Next Article in Journal
An Effective Strategy to Maintain the CALPHAD Atomic Mobility Database of Multicomponent Systems and Its Application to Hcp Mg–Al–Zn–Sn Alloys
Next Article in Special Issue
Torque Generation of the Endodontic Instruments: A Narrative Review
Previous Article in Journal
Superionic Solid Electrolyte Li7La3Zr2O12 Synthesis and Thermodynamics for Application in All-Solid-State Lithium-Ion Batteries
Previous Article in Special Issue
Post-Fatigue Fracture and Marginal Behavior of Endodontically Treated Teeth: Partial Crown vs. Full Crown vs. Endocrown vs. Fiber-Reinforced Resin Composite
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Distrontium Cerate as a Radiopaque Component of Hydraulic Endodontic Cement

1
Department of Pulp Biology and Endodontics, Graduate School of Medical and Dental Sciences, Tokyo Medical and Dental University, 1-5-45 Yushima, Bunkyo-ku, Tokyo 113-8549, Japan
2
Department of Conservative Dentistry and Prosthetics, Faculty of Dentistry, Srinakharinwirot University, 114 Sukhumvit 23, Wattana, Bangkok 10110, Thailand
3
National Research Centre of Egypt, Department of Restorative Dentistry and Dental Materials, Oral and Dental Research Division, El Buhouth Street, Dokki, Cairo 12622, Egypt
4
Department of Advanced Biomaterials, Graduate School of Medical and Dental Sciences, Tokyo Medical and Dental University, 1-5-45 Yushima, Bunkyo-ku, Tokyo 113-8549, Japan
5
Department of Oral and Maxillofacial Radiology, Graduate School of Medical and Dental Sciences, Tokyo Medical and Dental University, 1-5-45 Yushima, Bunkyo-ku, Tokyo 113-8549, Japan
*
Author to whom correspondence should be addressed.
Materials 2022, 15(1), 284; https://doi.org/10.3390/ma15010284
Submission received: 26 November 2021 / Revised: 24 December 2021 / Accepted: 28 December 2021 / Published: 31 December 2021
(This article belongs to the Special Issue Endodontics)

Abstract

:
This study aimed to synthesize distrontium cerate (2SrO·CeO2: S2Ce) and evaluate its properties as an alternative component of the endodontic cement. S2Ce cement was prepared through calcination of strontium hydroxide and cerium carbonate. Subsequently, the crystal phase was confirmed using X-ray diffraction. S2Ce cement exhibited a rapid setting time (121 min) and achieved a high compressive strength (72.1 MPa) at 1 d after mixing, comparable to the compressive strength of a commercial mineral trioxide aggregate (MTA) cement (ProRoot MTA) after 28 d post mixing. However, the compressive strength decreased after 28 d of storage when the W/P ratio was 0.30–0.40 (p < 0.05). Ion dissolution test of the S2Ce cement showed that strontium ions were released after immersion in water (5.27 mg/mL after 1 d), whereas cerium dissolution was not detected. S2Ce exhibited approximately three times higher radiopacity (9.0 mm aluminum thickness equivalent) compared to the commercial MTA (p < 0.05). These findings suggest that S2Ce is a possible component for hydraulic endodontic cement that demonstrates a rapid setting and high radiopacity.

1. Introduction

Mineral trioxide aggregate (MTA) has been used in pulp capping and retrograde filling and as a perforation repair material since the early nineties [1,2], owing to its remarkable capacity to induce hard tissue formation at the site of its application, such as in the case of direct pulp capping [3,4,5,6] and after full pulpotomy [7]. The main ingredient of MTA is tricalcium silicate (3CaO·SiO2: C3S), which is detectable in low contrast in X-ray radiography [8]. Therefore, heavy element oxides are added to commercial MTA cements to improve radiopacity. Bismuth oxide is a typical radiopacifier additive to MTA, which constitutes approximately 20% of the MTA composition [9]. However, the decrease in the compressive strength and tooth discoloration caused by bismuth oxide addition is of concern [10,11,12,13]. Therefore, the development of a novel cement ingredient, which has a high radiopacity and contributes to cement hydration and setting, can enhance the usability of MTA.
Previously, the authors developed strontium aluminate (3SrO·Al2O3: S3A) as a self-setting and radiopaque component for the MTA cement [14]. Strontium is an alkaline earth element like calcium and is naturally present in bones and teeth. Sr ions are rapidly incorporated into tooth hydroxyapatite from the surrounding fluid, and their effects on improving the acid resistance and remineralization have been reported [15,16,17,18,19,20]. In addition, Sr is a heavier element than Ca; therefore, the enhancement of radiopacity is expected [21]. Experimentally derived S3A cement exhibited a radiopacity similar to that of a commercial MTA cement (ProRoot MTA; Dentsply Tursa Dental, Johnson City, TN, USA) without the addition of a radiopacifier. While S3A exhibited a faster setting time, it demonstrated a lower compressive strength compared to commercial MTA. As the main component of endodontic cements, S3A exhibited sufficient radiopacity; however, the compressive strength is not sufficient. A mixture of S3A and C3S, which was the main component of MTA, exhibited an improved compressive strength, but the radiopacity of S3A was reduced to an insufficient level. Therefore, the development of novel cement components that can achieve both higher radiopacity and better mechanical properties than commercial MTA is required.
The synthesis and properties of distrontium cerate (2SrO·CeO2: S2Ce) have been reported for use as a matrix for rare-earth doping phosphors [22,23]. The possibility of using this compound as a component of the dental cement has not yet been investigated. Cerium is a lanthanoid and an adjacent element of lanthanum. Lanthanum oxide is widely used as a contrast agent in dental composite resins. Therefore, a higher radiopacity than that of S3A is expected for S2Ce. Additionally, bioactive effects may be present for both Sr and Ce. For example, CeO2 nanoparticles have been shown to promote the osteogenic differentiation and mineralization of osteoblasts [24], as well as the X-ray irradiation protection for cells by promoting the reduction of the reactive oxygen species [25]. If S2Ce exhibits similar hydration and setting behavior to those of calcium silicate, the main ingredient of MTA, S2Ce would be a promising candidate to improve the radiopacity of MTA cements without adding bismuth oxide.
The aim of this study is to synthesize S2Ce as a cement component that provides sufficient radiopacity, and to investigate the properties of S2Ce in terms of the setting time, compressive strength, relative flowability, and radiopacity.

2. Materials and Methods

2.1. Preparation of S2Ce and Experimental Cements

S2Ce cement was prepared according to a previously reported method [14]. Briefly, strontium hydroxide octahydrate (Sr(OH)2·8H2O; Kanto Chemical Co. Inc., Tokyo, Japan) and cerium carbonate octahydrate (Ce2(CO3)3·8H2O; Kanto Chemical Co. Inc., Tokyo, Japan) were mixed at a molar ratio of 4:1, heated for 2 h at 180 °C to allow the hydration water to evaporate, and ground using an agate mortar. The obtained powder was calcined at 800, 1000, and 1200 °C for 4 h and ground again in the agate mortar. X-ray diffraction (XRD, Miniflex, Rigaku Corp., Tokyo, Japan) was used to identify the crystal phase of the obtained powder at a scanning speed of 2°/min.
As a representative commercially available MTA product, white ProRoot MTA was used for comparison with the experimental cement.
The S2Ce cement was mixed with distilled water (DW) at water/powder (W/P) ratios from 0.25 to 0.5. ProRoot MTA was mixed with DW at a W/P ratio of 0.33, according to the instructions of the manufacturer.

2.2. Scanning Electron Microscopy (SEM) Observation

The microstructure of the S2Ce powder and the cement specimen cured at 37 °C with 100% relative humidity (RH) for 28 d after mixing were observed using SEM (TM4000Plus, Hitachi High-Technologies Corp., Tokyo, Japan); the observation was performed under an acceleration voltage of 15 kV and magnification of 1000.

2.3. Setting Time Evaluation

The setting time was determined according to the ISO 9917-1 (2007) specifications. The cement mixture was filled into a plastic mold with an inner diameter of 10 mm and a height of 2 mm placed in a sealed container and maintained at 37 °C with 100% RH. Each specimen was subjected to an indentation test using a Vicat needle (diameter: 1 mm) with a mass of 400 g. Indentations were made periodically until the needle failed to create a complete circular indentation in the cement. The setting time was calculated as the time elapsed from the beginning of cement mixing to the absence of indentation. Three replicates of each material were tested, and the results were averaged.

2.4. Compressive Strength Evaluation

The compressive strength was determined according to the ISO 9917-1 (2007) specifications. The cement mixture was filled into a separable cylindrical stainless-steel mold with inner dimensions of 4 mm diameter and 6 mm height. The mold was then covered on both sides with glass plates and maintained at 37 °C with 100% RH. The specimens were divided into two groups. One half was kept for 1 d, and the other half was kept for 28 d. After the given period, the specimen was carefully removed from the mold and its diameter and height were measured using a screw micrometer (QuantuMike series 293; Mitutoyo Corporation, Kawasaki, Japan). The compressive strengths were determined using a universal testing machine (EZ-LX, Shimadzu Corporation, Kyoto, Japan) at a test speed of 0.75 mm/min. Five replicates for each material were tested, and the results were averaged.

2.5. Relative Flowability

To estimate the rheological behavior of S2Ce cement, the relative flowability was evaluated according to a previously reported method [26]. A total of 0.06 g of powder for each cement was mixed with DW at the corresponding W/P ratio. The mixture was placed on a glass slab using a plastic ring of 6 mm diameter and 1 mm thickness. A precision balance (AG245, Mettler Toledo, Greifensee, Switzerland) was used to measure the mass of the cement. After removing the ring, a second glass slab was placed on top of the cement, and a weight of 1 kg was applied for 60 s at room temperature (24 °C). The surface of the spread cement was then digitized using a flat-bed scanner (ApeosPort-IV C3375, Fuji Xerox, Tokyo, Japan) at a resolution of 600 dpi, and the surface area was calculated using an image analysis software (ImageJ, Ver. 1.52K, National Institute of Health, Bethesda, MD, USA). The relative flowability was calculated as follows:
R e l a t i v e   F l o w a b i l i t y = a r e a   ( mm 2 ) w e i g h t   o f   p a s t e   ( g ) .
Five replicates of each material were tested, and the results were averaged.

2.6. Ion Dissolution from Cured Cement

The mixed cement specimen was filled into a plastic mold with an inner diameter of 10 mm and a height of 2 mm and cured in a sealed container maintained at 37 °C with 100% RH for 24 h. After curing, the cement-filled mold was immersed in 10 mL of DW in a sealed plastic container and kept for 1 and 3 d, respectively. The immersed solution was centrifuged at 3000 rpm and filtered with a syringe filter (pore diameter of 0.2 μm; Advanced Microdevices Pvt. Ltd., Ambala Cantt, India) to remove the cement particles. Then, the solutions were used for the analysis of dissolved ion concentrations. Sr and Ce contents were quantified using inductively coupled plasma atomic emission spectroscopy (ICP-AES: Spectro Arcos, Hitachi High-technologies, Tokyo, Japan). Sr (1000 ppm, Nacalai Tesque Inc., Kyoto, Japan) and Ce (1000 ppm, FUJIFILM Wako Pure Chemical Corp., Osaka, Japan) standard solutions were used as standard solutions for ICP-AES analyses.

2.7. Radiopacity

Radiopacity was estimated according to the ISO 6876 (2012) specifications. Disk-shaped specimens with the thickness of 0.4–0.5 mm were fabricated by filling the cement mixture into plastic molds. The thicknesses of the specimens were measured with a screw micrometer. The specimens and an aluminum step wedge (with a thickness of 1–10 mm) were placed on an X-ray imaging plate and exposed to X-rays with a dental X-ray equipment (MaxiX, Morita Corp., Kyoto, Japan) under the following conditions: voltage of 70 kV, current of 7 mA, exposure time of 0.63 s, and 15 cm distance between the imaging plate and cone end. An imaging plate reader (Carestream CS 7600, Carestream Health Japan Co., Ltd., Tokyo, Japan) was used to obtain the radiographs. The mean grey value (MGV) of the specimen was determined using image analysis software (ImageJ, Ver. 1.52K, National Institute of Health, Bethesda, MD, USA), and the aluminum thickness equivalent was calculated by normalizing the specimen thickness. Three replicates of each material were tested.

2.8. Statistical Analysis

One-way analysis of variance (ANOVA), followed by Tukey’s post-hoc test, was used to analyze the compressive strengths of samples with different W/P ratios after 1 d or 28 d from cement mixing. The compressive strengths of 1 d and 28 d samples at different W/P ratios were analyzed by an F-test followed by a t-test. The radiopacity of S2Ce and MTA was also analyzed by an F-test followed by a t-test. One-way ANOVA followed by the Dunnett post-hoc test was used to analyze the flowability of samples with different W/P ratios, and samples with a W/P ratio of 0.3, which showed the lowest flowability among the analyzed samples, were used as controls. The statistical significance was set at p < 0.05.

3. Results

3.1. XRD Analysis and Setting Time of the Synthesized S2Ce Powder

The XRD pattern of the synthesized S2Ce powder is shown in Figure 1. All observed peaks could be assigned to those of the S2Ce for the powders calcined at temperatures higher than 1000 °C. The powder calcined at 800 °C exhibited peaks assigned to SrCO3 and CeO2, indicating that the reaction of these two components did not occur. Thus, calcination temperatures higher than 1000 °C are necessary for S2Ce synthesis. Therefore, the powder calcined at 1200 °C was used in the following studies. The setting time of S2Ce was 121 ± 8 min at a W/P ratio of 0.4.

3.2. SEM Observation

Figure 2 shows the SEM images of S2Ce powders (a) and the cement after 28 d curing with W/P = 0.4 (b). The S2Ce powders consisted of small primary particles of a few μm in diameter and secondary particles, which had irregular shapes with sizes up to 20 μm. The S2Ce cement showed that small precipitates were filled among the resource particles.

3.3. Compressive Strength

The compressive strength evaluated for the S2Ce cement prepared with various W/P ratios at 1 d and 28 d after mixing is shown in Figure 3. After 1 d curing, specimens mixed with the 0.25 W/P ratio exhibited a significantly lower compressive strength than those mixed with the 0.30 W/P ratio. The mixture prepared at 0.25 W/P ratio had low flowability. Therefore, the preparation of test specimens by filling the mixture densely into the metal mold was challenging. Thus, the prepared specimens might have contained defects that resulted in the low compressive strength. The compressive strength was not significantly different in specimens mixed with the W/P ratio of 0.30–0.40. However, specimens mixed with the W/P ratio of 0.45–0.50 exhibited lower values than those mixed with the W/P ratio of 0.40. Specimens mixed after 28 d with the W/P ratio of 0.30–0.40 exhibited lower compressive strengths compared to those mixed after 1 d with the same W/P ratio.

3.4. Relative Flowability

Figure 4 shows the relative flowability of S2Ce cements mixed with various W/P ratios. The cement paste mixed with the 0.25 W/P ratio did not spread, and its flowability was not measurable. The flowability was improved by increasing the W/P ratio, and values similar to those of MTA presented in our previous report [14] were obtained at ratios ≥ 0.45.

3.5. Ion Dissolution from the Cured Cement

As shown in Table 1, the Sr concentration in the surrounding water, leached from the S2Ce cement mixed with the W/P ratio = 0.4, was 5.27 mg/mL (195 mM) after 1 d of immersion, and the concentration did not significantly increase after 3 d of immersion. In contrast, Ce was not detected at both 1 d and 3 d of immersion. Therefore, Sr rapidly and selectively dissolved into the surrounding water in the early stage and the water would be almost saturated with Sr ion.

3.6. Radiopacity

The S2Ce cement sample (W/P = 0.4) with a thickness of 0.4–0.5 mm exhibited a similar radiographic contrast, compared to the commercial MTA cement (ProRoot MTA) with a thickness of 1.1 mm, as shown in Figure 5a. The normalized Al thickness equivalence of the S2Ce cement was 9.0 ± 0.4 mm, which was roughly three times higher than that of the commercial MTA cement.

4. Discussion

Tricalcium silicate (C3S), the main ingredient of MTA, exhibits X-ray absorption properties similar to those of the tooth [8]. Therefore, heavy element oxides (e.g., bismuth oxide) are added as radiopacifiers. However, some negative effects of bismuth oxide, including tooth discoloration and setting deterioration, have been reported [10,11,12,13]. Therefore, we investigated an alternative cement component consisting of a heavier element complex oxide. In a previous study [14], we reported that S3A exhibited a radiopacity similar to that of commercial MTA (ProRoot MTA), while the compressive strength of S3A was not satisfactory for use as the main ingredient of the cement. In this study, we developed a novel component, S2Ce, which consisted of heavier element oxides than S3A, and its properties were investigated.
S2Ce was successfully synthesized from strontium hydroxide and cerium carbonate by calcination at 1200 °C. Compared to the calcination temperature of Portland cement, which is typically 1400–1500 °C, S2Ce could be synthesized at lower temperatures. The experimental S2Ce powders had larger particle sizes and irregular shapes, similar to the previously developed S3A powders [14].
In a previous study, we reported a setting time of 90.7 min for S3A and 153 min for C3S, the main ingredient of MTA [14]. In this study, the setting time of S2Ce was shorter (121 ± 8 min). Thus, Sr-containing complex oxides would exhibit a shorter setting time compared to calcium silicate-based cement ingredients. A long setting time of 261 min [27] has been reported for commercial MTA (ProRoot MTA) and is considered a major drawback of this material. The shorter setting time of S2Ce might help to shorten the setting time of MTA.
The compressive strength of S2Ce mixed with W/P = 0.4 achieved 72.1 MPa after 1 d of maturation, as shown in Figure 3. The compressive strength of commercial MTA (ProRoot MTA) is reported as 27.41 MPa after 1 d [28], and it increases to 86.02 MPa after 28 d [29]. Therefore, S2Ce exhibited fast setting, and a higher compressive strength was achieved after 1 d post mixing. However, S2Ce exhibited a significant reduction in the compressive strength at 28 d after mixing in samples with W/P ratios between 0.3 and 0.4, which could be associated with certain degradation during the curing period, such as the dissolution behavior. Thus, a fast setting is expected for S2Ce, while an improvement in stability is desirable for this material.
The relative flowability of the S2Ce mixture was similar to that of commercial MTA (ProRoot MTA) with W/P ratios ≥ 0.45. However, the compressive strength was low in those W/P ratios, and the flowability with W/P = 0.4, which is the optimum condition to obtain best compressive strength, was quite lower than that of commercial MTA. In this study, S2Ce powders were prepared through manual grinding by using an agate mortar. Therefore, coarse granules with irregular shapes resulted in low flowability.
The dissolution behavior could be considered as one of the reasons that the compressive strength of S2Ce decreased after 28 d of maturation. The solubility of strontium oxide in water is reported to be 6.9 mg/mL for cold water (30 °C), while cerium oxide is reported to be insoluble in water [30]. As shown in Table 1, the Sr content in the immersed water was 5.27 mg/mL after 1 d immersion that was close to the above solubility limit. Therefore, Sr dissolved rapidly in the surrounding water until saturation. In contrast, Ce has no solubility in water; therefore, only Sr dissolved selectively. This rapid dissolution of Sr considerably decreased the compressive strength after 28 d, which was maintained at 37 °C and 100% RH. The specimens were not in direct contact with the liquid water, while the condensed water from the vapor on the specimen surface might wash out Sr selectively; thus, the cement would possibly be weakened.
The effect of extraction solution from S3A on mouse dental papilla cells was studied to elucidate the effect of Sr released from the cement. The extraction solution containing Sr and Al ions exhibited higher mineralized nodule formation and mRNA expression of bone morphogenic protein 2, osteocalcin, and osteopontin than those of the MTA extract [31]. Therefore, a similar pro-mineralization effect could be expected for S2Ce cement, which we will investigate in future studies.
The flowability of the S2Ce cement (Figure 4) was lower than those of S3A and commercial MTA in a previous report [14]. Even with the largest W/P ratio (0.5), the flowability of the S2Ce cement was lower than that of the commercial MTA (W/P = 0.33) achieved in the previous report. The large particle size and irregular shape of S2Ce are the main reasons for the low flowability. Flowability is one of the important factors that dominate the handling properties of cement. Therefore, further studies on the particle size and shape control are required.
Regarding the radiopacity, as shown in Figure 5, the S2Ce cement exhibited three times higher contrast on X-ray radiography compared to the commercial MTA (ProRoot MTA), which contained bismuth oxide as the contrast agent. The typical dental X-ray emission spectrum, operated at 80 kV, has a spectrum peak at 34 keV, and the full width half maximum is approximately at 23 to 58 keV [32]. Therefore, the irradiated X-ray contains a higher energy X-ray component than that at 40 keV. The X-ray absorption by the atoms exhibits the discontinuous increase at certain energies called “absorption edges;” therefore, most efficient absorption occurs just above the absorption edges. The absorption edge energy is an atom characteristic. The absorption edge energies of the K-shell electrons of Sr and Ce are 16.1 and 40.4 keV, respectively [30]. Therefore, Sr exhibits high absorption for X-rays with energies of 16 keV or more; however, high-energy X-rays at energies higher than 40 keV are easily transmitted. In contrast, the K-edge of Ce is close to the spectrum peak of typical dental X-ray emission; therefore, Ce efficiently absorbs the higher energy component of the irradiated X-ray. This is the reason for the high radiopacity of S2Ce.
In this study, we synthesized S2Ce and demonstrated the feasibility of using it as a component of MTA. S2Ce exhibited a fast setting time as well as a high initial compressive strength. The radiopacity of S2Ce cement was approximately three times higher than that of the commercial MTA. Therefore, S2Ce could be considered a novel component for the hydraulic endodontic cement that provides both fast self-setting and radiopacity. The release rate of Sr ion from S2Ce cement was high; therefore, a bioactive effect might be expected for the released Sr ion. However, Sr dissolution is related to the hydrolysis of the cement and subsequent decrease in the compressive strength; thus, long-term in vivo stability is a concern. The relative flowability of S2Ce cement was lower than that of the commercial MTA, and this could be attributed to the large and irregularly shaped S2Ce particles. Therefore, improvement of particle shape and size control is required. Considering these properties, S2Ce could not be expected to be a main component of MTA. However, it can be used as an additive that exhibits fast self-setting and highly radiopaque properties.
Future studies should focus on improving the long-term stability and flowability of S2Ce cement by modifying the particle size and shape of S2Ce powders. Adhesion properties of S2Ce cement should also be studied as the adhesion between MTA and other restoration materials is weak [33]. Additionally, the biological effect of the Sr ion released from S2Ce cement should be investigated via in vitro and in vivo studies.

5. Conclusions

In this study, S2Ce was synthesized from strontium hydroxide and cerium carbonate by calcination at 1200 °C. S2Ce exhibited a faster setting time than commercial MTA (ProRoot MTA). In addition, it showed a higher compressive strength at 1 d after mixing than that of the commercial MTA. However, the compressive strength decreased for S2Ce after 28 d post mixing. Therefore, a fast setting and fast increase in the compressive strength could be expected for S2Ce, while its degradation is a property that requires further refinement.
S2Ce exhibited a large dissolution of Sr ions in water, but dissolution was not detected for Ce. This large dissolution is related to the decrease in the compressive strength of S2Ce. The radiopacity of S2Ce was three times higher than that of commercial MTA. Therefore, S2Ce is a possible cement component that provides a fast-setting time and sufficient radiopacity. Further studies are required to improve the long-term stability, particle shape, and size control as well as to investigate the potential biological effects.

Author Contributions

Conceptualization, M.U. and T.O.; methodology, K.D., M.U.; T.W. and H.W.; validation, M.U.; investigation, K.D., S.A., T.W. and N.K.; data curation, K.D., N.K. and M.U.; writing—original draft preparation, K.D. and M.U.; writing—review and editing, T.O., C.P. and T.K.; visualization, T.W. and N.K.; supervision, M.U. and T.O.; project administration, M.U. and T.O.; funding acquisition, M.U. and T.O. All authors have read and agreed to the published version of the manuscript.

Funding

This research was Supported by a Grant-in-Aid from the Japan Society for the Promotion of Science (JSPS No. 20H03869). A part of this work was also supported by the Global Public Leadership Program from the Japan International Cooperation Agency (JICA).

Institutional Review Board Statement

Not Applicable.

Informed Consent Statement

Not Applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

The authors would like to thank Ami Kuribayashi for the radiopacity measurement.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Torabinejad, M.; Hong, C.U.; McDonald, F.; Pitt Ford, T.R. Physical and Chemical Properties of a New Root-End Filling Material. J. Endod. 1995, 21, 349–353. [Google Scholar] [CrossRef]
  2. Arens, D.E.; Torabinejad, M. Repair of Furcal Perforations with Mineral Trioxide Aggregate: Two Case Reports. Oral Surg. Oral Med. Oral Pathol. Oral Radiol. Endod. 1996, 82, 84–88. [Google Scholar] [CrossRef]
  3. Faraco, I.M.; Holland, R. Response of the Pulp of Dogs to Capping with Mineral Trioxide Aggregate or a Calcium Hydroxide Cement. Dent. Traumatol. 2001, 17, 163–166. [Google Scholar] [CrossRef] [PubMed]
  4. Kuratate, M.; Yoshiba, K.; Shigetani, Y.; Yoshiba, N.; Ohshima, H.; Okiji, T. Immunohistochemical Analysis of Nestin, Osteopontin, and Proliferating Cells in the Reparative Process of Exposed Dental Pulp Capped with Mineral Trioxide Aggregate. J. Endod. 2008, 34, 970–974. [Google Scholar] [CrossRef] [PubMed]
  5. Gandolfi, M.G.; Taddei, P.; Tinti, A.; Prati, C. Apatite-Forming Ability (Bioactivity) of ProRoot MTA. Int. Endod. J. 2010, 43, 917–929. [Google Scholar] [CrossRef] [PubMed]
  6. Torabinejad, M.; Chivian, N. Clinical Applications of Mineral Trioxide Aggregate. J. Endod. 1999, 25, 197–205. [Google Scholar] [CrossRef]
  7. Santos, J.M.; Marques, J.A.; Diogo, P.; Messias, A.; Sousa, V.; Sequeira, D.; Palma, P.J. Influence of Preoperative Pulp Inflammation in the Outcome of Full Pulpotomy Using a Dog Model. J. Endod. 2021, 47, 1417–1426. [Google Scholar] [CrossRef] [PubMed]
  8. Formosa, L.M.; Mallia, B.; Camilleri, J. The Effect of Curing Conditions on the Physical Properties of Tricalcium Silicate Cement for Use as a Dental Biomaterial. Int. Endod. J. 2012, 45, 326–336. [Google Scholar] [CrossRef]
  9. Camilleri, J. The Chemical Composition of Mineral Trioxide Aggregate. J. Conserv. Dent. 2008, 11, 141–143. [Google Scholar] [CrossRef]
  10. Coomaraswamy, K.S.; Lumley, P.J.; Hofmann, M.P. Effect of Bismuth Oxide Radioopacifier Content on the Material Properties of an Endodontic Portland Cement–Based (MTA-Like) System. J. Endod. 2007, 33, 295–298. [Google Scholar] [CrossRef]
  11. Kang, S.H.; Shin, Y.S.; Lee, H.S.; Kim, S.O.; Shin, Y.; Jung, I.Y.; Song, J.S. Color Changes of Teeth After Treatment With Various Mineral Trioxide Aggregate–Based Materials: An Ex Vivo Study. J. Endod. 2015, 41, 737–741. [Google Scholar] [CrossRef] [PubMed]
  12. Palma, P.J.; Marques, J.A.; Santos, J.; Falacho, R.I.; Sequeira, D.; Diogo, P.; Caramelo, F.; Ramos, J.C.; Santos, J.M. Tooth Discoloration after Regenerative Endodontic Procedures with Calcium Silicate-Based Cements-An Ex Vivo Study. Appl. Sci. 2020, 10, 5793. [Google Scholar] [CrossRef]
  13. Camilleri, J.; Borg, J.; Damidot, D.; Salvadori, E.; Pilecki, P.; Zaslansky, P.; Darvell, B.W. Colour and Chemical Stability of Bismuth Oxide in Dental Materials with Solutions Used in Routine Clinical Practice. PLoS ONE 2020, 15, e0240634. [Google Scholar] [CrossRef]
  14. Adel, S.; Wada, T.; Kawashima, N.; Abdou, A.; Watanabe, H.; Kurabayashi, T.; Okiji, T.; Uo, M. Preparation and Properties of Tristrontium Aluminate as an Alternative Component of Mineral Trioxide Aggregate (MTA) Cement. Dent. Mater. J. 2021, 40, 184–190. [Google Scholar] [CrossRef]
  15. Uo, M.; Wada, T.; Asakura, K. Structural Analysis of Strontium in Human Teeth Treated with Surface Pre-Reacted Glass-Ionomer Filler Eluate by Using Extended X-Ray Absorption Fine Structure Analysis. Dent. Mater. J. 2017, 36, 214–221. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  16. Ogawa, A.; Wada, T.; Mori, Y.; Uo, M. Time Dependence of Multi-Ion Absorption into Human Enamel from Surface Prereacted Glass-Ionomer (S-PRG) Filler Eluate. Dent. Mater. J. 2019, 38, 707–712. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  17. Dedhiya, M.G.; Young, F.; Higuchi, W.I. Mechanism for the Retardation of the Acid Dissolution Rate of Hydroxyapatite by Strontium. J. Dent. Res. 1973, 52, 1097–1109. [Google Scholar] [CrossRef]
  18. Featherstone, J.D.B.; Shields, C.P.; Khademazad, B.; Oldershaw, M.D. Acid Reactivity of Carbonated Apatites with Strontium and Fluoride Substitutions. J. Dent. Res. 1983, 62, 1049–1053. [Google Scholar] [CrossRef]
  19. Spets-Happonen, S.; Luoma, H.; Seppä, L.; Räisänen, J. The Effect of Different Strontium Concentrations on the Efficacy of Chlorhexidine-Fluoride-Strontium Gel in Preventing Enamel Softening in Vitro. Arch. Oral Biol. 1993, 38, 107–112. [Google Scholar] [CrossRef]
  20. Thuy, T.T.; Nakagaki, H.; Kato, K.; Hung, P.A.; Inukai, J.; Tsuboi, S.; Nakagaki, H.; Hirose, M.N.; Igarashi, S.; Robinson, C. Effect of Strontium in Combination with Fluoride on Enamel Remineralisation in Vitro. Arch. Oral Biol. 2008, 53, 1017–1022. [Google Scholar] [CrossRef]
  21. Shahid, S.; Hassan, U.; Billington, R.W.; Hill, R.G.; Anderson, P. Glass Ionomer Cements: Effect of Strontium Substitution on Esthetics, Radiopacity and Fluoride Release. Dent. Mater. 2014, 30, 308–313. [Google Scholar] [CrossRef] [PubMed]
  22. Suriyamurthy, N.; Panigrahi, B.S.; Venkatraman, B.; Natarajan, V. Studies on Optical Properties of Blue Emitting Sr2CeO4 Phosphor Prepared Through Combustion Synthesis. J. Opt. 2012, 41, 48–53. [Google Scholar] [CrossRef]
  23. Gupta, S.K.; Sahu, M.; Krishnan, K.; Saxena, M.K.; Natarajan, V.; Godbole, S.V. Bluish White Emitting Sr2CeO4 and Red Emitting Sr2CeO4:Eu3+ Nanoparticles: Optimization of Synthesis Parameters, Characterization, Energy Transfer and Photoluminescence. J. Mater. Chem. C 2013, 1, 7054–7063. [Google Scholar] [CrossRef]
  24. Zhou, G.; Gu, G.; Li, Y.; Zhang, Q.; Wang, W.; Wang, S.; Zhang, J. Effects of Cerium Oxide Nanoparticles on the Proliferation, Differentiation, and Mineralization Function of Primary Osteoblasts In Vitro. Biol. Trace Elem. Res. 2013, 153, 411–418. [Google Scholar] [CrossRef] [PubMed]
  25. Wang, C.; Blough, E.; Dai, X.; Olajide, O.; Driscoll, H.; Leidy, J.W.; July, M.; Triest, W.E.; Wu, M. Protective Effects of Cerium Oxide Nanoparticles on MC3T3-E1 Osteoblastic Cells Exposed to X-Ray Irradiation. Cell. Physiol. Biochem. 2016, 38, 1510–1519. [Google Scholar] [CrossRef] [PubMed]
  26. Kang, D.; Wada, T.; Uo, M.; Okiji, T. Influence of Bentonite Addition on the Handling and Physical Properties of Tricalcium Silicate Cement. Asian. Pac. J. Dent. 2018, 18, 37–44. [Google Scholar]
  27. Choi, Y.; Park, S.J.; Lee, S.H.; Hwang, Y.C.; Yu, M.K.; Min, K.S. Biological Effects and Washout Resistance of a Newly Developed Fast-Setting Pozzolan Cement. J. Endod. 2013, 39, 467–472. [Google Scholar] [CrossRef]
  28. Hwang, Y.C.; Kim, D.H.; Hwang, I.N.; Song, S.J.; Park, Y.J.; Koh, J.T.; Son, H.H.; Oh, W.M. Chemical Constitution, Physical Properties, and Biocompatibility of Experimentally Manufactured Portland Cement. J. Endod. 2011, 37, 58–62. [Google Scholar] [CrossRef]
  29. Islam, I.; Chng, H.K.; Yap, A.U. Comparison of the Physical and Mechanical Properties of MTA and Portland Cement. J. Endod. 2006, 32, 193–197. [Google Scholar] [CrossRef]
  30. Weast, R.C.; Astle, M.J.; Beyer, W.H. CRC Handbook of Chemistry and Physics, 69th ed.; CRC Press Inc.: Boca Raton, FL, USA, 1989; pp. B68–B146, E189–B194. [Google Scholar]
  31. Adel, S.; Hashimoto, K.; Kawashima, N.; Wada, T.; Uo, M.; Okiji, T. Biocompatibility and Pro-mineralization Effect of Tristrontium Aluminate Cement for Endodontic Use. J. Dent. Sci. 2022; in press. [Google Scholar]
  32. Ozaki, Y.; Watanabe, H.; Kurabayashi, T. Effective Dose Estimation in Cone-Beam Computed Tomography for Dental Use by Monte-Carlo Simulation Optimizing Calculation Numbers Using a Step-and-Shoot Method. Dentomaxillofac. Radiol. 2021, 50, 20210084. [Google Scholar] [CrossRef] [PubMed]
  33. Palma, P.J.; Marques, J.A.; Falacho, R.I.; Vinagre, A.; Santos, J.M.; Ramos, J.C. Does Delayed Restoration Improve Shear Bond Strength of Different Restorative Protocols to Calcium Silicate-Based Cements? Materials 2018, 11, 2216. [Google Scholar] [CrossRef] [PubMed] [Green Version]
Figure 1. XRD pattern of S2Ce powders calcined at various temperatures.
Figure 1. XRD pattern of S2Ce powders calcined at various temperatures.
Materials 15 00284 g001
Figure 2. SEM images of S2Ce powder (a) and S2Ce cement (W/P = 0.4) at 28 d after mixing (b).
Figure 2. SEM images of S2Ce powder (a) and S2Ce cement (W/P = 0.4) at 28 d after mixing (b).
Materials 15 00284 g002
Figure 3. Compressive strengths of S2Ce cements after 1 d and 28 d from cement mixing. Columns with different letter(s) (lower case (a–d) for 1 d group and capitals (A–D) for 28 d group) are significantly different (p < 0.05). Asterisk (*) represents significant differences between the 1 d and 28 d maturing periods of the samples with the same W/P ratio.
Figure 3. Compressive strengths of S2Ce cements after 1 d and 28 d from cement mixing. Columns with different letter(s) (lower case (a–d) for 1 d group and capitals (A–D) for 28 d group) are significantly different (p < 0.05). Asterisk (*) represents significant differences between the 1 d and 28 d maturing periods of the samples with the same W/P ratio.
Materials 15 00284 g003
Figure 4. Relative flowability of the S2Ce cement paste mixed with various W/P ratios. Result of MTA was derived from a previous report [14]. Columns with different letter(s) (a–c) are statistically different (p < 0.05).
Figure 4. Relative flowability of the S2Ce cement paste mixed with various W/P ratios. Result of MTA was derived from a previous report [14]. Columns with different letter(s) (a–c) are statistically different (p < 0.05).
Materials 15 00284 g004
Figure 5. (a) Digital radiographs of S2Ce and MTA cement specimens and an Al step-wedge. Numbers in the photo show the thickness of the specimens. (b) Radiopacity values of cements are presented as Al thickness equivalent (mm). Asterisk (*) represents significant difference between S2Ce and MTA (p < 0.05).
Figure 5. (a) Digital radiographs of S2Ce and MTA cement specimens and an Al step-wedge. Numbers in the photo show the thickness of the specimens. (b) Radiopacity values of cements are presented as Al thickness equivalent (mm). Asterisk (*) represents significant difference between S2Ce and MTA (p < 0.05).
Materials 15 00284 g005
Table 1. Dissolved ion concentrations from S2Ce cement (W/P = 0.4) after 1 d and 3 d immersion.
Table 1. Dissolved ion concentrations from S2Ce cement (W/P = 0.4) after 1 d and 3 d immersion.
Species1 d3 d
Sr5.27 ± 0.15 mg/mL
(195 ± 5.5 mM)
5.68 ± 0.23 mg/mL
(211 ± 8.8 mM)
Cenot detectednot detected
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Dumrongvute, K.; Adel, S.; Wada, T.; Kawashima, N.; Piyachon, C.; Watanabe, H.; Kurabayashi, T.; Okiji, T.; Uo, M. Distrontium Cerate as a Radiopaque Component of Hydraulic Endodontic Cement. Materials 2022, 15, 284. https://doi.org/10.3390/ma15010284

AMA Style

Dumrongvute K, Adel S, Wada T, Kawashima N, Piyachon C, Watanabe H, Kurabayashi T, Okiji T, Uo M. Distrontium Cerate as a Radiopaque Component of Hydraulic Endodontic Cement. Materials. 2022; 15(1):284. https://doi.org/10.3390/ma15010284

Chicago/Turabian Style

Dumrongvute, Kunlanun, Sherif Adel, Takahiro Wada, Nobuyuki Kawashima, Chinalai Piyachon, Hiroshi Watanabe, Tohru Kurabayashi, Takashi Okiji, and Motohiro Uo. 2022. "Distrontium Cerate as a Radiopaque Component of Hydraulic Endodontic Cement" Materials 15, no. 1: 284. https://doi.org/10.3390/ma15010284

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop