Structure and Luminescent Characteristics of Y1−xEuxNbO4 (x = 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.4) Ceramic Solid Solutions

,
,
and
Tananaev Institute of Chemistry—Subdivision of the Federal Research Centre, Kola Science Centre of the Russian Academy of Sciences, 184209 Apatity, Russia
*
Author to whom correspondence should be addressed.

Abstract

This study focuses on Y1−x EuxNbO4 (x = 0.01–0.40) ceramic solid solutions. The precursor powders were obtained via a liquid-phase route, and the final ceramics were fabricated using conventional ceramic processing (conventional sintering). Using full-profile X-ray diffraction analysis of polycrystals, the phase composition was determined and the structural parameters of solid solution phases were refined as a function of Eu concentration. The morphological features of the microstructure of Y1−xEuxNbO4 ceramics were studied. The visible photoluminescence of Y1−xEuxNbO4 was systematically characterized. The emission spectra for all compositions are dominated by electric dipole 5D0 → 7F2 transition of Eu3+, peaking at ~613 nm. The effects of excitation wavelength (λex = 275, 392, 463, and 535 nm) and Eu content on the efficiency of energy transfer were examined. It was revealed that the concentration quenching of photoluminescence depended on the excitation energy, and at x > 0.2 multipole energy transfer between Eu3+ cations dominated due to the critical distances RC for Y0.8Eu0.2NbO4 was 8.9 Å.

1. Introduction

Orthoniobates of rare-earth elements (RENbO4) are widely recognized as superior host matrices for luminescent activators such as Sm3+, Eu3+, and Yb3+. This suitability stems from the specific electronic interaction between the RE3+ ions and the NbO43− anionic groups [1]. These materials are characterized by exceptional photostability, significant Stokes shifts, and spectrally narrow emission lines spanning from the UV to the NIR regions.
Therefore, these luminescent materials have found wide application [2] in solid-state white light-emitting diodes (LEDs) [3], X-ray displays, lasers, scintillation detectors of ionizing radiation, optical telecommunications, security inks, anti-counterfeiting labels [4], probes for luminescent immunoassays and sensitizers for photodynamic therapy [5].
Yttrium orthoniobate (YNbO4) is one of the most promising crystalline hosts for doping with rare-earth elements (REEs), as it possesses a favorable combination of structural stability and moderate phonon energy, and has non-centrosymmetric crystal sites, which contribute to intense luminescence. Monoclinic structure with the space group C/2c of YNbO4 provides a low-symmetry coordination environment for the activator ions, which enhances electric dipole transitions (for example, 5D0 → 7F2 transition in Eu3+). It, thereby, ensures the high color purity of phosphor. These features make YNbO4 particularly relevant material for applications in solid-state lighting and optical thermometry, where both radiative efficiency and spectral resolution are critically important.
Orthoniobates, such as GdNbO4, YbNbO4, ErNbO4, LuNbO4, and LaNbO4, are also studied for the activation of REEs. Similar hosts with a fergusonite structure have both strengths and limitations. For example, GdNbO4 exhibits strong self-activated luminescence, but its higher phonon energies often increase the rate of non-radiative relaxation, reducing quantum efficiency, especially at high temperatures [6,7,8].
LuNbO4 has a denser lattice and potentially higher thermal stability. However, the smaller ionic radius of Lu3+ can cause lattice deformation when doped with larger REE cations, which leads to defect formation, high electron–phonon interactions, and the activation of luminescence quenching mechanisms [9].
LaNbO4, being chemically stable, tends to crystallize in phases with higher site symmetry, which weakens electric dipole transitions and reduces the intensity of hypersensitive transitions [10].
Furthermore, in the Y3+ cation, in comparison with the Gd3+, Er3+, and Yb3+ ones, there are no transitions in the near-ultraviolet region which would partially absorb the excitation energy from the activator cations (Eu3+, Sm3+, Tb3+, …) and intrinsic luminescent centers [11,12].
Study of the YNbO4 host is highly relevant. For example, in Ref. [13] the host is doped by Ho3+, Tm3+, Yb3+ in order to study up- and down-conversion luminescence. For thermoluminescence applications, the host was doped with Bi, La, Dy, and Eu [14]. For the same applications, authors doped YNbO4 with other ions (Pr and Tb) [15]. For the study of luminescent properties in thin films based on the fergusonite YNbO4 host, authors [16] activated it with Nd, Sm, Eu. The structural, electronic and optical properties were investigated based on the density functional theory (DFT) in fergusonite-type structures [17].
In particular, the activation of YNbO4 by europium is of particular interest. In this work [18], Eu3+ ion together with bismuth (Bi3+) forms a dual-emitting center to create an optical thermometer. Eu3+ ion is a red-emitting activator that creates highly efficient red phosphors suitable for use in lighting devices, displays and, in particular, anti-counterfeiting inks [19]. In this study [20], Eu3+ ion serves as a model activator for the systematic study of its spectroscopic properties and the application of Judd-Ofelt theory over a wide concentration range (from 0.1 to 20 mol%). This fundamental spectroscopic study aims to understand the evolution of optical parameters with increasing Eu3+ concentrations.
Trivalent lanthanide ions that activate RENbO4 exhibit remarkable luminescent properties. The reason for this is the rich structure of energy levels in 4f configurations [21]. For luminescent inorganic materials RENbO4:RE3+, the sensitization process occurs as a result of non-radiative transfer of excitation energy from a rare earth ion, which behaves as an energy donor (sensitizer), to another rare earth ion, which behaves as an energy acceptor (activator). The absorption and emission spectra of 4f intraconfiguration transitions of RE3+ cations retain their atomic character to a greater or lesser extent, and this does not depend on the crystal host [22]. The 4f–4f transitions of RE3+ ions are realized either due to electric dipole or magnetic dipole interactions. Magnetic dipole transitions are parity-allowed, while electric dipole transitions are parity-forbidden, according to the Laporte rule. However, for these transitions, the Laporte rule is slightly relaxed: the reason lies in the mixing of electron configurations with different parities. The bias is caused by the odd components of the non-centrosymmetric ligand field. Furthermore, it has been shown that ligand polarization effects are of great importance for the 4f–4f transitions of RE3+ cations [22].
For example, Eu3+ (4f6) ions have relatively large energy gaps between the excited and ground states. Complexes of these ions usually exhibit strong luminescence since the excited energy levels of the ion are just below the triplet state of the ligand. In systems containing more than one electron in the 4fn orbital, such as the Eu3+ (4f6) ion [20,22], the degeneracy of the 4fn configuration is partially or completely lifted under the influence of several perturbing factors. The factors affecting the RE3+ ion include electron repulsion, spin–orbit interaction, and ligand field perturbation. Electron repulsion is an electrostatic interaction between different electrons in the 4f subshell. Spin–orbital interaction arises from the interaction of the spin magnetic moment and the orbital magnetic moment of the electron. The ligand field effect is due to the interaction between the 4f electrons and the electrons of the ligands.
When RE3+ ions are placed in inorganic hosts, the spherical symmetry of the free ion is broken. Each spectroscopic level is further split. This occurs under the influence of an asymmetric electric field generated by the chemical environment. This field is called a ligand field or a crystal field. The ligand field effect removes the degeneracy of the levels in the free ion. It depends solely on the symmetry point with respect to the RE3+ ion [22,23]. These levels are known as crystal field levels (or Stark levels).
Thus, the electronic excitation of lanthanide ions in host materials occurs through two mechanisms. The first is resonant energy transfer. The second is non-resonant energy transfer involving phonons as a result of ion–ion interactions [23,24,25,26]. Ions embedded in the host material’s crystal lattice do not have exactly the same energy level in their excited states. This is due to lattice stresses and defects. Because of this, the resulting luminescence is very sensitive to the local coordination environment and the symmetry of the site. In addition, at high concentrations of RE3+ ions in the crystalline host, concentration quenching of their luminescence is observed [26].
This research pursues several key goals: the liquid-phase preparation of finely divided Y1−xEuxNbO4 solid-solution powders; a comprehensive analysis of their phase purity and structural evolution; an investigation into the microstructural and crystallographic development of the ceramic bodies; and a systematic study of the luminescence response as a function of both excitation wavelength and Eu3+ content.

2. Materials and Methods

The synthesis of finely dispersed powders of yttrium orthoniobate doped with Eu with contents of x = 0.01, 0.1, 0.15, 0.2, 0.25, 0.3, 0.4 was carried out using nitrate solutions of REEs and niobium oxide. A high-purity niobium stock solution was prepared by dissolving Nb2O5 (99.9%, Solikamsk Magnesium Plant, Solikamsk, Russia) in concentrated HF (99.9 (not more than 10−5 of 27 impurities), Komponent-reaktiv Ltd., Moscow, Russia), yielding hexafluoroniobic acid (HNbF6):
Nb2O5 + 12HF = 2HNbF6 +5H2O
The subsequent addition of aqueous NH4OH (25%, 99.9 (not more than 10−5 of 23 impurities), Sigma Tek, Russia, Khimki) to this solution, maintaining a pH of 10–11, precipitated hydrated ammonium niobate (NH4)xH3−xNbO4. This precursor was isolated by filtration and thoroughly rinsed with deionized water (solid-to-liquid ratio of 1:3) until fluoride ions were effectively removed. The product was then dried at 90 °C until it reached a moisture level of about 65%.
(6 + x)NH4OH (conc.) + HNbF6 → (NH4)xH3−xNbO4 + 6NH4F+ (2 + x)H2O)
The resulting precipitate was filtered and washed with deionized water. This removed fluoride ions. Washing was performed at a solid-to-liquid ratio of T:Vl = 1:3. The precipitate was then dried at 90 °C to a moisture content of approximately 65%. It was then mixed for 3 h with nitric acid solutions of REEs (Y and Eu). The solid-to-liquid ratio during mixing was T:Vl = 1:1. Nitric acid solutions were obtained by dissolving the calculated amount of REE oxides in nitric acid. The oxides used were Y2O3 and Eu2O3 (99.9% purity, Himkraft, Kaliningrad, Russia). Ammonia was added to the resulting pulp until the pH reached ~10. When a solution of ammonium niobate is mixed with REE nitrate in an alkaline medium (provided by NH4OH), an exchange reaction occurs, resulting in the formation of a sparingly soluble REE orthoniobate. For x = 3 (fully substituted niobate):
(NH4)3NbO4 + RE(NO3)3 →RENbO4↓ + 3NH4NO3
Ammonia water NH4OH performs the function of maintaining an alkaline environment (pH~10), which is necessary so that niobium does not hydrolyze to Nb2O5·H2O. Furthermore, the excess NH4OH ensures the gradual formation of the RENbO4 precipitate, rather than RE(OH)3.
The mixture was stirred for 3 h, after which the precipitate was filtered and washed three times with deionized water to remove ammonium ions. Washing was performed at a T:Vl ratio of 1:(2–3). The precipitate was then dried at 150 °C, calcined at 700 °C for 2 h, and ground in a KM1 chalcedony ball mill (MLW, Leipzig, Germany) for 4 h. Finally, the powders were additionally calcined for 4 h at 1100 °C.
The niobium content in fluoride Nb-containing solutions during the synthesis of Y1−xEuxNbO4 powders was determined gravimetrically. The content of fluoride ions was determined potentiometrically using an EV-74 ion meter with an EVL-1M3 F-selective electrode by potentiometric method on ionomer EV-74 (Zavod izmeritel’nych priborov, Minsk, Belarus) with an F-selective electrode EVL-1MZ (Zavod izmeritel’nych priborov, Minsk, Belarus). Fluorine in the synthesized powders was analyzed using the pyrohydrolysis method. Y and Eu in filtrates and washing solutions were determined by atomic emission spectrometry on an ICPE 9000 spectrometer (Shimadzu, Kyoto, Japan) and when in powders were determined by XRD on a Spectroscan MAKS-GV device (Spectron, Saint Petersburg, Russia).
Chemical analysis confirmed that the residual fluorine content in the calcined powders was negligible, falling below the detection threshold of the pyrohydrolysis method (<1 × 10−3 wt%). Furthermore, the concentrations of Y, Nb, and Eu were found to be stoichiometric, with the analytical results deviating from the nominal values by no more than the standard measurement uncertainty of approximately 1%.
Using conventional sintering (CS), ceramic tablets 10 mm in diameter and 2–3 mm in height were prepared from the resulting powders. Polyvinyl alcohol was used as a binder. The tablets were pressed at a load of ~8.8 kg/cm2. The tablets were sintered in a KEP 14/1400P electric furnace (OOO MZVE, Russia, Saint-Petersburg) at 1400 °C for 4 h.
The phase composition and structure refinement of ceramic samples were performed using a Rigaku multifunctional X-ray diffractometer with SmartLab Studio II(with the program built in the plant) software (RIGAKU, Tokyo, Japan). The counter speed was 2 deg min−1 (CuKα radiation, scanning range 6–90°). The ICDD databases (PDF 4, relies 2022) were used for phase identification. The structural characteristics of the phases were refined using the WPPF (Whole Powder Pattern Fitting) method of full-profile analysis of X-ray diffraction patterns. Atomic coordinates and crystallographic lattice characteristics were entered from the cif files of the International Diffraction Data Center (ICDD) database (PDF 4, relies 2020). The reliability criteria for the obtained results were the values of the profile R-factor (Rp and Rwp) calculated using standard formulas.
X-ray density was calculated using the following formula:
ρ X-ray = 1.66 M V
where M is molecular mass per cell and V is cell volume. The crystallite size in Y1−xEuxNbO4 ceramic solid solutions was estimated from the coherent scattering region (CSR) calculated using the Scherrer equation,
D = 0.941 λ β cos θ
where D is CSR or average crystallite size, λ is wavelength of X-ray radiation (CuKα = 1.5405929 Å), and θ and β are diffraction angle and full width at half maximum (FWHM) of the observed peaks, respectively.
The ceramic microstructure was studied using a LEO 420 SEM scanning electron microscope (Carl Zeiss, Oberkochen, Germany) and analyzed using the program ScanMaster (National research nuclear university (MEPHI), Moscow Engineering Physics Institute, Russia) software. This software is designed for the mathematical processing of these images and for performing measurements on them.
Luminescence and excitation spectra of the studied samples were recorded using an FL970 spectrofluorimeter (Techcomp, Shanghai, China) in the wavelength range of 200–900 nm with ±2 nm resolution. A 150-watt xenon lamp was used as the luminescence excitation source. Edge filters (the cutoff wavelengths were 380 and 420 nm) were used to filter out the excitation band and Raman scattering to study the luminescence properties. The filter was mounted in front of the entrance slit of the monochromator. All used additional units belong to the FL970.

3. Results

3.1. Structure of Ceramic Solid Solutions

The results of X-ray phase analysis showed that all Y1−xEuxNbO4 (x = 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3 and 0.4) compositions crystallize in the monoclinic β-fergusonite phase with the space symmetry group C2/c, Z = 4.00 (ICDD Card 04-021-8433) correspond to the chemical formula Y0.99Eu0.01NbO4, (Figure 1). The array of initial data of X-ray diffraction spectra of samples is given in the Supplementary Materials.
Figure 1. XRD patterns of ceramic Y1−xEuxNbO4 (x = 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3 and 0.4).
The cell parameters of ceramic Y1−xEuxNbO4 refined by the WPPF (Whole Powder Pattern Fitting) method, as well as the X-ray density, are presented in Table 1, and the calculated sizes of the CSR for the directions [22 1 ¯ ], [021], [040], [20 2 ¯ ] and the average crystallite size are shown in Table 2.
Table 1. Refined values of the periods of unit cells of the main phases of Y1−xEuxNbO4 ceramic samples.
Table 2. Average crystallite size for the studied samples.
As can be seen from Table 1, the parameters a, b and c of the monoclinic lattice of the Y1−xEuxNbO4 ceramic samples vary monotonically with the Eu activator content. It should be noted that the ceramic sample with the highest Eu content (x(Eu) = 0.4) contains about 3% of the cubic phase Y3NbO7, with the space symmetry group Fm 3 ¯ m (ICDD Card 01-074-6421) and about 2% Nb2O5 (ICDD Card 04-007-0451).
Figure 2 shows the dependence of the unit cell volume on the europium concentration in Y1−xEuxNbO4 ceramic solid solutions. It is evident that an increase in the proportion of Eu3+ cations in the crystal structure of Y1−xEuxNbO4 leads to an increase in the unit cell volume. This is due to the fact that europium cations, having an ionic radius r(Eu3+) = 1.066 Å [27,28], replace smaller yttrium cations (r(Y3+) = 1.019 Å [27,28]) in distorted oxygen hexahedra (the coordination number of the cation is 8). This should also reduce the proportion of covalence and increase the proportion of ionic bonds in the oxygen polyhedra of the samples’ structures.
Figure 2. Dependence of the unit cell volume on the concentration of europium in a Y1−xEuxNbO4 ceramic solid solution. Filled squares is experimental data. Red curve is an approximating straight line.
The crystallite sizes are nearly isotropic in the calculated crystallographic directions for the studied Y1−xEuxNbO4 samples, with the exception of Y1−xEuxNbO4 (x = 0.1, 0.3 and 0.4). The greatest dispersion of crystallite sizes is 28.7, 38.5 and 21.2 nm for Y0.9Eu0.1NbO4, Y0.7Eu0.3NbO4 and Y0.6Eu0.4NbO4, respectively. In the Y0.8Eu0.2NbO4 sample, the average crystallite size significantly exceeds the average crystallite size of the other samples, Table 2.
In the monoclinic β-fergusonite structure (space symmetry group C2/c, Z = 4), Y is surrounded by 8 oxygen atoms, forming a distorted REEO8 polyhedron (Figure 3). The point symmetry group of the Y3+ cation is C2. Due to the C2 symmetry, the eight REE–O bonds are grouped into four pairs of unequal lengths (see Table 3), which reflects the low symmetry of the monoclinic phase. The REEO8 polyhedra share edges, forming zigzag chains along the c-axis, connected by NbO6 octahedra that share common vertices. When other rare earth ions—as in our case Eu3+—occupy the Y site, the oxygen hexahedron expands, and changes in the distances between the atoms of the crystal host and the dopant will also affect the luminescence properties of the dopant. The distances between the A3+ and B5+ cations and oxygen in Y1−xEuxNbO4 (x = 0.01–0.4) refined using the WPPF method are presented in Table 3.
Figure 3. Distorted oxygen polyhedron and crystal structure of the monoclinic phase Y1−xEuxNbO4.
Table 3. Interatomic distances between cations A3+, B5+ and oxygen in the monoclinic phase of fergusonite Y1−xEuxNbO4.
All distances between Eu and Nb increase successively as the dopant concentration increases, Table 3. The short distances between REE and oxygen decrease over the concentration range x(Eu) = 0.01–0.15. Then, the pattern has a non-monotonic “sawtooth” character in the area x(Eu) = 0.2–0.4. Long distances between REEs increase with increasing Eu concentration up to x(Eu) = 0.25. Then, there is a decrease and increase of this distance at x(Eu) = 0.3–0.4, respectively.

3.2. Morphology of Ceramic Solid Solutions Y1−xEuxNbO4 (x = 0.01–0.40)

Microstructural characterization and grain size evaluation of the studied ceramic samples were carried out using a series of SEM images, Figure 4. Using ScanMaster software for image analysis and mathematical processing, differential grain size distribution curves for Y1−xEuxNbO4 (x = 0.01–0.4) ceramics were obtained. They are shown in the corresponding insets in Figure 4a–h.
Figure 4. Microstructure and grain size distribution in ceramic samples: (a)—Y0.99Eu0.01NbO4; (b)—Y0.95Eu0.05NbO4; (c)—Y0.9Eu0.1NbO4; (d)—Y0.85Eu0.15NbO4; (e)—Y0.8Eu0.2NbO4; (f)—Y0.75Eu0.25NbO4; (g)—Y0.7Eu0.3NbO4; (h)—Y0.6Eu0.4NbO4.
All Y1−xEuxNbO4 (x = 0.01–0.4) ceramic samples consist of grains of similar morphology, with pronounced faceting elements. They are characteristic of this syngony. The grain size in the group of Y1−xEuxNbO4 (x = 0.01–0.25) samples is similar: from ~1.5 to ~20 μm (Figure 4a–f). Y0.7Eu0.3NbO4 ceramics are distinguished by significantly larger grains: from ~10 to ~50 μm (Figure 4g). The Y0.6Eu0.4NbO4 sample with the highest Eu content has the least uniform microstructure containing both large grains of the main phase and grains of a different columnar morphology. The grains apparently belong to the Nb2O5 impurity phase (Figure 4h).

3.3. Photoluminescence Study of Ceramic Solid Solutions Y1−xEuxNbO4 (x = 0.01–0.40)

Figure 5a shows a typical photoluminescence excitation (PLE) spectrum (λem = 613 nm) of the Y0.8Eu0.2NbO4 sample compared to the spectrum of the unactivated YNbO4 ceramic (λem = 440 nm). Figure 5b shows the PLE spectra of Y1−xEuxNbO4 ceramics. The PLE spectrum can be divided into two regions.
Figure 5. (a)—PLE spectra of Y0.8Eu0.2NbO4 (1, λem = 613 nm) and YNbO4 (2, λem = 408 nm) ceramics. (b)—the spectra of Y1−xEuxNbO4 samples for 613 nm emission.
The first region is located in the range from 200 to 350 nm and contains two broad excitation bands (Figure 5). The band at ~275 nm is associated with an optical transition between the 2p orbital of O2− and the 4d orbital of Nb5+ in the individual compound YNbO4. Similar patterns are described in the literature [28]. It should be noted that the presence of Eu in the ceramic lattice should lead to the appearance of a charge transfer band between O2− and Eu3+. There is probably an overlap of transfer bands from different components. The asymmetry of the ~275 nm band is attributed precisely to the O2−–Eu3+ charge transfer [29]. The nature of the band at ~300 nm is associated with charge transfer between Eu3+ and Nb5+ cations; in addition, part of the 4f–4f transitions may also contribute to this region of the spectrum [30].
The second region, from 350 to 580 nm, is associated with relatively narrow excitation bands. They reflect intraconfigurational 4f–4f transitions of the Eu3+ cation. The correlation of excitation bands and the corresponding transitions is presented in Table 4. The bands were determined on the basis of the literature data [20,22,31,32,33], taking into account the combination principle and data from the luminescence spectra.
Table 4. The ratio between excitation bands and cation transitions Eu3+.
Figure 6 shows the dependences of the position and intensity of the excitation band with a maximum at 275 nm on the Eu concentration in Y1−xEuxNbO4 ceramic solid solutions. The maximum excitation band intensity is achieved in the sample with the composition Y0.85Eu0.15NbO4. A further increase in the europium concentration leads to a decrease in the excitation efficiency according to the “host—REE” scheme. As the doping element concentration increases, a consistent shift of this band toward longer wavelengths is observed. As noted earlier, the band at ~275 nm is associated with interband charge transfer from the molecular 2p orbital of O2− to the molecular 4d orbital of Nb5+. Consequently, this band can be connected with the bandgap of YNbO4 and its behavior correlates well with the one of unit cell volume. The former is confirmed by optical measurements and DFT calculations [17]. Increasing the Eu3+ concentration may be accompanied by a decrease in the bandgap of the studied samples. To confirm this, it is necessary to conduct diffuse reflectivity measurements in UV region of samples.
Figure 6. Dependences of the intensity and position of the excitation band at ~275 nm on the concentration of Eu in Y1−xEuxNbO4 ceramic solid solutions.
Figure 7 shows the dependence of the intensity of the excitation bands at 392, 463 and 535 nm on the Eu concentration. These bands correspond to the 5L6, 5D2 ← 7F0, 5D1 ← 7F1 transitions [22].
Figure 7. Dependence of the excitation band intensity on the concentration of Eu3+ in Y1−xEuxNbO4 ceramic solid solutions.
It can be seen that as the Eu concentration increases, a consistent increase in excitation efficiency is initially observed across the three channels, but at x(Eu) > 0.2 it begins to decrease. Excitation at the indicated wavelengths is due exclusively to intraconfigurational 4f–4f transitions of the Eu3+ cation. Each excitation wavelength ensures the transition of the Eu3+ cation from the ground state (7F0) to one of the metastable states (5L6, 5D2 and 5D1). The excited Eu3+ cations then relax to the ground state via optical and non-optical transitions.
As follows from Figure 7, concentration quenching upon excitation in the 463 and 535 nm bands begins already at x(Eu) > 0.15, whereas upon excitation in the 392 nm band, it begins at x(Eu) > 0.2. This indicates that the relaxation mechanisms for two channels (7F0 → 5D2 → … → 5D0 → 7F2 and 7F1 → 5D1 → … → 5D0 → 7F2) are equivalent, while for the third channel (7F0 → 5L6 → … → 5D0 → 7F2) the mechanism is different. Thus, at a concentration of x(Eu) = 0.15 and an excitation wavelength of 392 nm (transition 5L6 ← 7F0), the maximum efficiency of radiation by Eu3+ cations in Y1−xEuxNbO4 ceramic solid solutions is not yet achieved (Figure 7). Thus, the concentration quenching of the Eu3+ cation and luminescence spectra of Y1−xEuxNbO4 ceramics depends on the luminescence excitation wavelength.
Figure 8 shows the photoluminescence (PL) spectra of Y1−xEuxNbO4 (x = 0.01, 0.15, and 0.3) ceramic solid solutions excited at λex = ~275 nm in comparison with the spectrum of unactivated YNbO4. The PL spectra of Y1−xEuxNbO4 ceramics reflect a typical pattern of radiative transitions 5D0 → 7FJ (J = 0, 1, 2, 3 and 4) of the Eu3+ cation in the YNbO4 host [33,34]. The predominance of the band at 613 nm indicates that Eu3+ cations occupy non-centrosymmetric positions in the YO8 polyhedra of the YNbO4 ceramic structure with the point symmetry group C2.
Figure 8. PL spectra of Y1−xEuxNbO4 (x = 0.01, 0.15 and 0.3) and YNbO4 ceramics upon excitation in the charge transfer band (λex ~ 275 nm). The inset shows the dependence of the luminescence intensity on the europium concentration.
At a low concentration of x(Eu) = 0.01, the PL spectrum, in addition to the characteristic bands of the Eu3+ cation, exhibits a broad band peaking at 415 nm due to NbO6 groups. The increase in dopant concentration leads to the disappearance of this band. This indicates complete energy transfer from the host to the Eu3+ cations, and some excited energy dissipates through interaction with lattice phonons. All radiative transitions of Eu3+ occur from the 5D0 level to the 7F term: 5D0 → 7F1 (595 HM), 5D0 → 7F2 (600–625 nm), 5D0 → 7F3 (660 nm), 5D0 → 7F4 (700–714 nm) [22].
The maximum luminescence intensity is observed in the sample with the composition Y0.85Eu0.15NbO4. At x(Eu) > 0.15 the luminescence intensity is decreased by concentration quenching. This is due to the interaction between europium cations, which increases non-radiative transitions.
To clarify the mechanism of energy exchange between interacting identical luminescence centers, an empirical formula is used to calculate the critical distance RC [1,34,35]:
R C = 2 3 V 4 π x c Z 1 / 3
where V is the volume of a unit cell, xc is the concentration at which the maximum value of luminescence intensity is observed, Z is the number of formula units in a unit cell [31,34,35]. Calculations using this formula showed that the distance between interacting luminescence centers at x(Eu) = 0.15 is 9.8 Å for the Y0.85Eu0.15NbO4 sample. This confirms that the energy transfer mechanism is realized through the multipole interaction between the Eu3+ luminescence centers. Initially, at ~275 nm NbO6 absorbs excited energy and, through non-radiative energy transfer, transfers it to Eu3+ cations (Figure 9). At a concentration x(Eu3+) < 0.15, the excited energy is localized on the Eu3+ cation, and emission processes occur at a single luminescence center. Then, when x(Eu) = 0.15, the single Eu3+ cations begin to interact with each other via a multipole mechanism, and the excitation energy starts to migrate through the Eu3+ sites (Figure 9). The subsequent increase in the concentration of x(Eu) leads to active interaction and energy migration to quenching centers, and as a result, the luminescence intensity decreases. According to the table of interatomic distances (Table 4), the Eu-Eu interaction does not occur with the adjacent EuO8 polyhedrons. Consequently, the interaction can occur both within a single unit cell (RC < b) and between two adjacent cells. One study [19] also found RC = 9.8 Å for a concentration of 15 mol% Eu3+. This confirms that the concentration quenching mechanism in YNbO4:Eu3+ is indeed related to multipole (dipole–dipole) interactions, and the critical distance is a characteristic value for this host.
Figure 9. Energy diagram of Y1−xEuxNbO4, where ET—energy transfer and NR—non-radiative transition.
Figure 10 shows the PL spectra of Y1−xEuxNbO4 ceramic solid solutions (x = 0.1, 0.2, and 0.4) excited at λex = ~392 nm. A gradual increase in the Eu concentration in the crystal structure leads to an increase in the luminescence intensity of the 5D0 → 7F2 electric dipole transition and reaches a maximum at x(Eu) = 0.2, (Figure 9). At concentrations above x(Eu) > 0.2, the luminescence intensity drops sharply. This indicates the activation of the quenching mechanism. The absorption and emission of radiation occur locally at a single luminescence center within the unit cell at low dopant concentrations. Increasing the Eu concentration increases the number of such single luminescence centers, resulting in increased luminescence intensity and the initialization of the process of energy transfer between Eu3+ cations. The critical distance RC for Y0.8Eu0.2NbO4 is 8.9 Å. It means that Eu-Eu energy transfer occurs via multipole mechanics. At x(Eu) > 0.2 the decrease in luminescence is observed. This is due to the donor–acceptor interaction between cations, which is made possible by the reduction in the Eu-Eu distance in the Y1−xEuxNbO4 ceramic crystal lattice. It is worth noting that the Y0.8Eu0.2NbO4 sample, compared to other compositions, is characterized by the largest CSR sizes in various crystallographic directions (Table 2).
Figure 10. PL spectra of Y1−xEuxNbO4 ceramic solid solutions (x = 0.1, 0.2 and 0.4) excited via the 5L6 ← 7F0 transition (λex = 392 nm). The inset shows the dependence of the luminescence intensity on the europium concentration.
Consequently, a larger number of single Eu3+ luminescence centers are formed in the Y0.8Eu0.2NbO4 ceramic. These centers interact weakly with defects at the CSR boundaries and adjacent Eu Y defects, resulting in a higher luminescence level. This is observed upon excitation at ~392 nm (Figure 10). Presumably, increasing the size of the CSR shifts the concentration effects toward higher dopant concentrations. At the same time, at other excitation wavelengths, the emission probability decreases. This is due to the fact that concentration quenching in Y1−xEuxNbO4 ceramics begins to manifest itself already at x(Eu) = 0.2 (Figure 8). It can be concluded that relaxation from the 5L6 state of the Eu3+ cation is more “stable” when interacting with other luminescence centers compared to other relaxation channels (Figure 6).

4. Conclusions

Finely dispersed powders of yttrium orthoniobates Y1−x EuxNbO4 (x = 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3 and 0.4) were obtained by liquid-phase synthesis using nitrate solutions.
Ceramic samples of Y1−xEuxNbO4 solid solutions were prepared from synthesized powders using CS technology. The morphological features of the Y1−xEuxNbO4 ceramic microstructure are presented, and coherent scattering regions are calculated. Using the full-profile analysis method of XRD patterns of polycrystals, it was established that all compositions of Y1−xEuxNbO4 (x = 0.01–0.4) solid solutions crystallize in the monoclinic β-fergusonite phase with the space symmetry group C2/c, Z = 4.00 (ICDD Card 04-021-8433).
A combined approach, involving the refinement of lattice parameters and interatomic distances via the WPPF method and a comprehensive PL analysis (λex = 275; 392; 463 and 535 nm), unveiled the concentration-dependent behavior of excitation energy migration among the luminescent centers in the Y1−xEuxNbO4 (x = 0.01–0.4) system.
Based on excitation spectra, it was established that the charge transfer band between the molecular 2p orbital of O2− and the 4d orbital of Nb5+ shifts toward longer wavelengths as the Eu concentration in Y1−xEuxNbO4 ceramics increases. This correlates well with the increase in unit cell volume. It is shown that the most efficient energy transfer via the multipole mechanism in "host-Eu" excitation scheme is achieved in the sample with the composition Y0.85Eu0.15NbO4, and that the luminescence of NbO6 groups does not appear when the non-radiative transfer process dominates. The Eu-Eu transfer is a multipole mechanism, as the critical distance RC is 9.8 Å, calculated from the structure data and the critical concentration (xc). Based on excitation and luminescence spectra, it was established that concentration quenching of europium in Y1−xEuxNbO4 ceramic solid solutions depends on the excitation wavelength. This is due to the relaxation from the 5L6 state of the Eu3+ cation, which is more stable for external interactions. The maximum luminescence intensity is observed in Y0.85Eu0.15NbO4 and Y0.8Eu0.2NbO4 ceramics at λex = 275 nm and 392 nm, respectively. Moreover, the luminescence intensity in the ~613 nm band for Y0.8Eu0.2NbO4 ceramics is almost 2.5 times higher than for Y0.85Eu0.15NbO4 ceramics.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/ceramics9100108/s1.

Author Contributions

Conceptualization—O.S. and M.P.; Methodology—O.S., M.S. and S.M.; Validation—M.S. and O.S.; Investigation—S.M., O.S. and M.S.; Data Curation—M.P. and S.M.; Writing—Original Draft—O.S., M.S. and S.M.; Writing—Review and Editing—O.S. and M.P.; Visualization—O.S. and M.S.; Funding acquisition—M.P.; Resources—O.S.; Supervision—O.S. All authors have read and agreed to the published version of the manuscript.

Funding

This work was financially supported by the Ministry of Science and Higher Education Russian Federation scientific topics FMEZ-2025-0055.

Data Availability Statement

The raw data supporting the conclusions of this article will be made available by the authors on request.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Blasse, G.; Bril, A. Luminescence of phosphors based on host lattices ABO4 (A is Sc, In; B is P, V, Nb). J. Chem. Phys. 1969, 50, 2974–2980. [Google Scholar] [CrossRef] [Scilit]
  2. Sato, M.; Kim, S.W.; Shimomura, Y.; Hasegawa, T.; Toda, K.; Adachi, G. Rare earth-doped phosphors for white light-emitting diodes. Handb. Phys. Chem. Rare Earths 2016, 49, 1–128. [Google Scholar] [CrossRef] [Scilit]
  3. Liu, Y.; Tu, D.; Zhu, H.; Chen, X. Lanthanide-doped luminescent nanoprobes: Controlled synthesis, optical spectroscopy, and bioapplications. Chem. Soc. Rev. 2013, 42, 6924–6958. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Bunzli, J.C.G. Lanthanide luminescence: From a mystery to rationalization, understanding, and applications. Handb. Phys. Chem. Rare Earths 2016, 50, 141–176. [Google Scholar] [CrossRef] [Scilit]
  5. Almeida, A.; Faustino, M.A.F.; Tome, J.P.C. Photodynamic inactivation of bacteria: Finding the effective targets. Futur. Med. Chem. 2015, 7, 1221–1224. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  6. Bouzayani, M.M.; Aydi, S.; Chkoundali, S.; Tliha, M.; Oueslati, A.; Aydi, A. Comprehensive investigation of the structural, dielectric relaxation, and hopping conduction mechanisms in fergusonite RENbO4 (RE = Gd, In) ceramics. Ceram. Int. 2026, 52, 33223–33235. [Google Scholar] [CrossRef] [Scilit]
  7. Wi, S.W.; Lee, Y.S. Effect of Eu3+, Bi3+, and Li+ doping on luminescent property of GdNbO4. J. Rare Earths 2024, 42, 66–75. [Google Scholar] [CrossRef] [Scilit]
  8. Palatnikov, M.N.; Shcherbina, O.B.; Smirnov, M.V.; Deyneko, D.V.; Masloboeva, S.M. Luminescence and mechanical properties of GdNbO4 ceramic phosphors doped by Eu3+, Sm3+, Tb3+, Er3+. J. Alloys Compd. 2025, 1037, 182432. [Google Scholar] [CrossRef] [Scilit]
  9. Sato, H.; Kodama, S.; Yanase, I.; Takeda, H. Photoluminescence properties of solid solutions of YNbO4, GdNbO4 and LuNbO4. J. Ceram. Soc. Jpn. 2025, 133, 353–357. [Google Scholar] [CrossRef] [Scilit]
  10. Shan, Y.J.; Kawaguchi, R.; Akizawa, R.; Tezuka, K. Crystal structure and ionic conductivity of novel rare-earth niobates LnNbO4 (Ln = Nd, Sm, Eu, Gd) by substituting Nb with W. Ionics 2023, 29, 2697–2703. [Google Scholar] [CrossRef] [Scilit]
  11. Zhang, D.-L.; Hua, P.-R.; Cui, Y.-M.; Chen, C.-H.; Pun, E.Y.B. Absorption and emission characteristics of Er3NbO7 phosphor: A comparison with ErNbO4 phosphor and Er:LiNbO3 single crystal. J. Lumin. 2007, 127, 453–460. [Google Scholar] [CrossRef] [Scilit]
  12. Palatnikov, M.N.; Smirnov, M.V.; Masloboeva, S.M.; Shcherbina, O.B.; Sidorov, N.V.; Steblevskay, N.I.; Belobeletskaya, M.V. Luminescence properties of Sol–Gel Derived Ceramic GdNbxTa1 − xO4 and YNbxTa1 − xO4 Solid Solutions. Inorg. Mater. 2020, 56, 437–442. [Google Scholar] [CrossRef] [Scilit]
  13. Zeng, Y.; Li, A.; Wu, W.; Wang, Z.; Hao, Y.; Deng, M.; Wang, J.; Xu, S.L.; Deng, W. Growth of Ho3+/Tm3+/Yb3+ co-doped monoclinic YNbO4 single crystal for intense up-conversion and down-conversion photoluminescence. Opt. Mater. 2025, 168, 117497. [Google Scholar] [CrossRef] [Scilit]
  14. Luo, Y.; Zhang, D.; Xu, S.; Li, L.; Chen, L.; Guo, H. Optical thermometry based on Bi3+, Ln3+ co-doped YNbO4 (Ln = Dy, Eu) phosphors. J. Lumin. 2023, 257, 119780. [Google Scholar] [CrossRef] [Scilit]
  15. Yuan, S.; Zhao, S.; Lou, L.; Zhu, D.; Mu, Z.; Wu, F. Fluorescence intensity ratio optical thermometer YNbO4: Pr3+, Tb3+ based on intervalence charge transfer. Powder Technol. 2022, 395, 83–92. [Google Scholar] [CrossRef] [Scilit]
  16. Brunckova, H.; Rocha, L.A.; Nassar, E.J.; Moscardini, S.B.; Kolev, H. Luminescence properties of neodymium, samarium, and europium niobate and tantalate thin films. Luminescence 2022, 37, 642–655. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  17. Lima, A.F. New insights into the bonding, electronic and optical properties of fergusonite and scheelite ReNbO4 (Re = Y, La and Lu) compounds. Ceram. Int. 2024, 50, 35161–35168. [Google Scholar] [CrossRef] [Scilit]
  18. Han, C.; Tan, J.; Xiong, A.; Zhang, T. Sensitive optical thermometer via efficient energy transfer in dual-emitting thermochromic YNbO4:Bi3+, Eu3+ phosphor. Ceram. Int. 2022, 48, 4732–4740. [Google Scholar] [CrossRef] [Scilit]
  19. Cho, S. Photoluminescence properties of YNbO4:RE3+ (RE = Dy or Eu) phosphors for anti-counterfeiting applications. Appl. Phys. A 2022, 128, 534. [Google Scholar] [CrossRef] [Scilit]
  20. Đačanin Far, L.; Ćirić, A.; Sekulić, M.; Periša, J.; Ristić, Z.; Antić, Ž.; Dramićanin, M.D. Judd-Ofelt description of radiative properties of YNbO4 activated with different Eu3+ concentrations. Optik 2023, 272, 170398. [Google Scholar] [CrossRef] [Scilit]
  21. Bünzli, J.-C.G. On the design of highly luminescent lanthanide complexes. Coord. Chem. Rev. 2015, 293–294, 19–47. [Google Scholar] [CrossRef] [Scilit]
  22. Binnemans, K. Interpretation of europium (III) spectra. Coord. Chem. Rev. 2015, 295, 1–45. [Google Scholar] [CrossRef] [Scilit]
  23. Reid, M.F. Theory of rare-earth electronic structure and spectroscopy. Handb. Phys. Chem. Rare Earths 2016, 50, 47–64. [Google Scholar] [CrossRef] [Scilit]
  24. Soules, T.F.; Duke, C.B. Resonant energy transfer between localized electronic states in a crystal. Phys. Rev. B 1971, 3, 262–274. [Google Scholar] [CrossRef] [Scilit]
  25. Malta, O.L. Mechanisms of non-radiative energy transfer involving lanthanide ions revisited. J. Non-Cryst. Solids 2008, 354, 4770–4776. [Google Scholar] [CrossRef] [Scilit]
  26. Liu, J.; Lu, L.; Liu, X.; Mi, X. Luminescence performance and energy transfer mechanism investigation of RE3+(Eu3+/Tb3+/Ce3+)-doped Y2O3 phosphors. CrystEngComm 2024, 26, 160–169. [Google Scholar] [CrossRef] [Scilit]
  27. Shannon, R.D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Cryst. 1976, A32, 751–767. [Google Scholar] [CrossRef] [Scilit]
  28. Buth, A.H.; Blasse, G. Luminescence and energy transfer in yttrium niobate (YNbO4). Phys. Status Solidi (A) 1981, 64, 669–676. [Google Scholar] [CrossRef] [Scilit]
  29. Li, Y.; Xiao, J.; Zhou, Y.; Meng, D.; Che, A.; Zhao, L. YNbO4:RE3+ (RE = Eu, Sm, Pr, Dy) phosphors: The luminescence properties and the energy transfer between the host and the RE3+ ions. Optik 2020, 208, 164126. [Google Scholar] [CrossRef] [Scilit]
  30. Zhang, L.; Yi, S.; Hu, X.; Liang, B.; Zhao, W.; Wang, Y. Synthesis and photoluminescence properties of multicolor tunable GdNbO4:Tb3+,Eu3+ phosphors based on energy transfer. Mod. Phys. Lett. B 2017, 31, 1750051. [Google Scholar] [CrossRef] [Scilit]
  31. Zhou, H.; Wang, Q.; Jin, Y. Temperature dependence of energy transfer in tunable white light-emitting phosphor BaY2Si3O10:Bi3+,Eu3+ for near UV LEDs. J. Mater. Chem. C 2015, 3, 11151–11162. [Google Scholar] [CrossRef] [Scilit]
  32. Carnall, W.T.; Fields, P.R.; Rajnak, K. Electronic energy levels of the trivalent lanthanide aquo ions. IV. Eu3+. J. Chem. Phys. 1968, 49, 4450–4455. [Google Scholar] [CrossRef] [Scilit]
  33. Aggarwal, V.; Dalal, S.; Malik, S.; Singh, D.; Sindhu, J.; Kumar, S.; Malik, R.S.; Kumar, P. A complete perspective on lanthanide coordination complexes: Fundamentals, mechanisms and applications. Coord. Chem. Rev. 2026, 562, 217948. [Google Scholar] [CrossRef] [Scilit]
  34. Liu, X.; Lü, Y.; Chen, C.; Luo, S.; Zeng, Y.; Zhang, X.; Shang, M.; Li, C.; Lin, J. Synthesis and luminescence properties of YNbO4:A (A = Eu3+ and/or Tb3+) nanocrystalline phosphors via a sol-gel process. J. Phys. Chem. C 2014, 118, 27516–27524. [Google Scholar] [CrossRef] [Scilit]
  35. Blasse, G. Energy transfer in oxidic phosphors. Phys. Lett. A 1968, 28, 444–445. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.