667. [Google Scholar] [CrossRef]
  24. Arbag, H.; Yasyerli, S.; Yasyerli, N.; Dogu, G. Activity and stability enhancement of Ni-MCM-41 catalysts by Rh incorporation for hydrogen from dry reforming of methane. Int. J. Hydrog. Energy 2010, 35, 2296–2304. [Google Scholar] [CrossRef]
  25. Sharifi, M.; Haghighi, M.; Rahmani, F.; Karimipour, S. Syngas production via dry reforming of CH4 over Co- and Cu-promoted Ni/Al2O3–ZrO2 nanocatalysts synthesized via sequential impregnation and sol–gel methods. J. Nat. Gas Sci. Eng. 2014, 21, 993–1004. [Google Scholar] [CrossRef]
  26. Park, J.-H.; Yeo, S.; Kang, T.-J.; Shin, H.-R.; Heo, I.; Chang, T.-S. Effect of Zn promoter on catalytic activity and stability of Co/ZrO2 catalyst for dry reforming of CH4. J. CO2 Util. 2018, 23, 10–19. [Google Scholar] [CrossRef]
  27. Schwarz, J.A.; Contescu, C.; Contescu, A. Methods for preparation of catalytic materials. Chem. Rev. 1995, 95, 477–510. [Google Scholar] [CrossRef]
  28. Hao, Z.; Zhu, Q.; Jiang, Z.; Hou, B.; Li, H. Characterization of aerogel Ni/Al2O3 catalysts and investigation on their stability for CH4-CO2 reforming in a fluidized bed. Fuel Process. Technol. 2009, 90, 113–121. [Google Scholar] [CrossRef]
  29. Osman, A.I.; Abu-Dahrieh, J.K.; McLaren, M.; Laffir, F.; Rooney, D.W. Characterisation of Robust Combustion Catalyst from Aluminium Foil Waste. ChemistrySelect 2018, 3, 1545–1550. [Google Scholar] [CrossRef] [Green Version]
  30. Jiménez-González, C.; Boukha, Z.; de Rivas, B.; González-Velasco, J.R.; Gutiérrez-Ortiz, J.I.; López-Fonseca, R. Behaviour of nickel–alumina spinel (NiAl2O4) catalysts for isooctane steam reforming. Int. J. Hydrog. Energy 2015, 40, 5281–5288. [Google Scholar] [CrossRef]
  31. Al-Fatesh, A.S.; Kumar, R.; Kasim, S.O.; Ibrahim, A.A.; Fakeeha, A.H.; Abasaeed, A.E.; Alrasheed, R.; Bagabas, A.; Chaudhary, M.L.; Frusteri, F.; et al. The effect of modifier identity on the performance of Ni-based catalyst supported on γ-Al2O3 in dry reforming of methane. Catal. Today 2020, in press. [Google Scholar] [CrossRef]
  32. Xu, J.; Zhou, W.; Wang, J.; Li, Z.; Ma, J. Characterization and Analysis of Carbon Deposited during the Dry Reforming of Methane over Ni/La2O3/Al2O3 Catalysts. Chin. J. Catal. 2009, 30, 1076–1084. [Google Scholar] [CrossRef]
  33. Hou, Z.; Yashima, T. Meso-porous Ni/Mg/Al catalysts for methane reforming with CO2. Appl. Catal. A Gen. 2004, 261, 205–209. [Google Scholar] [CrossRef]
  34. Asai, K.; Takane, K.; Nagayasu, Y.; Iwamoto, S.; Yagasaki, E.; Inoue, M. Decomposition of methane in the presence of carbon dioxide over Ni catalysts. Chem. Eng. Sci. 2008, 63, 5083–5088. [Google Scholar] [CrossRef]
  35. Li, X.; Li, D.; Tian, H.; Zeng, L.; Zhao, Z.-J.; Gong, J. Dry reforming of methane over Ni/La2O3 nanorod catalysts with stabilized Ni nanoparticles. Appl. Catal. B Environ. 2017, 202, 683–694. [Google Scholar] [CrossRef]
  36. Liu, D.; Lau, R.; Borgna, A.; Yang, Y. Carbon dioxide reforming of methane to synthesis gas over Ni-MCM-41 catalysts. Appl. Catal. A Gen. 2009, 358, 110–118. [Google Scholar] [CrossRef]
  37. Zhang, J.; Li, F. Coke-resistant Ni@SiO2 catalyst for dry reforming of methane. Appl. Catal. B Environ. 2015, 176–177, 513–521. [Google Scholar] [CrossRef]
Figure 1. N2 adsorption-desorption isotherms for non-promoted and promoted catalysts.
Figure 1. N2 adsorption-desorption isotherms for non-promoted and promoted catalysts.
Processes 08 00522 g001
Figure 2. Temperature-programmed reduction (TPR) profiles of the non-promoted and promoted catalysts.
Figure 2. Temperature-programmed reduction (TPR) profiles of the non-promoted and promoted catalysts.
Processes 08 00522 g002
Figure 3. (A) Conversion of CH4, (B) Conversion of CO2, and (C) the fraction of H2/CO at 700 °C, 1.0 atm and GHSV = 2990 h1.
Figure 3. (A) Conversion of CH4, (B) Conversion of CO2, and (C) the fraction of H2/CO at 700 °C, 1.0 atm and GHSV = 2990 h1.
Processes 08 00522 g003
Figure 4. Temperature programmed oxidation (TPO) profiles of the used catalysts.
Figure 4. Temperature programmed oxidation (TPO) profiles of the used catalysts.
Processes 08 00522 g004
Figure 5. Thermogravimetric analysis (TGA) curves of the spent catalysts.
Figure 5. Thermogravimetric analysis (TGA) curves of the spent catalysts.
Processes 08 00522 g005
Figure 6. SEM images of the fresh catalysts (A) 5Ni/Al, (B) 5Ni+1Gd/Al, (C) 5Ni+1Zn/Al, (D) 5Ni+1Cu/Al, and (E) 5Ni+1Ga/Al.
Figure 6. SEM images of the fresh catalysts (A) 5Ni/Al, (B) 5Ni+1Gd/Al, (C) 5Ni+1Zn/Al, (D) 5Ni+1Cu/Al, and (E) 5Ni+1Ga/Al.
Processes 08 00522 g006
Figure 7. Raman spectra for the spent catalysts.
Figure 7. Raman spectra for the spent catalysts.
Processes 08 00522 g007
Table 1. Textural properties (SBET, VP, dp) of the non-promoted and promoted catalysts.
Table 1. Textural properties (SBET, VP, dp) of the non-promoted and promoted catalysts.
CatalystSBET, m2·g−1VP, cm3·g−1dp, nm
5NiAl1820.6111.3
5Ni+1Cu/Al1850.5911.4
5Ni+1Zn/Al1870.6011.4
5Ni+1Ga/Al1850.6111.3
5Ni+1Gd/Al1930.6211.4
Table 2. Conversion of CH4, H2/CO ratio and deactivation factor (DF) for non-promoted and promoted catalysts.
Table 2. Conversion of CH4, H2/CO ratio and deactivation factor (DF) for non-promoted and promoted catalysts.
CatalystXi (CH4)Xf (CH4)H2/CO Mole Ratio aDF bCoke c
%% %%wt Loss
5Ni/Al79.378.60.970.90 4.0
5Ni+1Cu/Al77.476.10.971.705.8
5Ni+1Zn/Al80.079.41.000.754.8
5Ni+1Ga/Al79.078.70.990.385.5
5Ni+1Gd/Al83.483.21.000.246.5
a Average ratio; b Deactivation factor (DF) = [(initial CH4 conversion − final CH4 conversion)/initial CH4 conversion] × 100; c Coke Estimated using TGA data.

Share and Cite

MDPI and ACS Style

Fakeeha, A.H.; Bagabas, A.A.; Lanre, M.S.; Osman, A.I.; Kasim, S.O.; Ibrahim, A.A.; Arasheed, R.; Alkhalifa, A.; Elnour, A.Y.; Abasaeed, A.E.; et al. Catalytic Performance of Metal Oxides Promoted Nickel Catalysts Supported on Mesoporous γ-Alumina in Dry Reforming of Methane. Processes 2020, 8, 522. https://doi.org/10.3390/pr8050522

AMA Style

Fakeeha AH, Bagabas AA, Lanre MS, Osman AI, Kasim SO, Ibrahim AA, Arasheed R, Alkhalifa A, Elnour AY, Abasaeed AE, et al. Catalytic Performance of Metal Oxides Promoted Nickel Catalysts Supported on Mesoporous γ-Alumina in Dry Reforming of Methane. Processes. 2020; 8(5):522. https://doi.org/10.3390/pr8050522

Chicago/Turabian Style

Fakeeha, Anis H., Abdulaziz A. Bagabas, Mahmud S. Lanre, Ahmed I. Osman, Samsudeen O. Kasim, Ahmed A. Ibrahim, Rasheed Arasheed, Abdulmajeed Alkhalifa, Ahmed Y. Elnour, Ahmed E. Abasaeed, and et al. 2020. "Catalytic Performance of Metal Oxides Promoted Nickel Catalysts Supported on Mesoporous γ-Alumina in Dry Reforming of Methane" Processes 8, no. 5: 522. https://doi.org/10.3390/pr8050522

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.