Next Article in Journal
Investigation of Polyaniline and a Functionalised Derivative as Antimicrobial Additives to Create Contamination Resistant Surfaces
Previous Article in Journal
Hot Deformation Behavior and a Two-Stage Constitutive Model of 20Mn5 Solid Steel Ingot during Hot Compression
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Laser-Aided Directed Energy Deposition of Steel Powder over Flat Surfaces and Edges

Department of Industrial Engineering, University of Salerno, 84084 Fisciano, Italy
*
Author to whom correspondence should be addressed.
Materials 2018, 11(3), 435; https://doi.org/10.3390/ma11030435
Submission received: 30 January 2018 / Revised: 6 March 2018 / Accepted: 13 March 2018 / Published: 16 March 2018

Abstract

:
In the framework of Additive Manufacturing of metals, Directed Energy Deposition of steel powder over flat surfaces and edges has been investigated in this paper. The aims are the repair and overhaul of actual, worn-out, high price sensitive metal components. A full-factorial experimental plan has been arranged, the results have been discussed in terms of geometry, microhardness and thermal affection as functions of the main governing parameters, laser power, scanning speed and mass flow rate; dilution and catching efficiency have been evaluated as well to compare quality and effectiveness of the process under conditions of both flat and edge depositions. Convincing results are presented to give grounds for shifting the process to actual applications: namely, no cracks or pores have been found in random cross-sections of the samples in the processing window. Interestingly an effect of the scanning conditions has been proven on the resulting hardness in the fusion zone; therefore, the mechanical characteristics are expected to depend on the processing parameters.

1. Introduction

To prevent replacement of high-price sensitive metal products such as turbine blades, rotor shafts, tools and moulds, Additive Manufacturing is growing [1,2]. The driving idea is to provide additional metal over worn-out surfaces to restore nominal dimensions, thus preventing part disposal.
In this framework, a number of laser-based methods have been employed in demanding environments such as aerospace, defense, petrolchemical and nuclear industries [3,4]. In Directed Energy Deposition (DED), a laser beam is used as a heat source to scan the surface: a melting pool over an existing substrate is created and metal impinging of the pool is fed concurrently (i.e., in single stage processing) [5]. A deposited metal trace results, with metallurgical bonding to the substrate thanks to fusion and diffusion. Resistance metallic coatings can be laid [6]; functionally graded material parts can be manufactured by means of a dual powder feeding system [7]; and the fabrication of a 3D part is even possible by means of layer-by-layer deposition of consecutive, overlapping traces [8]. Reduction of waste is benefited in comparison with subtractive technologies [9]. Different names have been given to the same technology, depending on the Authors or the company [10].
In general, a number of advantages are reported in DED with respect to conventional welding technologies for repairing, such as tungsten inert gas or gas metal arc [5,11]. As focused heat is provided, thermal affection and residual stresses are reduced, and precision and production flexibility are enhanced [3]. New opportunities are hence expected for parts of complex geometry and difficult-to-cut materials [12].
At present, both powder and wire are being considered as feedstock. It is worth noting that metallic wires are considered to be easier to stock and to produce in comparison with powder [13]; on the other hand, process stability, proper surface quality, bonding strength and soundness are reported to be challenging [14]. Since powder feeding has been proven to be flexible in materials [15], as well as robust and effective, several studies in the literature have discussed the outcome as a function of the processing parameters [16,17].
Regarding steel deposition in the form of powder, the influence of the particle size distribution on the resulting relative density has been investigated [18]. Interestingly, since the cost of metal powder is among the main barriers in DED, the feasibility of a raw feedstock consisting of coarse and irregular steel swarf or chips resulting from machining has been proposed [19].
Clad thickness, depth of penetration and extent of the heat-affected zone (HAZ) are governed by the main parameters such as the laser power, the scanning speed and the specific energy of the beam [5,6]. In addition, depending on the carbon content and irrespective of the feedstock form [20], martensitic transformation occurs in the base metal [21], i.e., the microstructure morphology in terms of grain size and the mechanical properties in turn [22] have been found to definitely depend on solidification velocity and the temperature gradient as a consequence of the processing parameters [23], mainly the scanning speed [10]. The latter has been reported to significantly influence dilution [3], i.e., the percentage index of the affection of the substrate with respect to the reported metal [11]. Minor porosity and micro-cracking have been observed [6] due to residual thermal stresses, although these are not deemed to result in rejection of parts during quality checks when referring to usual international or customer standards for quality in laser welding [24], since no specific regulations are available at present for DED [25].
It is worth noting that, as for any emerging technology in the industry [26,27], flexible thermal modeling is crucial to prevent the usual trial-and-error approach. Indeed, much effort has been made in the literature to model the process of DED in terms of resulting geometry and induced thermal cycles [28].
Numerous studies have been conducted over flat surfaces. These results are suitable for actual applications in repair process chains, where damaged areas or cracks are preliminarily removed by milling, then reconditioned with new material deposition [29]. Nevertheless, processing of sharp edges is required to be investigated as well, since this processing configuration is expected to be useful in many applications, e.g., for the purpose of overhauling cores and mould sections for investment casting. As a consequence, deposition over both flat surfaces and corners has been considered in this paper.

2. Materials and Methods

A base metal corresponding to standard UNS S43100 chromium-nickel stainless steel in terms of nominal chemical composition (Table 1) has been considered. Pre-alloyed, spherical shaped, gas-atomized virgin commercial powder of the same composition has been used; the particle size ranges from 20 µm to 60 µm. Since a steady feeding rate must be provided consistently [11], the powder has been preliminary dried, in furnace, 180 °C, 2 h, to flow properly via an antistatic conveyor to the working area.
To perform DED, a deposition line (Figure 1) is required, and a number of base components must be arranged [25], irrespective of the form of the feedstock supply. For the purpose of this work, a fibre-delivered Yb:YAG disc laser source, operating in continuous wave emission (Table 2), has been considered. The movement of the laser head has been accomplished by a 6-axis industrial robot with a dedicated controller, and an in-built 3-way feeding nozzle has been moved with the laser head (Figure 2); the base metal has been provided by a powder feeder with oscillating conveyor.
Argon has been supplied: it has been injected with each stream of powder as a carrier gas at a flow rate of 3 L/min; it has been blown coaxially to the laser beam at a flow rate of 10 L/min as a shielding gas over the melting pool. A tilting angle of 4° has been set for the laser head, in agreement with common practice to process high-reflective metals [30] to prevent back-reflections from entering the optics train. A given positive defocusing providing a processing laser beam diameter of 3 mm on the substrate has been set, thus benefiting from reduced irradiance and increased catchment of powder in the melting pool with respect to a focused condition.
The main processing factors of the experimental plan have been selected based on the literature and past experience: namely, laser power P, scanning speed s and powder feeding rate m′ have been considered. Two levels for each factor have been set upon preliminary trials and adjusted to result in valuable outcomes, preventing detachment, balling, lack of clad or excessive dilution. A full-factorial, 3-factor, 2-level experimental plan has been arranged (Figure 3); eight deposition conditions have resulted (Table 3) and have been performed over both flat surfaces and edges. A total deposition length of 100 mm has been set. A 0.3 mm beveled edge has been produced by machining prior to deposition to resemble an actual condition of wear. Three runs have been planned for each processing condition in random order. The geometry has been evaluated upon cross-cutting and mechanical preparation; three samples from each trace have been considered, the results have been averaged to assess the statistical significance. Polishing to mirror finish and chemical etching with a solution consisting of 5% nitric acid and 95% ethanol at room temperature [31] have eventually been performed.
In agreement with common practice in DED, a number of geometrical responses in the cross-sections have been measured using conventional optical microscopy. Namely, in case of deposition over flat surfaces (Figure 4a): width w, height h, depth d, shape angle α at both sides of the trace, areal extent Ah and Ad of the deposition above and below the reference plane, respectively. In case of deposition over edges (Figure 4b): height h1 and h2 with respect to the reference planes, areal extent Ah and Ad of the deposition outside and inside the theoretical edge, respectively.
Dilution has been considered as well: Although a chemical definition is usually given involving the weight percentage composition of the main alloying elements in the substrate with respect to the reported metal [11], it has been shown that an alternative geometric definition can be given [32]; namely, the ratio of the fused (i.e., mixing) area of the substrate to the total area in the transverse cross-section can be measured. Therefore, dilution in this paper has been evaluated as:
d i l u t i o n = A d A h + A d [ % ]
Moreover, the catching efficiency η has been rated as a measure of the process effectiveness [11]: the ratio of the deposited metal md to the total amount of delivered powder mt in the processing time has been evaluated. The higher this ratio, the better the efficiency, since a larger amount of powder is caught by the fused pool.
In practice, the mass of deposited metal has been found by mere weighing of the samples, whereas the total mass of delivered powder has been found based on the flow rate m′ and the deposition time td to provide the trace length L:
η = m d m t = m d m × t d = m d m × L s [ % ]
Eventually, Vickers microhardness testing has been performed to assess the extent of the HAZ between the fusion zone and base material, as well as to discuss the microstructural changes upon deposition; an indenting load of 0.2 kg has been used for a dwell period of 10 s, a step of 200 μm has been allowed between consecutive indentations, in compliance with the usual ISO standard [33] for hardness testing of metallic materials.

3. Results and Discussion

3.1. Deposition over Flat Surfaces

3.1.1. Geometry

Since all of the processing conditions of the experimental plan resulted in a valuable outcome (Table 4), all of them can be effectively considered and discussed (Table 5); the catching efficiency has been rated as well.
No cracks or pores have been found. Interesting findings can be drawn based on multifactor trends of the geometrical responses. At first, width w increases for increasing power and decreasing speed (Figure 5); therefore, any increase in thermal input (i.e., the power to speed ratio) yields a corresponding increase in trace width, in agreement with past research on DED of metals [25]; the shape angle is affected, accordingly. The effect of the feeding rate is not significant with respect to trace width; hence, one may infer the attenuation of the laser beam due to powder blowing [11] is negligible in the investigating domain.
On the other hand, a considerable dependence on the powder feeding rate has been found for both the trace height h (Figure 6) and the transverse areal extent of reported metal Ah (Figure 7), as expected: namely, a 50% increase in delivered powder results in the same increase in transverse size of the reported metal; the catching efficiency is not affected. Since the fusion zone below the reference plane is negligible with respect to the fusion zone above, the same trends have been found when considering the total size of fusion area. As an additional consequence, dilution is mainly governed by Ah and rather approaches its inverted trend (Figure 8). It is worth noting that although limited dilution below 10% results in some of the processing conditions, the process is expected to be successful thanks to diffusion bonding [25].
The approximation of certain transverse profiles for the fused area Ah above the reference plane has been addressed in the literature [8,34] to provide assistance to modelling. Namely, an approximation for Ah can be given by a parabolic or circular segment. The effectiveness of these has been further investigated here, based on the real measurements in the cross-section (Table 5). A comparison has been made (Table 6): interestingly, the parabolic approximation is effective in a measure of 5.6% on average, although the circular segment is affected by a 6.4% average absolute mismatch. The result is relevant to real applications: a geometric model, as simple as a parabolic profile, is useful when a processing strategy for consecutive, and overlapping traces must be set to properly scan wider surfaces or manufacture a real part [8].

3.1.2. Micro-Hardness

In order to give a full description of the outcome upon DED, the mechanical properties have been investigated by means of Vickers micro-hardness testing. All of the processing conditions have been addressed, and random cross-sections have been indented; hence, the trend of micro-hardness has been evaluated as a function of the distance from the top surface of the reported metal (Figure 9). Based on this, the average hardness in two sites of interest (i.e., the reported metal and the HAZ) can be discussed as a function of the processing parameters (Table 7); it is worth noting that larger standard deviations result in the HAZ with respect to the reported metal as a consequence of ranging in a wider window.
Interestingly, hardness in the fusion zone is clearly governed by the processing conditions because the cooling rate is affected, and the resulting microstructure and grain size in turn, in agreement with similar findings in the referred literature [10,22,23]. Indeed, an increase of hardness has been found ranging from 270 HV0.2 to 450 HV0.2 in the fusion zone, depending on the processing conditions, with respect to a reference 115 HV0.2 in the parent metal. Power is deemed to exert the main effect, whereas any dependence on the feeding rate is not significant; as a consequence, the response surfaces for hardness have been averaged for each given condition of power and speed (Figure 10).
When this approach is taken to draw the response surface, the resulting hardness in the HAZ appears to be unaffected by the processing conditions. Nevertheless, the extent of the HAZ can be inferred (Table 8) based on the distance to recover the reference hardness in the parent metal. As expected, larger HAZs have been found when a higher thermal input is provided (Figure 11), i.e., when a lower processing speed is set. Again, any dependence on the flow rate is weak.

3.2. Deposition over Edges

3.2.1. Geometry

All of the processing conditions of the experimental plan resulted in a valuable outcome over edges as well (Table 9). It is worth noting that a proper metal allowance must be provided in order to result in effective addition of metal upon eventual post processing machining when a sharp edge is recovered. The shape in the cross-section and the corresponding dilution and catching efficiency have been considered (Table 10). Due to the peculiar shape of the reported metal in the cross-section, approximations via a parabolic or circular segment profile are prevented. Further studies are planned to find a proper geometric approximation to set the processing path.
As for deposition over flat surfaces, no cracks or pores have been found. Again, a 50% increase in delivered powder results in a comparable increase in the transverse size of reported metal (Figure 12). The overall geometry depends on the thermal input. Nevertheless, as a consequence of a different shape of the substrate, the catchment is affected: in general, a reduction of 20% on average results in the catching efficiency, as a consequence of the powder flow impinging an edge instead of a flat surface. Conversely, dilution is increased up to 58%, although the same trend is observed (Figure 13), approximately, with respect to deposition over flat surfaces, since the amount of reported metal is reduced due to the edge.

3.2.2. Micro-Hardness

Regarding the mechanical properties of the reported metal, the trend of Vickers micro-hardness has been evaluated along a 45°-tilted path with respect to the theoretical edge, starting from the trace top (Figure 14). Dependence on the processing conditions is considered (Table 11, Figure 15), although higher hardness has been measured for each given processing condition with respect to the same condition of deposition over flat surfaces. Again, one may infer the cooling rate in case of deposition over edges is affected, thus resulting in different microstructure and grain size in the fusion zone. Aimed at to a real application, the proper condition of processing must be selected based on the damage to be addressed; an approach of optimization to take account of a number of requirements, both geometrical and mechanical with specific weights depending on the application, is suggested in the literature [25].

4. Conclusions

The effectiveness of the process of Directed Energy Deposition has been addressed over both flat surfaces and edges, aimed at real applications where coating or overhauling for the purpose of restoring the nominal dimensions is required. Convincing findings have been achieved.
Namely, a proper processing window has been found to perform the process over UNS S43100 chromium-nickel stainless steel. Based on the application, the proper condition must be selected in a multi-constraint optimization approach. Nevertheless, a number of main findings can be given here:
  • the approximation of a parabolic profile in the cross-section is suitable in case of flat deposition; hence, a simple description is benefited when setting a proper deposition strategy for overlapping, multi-layer traces at the pre-processing stage;
  • no cracks or pores are produced in random cross-sections of the samples in the suggested processing window;
  • the catching efficiency depends on the processing parameters; half the amount of the total delivered powder is effectively deposited on average for both flat and edge depositions;
  • dilution, hence the affection of the parent metal, is mainly governed by the thermal input and is increased when moving from flat to edge deposition as a consequence of modified thermal exchange.
Tensile and fatigue strengths are expected to depend on the processing condition of deposition. Dependence of the Vickers microhardness on the thermal input has been found.

Author Contributions

Both authors conceived and designed the experiments, analyzed the data, and wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Graf, B.; Ammer, S.; Gumenyuk, A.; Rethmeier, M. Design of experiments for laser metal deposition in maintenance, repair and overhaul applications. Procedia CIRP 2013, 11, 245–248. [Google Scholar] [CrossRef]
  2. Song, J.; Qilin, D.; Changyuan, C.; Hu, D.; Yongtang, L. Rebuilding of metal components with laser cladding forming. Appl. Surf. Sci. 2006, 252, 7934–7940. [Google Scholar] [CrossRef]
  3. Segerstark, A.; Andersson, J.; Svensson, L. Investigation of laser metal deposited Alloy 718 onto an EN 1.4401 stainless steel substrate. Opt. Laser Technol. 2017, 97, 144–153. [Google Scholar] [CrossRef]
  4. Brandl, E.; Baufeld, B.; Leyens, C.; Gault, R. Additive manufactured Ti-6Al-4V using welding wire: comparison of laser and arc beam deposition and evaluation with respect to aerospace material specification. Phys. Procedia 2010, 5, 595–606. [Google Scholar] [CrossRef]
  5. Steen, W.; Mazumder, J. Laser Material Processing; Springer: London, UK, 2010. [Google Scholar]
  6. Rahman Rashid, R.; Abaspour, S.; Palanisamy, S.; Matthews, N.; Dargush, M. Metallurgical and geometrical characterisation of the 316L stainless steel clad deposited on a mild steel substrate. Surf. Coat. Technol. 2017, 327, 174–184. [Google Scholar] [CrossRef]
  7. Kadekar, V.; Prakash, S.; Liou, F. Experimental investigation of laser metal deposition of functonally graded copper and steel. In 2004 Solid Freeform Fabrication; University of Texas Press: Austin, TX, USA, 2004. [Google Scholar]
  8. Ocelik, V.; Nenadl, O.; Palavra, A.; De Hosson, T. On the geometry of coating layers formed by overlap. Surf. Coat. Technol. 2014, 242, 54–61. [Google Scholar] [CrossRef]
  9. Gibson, I.; Rosen, D.; Stucker, B. Additive Manufacturing Technologies; Springer: London, UK, 2015. [Google Scholar]
  10. Zhang, K.; Wang, S.; Shang, X. Characterization of stainless steel parts by Laser Metal Deposition Shaping. Mater. Des. 2014, 55, 104–119. [Google Scholar] [CrossRef]
  11. Toyserkani, E.; Khajepour, A.; Corbin, S. Laser Cladding; CRC Press: Boca Raton, FL, USA, 2005. [Google Scholar]
  12. Artetxe, E.; González, H.; Calleja, A.; Valdivielso, A.; Polvorosa, R.; Lamikiz, A.; Lacalle, N.L.D.L. Optimised methodology for aircraft engine IBRs five-axis machining process. Int. J. Mechatron. Manuf. Syst. 2016, 9, 385. [Google Scholar] [CrossRef]
  13. Demir, A. Micro laser metal wire deposition for additive manufacturing of thin-walled structures. Opt. Lasers Eng. 2018, 100, 9–17. [Google Scholar] [CrossRef]
  14. Abioye, T.; Folkes, J.; Clare, A. A parametric study of Inconel 625 wire laser deposition. J. Mat. Process. Technol. 2013, 213, 2145–2151. [Google Scholar] [CrossRef]
  15. Boussaha, E.; Aouici, S.; Bahloul, A.; Sahour, M.C. Optimization of geometrical features of laser cladding obtained by powder injection. Phys. Procedia 2009, 2, 1147–1152. [Google Scholar] [CrossRef]
  16. Riveiro, A.; Mejias, A.; Lusquinos, F.; Del Val, J.; Comesana, R.P.J.; Pou, J. Laser cladding of aluminium on AlSi 304 stainless steel with high-power diode lasers. Surf. Coat. Technol. 2014, 253, 214–220. [Google Scholar] [CrossRef]
  17. Grigoriev, S.; Tarasova, T.; Gvozdeva, G.; Nowotny, S. Solidification behaviour during laser microcladding of Al-Si alloys. Surf. Coat. Technol. 2015, 268, 303–309. [Google Scholar] [CrossRef]
  18. Hentschel, O.; Scheitler, C.; Fedorov, A.; Junker, D.; Gorunov, A.; Haimerl, A.; Merklein, M.; Schmidt, M. Experimental investigations of processing the hig carbon cold-work tool steel 1.2358 by laser metal deposition for the additive manufacturing of cold forging tools. J. Laser Appl. 2017, 29, 022307. [Google Scholar] [CrossRef]
  19. Mahmood, K.; Khan, A.; Pinkerton, A. Laser Metal Deposition of steel components using machine waste as build material. In Proceedings of the Conference on Lasers and Electro-Optics, CLEO 2011, Baltimore, MD, USA, 1–6 May 2011. [Google Scholar]
  20. Xu, X.; Mi, G.; Luo, Y.; Jiang, P.; Shao, X.; Wang, C. Morphologies, microstructures and mechanical properties of samples produced using laser metal deposition with 316L stainless steel wire. Opt. Lasers Eng. 2017, 94, 1–11. [Google Scholar] [CrossRef]
  21. Adeyemi, A.; Akinlabi, E.; Mahamood, R.; Sanusi, K.; Pityana, S.; Tlotleng, M. Influence of laser power on microstructure of laser metal deposited 17-4 PH stainless steel. Mater. Sci. Eng. 2017, 225. [Google Scholar] [CrossRef]
  22. Ma, M.; Wang, Z.; Zeng, X. A comparison on metallurgical behaviors of 316L stainless steel by selective laser melting and laser cladding deposition. Mater. Sci. Eng. A 2017, 685, 265–273. [Google Scholar] [CrossRef]
  23. Fang, J.; Dong, S.; Wang, Y.; Xu, B.; Zhang, Z.; Xia, D.; Ren, W.; He, P. Microstructure and properties of an as-deposited and heat treated martensitic stainless steel fabricated by direct laser deposition. J. Manuf. Process. 2017, 25, 402–410. [Google Scholar] [CrossRef]
  24. AWS D17. 1M:2017. Specification for Fusion Welding for Aerospace Applications; American Welding Society: Miami, FL, USA, 2017. [Google Scholar]
  25. Caiazzo, F.; Alfieri, V.; Argenio, P.; Sergi, V. Additive manufacturing by means of laser-aided directed metal deposition of 2024 aluminium powder: Investigation and optimization. Adv. Mech. Eng. 2017, 9, 1–12. [Google Scholar] [CrossRef]
  26. Ukar, E.; Lamikiz, A.; Lopez De Lacalle, L.; Del Pozo, D.; Liebana, F.; Sanchez, A. Laser polishing parameter optimisation on selective laser sintered parts. Int. J. Mach. Machinab. Mater. 2010, 8, 417–432. [Google Scholar] [CrossRef]
  27. Mackwood, A.; Crafer, R. Thermal modelling of laser welding and related processes: a literature review. Opt. Laser Technol. 2005, 37, 99–115. [Google Scholar] [CrossRef]
  28. Ya, W.; Pathiraj, B.; Liu, S. 2D modelling of clad geometry and resulting thermal cycles during laser cladding. J. Mater. Process. Technol. 2016, 230, 217–232. [Google Scholar] [CrossRef]
  29. Graf, B.; Gumenyuk, A.; Rethmeier, M. Laser metal deposition as repair technology for stainless steel and titanium alloys. Phys. Procedia 2012, 39, 376–381. [Google Scholar] [CrossRef]
  30. Alfieri, V.; Caiazzo, F.; Sergi, V. Autogenous laser welding of AA2024 aluminium alloy: process issues and bead features. In Proceedings of the 9th Conference on Intelligent Computation in Manufacturing Engineering (CIRP ICME 2014), Capri, Italy, 23–25 July 2014. [Google Scholar]
  31. Davis, J.R. Aluminum and Aluminum Alloys; ASM International: Materials Park, OH, USA, 1993. [Google Scholar]
  32. Abbas, G.; West, D. Laser surface cladding of stellite and stellite-SiC composite deposits for enhanced hardness and wear. Wear 1991, 143, 353–363. [Google Scholar] [CrossRef]
  33. International Organization for Standardization (ISO). E.I. 6507-1. Metallic Materials-Vickers Hardness Test—Part 1: Test Method; ISO: Geneva, Switzerland, 2005. [Google Scholar]
  34. Cao, Y.; Zhu, S.; Liang, X.; Wang, W. Overlapping model of beads and curve fitting of bead section for rapid manufacturing by robotic MAG welding process. Robot. Comput. Integr. Manuf. 2011, 27, 641–645. [Google Scholar] [CrossRef]
Figure 1. Main components in the deposition line.
Figure 1. Main components in the deposition line.
Materials 11 00435 g001
Figure 2. Laser head performing DED over a flat surface.
Figure 2. Laser head performing DED over a flat surface.
Materials 11 00435 g002
Figure 3. Testing scheme, full-factorial, 3-factor, 2-level plan.
Figure 3. Testing scheme, full-factorial, 3-factor, 2-level plan.
Materials 11 00435 g003
Figure 4. Scheme of the cross-section resulting from deposition (a) over flat surface and (b) edge.
Figure 4. Scheme of the cross-section resulting from deposition (a) over flat surface and (b) edge.
Materials 11 00435 g004
Figure 5. Trace width w as a function of the governing variables; flat deposition.
Figure 5. Trace width w as a function of the governing variables; flat deposition.
Materials 11 00435 g005
Figure 6. Trace height h as a function of the governing variables; flat deposition.
Figure 6. Trace height h as a function of the governing variables; flat deposition.
Materials 11 00435 g006
Figure 7. Transverse areal extent of reported metal Ah as a function of the governing variables; flat deposition.
Figure 7. Transverse areal extent of reported metal Ah as a function of the governing variables; flat deposition.
Materials 11 00435 g007
Figure 8. Dilution as a function of the governing variables; flat deposition.
Figure 8. Dilution as a function of the governing variables; flat deposition.
Materials 11 00435 g008
Figure 9. Example of the trend of Vickers micro-hardness under condition F; flat deposition.
Figure 9. Example of the trend of Vickers micro-hardness under condition F; flat deposition.
Materials 11 00435 g009
Figure 10. Example of the trend of Vickers micro-hardness in condition F; flat deposition.
Figure 10. Example of the trend of Vickers micro-hardness in condition F; flat deposition.
Materials 11 00435 g010
Figure 11. Extent of the HAZ as a function of the processing conditions; flat deposition.
Figure 11. Extent of the HAZ as a function of the processing conditions; flat deposition.
Materials 11 00435 g011
Figure 12. Transverse extent of reported metal Ah as a function of the governing variables; edge deposition.
Figure 12. Transverse extent of reported metal Ah as a function of the governing variables; edge deposition.
Materials 11 00435 g012
Figure 13. Dilution as a function of the governing variables; edge deposition.
Figure 13. Dilution as a function of the governing variables; edge deposition.
Materials 11 00435 g013
Figure 14. Example of the trend of Vickers microhardness under condition F; edge deposition.
Figure 14. Example of the trend of Vickers microhardness under condition F; edge deposition.
Materials 11 00435 g014
Figure 15. Average Vickers micro-hardness in the deposited metal; edge deposition.
Figure 15. Average Vickers micro-hardness in the deposited metal; edge deposition.
Materials 11 00435 g015
Table 1. Nominal chemical (wt.%) composition of base and fed metals.
Table 1. Nominal chemical (wt.%) composition of base and fed metals.
CrNiMnSiCPSFe
15.0 ÷ 17.01.25 ÷ 2.501.01.00.200.040.03Balanced
Table 2. Main technical features of the laser source.
Table 2. Main technical features of the laser source.
ParameterValue
Maximum output power (kW)4.0
Operating nominal wavelength (nm)1030
Beam Parameter Product (mm × mrad)8.0
Core diameter of the delivering fibre (µm)300
Spot size of the laser beam on the surface (mm)3.0
Table 3. Processing condition of the experimental plan for deposition over flat surface and edges.
Table 3. Processing condition of the experimental plan for deposition over flat surface and edges.
ConditionP (kW)s (mm∙s−1)m′ (g∙min−1)
A1200129
B12001218
C1200169
D12001618
E1500129
F15001218
G1500169
H15001618
Table 4. Trace surface aspect and corresponding cross-section for deposition over a flat surface.
Table 4. Trace surface aspect and corresponding cross-section for deposition over a flat surface.
ConditionTrace AspectCross-Section
A Materials 11 00435 i001 Materials 11 00435 i002
B Materials 11 00435 i003 Materials 11 00435 i004
C Materials 11 00435 i005 Materials 11 00435 i006
D Materials 11 00435 i007 Materials 11 00435 i008
E Materials 11 00435 i009 Materials 11 00435 i010
F Materials 11 00435 i011 Materials 11 00435 i012
G Materials 11 00435 i013 Materials 11 00435 i014
H Materials 11 00435 i015 Materials 11 00435 i016
Table 5. Average geometrical responses in the cross section for deposition over a flat surface.
Table 5. Average geometrical responses in the cross section for deposition over a flat surface.
Conditionw (mm)h (mm)d (mm)Ah (mm2)Ad (mm2)α (°)Dilution (%)η (%)
A2.730.600.141.070.16351356
B2.491.320.032.380.0874360
C2.420.470.020.720.0637850
D1.931.190.041.770.0276160
E3.170.540.231.180.44312762
F3.151.020.142.230.26481056
G3.070.400.200.760.47203853
H2.880.750.101.450.17461049
Table 6. Comparison between real and approximated fused area above the reference plane in the cross-section.
Table 6. Comparison between real and approximated fused area above the reference plane in the cross-section.
ConditionActual Ah (mm2)Parabolic Approx. (mm2)Mismatch (%)Circular Approx. (mm2)Mismatch (%)
A1.071.091.91.135.6
B2.382.19−8.02.6210.1
C0.720.765.60.788.3
D1.771.53−13.61.928.5
E1.181.14−3.41.17−0.8
F2.232.14−4.02.313.6
G0.760.827.90.839.2
H1.451.44−0.71.524.8
Table 7. Average Vickers micro-hardness as a function of the processing conditions; flat deposition.
Table 7. Average Vickers micro-hardness as a function of the processing conditions; flat deposition.
ConditionReported MetalHAZ
HV0.2Std. dev.HV0.2Std. dev.
A29724.216950.3
B30119.516236.3
C3117.717551.9
D27223.916326.1
E39624.617351.7
F41025.616444.2
G4213.518165.2
H4424.219069.8
Table 8. Average extent of the HAZ as a function of the processing conditions; flat deposition.
Table 8. Average extent of the HAZ as a function of the processing conditions; flat deposition.
ConditionABCDEFGH
HAZ extent (mm)2.202.052.032.022.542.402.501.90
Table 9. Trace surface aspect and corresponding cross-section for deposition over edges.
Table 9. Trace surface aspect and corresponding cross-section for deposition over edges.
ConditionTrace AspectCross-Section
A Materials 11 00435 i017 Materials 11 00435 i018
B Materials 11 00435 i019 Materials 11 00435 i020
C Materials 11 00435 i021 Materials 11 00435 i022
D Materials 11 00435 i023 Materials 11 00435 i024
E Materials 11 00435 i025 Materials 11 00435 i026
F Materials 11 00435 i027 Materials 11 00435 i028
G Materials 11 00435 i029 Materials 11 00435 i030
H Materials 11 00435 i031 Materials 11 00435 i032
Table 10. Average geometrical responses in the cross section for deposition over edges.
Table 10. Average geometrical responses in the cross section for deposition over edges.
Conditionh1 (mm)h2 (mm)Ah (mm2)Ad (mm2)Dilution (%)η (%)
A0.350.390.840.413344
B0.940.711.740.15844
C0.270.320.550.333838
D0.670.570.900.06630
E0.410.340.981.355851
F0.870.622.180.381555
G0.300.380.690.715148
H0.570.581.390.271647
Table 11. Average Vickers micro-hardness as a function of the processing conditions; edge deposition.
Table 11. Average Vickers micro-hardness as a function of the processing conditions; edge deposition.
ConditionReported MetalHAZ
HV0.2Std. dev.HV0.2Std. dev.
A52710.917742.2
B59727.518256.2
C5185.217951.4
D58919.019477.5
E43512.417243.8
F57611.016737.3
G4386.218756.8
H44065.718644.7

Share and Cite

MDPI and ACS Style

Caiazzo, F.; Alfieri, V. Laser-Aided Directed Energy Deposition of Steel Powder over Flat Surfaces and Edges. Materials 2018, 11, 435. https://doi.org/10.3390/ma11030435

AMA Style

Caiazzo F, Alfieri V. Laser-Aided Directed Energy Deposition of Steel Powder over Flat Surfaces and Edges. Materials. 2018; 11(3):435. https://doi.org/10.3390/ma11030435

Chicago/Turabian Style

Caiazzo, Fabrizia, and Vittorio Alfieri. 2018. "Laser-Aided Directed Energy Deposition of Steel Powder over Flat Surfaces and Edges" Materials 11, no. 3: 435. https://doi.org/10.3390/ma11030435

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.