Surface Coating Technologies: From Deposition Methods to Engineering Applications

,
and
1
Department of Materials and Ceramic Engineering, University of Aveiro, 3810-193 Aveiro, Portugal
2
CICECO-Aveiro Institute of Materials, University of Aveiro, 3810-193 Aveiro, Portugal
*
Author to whom correspondence should be addressed.

Abstract

Coating technologies are essential for improving material surface properties while preserving bulk performance. They are widely used to enhance wear resistance, corrosion protection, thermal stability, biocompatibility, and functional behavior in aerospace, automotive, biomedical, electronics, and energy applications. Together with conventional electrochemical methods, the field has advanced to sophisticated techniques such as physical vapor deposition (PVD), laser cladding, chemical vapor deposition (CVD), atomic layer deposition (ALD), and other precision surface modification processes, enabling greater control over coating composition, thickness, microstructure, and adhesion. Recent progress in materials science, nanotechnology, and process engineering has led to multifunctional coatings with enhanced mechanical, thermal, chemical, and biological properties. At the same time, growing sustainability demands have encouraged the development of coating systems with improved durability, reduced environmental impact, and greater process efficiency. This review summarizes recent advances in coating technologies, focusing on major deposition methods (such as PVD, CVD, laser cladding, and electrodeposition), coating materials, and applications for high-performance and sustainable material systems.

1. Introduction

Surface engineering has become an essential strategy for tailoring the interfacial properties of materials to meet the increasingly stringent requirements of advanced engineering applications. Since many forms of material degradation initiate at the surface, coatings provide an effective means of improving wear resistance, corrosion protection, oxidation resistance, thermal stability, electrical performance, and biocompatibility while preserving the bulk properties of the substrate. Consequently, coating technologies are widely employed to extend component lifetime and enhance functionality in aerospace, energy, electronics, automotive engineering, biomedical engineering, and many other industrial sectors [1].
Over the past decades, a wide range of coating technologies has been developed to satisfy increasingly diverse engineering requirements. These include solution-based methods (e.g., dip coating, spin coating, blade coating, and spray coating) [2,3,4], electrochemical techniques (e.g., electrodeposition and anodizing) [5,6,7], thermal spraying processes (e.g., plasma spraying, HVOF, and cold spraying) [8,9,10], laser-based surface engineering [11,12], vapor deposition methods [13,14,15,16], and more recently, colloidal self-assembly and other nanostructured coating strategies [17,18,19,20]. Each class of coating technologies offers distinct advantages regarding processing temperature, achievable coating thickness, deposition rate, cost, scalability, and compatibility with different substrates. Consequently, no single deposition technique is universally applicable, and the selection of a coating process depends strongly on the required material properties, component geometry, service environment, and manufacturing constraints.
Among this broad spectrum of coating technologies, PVD, CVD, ALD, laser cladding, and electrodeposition were selected for this review. Collectively, they represent complementary approaches to advanced surface engineering, spanning a wide range of coating thicknesses, deposition mechanisms, processing conditions, and engineering applications [1,2,21]. These techniques provide different levels of control over coating composition, microstructure, adhesion, thickness, and surface functionality, while covering applications ranging from nanoscale and thin-film technologies to thick protective coatings and surface restoration. Figure 1 presents the timeline of the development of various coating technologies. This combination provides a useful framework for evaluating coating technologies from an application-oriented perspective, in which the appropriate process is determined by requirements such as coating thickness, conformality, substrate compatibility, deposition rate, surface functionality, and the intended service environment. While PVD and CVD are widely used to produce dense, adherent, and functional thin films, ALD offers exceptional conformality and atomic-scale thickness control for high-aspect-ratio structures, making it particularly valuable for nanostructured coatings, microelectronics, energy devices, and biomedical surfaces. Laser cladding, in contrast, enables the formation of thick, metallurgically bonded coatings for surface repair and wear- or corrosion-resistant applications. Electrodeposition remains one of the most practical and scalable methods for depositing metallic, alloy, composite, and functional coatings on conductive substrates, including components with complex geometries.
Figure 1. Timeline of the development of major surface coating technologies.
In parallel with advances in processing methods, the range of coating materials has expanded considerably. Carbon-based coatings, including graphene-based films and diamond-like carbon, nanostructured ceramics, metallic alloys, composite coatings, and bioactive polymers, have opened new possibilities for multifunctional surface design. These materials allow coatings to move beyond conventional passive protection and provide additional functions such as antimicrobial activity, self-cleaning behavior, controlled drug release, thermal insulation, electrical conductivity, and catalytic activity. Consequently, modern coating systems are increasingly designed not only to protect substrates but also to actively enhance their performance in specific service environments.
A major direction in contemporary surface engineering is the development of multifunctional, hybrid, and smart coatings. Such systems can combine several properties within a single coating architecture, for example, simultaneous wear and corrosion resistance, or mechanical durability combined with biological activity. Smart coatings that respond to external stimuli such as temperature, pH, light, or mechanical damage are also gaining importance. Self-healing coatings, for instance, can repair micro-cracks and extend the operational life of structural components, while drug-eluting and bioactive coatings have significantly improved the performance of biomedical implants. These developments are particularly relevant for addressing challenges related to energy efficiency, healthcare, infrastructure durability, and sustainable manufacturing.
Despite these advances, several limitations continue to restrict the wider implementation of advanced coating technologies. Many deposition processes involve high equipment costs, complex processing conditions, limited scalability, high energy consumption, or the use of hazardous precursors and electrolytes. In addition, the relationship between processing parameters, coating microstructure, and final functional performance is not always systematically established, making it difficult to optimize coatings for specific applications. Environmental considerations, including material utilization, emissions, waste generation, and life cycle impact, are also becoming increasingly important in the selection and development of coating processes.
While numerous reviews have compared deposition technologies primarily from the perspectives of processing principles and operating parameters, the present review adopts an application-oriented framework, examining how major coating technologies, including PVD, CVD, ALD, laser cladding, and electrodeposition, address the functional requirements of different engineering sectors and how these requirements influence coating selection. Where appropriate, the advantages, limitations, and selection criteria of each technology are discussed to provide practical guidance for researchers and engineers. Finally, emerging trends, including multifunctional coatings, sustainable manufacturing, digital process optimization, and hybrid deposition strategies, are highlighted to identify future research directions.

2. Deposition Techniques

Modern deposition techniques are the cornerstone of advanced coating technologies, enabling precise control over material properties, thickness, and functionality. These methods, including Physical Vapor Deposition (PVD), laser cladding, Chemical Vapor Deposition (CVD), Atomic Layer Deposition (ALD), and electrodeposition, enable precise control over coating properties and therefore cater to diverse industrial demands, from aerospace to flexible electronics. ALD excels in creating ultra-thin films for electronics, while laser cladding produces wear-resistant coatings for aerospace components. Electrodeposition has evolved to fabricate nanostructured coatings with enhanced corrosion resistance and catalytic activity, crucial for energy applications. Hybrid techniques combining electrochemical synthesis with other methods are emerging, offering multifunctional layers for sensors and smart coatings.
Although each deposition technique relies on different processing principles, their selection is ultimately governed by the functional requirements of the target application, including coating performance, substrate compatibility, component geometry, production scalability, and economic considerations. The following section discusses the different deposition techniques, their applications, along with recent advancements, challenges, and outlook.

2.1. Physical Vapor Deposition (PVD)

Physical vapor deposition (PVD) comprises a group of vacuum-based coating techniques in which material is physically removed from a solid source and transported in the vapor phase to a substrate, where it condenses to form a thin film [22]. Unlike chemical vapor deposition, PVD relies on physical processes such as evaporation or momentum transfer rather than chemical reactions, enabling relatively lower processing temperatures and high-purity coatings.
PVD techniques are widely used for depositing metals, alloys, and compound coatings such as nitrides, carbides, and oxides. These coatings typically exhibit high hardness, good adhesion, and controlled microstructure, making PVD particularly suitable for applications in tribology, optics, microelectronics, and decorative coatings.

2.1.1. Classification of PVD Techniques

PVD processes can be broadly categorized based on the mechanism used to generate vapor species.
(a)
Evaporation-based techniques
In evaporation processes, the coating material is heated to its vaporization temperature in a vacuum environment and subsequently condenses on the substrate (Figure 2a). Evaporation techniques are commonly used in optical coatings and microelectronics but are inherently limited by their line-of-sight nature, which restricts coating uniformity on complex geometries.
Figure 2. Schematic of conventional PVD processes: (a) sputtering and (b) evaporation using ionized Argon (Ar+) gas. Reprinted with permission from ref. [22].
Thermal Evaporation: Material is heated using resistive heating or crucibles until evaporation occurs. This method is relatively simple and provides high deposition rates, but it offers limited control over film density and adhesion.
Electron Beam Evaporation: A focused electron beam is used to heat and evaporate the target material. This allows the deposition of high-melting-point materials and provides improved control over film purity and deposition rate compared to thermal evaporation.
(b)
Sputtering-based techniques
Sputtering involves the ejection of atoms from a target material due to bombardment by energetic ions (typically form a plasma). These ejected atoms then deposit onto the substrate (Figure 2b). Sputtering techniques are favored for their excellent film uniformity, strong adhesion, and ability to deposit a wide range of materials, including hard coatings such as TiN, CrN, and AlTiN.
Direct Current (DC) Sputtering: Suitable for conductive targets, offering stable deposition and good film uniformity.
Radio Frequency (RF) Sputtering: Enables deposition of insulating materials by alternating the electric field, preventing charge buildup on the target.
Magnetron Sputtering: Utilizes magnetic fields to confine electrons near the target surface, increasing plasma density and improving deposition efficiency. This is one of the most widely used industrial PVD techniques.
High-Power Impulse Magnetron Sputtering (HiPIMS): An advanced variant that employs high-power pulses to generate a highly ionized plasma. HiPIMS produces dense, defect-free coatings with superior adhesion and mechanical properties, making it particularly suitable for demanding applications such as aerospace and high-performance tooling.
(c)
Arc-based deposition
Cathodic Arc Deposition: In this technique, a high-current, low-voltage arc is used to vaporize material from the cathode target. The resulting plasma contains highly ionized species, which contribute to dense coatings with excellent adhesion. However, the presence of macroparticles (droplets) can negatively affect surface quality and may require additional filtering techniques.
Overall, the various PVD techniques offer distinct combinations of coating quality, deposition efficiency, and process complexity. Magnetron sputtering remains one of the most versatile industrial PVD methods because of its excellent coating uniformity, strong adhesion, and broad material compatibility. HiPIMS further improves coating density and mechanical performance through enhanced plasma ionization, although at the expense of lower deposition rates and increased equipment complexity. Cathodic arc deposition offers exceptionally dense coatings and high productivity but requires mitigation of macroparticle formation to achieve high surface quality. Consequently, the selection of a specific PVD technique depends on balancing coating performance requirements with manufacturing efficiency and cost.

2.1.2. Applications of PVD Coatings

The versatility of PVD enables its application across a wide range of engineering sectors. The following sections highlight representative application areas in which the combination of high coating quality, controlled microstructure, and relatively low processing temperatures provides significant technological advantages.
Cutting Tools and Tribological Components
Single-layer and multilayer PVD coatings have become one of the most widely adopted surface engineering solutions for cutting tools, molds, and dies because they significantly improve hardness, wear resistance, and service life while avoiding the higher deposition temperatures associated with many CVD processes. They are also vital for molds and dies, where they provide better wear and corrosion resistance while helping parts release more easily. Although arc evaporation-PVD has a significantly higher deposition rate, magnetron sputtering is favored for wear-resistant coatings in cutting tools and automotive components due to its excellent adhesion, uniformity, surface smoothness, and precision [23]. Moreover, it allows coating of steel tools without exposing the substrate to excessive heat, which maintains the tool’s structural integrity. Sputtered coatings, particularly when optimized with techniques like ion-beam assistance or bias, produce dense microstructures that improve wear and corrosion resistance. However, the induction of residual stress is inevitable in the PVD process [24]. Although the relatively low processing temperature of PVD is advantageous for retaining the mechanical integrity of tool substrates, the energetic particle bombardment involved in many PVD processes can introduce significant residual stresses within the coating. Such compressive stress can contribute to coating densification and, in some cases, improved resistance to crack initiation, whereas excessive residual stress can promote cracking or delamination and thereby compromise coating durability. Thus, the selection and optimization of PVD parameters require a balance among coating densification, residual stress, adhesion, and substrate temperature rather than maximizing hardness alone.
Transition-metal nitrides (such as Titanium Nitride (TiN), Titanium carbonitride (TiCN), Titanium carbide (TiC), Titanium Aluminum Nitride (TiAlN), Aluminum Titanium Nitride (AlTiN), Chromium Nitride (CrN)), alumina (Al2O3) coatings, and combinations of these materials are widely used in engineering applications due to their superior physical and chemical properties. Hard coatings of these materials significantly enhance wear and corrosion resistance, reduce friction, and improve tool lifespan in machining and forming operations [25,26,27,28,29,30,31,32]. Diamond-like carbon coatings are also hard but suffer from higher friction than the hard nitride coatings [23]. Among the several PVD techniques available for deposition of hard coatings, magnetron sputtering and cathodic arc vapor deposition methods are widely used to deposit wear-resistant Ti-Al-based coatings [33,34,35,36,37,38,39].
Comparative studies have shown that the deposition technique strongly influences the microstructure and tribological performance of hard PVD coatings [40,41,42,43]. For instance, Panjan et al. [40] performed a comparative study of microstructural, mechanical, and tribological behavior of TiN hard coatings deposited by different PVD deposition techniques, including low-voltage electron beam evaporation, magnetron sputtering, and cathodic arc deposition. The SEM micrographs presented in Figure 3 show that TiN coatings produced by different PVD techniques differ in columnar morphology, coating porosity, preferred crystallographic orientation, and surface roughness [40]. Figure 4 compares the wear coefficients of TiN coatings deposited by the three techniques under nitrogen, oxygen, and ambient air. The results indicate that wear increased with coating surface roughness, with the cathodic arc (AIP) coating exhibiting the highest wear coefficient. These results demonstrate that coating composition alone does not determine tribological performance; the deposition route can substantially modify coating morphology, density, texture, and surface roughness, which in turn influence wear behavior. Therefore, selecting a PVD technique solely on the basis of nominal coating composition may be insufficient for tribological applications, and process selection should also consider the microstructural characteristics and surface condition produced by the deposition route.
Figure 3. Comparison of SEM images from fracture-cross sections and FIB cross-sections of the various coatings deposited on D2 tool steel substrate (a–c), FIB secondary electron images of cross-sections (d–f), and FIB secondary electron top view images (g–i) of TiN coatings deposited by low-voltage electron beam evaporation (BAI), magnetron sputtering (CC7), and cathodic arc deposition techniques (AIP). Reprinted with permission from ref. [40].
Figure 4. Wear rates of BAI, CC7, and AIP coatings as a function of surface roughness Sa. The wear tests were performed in (a) nitrogen, (b) ambient air, and (c) oxygen atmospheres. Reprinted with permission from ref. [40].
In another similar work [43], a preferential growth of as-deposited CrN film on the (200) facet was realized by HiPIMS when compared with DCMS on the (111) facet. Consequently, the HiPIMS-deposited coatings had a very compact microstructure with high hardness and a corrosion current approximately one order of magnitude lower than that of CrN films deposited by DCMS. The friction coefficient and wear resistance studies showed that CrN coatings deposited by HiPIMS exhibited lower friction coefficients compared to DCMS (Figure 5). Figure 3, Figure 4 and Figure 5 clearly illustrate how differences in plasma generation and ionization influence coating morphology, microstructure, and wear behavior, thereby explaining the performance differences observed among the various PVD techniques. The improved coating properties obtained with HiPIMS should nevertheless be considered against its greater process complexity and the process conditions required to generate highly ionized plasma. Consequently, HiPIMS is particularly attractive when coating density, adhesion, and wear or corrosion performance are prioritized over process simplicity and maximum deposition productivity.
Figure 5. (a) The friction coefficient and (b) wear groove width obtained from the friction and (c) wear tests on CrN coatings prepared via HiPIMS and DCMS. Reprinted with permission from ref. [43].
Hybrid CVD–PVD multilayer coating strategy has been reported to significantly enhance cutting tool performance and longevity in demanding machining applications. Machining tests on advanced ceramic multilayer coatings on AISI 316 stainless steel by Codau et al. [44] revealed that the hybrid CVD- and HiPIMS-PVD-coated tools exhibited significantly better tool life compared to the CVD-coated tools. This result suggests that the performance of a coating system may depend not only on the individual deposition technology but also on the architecture and combination of coating processes. The superior tool life obtained with the hybrid CVD–HiPIMS-PVD approach indicates that sequential integration of different deposition methods can provide performance advantages over a single-process coating, although additional processing steps and associated manufacturing complexity should also be considered when evaluating industrial applicability.
In the automotive sector, coatings are extensively used for engine components (piston rings, valves), bearings, and fuel cells to reduce friction and improve durability [45,46,47,48]. Among the several PVD techniques, magnetron sputtering is most favored for coating the piston ring of an internal combustion engine [46,49]. Tribological tests have confirmed that carbon-, nitride-, and carbide-based coatings (such as CrN, MoN, CrAlN, TiSiN, TiC, and DLC) effectively reduce the wear rate compared with uncoated piston rings [47,49,50,51,52,53,54,55].
Collectively, these studies demonstrate that the choice of PVD deposition technique has a profound influence on coating microstructure and, consequently, tribological performance. Magnetron sputtering generally produces smoother coatings with lower surface roughness, whereas HiPIMS promotes denser microstructures through enhanced plasma ionization, resulting in higher hardness and improved corrosion and wear resistance. Cathodic arc deposition offers significantly higher deposition rates but may compromise surface quality because of macroparticle formation. Therefore, the selection of a PVD technique should be guided by the specific application requirements rather than by any single performance metric. In practice, the optimum process depends on balancing deposition rate, coating density, surface finish, component geometry, and manufacturing cost.
Aerospace and High-Temperature Coatings
Aerospace components operate under extreme thermal, mechanical, and oxidative conditions, requiring coatings that combine excellent adhesion, thermal stability, and long-term durability. The precise microstructural control achievable by advanced PVD techniques makes them particularly attractive for these demanding applications.
Thermal barrier coatings are widely utilized protective coatings in the aerospace industry to improve oxidation resistance, thermal stability, functional performance, and lifespan of components such as gas turbine engines, turbine blades, aircraft landing gear, and engine blocks [56,57,58,59]. Several PVD-based thermal barrier coating methods have been studied. HIPIMS enhances coating density and reduces defects, critical for aerospace turbine blades exposed to extreme temperatures, while the EB-PVD coating method has also been used in aircraft engine applications of gas turbines [56,60,61]. For instance, Shen et al. [56] studied LaNdZrO and YSZ ceramic coatings deposited by EB-PVD, and NiCoCrAlYHf metallic coating using AIP-PVD. Protective Cr/CrN coatings deposited using magnetron sputtering-PVD have been utilized for space applications [62]. Furthermore, hybrid CVD-PVD has also been used for barrier coatings of aircraft engines [57]. These examples indicate that PVD is not a single uniform solution for aerospace applications; rather, the choice among EB-PVD, HiPIMS, AIP-PVD, and magnetron sputtering depends on the required combination of coating architecture, density, surface quality, thermal stability, and component-specific performance requirements.
Microelectronics and Thin-Film Devices
Microelectronic devices require extremely thin, uniform, and high-purity coatings with excellent electrical and diffusion-barrier properties. The precise thickness control and cleanliness associated with PVD processing have therefore made these techniques indispensable in semiconductor manufacturing.
PVD is employed for the deposition of metal interconnects, barrier layers, and functional thin films in semiconductor devices [63,64,65,66,67]. TiN, due to its relatively high thermal and structural stability and low electrical resistivity, is employed in microelectronic and photovoltaic devices [63,67]. High carrier mobility of 800 cm3/Vs and a resistance of 5 × 10−4 Ohm-cm have been reported in TiN films [67]. For instance, Mühlbacher et al. [63] sputter-deposited single-crystalline TiN/Cu bilayers on MgO (001) substrates and demonstrated the excellent diffusion-barrier properties of single-crystalline TiN. These applications highlight the suitability of PVD for microelectronic systems where thin-film uniformity, electrical performance, and diffusion-barrier functionality are critical; however, the increasing complexity and aspect ratio of device architectures can make conformal coating increasingly challenging, providing a rationale for considering more conformal deposition approaches such as ALD when required.
Decorative and Optical Coatings
In addition to engineering applications, PVD has become an important industrial technology for decorative and optical coatings, where precise color control, surface finish, and long-term durability are essential.
PVD enables the fabrication of reflective, anti-reflective, and aesthetically appealing coatings with precise thickness control [68,69,70,71]. Hard transition-metal nitrides exhibit different colors such as gold-yellow, bronze, brown, violet, dark-blue, and almost black by small variations in their stoichiometric composition. In particular, the characteristic golden color, abrasion resistance, and chemical inertness of TiN coatings are attractive for decorative purposes, including watch cases, sanitary hardware, household appliances, door handles, jewelry items, and architectural glass. PVD is also used to develop optical coatings on display screens, enabling anti-reflective or reflective properties.
Biomedical Coatings
Biomedical applications demand coatings that combine excellent biocompatibility, corrosion resistance, wear resistance, and chemical stability while minimizing adverse biological responses. These requirements have led to widespread adoption of PVD coatings for medical devices and implants.
PVD coatings are excellent for wear protection of orthopedic implants (hips, knees, and other prosthetic joints) and dental implants (screws, abutments) [72,73]. Besides implants, PVD coatings are used to provide corrosion protection, antimicrobial properties, sharpness, and cutting-edge retention for surgical tools (e.g., scalpels, blades, drills, reamers, orthopedic bone saw blades).
Owing to its intrinsic biocompatibility, antibacterial properties, chemical inertness, and good tribological properties, coatings of Ti and its alloys, such as TiN, are extensively used for wear protection of medical implants [74]. Moreover, the haemocompatibility of TiN encouraged TiN coatings in cardiology for ventricular assist devices and for pacemaker leads [72,75,76]. These applications illustrate the potential of PVD coatings to improve the wear and surface durability of biomedical devices; however, coating selection in biomedical applications must also consider long-term biocompatibility, interfacial stability, and the biological response to the coating system, rather than relying solely on mechanical or tribological performance.
From an application perspective, conventional magnetron sputtering is generally preferred for cutting tools, automotive components, and decorative coatings because it provides an excellent balance between coating quality, process stability, and industrial scalability. HiPIMS is increasingly selected where superior coating density, adhesion, and corrosion resistance justify higher processing costs, particularly in aerospace and biomedical applications. Cathodic arc deposition remains attractive for wear-resistant coatings requiring high deposition rates, whereas evaporation-based techniques continue to play an important role in optical coatings and selected microelectronic applications because of their simplicity and excellent thickness control. Thus, the selection among PVD variants is application-dependent and requires balancing coating performance against deposition productivity, surface quality, process complexity, and cost.

2.1.3. Advantages, Challenges and Outlook

PVD offers several advantages, including relatively low deposition temperatures compared to CVD, high coating purity due to vacuum processing, and good control over film thickness and composition. Recent developments in PVD technologies have focused on enhancing plasma characteristics and ionization efficiency to improve coating density, adhesion, and microstructural control. High-power impulse magnetron sputtering has emerged as a significant advancement, generating a highly ionized metal flux that promotes dense film growth, reduced defect density, and improved interfacial bonding compared to conventional sputtering techniques. However, these improvements are accompanied by greater process complexity and, in general, lower deposition productivity than conventional magnetron sputtering, making HiPIMS particularly attractive when coating performance is prioritized over maximum throughput. In addition, strategies such as ion-assisted deposition, substrate biasing, and reactive sputtering have enabled improved control over residual stress, phase composition, and functional properties of coatings.
However, PVD techniques are generally limited by their line-of-sight deposition nature, which restricts their ability to uniformly coat substrates with complex geometries. Also, achieving strong and consistent adhesion on certain substrates often requires additional surface treatments or interlayers. Furthermore, issues related to scalability, process cost, and energy consumption can restrict large-scale industrial implementation. To overcome the intrinsic line-of-sight limitation of conventional PVD processes, hybrid approaches combining PVD with techniques such as atomic layer deposition have been developed. These systems enable the formation of conformal multilayer and nanolaminate coatings, integrating the high density of PVD films with the excellent conformality of ALD.
Looking forward, future developments in PVD are expected to focus on improving coating conformality, enhancing process scalability, and reducing energy consumption. A persistent challenge is therefore to improve coating conformality and process productivity simultaneously, without compromising coating density, adhesion, or microstructural control. The integration of advanced plasma diagnostics, real-time monitoring, and data-driven process optimization is likely to enable greater control over the coating quality and reproducibility. In addition, continued development of hybrid and multifunctional coating systems is expected to expand the applicability of PVD in emerging fields such as flexible electronics, energy systems, and environmentally sustainable surface engineering.
Overall, PVD is expected to remain one of the dominant thin-film deposition technologies for applications requiring high coating quality, excellent adhesion, and precise microstructural control. However, its selection should be based on the specific balance between coating performance, conformality, deposition productivity, substrate compatibility, and manufacturing cost. ALD may be preferred when exceptional conformality and atomic-scale thickness control are required, whereas laser cladding is more suitable when thick, metallurgically bonded protective or restorative layers are needed.

2.2. Laser Cladding

Laser cladding is an advanced surface modification and additive manufacturing technique in which a high-energy laser beam is used to melt and deposit a coating material onto a substrate, forming a metallurgically bonded layer (Figure 6). The laser cladding process involves complex interactions between laser energy, material feedstock, and substrate. Key parameters include laser power, scanning speed, powder feed rate, and shielding environment, all of which influence melt pool dynamics, microstructure evolution, and final coating properties. The feedstock material, typically in the form of powder or wire, is delivered into the laser-induced melt pool and rapidly solidifies to produce a dense coating with a refined microstructure.
Figure 6. Laser cladding using powdered feedstock. Adapted from webpage: https://www.laserline.com/en-int/laser-cladding/ (accessed on 14 April 2026).
As a directed energy deposition process, laser cladding enables precise control over heat input, dilution, and coating geometry. The localized nature of the process minimizes the heat-affected zone (HAZ), thereby reducing thermal distortion and preserving substrate properties. Rapid solidification during processing promotes fine microstructures, which are often associated with improved mechanical and tribological performance. Unlike vapor-phase deposition techniques, laser cladding produces coatings through localized melting and rapid solidification of metallic feedstock, resulting in dense, metallurgically bonded layers with thicknesses ranging from several hundred micrometers to several millimeters. Consequently, laser cladding is particularly suited for surface repair, hardfacing, and structural reinforcement, whereas vapor deposition techniques are generally preferred for thin functional coatings requiring precise control of composition and thickness. The ability to produce relatively thick, metallurgically bonded layers is therefore a major advantage of laser cladding for component restoration and surface strengthening; however, this advantage is accompanied by process-specific challenges associated with heat input, dilution, residual stress, and surface finish, which must be controlled to achieve reliable coating performance.
Laser cladding using titanium and high-entropy alloys (HEAs) offers significant surface modification advantages, primarily by creating high-performance, metallurgically bonded coatings on materials like steel, aluminum, and titanium alloys [77,78,79,80]. HEAs, typically comprising multiple principal metallic elements, are promising for applications such as oil drilling, aerospace, and marine engineering because their compositional flexibility can be exploited to obtain combinations of high strength, hardness, corrosion resistance, and high-temperature stability [81,82,83,84,85,86,87,88]. However, the selection of an HEA composition involves trade-offs among hardness, toughness, corrosion resistance, and environmental stability; consequently, recent research has increasingly focused on application-specific composition design rather than maximizing a single property. Advances in real-time monitoring and multi-material cladding (e.g., metal-ceramic composites) enhance process reliability and enable functionally graded coatings by dynamically adjusting feedstock composition during deposition.
Several laser cladding configurations have been developed to address different coating thicknesses, deposition rates, component geometries, and manufacturing requirements.

2.2.1. Variants of Laser Cladding

Laser cladding processes can be categorized based on feedstock delivery, processing speed, and application configuration.
(a) Powder-Fed Laser Cladding: In this widely used configuration, powder is delivered through a nozzle into the laser beam. It offers high flexibility in material selection and is suitable for both coating applications and additive manufacturing.
(b) Wire-Fed Laser Cladding: This method employs a continuous metallic wire as feedstock. Compared with powder-fed systems, it provides higher material utilization efficiency and reduced material waste, making it attractive for large-scale deposition.
(c) Extreme High-Speed Laser Application (EHLA): EHLA is an advanced variant characterized by very high processing speeds and the ability to produce thin coatings (typically <0.1 mm). The process significantly reduces heat input, resulting in minimal dilution and a very narrow heat-affected zone.
(d) Internal Bore Laser Cladding: This specialized configuration is designed for coating the internal surfaces of cylindrical components such as pipes and tubes, enabling in situ repair and protection of otherwise inaccessible regions.
(e) 3D Freeform/Direct Energy Deposition (DED): This approach utilizes multi-axis systems to enable additive manufacturing of complex three-dimensional geometries. It extends laser cladding beyond surface coating to full component fabrication.
(f) Conventional (low-speed) Laser Cladding: The traditional form of laser cladding operates at relatively lower speeds and higher heat input. It is commonly used for industrial repair, hardfacing, and deposition of thick coatings.
These configurations involve important trade-offs in deposition rate, material utilization, coating thickness, heat input, geometric accessibility, and surface finish. Powder-fed systems offer greater flexibility in feedstock selection and are well suited to localized coating and repair, whereas wire-fed systems can provide higher material utilization and are attractive for larger-scale deposition. EHLA extends laser cladding toward high-speed deposition of relatively thin layers with reduced heat input, while internal-bore configurations address geometries that are inaccessible to conventional external cladding. Multi-axis DED systems further extend the process from surface coating and repair toward three-dimensional component fabrication. Consequently, the selection of a laser-cladding configuration should be based on component geometry, required coating thickness, deposition productivity, material utilization, accessibility, and the thermal sensitivity of the substrate rather than on deposition capability alone.

2.2.2. Applications

Laser cladding is an economical and effective process for a wide range of coating applications. It is extensively applied in industries requiring high-performance and repairable coatings.
Aerospace Industry
Laser cladding is used for the repair and protection of turbine blades and engine components, where wear- and oxidation-resistant alloys such as nickel- and cobalt-based high-entropy alloy systems provide improved durability under high-temperature and oxidative environments [89,90,91,92,93,94,95,96,97,98]. Wang et al. [96] fabricated a new refractory high-entropy alloy Ti35Ni34Cu10Zr10Nb8Ta3 coating on a copper substrate, significantly improving hardness and wear resistance. Morais et al. [93] exhibited that laser surface treatment enhanced metallurgical bonding between the coating and the substrate, preventing delamination and peel-off in Al-cladded AA2024-T3, an aluminum alloy widely used in the aerospace industry.
Recently, Liu et al. [99] prepared AlCoFeCuMox high-entropy alloy coatings with excellent mechanical and corrosion properties, rendering them suitable for aerospace applications, including unmanned aerial systems. In another work, Guan et al. [100] investigated the mechanical properties of 30CrMnSiNi2A steel repaired by laser cladding with AerMet100 Steel, providing an effective solution for critical aerospace components such as landing gear. Zhao et al. [101] improved wear and corrosion resistance in laser-cladding-fabricated TC11-xMo coatings. The worn surface of the TC11–10Mo coating showed the highest degree of smoothness and minimum wear depth, wherein the coating was rubbed against GCr15 steel balls measuring 6 mm in diameter.
Collectively, these studies indicate that the principal value of laser cladding in aerospace applications lies in its ability to combine material addition with localized surface repair and property enhancement. The reported coating systems differ substantially in composition and targeted performance, reflecting the application-specific nature of laser-cladded surfaces: alloy selection must account for the required balance among wear resistance, corrosion resistance, mechanical strength, and high-temperature stability. At the same time, the effectiveness of laser cladding is not determined solely by the nominal coating composition; metallurgical bonding, dilution, and the resulting coating microstructure are also important in determining the durability of the repaired or protected component. Thus, laser cladding is particularly attractive where localized restoration or relatively thick protective layers are required.
Energy Sector
In the energy sector, laser cladding is employed to protect critical components and boost the efficiency and durability against corrosion, erosion, and high-temperature degradation of power-generation equipment such as parts of oil and gas systems, including turbines, boilers, heat exchangers, deep-earth drilling tools, pipelines, and valves. These coatings are essential for maintaining structural integrity and operational efficiency in aggressive service conditions. Compared with conventional alloys, high-entropy alloys have garnered much attention for surface protection of engineering components operating under complex mechanical and corrosive environments, as in deep-earth engineering applications such as ultra-deep drilling and geothermal exploitation [102]. Wu et al. [88] studied the tribological behavior of 1 wt% hBN-reinforced CoCrFeNiMo0.5Tix (x = 0, 0.2, 0.4, 0.6) high-entropy alloy composite coatings on 42CrMo material used for oil drill pipe joints. Results indicated that the CoCrFeNiMo0.5Ti0.4-hBN exhibited the best resistance to dry wear and tribocorrosion. Wang et al. [103] reported on the Ni-WC laser-clad coating in a mineralizing solution. Cui et al. [104] designed laser cladding of FeCoNiCrMox (x = 0, 0.5, 1.0, 1.5) coatings for strengthening Ti6Al4V components for drilling equipment in deep, complex environments. The potentiodynamic polarization studies of Ti6Al4V and FeCoNiCrMox coatings in 3.5% NaCl solution revealed that the Mo-0.5 and Mo-1.0 coatings significantly enhanced the corrosion resistance.
These studies illustrate that laser-cladding performance in energy-related applications depends strongly on the service environment and the specific degradation mechanism being addressed. The incorporation of hBN, WC, or Mo, for example, represents different approaches to improving tribological or corrosion performance rather than a universally superior material solution. The reported results therefore support an application-specific approach to feedstock selection, in which coating composition and reinforcement are tailored to the dominant combination of wear, tribocorrosion, and corrosive exposure. This is an important advantage of laser cladding, because the feedstock composition can be modified to address different service requirements while retaining the benefits of a metallurgically bonded protective layer.
Automotive Industry
Laser cladding in the automotive industry is a high-precision surface engineering process used to enhance the wear and corrosion resistance of components, such as brake disks, engine valves, camshafts, and crankshafts. The automotive industry extensively uses laser surface treatments for repair/remanufacturing and the aesthetic appeal of automotive parts, allowing restoration of worn components with minimal distortion and reduced material waste, enabling cost-effective repair and remanufacturing strategies. The process is particularly beneficial for automotive components made of aluminum alloys [91,105,106,107,108].
Laser Cladding, a directed energy deposition process, is extremely favorable to improve durability of brake disks and reduce brake dust emissions that can cause health issues. With the introduction of the Euro 7 emissions standard, which limits brake dust emissions (brake particle emission < 7 mg·km−1), new coating solutions such as metal matrix composites (MMC) are gaining importance. Laser cladding provides protective, defect-free, metallurgically bonded layers with high adhesion, creating strong and durable coatings for brake disks that improve brake disk lifetime and performance while helping to meet environmental regulations [11,106,109,110]. Wang et al. [106] utilized rotatable inner-surface laser cladding to generate a stainless steel cladding layer to enhance the wear resistance of the inner surface of car engine cylinders. They explored the process parameters for laser cladding an Fe-based layer onto an AlSi9Mg surface employing low-speed (LSLC) and high-speed laser cladding (HSLC) layers. In comparison to the AlSi9Mg substrate, the microhardness was significantly greater in cladded layers, while the wear depth was nearly ten times shallower. Zhang et al. [111] successfully deposited a Co-Cr-Ti composite coating on Ti6Al4V (TC4) alloy, which is extensively used in various automotive components such as connecting rods, intake valves, and turbochargers, to achieve higher fuel efficiency and reduced energy consumption targets. The Co-Cr-Ti composite coating on a TC4 alloy substrate by laser cladding enhanced microhardness, wear, and corrosion resistance. In particular, the coating demonstrated a notable enhancement in friction and wear resistance at both room temperature and 500 °C. Altuncu et al. [110] systematically investigated the efficiency of HSLC for enhancing the wear and corrosion resistance of automotive brake disks, meeting the Euro-7. Three distinct MMC coatings were fabricated on a GG25 gray cast iron substrate. Consistent coating quality and high performance under challenging conditions such as wear, corrosion, and thermal-cycle loads were reported. Moreover, the coated brake disks complied with the Euro-7 regulations and with ECR90 standards.
These results highlight the particular relevance of laser cladding to automotive components subjected to simultaneous wear, corrosion, and thermal-cycle conditions. The comparison between low-speed and high-speed laser cladding also indicates that process configuration can influence the balance between coating performance, heat input, and processing productivity. For repair and remanufacturing, the ability to deposit material selectively on worn regions provides an additional advantage by reducing the need for complete component replacement. However, the suitability of laser cladding for automotive production depends on whether the achievable coating performance and material savings can offset the requirements for process control and subsequent surface finishing.
Functionally Graded Coatings
Beyond conventional protective applications, laser cladding enables the fabrication of advanced surface layers such as functionally graded coatings in which the composition and properties change gradually across the coating thickness [112,113,114,115]. Instead of a single uniform layer, the material is tailored step by step, for example, transitioning from a tough, compatible base layer to a hard, wear-resistant top layer. This gradual variation in composition and microstructure improves stress distribution and thermal compatibility, creating a strong metallurgical bond between the coating and the substrate. A gradual composition shift creates a steady gradient in the coefficient of thermal expansion (CTE), preventing sharp stress concentrations at the interface. By spreading thermal and mechanical stresses over a transitional layer, FGCs minimize the destructive residual stresses and eliminate sharp interfaces, preventing delamination and warping, particularly in dissimilar material systems such as ceramics on metals. Particularly, key advantages of functionally graded coatings include low dilution and a minimal heat-affected zone, high density and purity, and the ability to smoothly transition from hard surface layers to more ductile substrates. The principal advantage of this graded architecture is therefore the ability to manage the incompatibility between a hard, wear-resistant surface and a relatively tough substrate, rather than simply maximizing surface hardness. However, achieving the intended compositional and property gradient requires careful control of feedstock composition and deposition conditions, since deviations in the gradient can influence dilution, residual stress, phase formation, and resulting mechanical performance.
These coatings are widely used for wear and corrosion protection (e.g., Ni-WC or TiC on steel or magnesium alloys), high-temperature applications such as thermal barrier coatings, and repair or additive manufacturing of high-value components. Common material systems include Ni-WC/Al-Ni, AlCuTiVCr/Cu-Al high-entropy alloys, and TiC/Ni composites for high-strength applications [115,116,117,118,119,120,121,122,123]. For instance, Wan et al. [117] reported on a novel laser-cladded AlCuTiVCr/Cu-Al lightweight, high-melting-point HEA graded coating on the surface of a low-melting-point Mg-Li substrate. The design of the gradient coating comprising an AlCuTiVCr protective layer, a Cu-Al transition layer, and a Mg-Li alloy substrate formed excellent metallurgical bonding, and the protective layer achieved superior corrosion resistance. Müller et al. [124] applied a functionally graded coating by laser cladding to improve the lifetime of die-casting dies. They studied the hardness distribution of the gradient structure before and after heat treatment (for two hours at 580 °C) [124]. The heat treatment did not affect the hardness of the base material and the three top layers, which is essential to maintain its mechanical properties. In another work, Wang et al. [122] formed an H13/Ni60 functional gradient coating on the surface of H13 steel by using the laser cladding method, improving the hardness and wear resistance of the substrate significantly. Taken together, these studies demonstrate that functionally graded laser-cladded coatings can be designed to address the interface and property-mismatch problems that may arise in dissimilar material systems. The reported approaches differ in both composition and application, indicating that there is no universal gradient architecture; instead, the composition profile must be designed according to the substrate, required surface properties, and service conditions. The additional compositional control, however, also increases process complexity compared with deposition of a single homogeneous coating.

2.2.3. Advantages, Challenges and Outlook

Laser cladding offers significant advantages in producing high-performance coatings with strong metallurgical bonding and minimal dilution, ensuring that the deposited layer retains its designed composition and properties. The localized heat input reduces thermal damage to the substrate and enables precise control over coating geometry, making it particularly suitable for repair and remanufacturing of high-value components. Additionally, the ability to process a wide range of materials, including metal alloys and composite systems, and to fabricate functionally graded structures enhances its versatility. These advantages distinguish laser cladding from thin-film deposition techniques, particularly where relatively thick protective layers, localized material addition, or component restoration are required. However, the benefits of strong metallurgical bonding and high deposition thickness must be considered together with the associated thermal effects, dilution, residual stress, and post-processing requirements. Thus, laser cladding is most advantageous when the functional and economic benefits of localized material addition outweigh the additional process and finishing requirements. Recent developments in laser cladding have focused on improving process reliability, material performance, and functional versatility. The integration of real-time monitoring and closed-loop control systems has significantly enhanced process stability and reproducibility. In addition, multi-material and composite cladding approaches have enabled the fabrication of metal–ceramic coatings with superior wear resistance and thermal stability. The convergence of laser cladding with additive manufacturing technologies, particularly directed energy deposition, is further expanding its role in the fabrication and repair of complex, high-value components.
However, the process also presents several limitations. Rapid thermal cycles can produce steep temperature gradients, causing residual stresses, distortion, and in some cases cracking. Maintaining tight control of the process window to achieve the desired microstructure while minimizing defects (e.g., porosity, cracking, incomplete fusion/overlap) remains challenging and typically requires specialized expertise. Surface finish can be relatively rough and may necessitate post-processing. In addition, high capital and operating costs for laser systems (and, where applicable, consumables such as feedstock) can hinder adoption in cost-sensitive sectors. Process parameter complexity, scalability to consistent high-throughput production, integration into existing lines, and material/absorptivity constraints are additional barriers. Finally, applicability can be limited by material-laser interactions such as low absorptivity or narrow processing windows for certain substrates. These limitations indicate that the principal challenge for wider industrial adoption is not the ability to produce a high-performance clad layer but achieving consistent coating quality and process reproducibility at the required production rate and cost.
Looking forward, research in laser cladding is expected to focus on physics-based process modeling (including thermal–fluid flow and dilution), in situ diagnostics, and closed-loop control to improve reproducibility and part-to-part quality. Data-driven optimization, including machine learning for parameter selection, defect detection, and predictive maintenance, is likely to accelerate process qualification. On the hardware side, wider adoption of efficient fiber/diode laser sources, improved beam delivery, and higher-throughput systems, combined with automation and robotics, should enhance scalability for industrial production. Continued development of cost-effective laser platforms and optimized feedstock powders/wires will be essential for broader deployment. In parallel, functionally graded and multi-material coatings will expand performance tailoring for aerospace, energy, and biomedical components, and hybrid additive–subtractive repair and remanufacturing workflows are expected to grow. A key research priority will therefore be to integrate process monitoring, predictive modeling, and adaptive control into a unified manufacturing framework, so that coating quality can be controlled during deposition rather than assessed primarily after processing. Futuristic applications are emerging, with powder-based laser cladding being investigated for in-space metal repair and on-demand manufacturing in microgravity; however, robust powder handling and process stability remain key challenges [125,126].

2.3. Chemical Vapor Deposition (CVD)

Chemical vapor deposition (CVD) is a widely employed thin-film deposition technique in which volatile precursor species undergo chemical reactions at or near a heated substrate surface to form a solid coating. The process typically involves the transport of gaseous precursors into a reaction chamber, followed by their decomposition and/or reaction under controlled temperature and pressure conditions. The resulting solid material is deposited on the substrate, while gaseous by-products are continuously removed [127,128,129]. Figure 7 shows the schematic of the main steps involved during the CVD process [130].
Figure 7. Schematic of the main steps of the CVD process. Reprinted with permission from ref. [130].
CVD can produce dense, uniform, and well-adhered coatings with controlled composition and microstructure. Due to its non-line-of-sight nature, it is particularly suitable for coating substrates with complex geometries. The technique supports a broad range of material systems, including metals, oxides, nitrides, carbides, borides, and carbon-based materials such as diamond and diamond-like carbon (DLC). Consequently, CVD is extensively used in applications requiring high-performance coatings, including wear-resistant layers, corrosion protection, semiconductor devices, optical coatings, and thermal barrier systems. Compared with PVD, CVD generally provides superior conformal coverage on complex three-dimensional geometries because the coating is formed through surface chemical reactions rather than line-of-sight deposition. However, this advantage is often accompanied by higher processing temperatures, greater precursor complexity, and more demanding safety requirements. Consequently, CVD is particularly attractive when coating quality, uniformity, and compositional control are prioritized over process simplicity and operating cost.

2.3.1. Classification of CVD Techniques

(a)
Activation method
Thermal CVD: In thermal CVD, chemical reactions are driven by elevated temperatures, typically in the range of 500–1400 °C. This method often utilizes inorganic precursors such as halides or hydrides and is known for producing coatings with high crystallinity and purity. However, the high processing temperatures may limit its applicability to thermally sensitive substrates [127,131].
Plasma-Enhanced CVD (PECVD): PECVD employs plasma to generate reactive species, thereby reducing the required substrate temperature (typically 200–300 °C). Plasma activation enhances reaction kinetics and enables deposition on temperature-sensitive materials. Additionally, PECVD allows improved control over film properties such as density, stress, and composition. It is widely used for depositing dielectric layers, silicon-based films, and DLC coatings [127,128,132]. For example, Zhang et al. [133] deposited silicon nitride films at 80 °C under plasma-enhanced conditions.
Photo-Assisted CVD: In this approach, ultraviolet or laser radiation is used to initiate or enhance chemical reactions. This enables lower processing temperatures and selective area deposition, although its industrial application remains comparatively limited [127].
Microwave CVD (MWCVD): In this deposition technique, microwave energy is utilized to generate a plasma, which activates gaseous precursor molecules and enables the growth of high-quality materials on a substrate. Unlike conventional thermal CVD, Microwave CVD relies on microwave-generated plasma to activate chemical reactions, thereby reducing the substrate temperature required for deposition while maintaining excellent film quality.
MWCVD is widely used for the synthesis of diamond films, graphene, silicon-based coatings, and other advanced materials, and is valuable for applications in electronics, optics, energy devices, and protective coatings.
(b)
Precursor type
Metal–Organic CVD (MOCVD): MOCVD utilizes metal–organic precursors that can be vaporized at relatively low temperatures. This technique provides excellent control over film composition and uniformity, making it particularly suitable for the deposition of compound semiconductors, oxides, and nitrides [127,128,134]. Compared to conventional CVD, MOCVD enables lower-temperature processing and is widely used in optoelectronic and microelectronic applications.
Other specialized variants include initiated CVD (iCVD) and oxidative CVD (oCVD) [135,136,137,138]. The iCVD is an all-dry method for designing organic and hybrid polymers, enabling uniform, high-purity, and pinhole-free films with thicknesses ranging from >15 µm to <5 nm via free-radical mechanisms (Figure 8) [137,139]. While oxidative CVD (oCVD) is a liquid-free technique used for depositing electrically conductive conformal polymer coatings directly on the substrate as both monomer and oxidant in the vapor phase are introduced into the reactor simultaneously. For example, Kaviani et al. [136] deposited oCVD PEDOT polymer coatings on carbon cloth, imparting stable all-organic electrodes for oxygen electroreduction. Baek et al. [140] fabricated highly sensitive and fast-response pressure sensors through conformal oCVD polymers.
Figure 8. Electron micrographs of conformal coverage of iCVD polymers over complex geometries. SEM images of TiO2 nanopillars (a) before and (b) after CSE95 deposition, TiO2 nanopores (c) before and (d) after CSE10 deposition, and CSE10-coated. Reprinted with permission from ref. [139]. Copyright 2019 American Chemical Society.
(c)
Operating pressure
Atmospheric Pressure CVD (APCVD): APCVD operates at atmospheric pressure and is characterized by high deposition rates and relatively simple equipment [141]. However, film uniformity and thickness control may be limited compared to low-pressure systems, making this method more suitable for applications where high deposition rates are more important than precise thickness uniformity.
Low-Pressure CVD (LPCVD): LPCVD is conducted under reduced pressure, which enhances film uniformity and step coverage while minimizing gas-phase reactions [141]. In contrast to the APCVD, the low-pressure CVD allows thin-film deposition. LPCVD is therefore preferred when excellent film uniformity, conformality, and reproducibility are required, particularly in semiconductor manufacturing.
Ultra-High Vacuum CVD: This variant operates under ultra-high vacuum conditions to achieve superior purity and precise control over film growth, particularly in advanced semiconductor applications [141].
(d)
Other CVD variants
Additional CVD-based processes include hot-filament CVD, chemical vapor infiltration (CVI), fluidized-bed CVD, and electrochemical vapor deposition (EVD) [127,142]. Chemical vapor infiltration is particularly useful for producing ceramic matrix composites by infiltrating porous structures, while fluidized-bed CVD is employed for coating powders. Although atomic layer deposition (ALD) is often considered a specialized form of CVD due to its reliance on sequential surface reactions, it is treated separately in this review due to its distinct self-limiting growth mechanism.
The various CVD techniques primarily differ in the method used to activate the chemical reactions and the resulting processing temperature. Thermal CVD generally produces highly crystalline coatings but requires elevated temperatures, whereas PECVD significantly lowers the thermal budget, enabling deposition on temperature-sensitive substrates. MOCVD offers excellent compositional control for compound semiconductors, while specialized techniques such as iCVD and oCVD extend CVD to polymeric and organic coatings. Overall, the selection of the appropriate CVD variant depends primarily on substrate temperature limitations, coating chemistry, and the required film performance rather than deposition rate alone. This distinction also highlights an important trade-off within the CVD family: lowering the deposition temperature through plasma or other activation mechanisms can broaden substrate compatibility, but the resulting film properties and process characteristics should be evaluated against those achievable by conventional thermal CVD. Thus, the choice between thermal CVD, PECVD, MOCVD, and other variants is not simply a matter of selecting the lowest processing temperature; it depends on whether thermal budget, film composition, conformality, deposition environment, or application-specific performance is the dominant constraint.

2.3.2. Applications of CVD Coatings

CVD is extensively applied across multiple industries. Here, only a few selected applications will be discussed.
Cutting Tools and Wear-Resistant Components
Cutting performance and wear resistance can be significantly improved by coatings [44,143,144,145]. Components such as piston rings, cylinder bodies for injection molding, screws for extrusion, and bearings are prone to wear during sliding [146]. Using CVD-coated cutting tools and components offers excellent wear resistance and good adhesion to the substrate. Hard coatings of advanced materials such as titanium carbide (TiC), titanium nitride (TiN), titanium carbonitride (TiCN), titanium aluminum nitride (TiAlN), and aluminum oxide (Al2O3) significantly improve wear resistance, reduce friction, and extend tool life [44,147]. For instance, Zhu et al. [147] studied the mechanical and tribological properties of TiN/Ti(C,N)/Al2O3 multilayer coatings deposited using a thermal CVD system and investigated the effects of operational conditions on tool wear. Tool-life tests (Figure 9) revealed good adhesion between κ-Al2O3 and Ti(C,N)-based layers and exhibited the longest tool life, double that of a commercial CVD Al2O3 multilayer coating [147].
Figure 9. Tool-life plots for cutting tests of 24CrMoV5-1 steel. Reprinted from ref. [147].
In another study, Chen et al. [148] successfully enhanced the wear resistance of the CVD-coated inserts employing a composite process for CVD post-treatment. In their work, a TiN/MT-TiCN/TiN/α-Al2O3 composite coating was deposited on a cemented carbide substrate through CVD and assessed to evaluate the influence of different post-treatment processes. The longest tool life was achieved with the inserts that underwent the combined process.
Apart from ceramic coatings, CVD diamond and related hard carbon allotrope films exhibit extremely high hardness, wear resistance, and low coefficients of friction and are therefore widely used in the machining industry for various wear and antiwear tools [149,150]. Synthetic diamond coatings deposited via microwave plasma CVD exhibit very high hardness (90–100 GPa) and thermal conductivity (2000 W/m·K and have been investigated for machining high-strength alloys. Under the reported machining conditions, tool-life improvements of 10–20 times relative to tungsten-carbide tools have been demonstrated [151]. Zhang et al. [152] studied the tribology and cutting performance of a boron-doped diamond composite-coated tool using the hot-filament CVD technique. Cutting experiments show that the boron-doped microcrystalline diamond-nanocrystalline diamond film showed excellent wear resistance and the best cutting performance [152]. Zhao et al. [153] demonstrated superior performance of a CVD diamond tool when compared with a coated cemented carbide tool. In another work, Parray et al. [154] showed that, in contrast to ordinary cemented tungsten carbide (WC-Co) cutting tools, the CVD diamond coatings on WC-Co inserts enhanced the machining performance of EN24 steel.
Collectively, these studies demonstrate that CVD is particularly attractive for cutting tools and wear-resistant components where high coating durability, strong adhesion, and resistance to severe mechanical and thermal loading are prioritized. The reported improvements in tool life also indicate that coating performance depends not only on the deposited material but on the multilayer architecture, deposition conditions, and post-treatment strategy. Compared with PVD, CVD can provide thicker and highly stable ceramic coatings, which is advantageous for demanding machining conditions; however, the higher processing temperature imposes greater restrictions on substrate selection. Therefore, the choice of CVD over PVD is not determined solely by the intrinsic hardness or wear resistance of the coating, but by the balance between required coating performance and the thermal limitations of the substrate. For temperature-sensitive substrates, lower-temperature CVD variants such as PECVD may offer an alternative, although the resulting coating characteristics must be assessed against the requirements of the specific application.
Microelectronics
Among the different deposition techniques for fabricating functional coating systems, CVD has been employed industrially in microelectronics and several other sectors [16,155,156]. CVD is fundamental to semiconductor fabrication, enabling deposition of polysilicon, dielectric films, and metal interconnects with high precision and uniformity. CVD is used for achieving thin films of polycrystalline silicon (poly-Si) or doped poly-Si for use as carrier-selective passivating contacts, which are one of the key enabling technologies for the tremendous efficiency improvements in crystalline silicon solar cells [16,157,158,159]. Particularly, the APCVD technique enables a low-cost, simple manufacturing process to achieve poly-Si passivating contacts [160]. For integration of transistors in the semiconductor industry, metal lines and low-dielectric-constant films are used as intermetal dielectrics (IMDs) to reduce RC delays and crosstalk in multilevel metallization processes. In this regard, silicon carbon-nitride (SiCN) films or porous low-k SiCOH deposited by PECVD are widely used as a metal diffusion barrier [161,162,163,164].
These examples illustrate that CVD variant selection in microelectronics involves a trade-off between deposition throughput, thermal budget, film uniformity, and functional requirements. APCVD can be attractive where process simplicity and high-throughput production are important, whereas PECVD provides greater flexibility when lower-temperature deposition is required for dielectric and barrier layers. Thus, increasing device complexity does not necessarily favor a single CVD variant; rather, the appropriate process depends on the thermal sensitivity of the underlying structure and the specific electrical, barrier, and dimensional requirements of the deposited film.
Superconducting Materials
CVD is used to produce high-quality coatings of superconducting materials such as MgB2 and Nb3Sn with controlled thickness for superior RF performance levels in Superconducting Radio-Frequency (SRF) cavities [165,166,167,168,169].
Although representing a comparatively specialized application, these studies demonstrate the capability of CVD to fabricate dense, compositionally controlled superconducting coatings required for advanced accelerator and quantum technologies. In this context, the value of CVD lies primarily in its ability to achieve controlled coating composition and thickness over technically demanding substrates, while the relatively specialized application limits the extent to which these advantages can be generalized to conventional industrial coating systems.
Superhydrophobic Coatings
Transparent, wear-resistant, superhydrophobic inorganic coatings on glass substrates are desirable for applications in high-rise building glass curtain walls, windshield glass, and solar-cell cover glass. Zheng et al. [170] prepared a transparent and wear-resistant superhydrophobic film on glass via a two-step phase separation and CVD process. Transparent, superhydrophobic polymer nanocone array coatings with excellent mechanical durability and anti-icing performance were fabricated via a facile one-step iCVD process [171].
Besides, ceramic-based superhydrophobic coatings on metal surfaces provide a protective layer against corrosion [172,173]. For instance, Cao et al. [172] in their study showed better anti-icing performance of the F-SiO2-coated surface as compared to the uncoated surface.
These examples illustrate the versatility of CVD in tailoring surface chemistry and hierarchical surface morphology, enabling functional coatings that combine water repellency with durability, transparency, or corrosion protection depending on the target application. However, the multifunctionality achieved in these systems also highlights a key design challenge: improving water repellency, transparency, mechanical durability, and corrosion protection simultaneously may require compromises in coating composition and surface architecture. Consequently, CVD selection for superhydrophobic applications should be based on the dominant functional requirement rather than hydrophobicity alone.
Biomedical Coatings
Biomedical coatings are revolutionizing healthcare by enhancing the integration, safety, and functionality of medical devices. These coatings address critical challenges such as infection, biocompatibility, and therapeutic delivery, enabling advancements in implants, prosthetics, and drug delivery systems. Chemically inert passivation layers or antimicrobial coatings on implantable devices not only isolate adjacent channels electrically but also protect the implanted device from implant-associated infections [174,175,176,177,178,179]. CVD-based coating techniques particularly show distinct advantages for antibacterial applications since they allow precise control over coating chemistry and thickness regardless of the substrate characteristics [177,178,179,180]. CVD transforms medical implants by not only adding a high-performance layer that boosts biocompatibility and durability, but also by making surfaces harder and more resistant to wear or corrosion, thereby extending their lifespan [178]. Beyond protection, these coatings can even be engineered to assist with controlled drug delivery directly at the implant site.
Amorphous silicon carbide (a-SiC) coating is widely considered for the biocompatible coating of implantable devices [181]. Su et al. [180] fabricated self-regenerating antibacterial coating surfaces via vapor deposition (iCVD) of layered polymer nanocoatings. The trilayered coating consisted of top and bottom antibacterial PDE layers and an intermediate biodegradable PMAH-based layer, as depicted in Figure 10. Rico et al. [177] deposited graphene on a medical-grade cobalt-chromium alloy surface by RF-PECVD, which exhibited high biocompatibility, antibacterial, and antifouling properties.
Figure 10. Schematic of a three-stage deposition process of the layered degradable coating using iCVD. Sequentially deposited were PDE as the antibacterial layer, PMAH or its copolymer as the biodegradable layer, and another PDE antibacterial layer. Reproduced with permission from ref. [180]. Copyright 2021 American Chemical Society.
Carbon-based and tantalum (Ta) coatings by CVD on metal alloy substrates such as austenitic stainless steel, SiC, Co-Cr, and Ti alloys are promising for orthopedic, vascular stent, and dental implants [182,183,184,185,186,187,188].
Compared with many alternative deposition techniques, CVD offers flexibility in tailoring surface chemistry while maintaining coating uniformity on complex implant geometries. However, biomedical application introduces additional constraints beyond coating uniformity and functional performance, including substrate compatibility, processing temperature, and the biological response to both the coating and any residual process-related species. Therefore, the suitability of CVD for biomedical coatings depends on achieving the required surface functionality without compromising the integrity and biological compatibility of the underlying implant.
From an application perspective, CVD is generally attractive when excellent coating uniformity, conformal coverage of complex geometries, and high-quality ceramic, semiconductor, or diamond coatings are required. However, when lower processing temperatures, atomic-scale thickness control, or thick structural coatings are the primary design requirements, PVD, ALD, or laser cladding, respectively, may represent more appropriate alternatives.

2.3.3. Advantages, Challenges, and Outlook

CVD offers several key advantages, including excellent coating conformality, high density, strong adhesion, and broad material compatibility. The ability to tailor microstructure through process parameters makes it highly versatile for advanced applications. Recent developments in CVD have focused on reducing processing temperatures, improving precursor efficiency, and enabling environmentally sustainable processes. Plasma-enhanced techniques have significantly expanded the applicability of CVD to temperature-sensitive substrates by lowering reaction temperatures while maintaining film quality. In parallel, advances in precursor chemistry have enabled the controlled growth of nanostructured and functional materials, including graphene, diamond-like carbon (DLC), and other two-dimensional materials, with tailored microstructures and properties.
However, several challenges remain. High processing temperatures in conventional CVD can restrict substrate selection and induce thermal stresses. Additionally, the use of toxic, corrosive, or hazardous precursor gases and the relatively high energy consumption present environmental and safety concerns, while also increasing operational costs and posing economic challenges. Achieving uniform deposition over large areas and complex geometries, particularly in industrial-scale systems, remains another critical challenge.
These limitations reveal a fundamental trade-off in CVD between deposition performance and process sustainability. The same chemical reactivity and elevated temperatures that enable dense, adherent, and compositionally controlled coatings can also increase the thermal budget, energy demand, and environmental and safety burden of the process. Lower-temperature approaches such as PECVD can broaden substrate compatibility, but reducing the thermal budget does not by itself eliminate the need to control film quality, residual stress, precursor utilization, and process stability. Similarly, improving conformality and coating uniformity at larger scales remains challenging because reactor conditions, precursor transport, and surface reactions must be controlled simultaneously. Therefore, an important research gap is the development of CVD processes that can achieve the coating quality and compositional control associated with conventional CVD while simultaneously reducing temperature, energy consumption, hazardous precursor use, and scale-up complexity.
Looking forward, future developments in CVD should focus not only on lowering deposition temperature but on simultaneously improving energy efficiency, precursor utilization, process stability, and scalability. Low-temperature routes, including further refinement of plasma-assisted and catalytic CVD techniques, may expand substrate compatibility; however, their industrial significance will ultimately depend on whether reductions in thermal budget can be achieved without compromising coating quality and reproducibility. Similarly, safer and more sustainable precursor chemistry is essential, but precursor substitution must be evaluated together with deposition efficiency, film properties, waste generation, and overall process economics. Integration with hybrid deposition approaches and advanced process-control strategies therefore represents an important pathway toward balancing coating performance with manufacturing and environmental constraints.
Emerging approaches such as artificial intelligence and machine learning could further address the strong coupling between CVD process parameters, precursor chemistry, reactor conditions, and coating properties by enabling data-driven process optimization and predictive modeling. However, the practical value of such approaches will depend on the availability of reliable and sufficiently representative process data and on their ability to generalize across different reactor configurations and material systems. Similarly, high-entropy materials and two-dimensional materials offer opportunities to expand the functional range of CVD coatings, but challenges associated with compositional control, phase stability, defect formation, and reproducible large-scale deposition remain to be resolved. Hybrid manufacturing approaches may provide another route to overcome the limitations of individual processes by combining the complementary capabilities of different deposition and surface-engineering technologies.

2.4. Atomic Layer Deposition (ALD)

Atomic layer deposition (ALD) is an advanced vapor-phase thin-film deposition technique based on sequential, self-limiting surface reactions that enable atomic-scale control over film thickness and composition. In a typical ALD cycle, precursor gases are introduced alternately into the reaction chamber, where each precursor reacts with the substrate surface in a controlled manner to form approximately one atomic layer per cycle (Figure 11). Excess precursor molecules and gaseous reaction by-products are removed during intervening purge steps, ensuring uniform film growth and excellent conformality. Owing to its unique self-limiting growth mechanism, ALD is particularly well suited for depositing highly conformal coatings on complex three-dimensional and high-aspect-ratio structures, making it indispensable for nanoscale applications.
Figure 11. Schematic illustration of a typical ALD cycle. Reprinted with permission from ref. [189]. Copyright 2026 Wiley-VCH GmbH.

2.4.1. Classification of ALD Techniques

ALD processes can be categorized based on activation method and reactor configuration.
(a) Thermal ALD: It is the most conventional form of ALD and relies purely on thermal energy rather than plasma to activate precursors. It typically operates within a defined ALD temperature window (150–350 °C), providing excellent conformality over high-aspect-ratio structures and precise control over film thickness; however, its applicability is limited to precursor chemistries that exhibit sufficient surface reactivity within the ALD temperature window.
(b) Plasma-enhanced ALD (PEALD): Also known as plasma-assisted ALD, it is a thin-film deposition technique that uses plasma-generated reactive species (such as radicals) rather than thermal energy to grow high-quality, ultra-thin coatings at low temperatures. It is used in semiconductor manufacturing to deposit materials like titanium nitride (TiN), silicon nitride (SiN), and aluminum oxide (Al2O3) on temperature-sensitive substrates, offering improved material density, reduced impurities, higher growth rates, and shorter processing times [190,191,192].
(c) Spatial ALD (SALD): It is an advanced, high-throughput thin-film coating technique where precursor gases are separated physically in space rather than time, allowing for continuous, rapid deposition at atmospheric pressure. Unlike traditional ALD, which is slow due to sequential gas purging, Spatial ALD continuously injects precursors, with inert gas barriers keeping them separate. The process is easily scaled up and compatible with roll-to-roll (R2R) and sheet-to-sheet (S2S) processing, while maintaining the high-quality, pinhole-free, conformal, atomic-level thickness control of traditional ALD. Spatial ALD represents a major advancement toward the industrialization of ALD by substantially increasing deposition throughput while reducing processing cost and energy consumption. SALD is used for developing flexible electronics and display technology; coating electrodes, membranes, and separators for lithium-ion batteries and fuel cells (e.g., Al2O3, TiO2, ZnO); applying passivation layers to high-efficiency solar cells and as barrier layers for creating thin films to protect against moisture and oxygen [193].
(d) Area-Selective ALD (AS-ALD): It is a bottom-up, thin-film deposition technique that selectively grows material only on designated surface areas rather than the entire substrate. By using inhibitor molecules or inherent surface differences to block deposition elsewhere, it achieves nanoscale thickness control, thereby eliminating complex masking steps, reducing fabrication cost, and minimizing edge-placement errors. AS-ALD is crucial in advanced semiconductor manufacturing and nanotechnology, including next-generation nanoelectronics [194] and patterning 2D materials (e.g., selective growth on 2D materials like MoS2 or graphene) [195].
(e) Molecular Layer Deposition (MLD): It is a variant of ALD that uses sequential, self-limiting surface reactions to deposit organic or organic-inorganic hybrid materials at the molecular level, producing polymer-like thin films and hybrid coatings with subnanoscale precision. MLD is often used for flexible coatings, battery electrodes, biomedical devices, and barrier layers [196,197].
The various ALD techniques differ primarily in their activation mechanism and processing strategy. Thermal ALD remains the benchmark for producing highly uniform, conformal films with precise atomic-scale thickness control, whereas plasma-enhanced ALD (PEALD) enables deposition at significantly lower temperatures while improving film density and material quality. Spatial ALD (SALD) addresses one of the principal limitations of conventional ALD by substantially increasing deposition throughput, making large-area and roll-to-roll manufacturing feasible. Area-selective ALD (AS-ALD) enables direct nanoscale patterning without complex lithographic masking, while molecular layer deposition (MLD) extends the ALD concept to organic and hybrid organic–inorganic materials. Consequently, the selection of an appropriate ALD technique depends primarily on substrate temperature limitations, throughput requirements, patterning needs, and the desired coating chemistry rather than on film thickness alone.

2.4.2. Applications of ALD Coatings

Owing to its exceptional conformality and atomic-scale thickness control, ALD has found widespread application in several advanced technologies. Representative examples are discussed below.
Microelectronics
ALD has become indispensable in semiconductor device fabrication, enabling deposition of high-k dielectric (such as ZrO2, Al2O3, and HfO2) layers, channel materials, metal gate electrodes, diffusion barriers, and gate oxides [198,199,200,201]. Intel was the first to implement ALD in CMOS circuits with HfO2-based high-k films, replacing traditional thermally grown SiO2 gate dielectrics. Figure 12 shows a TEM image of an ALD-deposited SiNx film having a conformality of >95% [202].
Figure 12. Cross-sectional TEM image of a SiNx film deposited using ALD process at 400 °C ref. [202]. Copyright 2018 American Chemical Society.
Recently, Liu et al. [203] successfully fabricated high-performance ZnO thin-film transistors at few-μm resolution using low-temperature ALD (at 150 °C), patterned by high-resolution reverse-offset printing (Figure 13). Highly conductive ultrathin niobium carbide thin films (2.6 nm) as diffusion barriers for Cu and Ru interconnects were grown by PE-ALD on SiO2 substrates at 100–400 °C [204]. Figure 14a,b shows the four-point bending test performance of the PEALD-NbCx coatings as an adhesion-promoting layer for Cu and Ru interconnects, showing high critical loads and scratch resistance in the mechanical tests [204]. Figure 14c shows the uniform and conformal coating of NbCx film onto the complex topography of the 3D trench, with a step coverage of ~100% achieved using PE-ALD [204]. Development of flexible wearable electronics has also benefited from advances in ALD nano-coating [205,206,207]. Li et al. [206] fabricated high-performance flexible field-effect transistors based on ferroelectric Zr-doped HfO2 (HZO) and ultrathin ITO channels on a flexible MICA substrate (Figure 15), where 100 nm Al2O3 and 11.4 nm HZO were grown by ALD at 250 °C.
Figure 13. (a) Low-temperature ALD-grown 10 cm × 10 cm sample with 2 cm × 2 cm reticles and (b) ZnO TFT array. ref. [203]. Copyright 2025 American Chemical Society.
Figure 14. Load vs. displacement curves for (a) Cu (40 nm)/NbCx (2.6 nm)/SiO2 (100 nm) and (b) Ru (40 nm)/NbCx (2.6 nm)/SiO2 (100 nm) structures. (c) TEM image of the 3D trench substrate (depth: 400 nm; bottom width: ∼275 nm) coated by the PEALD-grown NbC layer. Reprinted with permission from ref. [204]. Copyright 2025 American Chemical Society.
Figure 15. (a) Photograph of the highly transparent and flexible device in a bent state. (b) Schematic of the flexible ITO FeFET memory devices. (c) The key experimental method flow of the HZO-based FeFET fabrication process. (d) HRTEM image of the Ni/ITO/HZO/W/Ti/Al2O3 gate stack. HRTEM shows clear crystallization of the HZO material and an ultra-thin 3.4 nm ITO channel. Reprinted with permission from ref. [206].
Energy Conversion and Storage Applications
ALD coatings improve the stability and performance of lithium-ion batteries, supercapacitors, and perovskite solar cells by enhancing interfacial stability and preventing degradation. In solar cells (including silicon, organic, thin film, perovskite, and quantum dot cells), ALD coatings are used as a surface passivation layer, buffer layer, window layer, absorber layer, electron/hole contact, or transparent conductive oxide [157,208,209,210,211,212,213,214,215]. For example, research has shown that ALD facilitates controllable ultra-thin and dense surface coating of quantum dots (QDs) at the atomic scale, enabling stability and longevity of their exceptional optoelectronic performance, indispensable for QD-based devices such as QLEDs, solar cells, and microLED displays [216,217,218,219]. Cheng et al. [217] reported on photo-stability enhancement of Al2O3-passivated colloidal CdSe/ZnS QDs. Selective surface passivation via ALD protects QDs from photo-oxidation and enhances photo-stability, critical for LED applications. Xie et al. [216] coated TiO2 nanorod arrays/CdS quantum dots via ALD, enhancing their photoelectrochemical and photocatalytic performance.
Leveraging conformal coatings and pinhole-free films with atomic-level thickness, ALD has shown great potential in deposition and surface modification of advanced electrode materials in electrochemical energy storage devices [216,220,221,222,223,224,225,226,227,228]. For example, Lopa et al. [228] fabricated ALD-deposited tungsten trioxide/molybdenum trioxide (WO3/MoO3) nanohybrid heterostructure electrodes, achieving high energy storage capacity and stability.
These examples demonstrate that the precise thickness control and conformal nature of ALD coatings play a critical role in enhancing interfacial stability, suppressing degradation, and improving the long-term performance of advanced energy conversion and storage devices.
Protective and Barrier Coatings
Thin ALD coatings serve as barrier films and membrane coatings that are used for filtration of water and air, and also act as effective moisture and gas barriers in flexible electronics and packaging applications [229,230,231,232,233,234]. For instance, Yang et al. [234] prepared a protein-activated ALD-TiO2-coated membrane, resulting in superhydrophilic nanoarmour on the membrane that demonstrated robust wettability and crude-oil-repellent stability.
Catalyst Surface Engineering
ALD enables atomic-scale surface engineering of catalysts and nanostructured materials with exceptional control over thickness, composition, and conformality. For designing efficient and durable catalysts, ALD has shown unique merits by allowing precise tuning of active sites and surface chemistry through the deposition of highly dispersed nanoparticles or even single atoms, and ultrathin overcoats, thereby tailoring the support-catalyst interface for enhancing electrochemical performance [235,236,237,238,239,240]. Currently, the molecular- and plasma-enhanced ALD techniques are widely used for the development of advanced catalysts [240]. Song et al. [241] presented a pioneering work on creating a sub-nano WO3 bridge layer between Pt nanoparticles and a carbon substrate (nitrogen-doped carbon nanotubes, NCNT) through ALD, resulting in a Pt-WO3-NCNT catalyst exhibiting remarkable stability and catalytic activity. Chen et al. [237] prepared a highly efficient and stable Pt-MoO3/CNT electrocatalyst via ALD for methanol oxidation and oxygen reduction reaction.
These studies demonstrate that ALD provides exceptional control over catalyst architecture at the atomic scale, enabling precise engineering of active sites and support interfaces for improved catalytic activity and long-term stability.
From an application perspective, ALD is the preferred deposition technique when atomic-scale thickness control, excellent conformality, and uniform coating of high-aspect-ratio structures are required. Thermal ALD remains the benchmark for high-quality conformal films, whereas PEALD is favored for temperature-sensitive substrates and improved film density. SALD addresses industrial throughput limitations, while AS-ALD and MLD enable specialized applications requiring selective deposition or organic–inorganic hybrid coatings. Consequently, ALD is particularly well suited for advanced microelectronics, energy storage devices, catalyst engineering, and other nanoscale technologies where precise interfacial control is essential.

2.4.3. Advantages, Challenges, and Outlook

ALD offers several distinct advantages over conventional deposition techniques, including atomic-scale thickness control, excellent conformality, high film uniformity, and the ability to deposit coatings at relatively low temperatures. Film thickness can be precisely controlled through the number of deposition cycles, while the self-limiting surface reactions enable uniform coating of complex geometries, porous materials, and high-aspect-ratio structures. Recent developments in ALD have focused on improving scalability and expanding its applicability. Spatial ALD has emerged as a promising approach for increasing deposition throughput by spatially separating precursor exposure, thereby enabling continuous processing. In addition, roll-to-roll ALD systems have been developed for large-area and flexible substrates, facilitating applications in flexible electronics and advanced coatings. Another significant advancement is area-selective ALD, which enables material growth on predefined surface regions and can reduce or potentially eliminate the need for conventional lithographic patterning in selected applications, making it attractive for next-generation nanofabrication and device integration.
Despite its advantages, several challenges limit the widespread industrial adoption of ALD. The cyclic nature of self-limiting surface reactions generally results in relatively low deposition rates, restricting throughput, particularly for thick coatings and large-area production. Furthermore, the availability of suitable precursors is constrained by requirements such as sufficient volatility, thermal stability, and surface reactivity, which can limit material versatility and increase process cost. The precise control of precursor exposure, reaction, and purge steps also increases reactor and process complexity, particularly when uniform deposition must be maintained over large or complex substrates.
Looking forward, ongoing research is directed toward overcoming the throughput, precursor, and process-complexity limitations of ALD through the development of higher-throughput configurations, including spatial ALD, together with improved precursor chemistries and process optimization. Plasma-enhanced ALD is expected to remain important for extending low-temperature deposition and improving film properties on temperature-sensitive substrates. Hybrid deposition strategies combining ALD with PVD or CVD may provide a practical route to balance atomic-scale control and conformality with higher deposition productivity and broader process scalability. Furthermore, emerging ALD-enabled approaches for three-dimensional device architectures are being explored for increasing integration density and functional complexity in advanced nanoelectronic systems, including applications such as neuromorphic computing, integrated photonic circuits, and flexible electronics [189].

2.5. Electrodeposition

Electrodeposition is a versatile electrochemical technique used to deposit metallic, alloy, and composite coatings from electrolyte solutions onto conductive substrates [242]. The process commonly involves electrochemical reduction or oxidation of dissolved species at an electrode under an applied potential or current, enabling control over coating thickness, composition, and microstructure [243]. According to IUPAC, electrodeposition incorporates the deposition of dissolved or suspended species onto an electrode under an applied electric field and therefore includes a broader range of electrochemically driven deposition processes. In coating applications, however, the term is often used more narrowly to describe cathodic metal deposition, or electroplating, in which metallic ions are reduced at the cathode to form a coating on the substrate. In such systems, the deposited amount is primarily governed by the charge passed, although the actual deposition rate also depends on current efficiency and competing electrochemical reactions [244].
A major advantage of electrodeposition is its ability to produce metallic, alloy, and composite coatings with controlled microstructure through manipulation of parameters such as current density, applied potential, electrolyte composition, temperature, and mass transport conditions. Modified approaches, including pulse and pulse-reverse electrodeposition, provide additional control over nucleation and growth, enabling grain refinement, improved coating density, and tailored functional properties. The relatively low processing temperature provides a low thermal budget compared with thermally intensive deposition processes, making electrodeposition attractive for coating a wide range of engineering substrates. However, achieving uniform deposition on geometrically complex or recessed surfaces can be challenging because local current-density distribution and mass transport vary across the substrate. Consequently, careful control of bath chemistry, electrode configuration, agitation, and deposition parameters is required to obtain reproducible coating thickness, composition, and microstructure [245,246,247,248,249,250,251,252,253].

2.5.1. Classification of Electrodeposition Techniques

Electrodeposition-based coating processes can be broadly classified according to the nature of the deposited species and the mechanism by which the coating is formed. For metallic and alloy coatings, conventional electroplating is primarily governed by electrochemical reduction of metal ions at the cathode, whereas electrophoretic deposition involves the migration and deposition of charged particles from a suspension. In addition, several modified electrodeposition routes have been developed to control coating microstructure and functionality.
(a) Cathodic and anodic electrodeposition
Cathodic electrodeposition and anodic electrodeposition are commonly used terms in electrocoating, particularly for polymeric coating systems. In cathodic electrodeposition (CED), positively charged resin species migrate toward the negatively charged cathode, where electrochemical reactions at the electrode surface promote resin deposition. In anodic electrodeposition (AED), negatively charged resin species migrate toward the positively charged anode and are deposited through the corresponding electrochemical process [254,255].
Cathodic electrodeposition (CED) has become an important industrial coating process, particularly for corrosion protection, owing to its ability to produce highly uniform films with strong adhesion and broad coverage, including on complex geometries. The use of waterborne resin systems can reduce VOC emissions relative to solvent-borne systems.
Compared with traditional solvent-based coating approaches, CED relies primarily on water-based resin systems such as acrylic, epoxy, epoxy–acrylate, and polyurethane. The process requires specially engineered resins that can be rendered electrophoretically mobile and deposited onto cathodic substrates. As a result, CED coatings typically provide improved corrosion protection, strong adhesion to metallic substrates, and effective coverage of irregular surfaces and intricate designs. However, CED is more appropriately regarded as an electrocoating process involving charged polymeric species rather than as a direct equivalent of conventional metallic electroplating.
(b) Electrophoretic Deposition (EPD)
A closely related but distinct technique is electrophoretic deposition (EPD), which involves the movement and deposition of charged particles, often non-conductive materials such as ceramics or polymers, under an applied electric field [256]. Unlike conventional metal electroplating, EPD enables the fabrication of coatings from suspensions of colloidal particles and is therefore particularly suitable for depositing ceramic, polymeric, and composite materials on conductive substrates. Because charged particles migrate electrophoretically toward an electrode, coating formation depends strongly on particle charge, suspension stability, and the solvent–binder–dispersant system. EPD is increasingly applied beyond traditional wear-resistant and antioxidant coatings, including functional films for microelectronics and solid oxide fuel cells, bioactive coatings for implants, nanoscale assembly, complex compounds, and ceramic laminates [257,258,259,260,261,262]. Its main intrinsic limitation is that aqueous suspensions can promote gas evolution at the electrodes during deposition, which may affect coating quality; this limitation can be mitigated using suitable non-aqueous solvents and optimized deposition conditions.
A related variant, electrophoretic co-deposition, extends conventional EPD by enabling the simultaneous deposition of two or more particle populations, such as ceramic nanoparticles and carbon nanotubes, to form multifunctional nanostructured coatings. Such coatings are frequently investigated for functional applications, including fuel cell components.
(c) Related and Specialized Electrodeposition variants
In addition to conventional electrodeposition and EPD, several related or modified coating processes are sometimes discussed alongside electrodeposition because of their applications or process similarities, although not all are strictly electrochemical electrodeposition processes. Some of them are outlined below.
Pulse Electrodeposition (PED): Pulse electrodeposition employs a time-varying current or potential waveform, including pulse and pulse-reverse modes, rather than continuous direct current, enabling improved control over nucleation and growth processes and resulting in refined grain structures and enhanced mechanical and corrosion-resistant properties [263,264].
Composite Electrodeposition: Composite electrodeposition involves the incorporation of dispersed solid particles, such as Al2O3, SiC, or carbon-based nanomaterials, into a growing metallic matrix to produce coatings with superior hardness, wear resistance, or self-lubricating characteristics.
Brush Electrodeposition: Brush electrodeposition is a localized variant used for repair and selective coating, in which the electrolyte is supplied through a moving electrode or brush, allowing precise deposition on targeted regions. This approach is particularly attractive for localized repair or dimensional restoration of worn or damaged surfaces without requiring complete component recoating.
Ultrasound-assisted electrodeposition (UAED): UAED has gained attention as a practical route to improve the quality and performance of electrodeposited metallic coatings compared with conventional depositions. UAED combines electrodeposition with ultrasonic irradiation to enhance mass transport through cavitation and acoustic streaming. These effects can reduce concentration polarization and improve ion transport to the electrode surface, often promoting finer-grained, denser, and more uniform deposits with improved mechanical, wear, and corrosion properties. However, scale-up, additional energy requirements, and possible electrolyte instability under prolonged sonication remain challenges.
Autodeposition: Autodeposition is a chemically driven coating process that does not require an external power supply. Film formation occurs through chemical and/or redox reactions at the substrate surface. Because the process is not driven by an externally applied electric field, autodeposition is mechanistically distinct from electrodeposition; it is nevertheless sometimes discussed alongside electrodeposition-based coating technologies because of its application in corrosion protection and surface finishing.
The various processes discussed in this classification differ primarily in deposition mechanism, deposited material, electrical waveform, process configuration, and the use of external-field or particle-assisted strategies. Conventional electroplating enables controlled deposition of metals and alloys, whereas EPD extends the approach to particulate ceramic, polymeric, and composite systems. Pulse and pulse-reverse methods provide greater control over nucleation and growth, while composite and electrophoretic co-deposition enable multifunctional coatings. Localized approaches such as brush electrodeposition are particularly suited to repair and dimensional restoration, whereas assisted processes such as ultrasound-assisted electrodeposition can improve mass transport and deposit uniformity. Consequently, the selection of an appropriate electrodeposition route depends primarily on the coating material, substrate geometry, required microstructure and functionality, deposition rate, and process-control requirements.

2.5.2. Applications of Electrodeposition

Electrodeposition and related electrically assisted deposition processes are widely used for preparing metallic, alloy, polymeric, composite, and particulate coatings on conductive substrates, with applications ranging from corrosion protection and decorative finishing to energy systems, electronics, and biomedical devices. Their versatility arises from the ability to control coating thickness, composition, morphology, and microstructure through the applied current or potential and electrolyte or suspension conditions.
Common applications include:
Corrosion Protection and Wear-Resistance
Electrodeposited coatings such as nickel, zinc, and chromium can provide adherent protective layers with controlled thickness and good corrosion and wear resistance, thereby protecting metal substrates from corrosive degradation in marine, automotive, and tribological applications. Nanocomposite coatings (e.g., Ni-P-SiC, Ni-B-TiN, Ni-CeO2, Ni-Co-Al2O3) can further enhance hardness, wear resistance, and frictional performance, extending the service life of mechanical components, gears, and cutting tools [265]. Besides a broad spectrum of coating materials, including chromium, nickel, cobalt, zinc, and copper, the incorporation of alloying elements into single-metal coatings can further improve their in-service performance by enhancing mechanical, tribological, and corrosion-resistant properties. Extensive work has been conducted to investigate the influence of nanoparticle co-deposition (e.g., SiC, CNTs, Al2O3), electrodeposition conditions, and process parameters on the mechanical, tribological, wear, and corrosion performance of these coatings [266,267,268,269,270,271,272,273,274,275,276,277,278,279].
Collectively, these studies demonstrate that electrodeposition provides a versatile route for tailoring metallic and metal–matrix composite coatings to simultaneously improve corrosion resistance, hardness, wear behavior, and frictional performance.
Decorative Finishing
Electrodeposition enables highly uniform and aesthetically appealing finishes for consumer products, jewelry, and architectural metals, while simultaneously providing corrosion protection and mechanical durability [280,281,282,283,284,285]. For decorative applications, electrodeposited coatings provide lustrous and durable surfaces on metallic and, in some cases, plastic substrates, thereby combining aesthetic appeal with functional protection. Common materials include gold, silver, nickel, copper, brass, and chromium alternatives such as tin-cobalt. Electrodeposition offers excellent decorative control, but traditional decorative plating has significant environmental and regulatory challenges associated with hazardous electrolyte chemistries.
Traditional decorative plating commonly employs copper, nickel, gold, silver, and other noble or functional metals to obtain controlled appearance, reflectivity, hardness, and corrosion resistance [286,287,288]. However, several established plating chemistries raise environmental, occupational, and regulatory concerns, particularly those involving cyanide-containing electrolytes and hexavalent chromium. This has stimulated the development of alternative bath chemistries and lower-hazard plating systems, although these alternatives may involve trade-offs in bath stability, deposition efficiency, appearance, or process control.
Modern techniques, such as pulsed-current electrodeposition, can improve deposit morphology, thickness uniformity, surface appearance, and deposition efficiency, depending on the waveform and bath chemistry. For instance, Mariani et al. [289] demonstrated that Au-Ni deposits obtained using pulsed currents exhibited finer and more compact grains, resulting in a smoother, glossier, and brighter finish and markedly improved corrosion resistance compared with deposits obtained using direct current. In another work, Mariani et al. [290] presented a systematic study of pulse and pulse-reverse plating using an acid copper bath for decorative and functional applications, and concluded that pulsed-current deposition produced improved characteristics compared with direct-current deposition, whereas reverse-pulsed currents are preferable when coating-thickness homogeneity is prioritized over surface esthetics. Verrucchi et al. [283] reported on the electrodeposition of Sn-Ru alloys using direct, pulsed, and pulsed-reverse currents for decorative applications. The uniformity of the electrodeposited layer was analyzed by XRF (Figure 16). The sample deposited using pulsed-reverse current (tC = 2 ms) exhibited remarkably homogeneous thickness, with a standard deviation of only 2 nm.
Figure 16. XRF thickness maps of the Sn-Ru deposit. (a) direct current sample 1 A/dm2, (b) pulsed current 2 ms, (c) pulsed current 5 ms, (d) pulsed current 10 ms, (e) pulsed reverse current 2 ms, (f) pulsed reverse current 5 ms, (g) pulsed reverse current 10 ms. Reprinted with permission from ref. [283].
Functional Surfaces
Electrodeposition enables the fabrication of functional coatings with tailored electrochemical, magnetic, and electrical properties. Electrodeposited materials, including cobalt- and nickel–iron-based alloys and cobalt phosphide, have been investigated for electrocatalysis, energy storage, and magnetic applications. In the field of energy, electrodeposited materials such as cobalt phosphide on conductive substrates have demonstrated excellent electrocatalytic activity for hydrogen evolution reactions, highlighting the technique’s relevance to sustainable energy technologies. Jia et al. [254] successfully deposited a two-dimensional conductive metal–organic framework on nickel foam for use as electrodes in supercapacitors, which demonstrated outstanding electrochemical performance.
Besides corrosion and wear resistance, the electrodeposited Ni-Fe coatings are widely employed for magnetic applications, including pole pieces in magnetic valves, magnetic heads for tape recorders, flux guides in thin-film write heads, magnetic recording shields, and cores of on-chip inductors, as well as for electronic applications such as memory, recording and storage devices, null-balance transformers, pulse transformers, and relay components [291,292,293,294,295,296]. Rasmussen et al. [292] developed a new bath formulation for pulse-reverse electroplating of CoNiFe for magnetic microsystem applications. Sun et al. [295] electrodeposited Ni80Fe20 Permalloy for use as the magnetic core of integrated flexible parylene-based MEMS inductors, achieving increased inductance and quality factor. In another work, a giant magnetoresistance ratio of 5.4% was achieved for electrodeposited [Ni80Fe20/Cu/Co/Cu] spin-valve multilayers on NiFe buffer layers [294].
Electronics and Microfabrication
Electrodeposition is widely used to fabricate metallic interconnects, conductive traces, and microstructures for printed circuit boards (PCBs), microelectronic devices, and MEMS components, benefiting from precise thickness control and high reproducibility [297,298,299,300,301]. In this context, electrodeposited nanotwinned metals have been studied extensively for interconnect applications in nanoelectronic devices and nanoelectromechanical systems because of their high strength, ductility, and electrical conductivity [299]. Nanoscale twin-metal formation has been achieved using both direct-current and pulsed-current deposition [302,303,304,305,306,307,308,309,310,311,312]. For example, Dong et al. [311] reported nanotwinned Cu micro-cone arrays fabricated by pulse electrodeposition without any template. The morphology of the micro-cones was found to be controllable through the Cl− concentration in the electrolyte. Furthermore, the nano-twinned micro-cone arrays enabled low-temperature bonding with a 50% enhancement in bonding performance, rendering them promising for advanced 3D electronic packaging applications.
Metal-Recovery
Beyond surface coating, electrodeposition is also widely employed for electrochemical metal recovery, particularly in hydrometallurgical and waste-treatment processes. Examples include the recovery of precious metals such as gold, silver, and copper from solution through electrodeposition or electrochemistry-based recovery processes [313,314,315,316,317]. Li et al. [314] recovered nickel from real electroplating wastewater using an integrated process combining electrodeposition with adsorption pretreatment in a cost-effective manner. Wang et al. [317] performed stepwise recovery of gold and silver from e-waste through sequential electrodeposition. In another work, Li et al. [316] employed a flotation-assisted electrodeposition process to recover copper from waste printed circuit boards.
Thus, electrodeposition can function not only as a coating technology but also as a route for recovering valuable metals from secondary resources, although recovery efficiency depends strongly on solution composition, competing ions, and electrochemical selectivity.
Biomedical Coatings
Electrodeposition of biocompatible materials such as hydroxyapatite (HAp) and calcium phosphate on implants improves osseointegration, corrosion resistance, and overall biocompatibility in physiological environments [318,319]. Chitosan-based coatings modified with gold or zinc nanoparticles are also considered effective strategies for preventing bacterial infections associated with implants [320,321]. Among wet-processing methods, various electrically assisted and related deposition approaches have been investigated for chitosan, HAp, and reinforced HAp nanocomposite coatings, including direct and pulse electrodeposition and electrophoretic deposition, while electroless deposition represents a separate chemically driven route [318,319,322,323,324,325,326,327,328].
Coatings on titanium and titanium alloys, such as Ti6Al4V and NiTi, are widely used for implants because of their outstanding biocompatibility and osseointegration, low density, corrosion resistance, and high mechanical strength [329,330,331,332,333,334,335,336,337,338,339]. Besides these materials, Zn- and Mg-based alloys, Co-Cr alloys, and 316 L stainless steels are also used in load-bearing implant applications [340,341,342,343,344,345,346,347].
For example, electrodeposition of HAp-TiO2 composite coating improved the corrosion resistance of NiTi by almost 50% [330], while pulsed electrodeposition of HAp-Ta2O5 composite coatings on NiTi substantially improved corrosion resistance and reduced Ni-ion release [338]. In a recent work, Souri et al. [348] reported the electrochemical deposition of a homogeneous HAp-Ag nanostructured coating, which enhanced the antibacterial performance and corrosion resistance of Ti6Al4V alloy.
From an application perspective, electrodeposition is particularly attractive where scalable, low-temperature deposition of metallic, alloy, polymeric, or composite coatings is required. Its ability to tailor composition and microstructure through electrochemical parameters makes it suitable for protective, decorative, functional, electronic, and biomedical surfaces. However, coating uniformity on complex geometries and the environmental compatibility of electrolyte chemistries remain important considerations in process selection. Consequently, electrodeposition is most advantageous when scalability, cost-effectiveness, and compositional flexibility are prioritized, whereas CVD or, particularly, ALD may be preferred when highly conformal coatings on complex structures and, in the case of ALD, atomic-scale thickness control are required

2.5.3. Advantages, Challenges, and Outlook

Electrodeposition offers several compelling advantages that make it a versatile and widely used surface-engineering technique. Its electrochemical nature enables control over coating thickness, composition, and microstructure through parameters such as current density, bath composition, temperature, deposition time, and waveform. This flexibility allows the fabrication of uniform and adherent coatings on a wide range of conductive substrates, including components with moderate geometric complexity. Compared with techniques such as PVD and CVD, electrodeposition generally offers simpler equipment requirements, lower processing temperatures, and lower capital costs. PVD typically requires vacuum systems and is subject to line-of-sight limitations, whereas CVD can provide highly conformal coatings but may require elevated temperatures and, depending on the process, reactive or hazardous precursor chemistries. Electrodeposition therefore offers an attractive combination of process simplicity, scalability, and compositional flexibility for applications in which atomic-scale thickness control or vacuum-based processing is not essential.
Another important advantage is the ability to tailor coating microstructure and functionality through process modification. Pulse and pulse-reverse electrodeposition can refine grain structure and influence deposit morphology, while composite electrodeposition enables the incorporation of reinforcing particles to produce coatings with enhanced hardness, wear resistance, corrosion resistance, or other functional properties. The process can accommodate a broad range of metals, alloys, and particle-reinforced composite systems and is readily adaptable to components ranging from small parts to large industrial surfaces. In addition, alternative electrolyte systems, including deep eutectic solvents, have attracted increasing attention as potential routes toward more sustainable metal electrodeposition. Their relatively low volatility, thermal stability, and potentially lower environmental burden compared with some conventional electrolytes make them promising candidates, although their practical sustainability must be assessed in relation to electrolyte preparation, stability, recycling, deposition efficiency, and overall process life cycle [349].
Despite these advantages, several limitations constrain the performance and broader industrial applicability of electrodeposition. Achieving uniform deposition on highly complex, recessed, or poorly accessible geometries remains challenging because local current density and mass transport can vary substantially across the substrate. These variations may produce non-uniform thickness, particularly at edges and recessed regions. Coatings may also develop internal stresses and defects such as porosity, cracks, nodules, or inclusions, depending on electrolyte chemistry and deposition conditions, which can compromise mechanical integrity and long-term durability. Furthermore, electrolyte composition, additives, pH, temperature, agitation, and particle dispersion must be carefully controlled because relatively small changes in bath conditions can significantly affect nucleation, growth, morphology, and coating properties. The use of hazardous metal salts, complexing agents, additives, or other electrolyte constituents can create environmental and occupational concerns, making bath management, waste treatment, and electrolyte recycling important considerations for sustainable implementation.
Advanced electrodeposition methods can address some of these limitations, but often at the expense of greater process complexity. Pulse and pulse-reverse deposition provide additional control over nucleation and growth but require optimization of waveform parameters and may increase equipment and process-control requirements. Similarly, composite electrodeposition depends on stable particle dispersion and reliable incorporation of the dispersed phase into the growing coating. Magnetic- and ultrasound-assisted electrodeposition can enhance mass transport and modify deposit morphology, but their effectiveness is system-dependent, and their scale-up introduces additional engineering and energy considerations. Consequently, improving coating performance cannot be considered independently of process complexity, reproducibility, energy consumption, and manufacturing cost.
Recent developments have therefore increasingly focused on electrolyte engineering, advanced waveform control, and external-field-assisted deposition. Pulse and pulse-reverse electrodeposition have been widely investigated for producing fine-grained and nanostructured coatings with improved mechanical and corrosion-related properties, while incorporation of nanoparticles has expanded the functionality of metal–matrix composite coatings. Magnetic and ultrasonic fields have also been investigated as strategies for modifying mass transport and reducing concentration polarization. These developments demonstrate that further improvements in electrodeposition are increasingly dependent not simply on increasing deposition rate, but on achieving simultaneous control of mass transport, interfacial reactions, microstructure, and coating uniformity.
Looking forward, research should focus on developing safer, more sustainable electrolyte systems, improving bath stability and recycling, and implementing advanced monitoring and process-control strategies. Particular attention should be given to real-time measurement of parameters such as current distribution, electrolyte composition, temperature, and deposition behavior, with the objective of establishing more direct relationships between process conditions, coating microstructure, and functional performance. The development of greener electrolytes, including deep eutectic and other alternative solvent systems, should similarly be evaluated not only based on toxicity or volatility but also in terms of deposition efficiency, durability, recyclability, waste generation, and overall process economics. Integration of electrodeposition with complementary surface-engineering and additive-manufacturing approaches may further enable hybrid coatings and component-scale manufacturing strategies that combine the scalability and low-temperature processing of electrodeposition with the microstructural or geometric capabilities of other technologies. Such developments could strengthen the role of electrodeposition in energy storage, catalysis, electronics, biomedical devices, and advanced manufacturing, provided that improvements in coating performance are achieved without disproportionate increases in process complexity or environmental burden.
To facilitate practical selection among the coating technologies discussed in this review, Table 1 summarizes their principal processing characteristics, material and substrate compatibility, distinctive features, advantages, limitations, and representative application scenarios. The comparison highlights that coating-process selection is governed by the balance among coating thickness, conformality, processing temperature, deposition rate, substrate compatibility, functional requirements, scalability, and overall manufacturing constraints.
Table 1. Comparative characteristics, advantages, limitations, and application scenarios of the coating technologies reviewed in this work.

3. Conclusions and Future Perspectives

Surface coating technologies have become indispensable in modern manufacturing and materials engineering, offering effective routes to enhance durability, functionality, surface protection, and overall component performance. This review has examined major coating technologies, including PVD, laser cladding, CVD, ALD, and electrodeposition, highlighting their distinct deposition mechanisms, capabilities, advantages, and limitations. Collectively, these technologies provide control over coating thickness, composition, microstructure, adhesion, and surface functionality, enabling their application across a wide range of industrial sectors. The comparison of these techniques demonstrates that no single coating process can satisfy all application requirements; rather, the appropriate technology must be selected according to substrate characteristics, required coating thickness and conformality, processing temperature, deposition rate, surface functionality, scalability, and economic and environmental constraints.
The development of modern coating technologies is increasingly characterized by the integration of advanced deposition processes, novel coating materials, and application-specific design strategies. Combining PVD, CVD, ALD, and electrodeposition, either sequentially or through hybrid approaches, can allow the complementary advantages of individual techniques to be exploited while mitigating their respective limitations. For example, ALD provides exceptional control over ultrathin interfaces and conformal nanoscale structures; CVD enables high-quality coatings with good conformality and broad material compatibility; PVD can produce dense, wear-resistant thin films; and electrodeposition offers a relatively simple and scalable route for metallic, alloy, and composite coatings. Laser cladding, in contrast, enables the deposition of relatively thick protective or functional layers while simultaneously providing opportunities for surface restoration, localized material addition, and component remanufacturing. Such complementary approaches create opportunities for designing multifunctional coating systems with performance beyond that achievable through a single deposition technique.
Recent progress has been driven by advances in materials design, process optimization, and digital technologies. Artificial intelligence and data-driven approaches are expected to play an increasingly important role in coating development by enabling process-parameter optimization, prediction of coating properties and defects, real-time process adjustment, and accelerated identification of suitable material–process combinations. However, the practical value of these approaches will depend on the availability of reliable, representative datasets and their ability to generalize across different materials, process conditions, and equipment configurations. At the same time, emerging concepts such as self-healing coatings, biomimetic surfaces, smart responsive coatings, and hybrid deposition processes are expanding the functional scope of coated materials. Furthermore, two-dimensional materials, including MXenes, are also being explored as constituents of multifunctional coatings for applications such as corrosion protection, electromagnetic interference shielding, sensing, and photothermal functionality, although challenges related to environmental stability, interfacial compatibility, processing, and large-scale integration remain [350,351]. The integration of in situ monitoring with advanced process control is particularly promising for improving reproducibility, reducing defects, and enabling more reliable scale-up from laboratory systems to industrial production.
Sustainability will be a decisive factor in the future development of coating technologies. Many conventional processes still involve high energy consumption, hazardous chemicals, solvent use, or volatile organic compound emissions, although the magnitude and nature of these burdens vary substantially among technologies and process configurations. Future development should therefore place greater emphasis on low-temperature and energy-efficient deposition, less hazardous precursor and electrolyte chemistries, reduced solvent use, recyclable materials, and bio-based coating systems where technically feasible. Life-cycle assessment can support the selection of materials and processes with lower environmental impact, reduced waste, and improved resource efficiency. Importantly, sustainability should be considered together with coating performance, durability, and service life, since extending component lifetime can itself contribute substantially to resource conservation. Aligning coating technologies with circular-economy principles will therefore be essential for achieving both high performance and environmental responsibility.
Future research should also address several persistent challenges, including process scalability, coating uniformity over complex geometries, deposition rate, residual stress, interfacial adhesion, precursor and electrolyte sustainability, process reproducibility, and the cost and complexity of advanced equipment. Addressing these challenges will require closer integration of materials science, electrochemistry, surface engineering, computational modeling, and manufacturing technologies. Hybrid and sequential deposition strategies are particularly promising because they can combine nanoscale precision with higher deposition rates or thicker protective architectures, thereby helping to bridge the gap between advanced laboratory-scale coatings and industrially viable systems. At the same time, process selection should increasingly be guided by application-specific performance requirements and life-cycle considerations rather than by optimization of individual coating properties in isolation.
Overall, surface coating technologies are expected to remain a key driver of innovation in materials science and industrial engineering. Their future development will depend not on the dominance of a single deposition technology, but on the intelligent selection and integration of complementary processes according to specific performance and manufacturing requirements. The convergence of advanced materials, precise processing, AI-assisted optimization, multifunctional design, and sustainable manufacturing is expected to enable coating systems with improved reliability, longer service life, reduced environmental impact, and greater functional complexity. By addressing current challenges related to scalability, durability, cost, and environmental impact, surface coatings can continue to support safer, more resource-efficient, and higher-performance technologies across diverse application areas.

Author Contributions

Conceptualization, I.C.; methodology, I.C.; writing—original draft preparation, I.C.; writing—review and editing, I.C.; visualization, I.C.; supervision, F.J.O. and G.M.; project administration, F.J.O.; funding acquisition, F.J.O. All authors have read and agreed to the published version of the manuscript.

Funding

The author I.C. would like to acknowledge funding from the “Agenda DRIVOLUTION—Transition to the factory of the future” project supported by the PRR—Recovery and Resilience Plan and by NextGenerationEU, through the scheme Capitalisation and Business Innovation (Ref: 02-C05-i01.02-2022.PC644913740-00000022). The authors acknowledge funding from Project “SINT3R” (ref: COMPETE2030-FEDER-02219100).

Data Availability Statement

No new data were created or analyzed in this study. All analyzed data were obtained from previously published articles listed in the references.

Acknowledgments

I. Coondoo would also like to acknowledge financial assistance from national funds provided by FCT—Fundação para a Ciência e a Tecnologia, I.P., through an individual FCT-CEEC Assistant Researcher contract (2024.09019.CEECIND). This work was partly developed within the scope of the project CICECO Aveiro Institute of Materials, UID/50011/2025 (DOI 10.54499/UID/50011/2025) & LA/P/0006/2020 (DOI 10.54499/LA/P/0006/2020), financed by national funds through the FCT/MCTES (PIDDAC). We are thankful to Phalguni Coondoo for enhancing the resolution and readability of the figures.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Sun, H.; Song, B.; Sun, X.; Cui, X.; Liu, Z.; Cong, M.; Sun, M.; Zhu, Z.; Tian, Y.; Liu, S.; et al. Recent Representative Progress of Surface Coating Technology. Chem. Rec. 2025, 25, e202500054. [Google Scholar] [CrossRef] [Scilit]
  2. Butt, M.A. Thin-Film Coating Methods: A Successful Marriage of High-Quality and Cost-Effectiveness—A Brief Exploration. Coatings 2022, 12, 1115. [Google Scholar] [CrossRef] [Scilit]
  3. Jeong, K.; Lee, D. Colloidal Wet Coating Techniques of Two-Dimensional Materials. Adv. Mater. Technol. 2026, 11, e01805. [Google Scholar] [CrossRef] [Scilit]
  4. Kumar, R.S.N.; Ramirez, A.V.; Verding, P.; Nivelle, P.; Renner, F.; D’hAen, J.; Deferme, W. Deposition of ultra-thin coatings by a nature-inspired Spray-on-Screen technology. Commun. Eng. 2023, 2, 42. [Google Scholar] [CrossRef] [Scilit]
  5. Mesbah, M.; Yazdani, S.; Vitry, V. A state-of-the-art review on electrodeposited metal matrix composite coatings: Recent innovations and challenges. Surf. Eng. 2024, 40, 400–417. [Google Scholar] [CrossRef] [Scilit]
  6. Gajagouni, S.P.; Bose, R.; Barsoum, I.; Cho, S.O.; AlFantazi, A. Electrochemical anodization of stainless steels: Advances in nanostructured oxide synthesis for corrosion-resistant and functional surfaces. Chem. Eng. J. Adv. 2026, 25, 100972. [Google Scholar] [CrossRef] [Scilit]
  7. Iwai, M.; Nagao, T.; Noguchi, T.; Kikuchi, T.; Kitano, S.; Fushimi, K.; Habazaki, H. Fundamental study on anodizing of aluminum and aluminum alloys in a sodium tetraborate electrolyte solution and evaluating their high-temperature wettability behavior. J. Alloys Compd. 2025, 1041, 183822. [Google Scholar] [CrossRef] [Scilit]
  8. Dash, S.S.; Cojocaru, C.V.; Choi, H.S.; Qu, N.; Chen, R.; Wei, J.; Aghasibeig, M.; Irissou, E.; Zou, Y. Wear behavior of eutectic high entropy alloy coatings made by cold spray and thermal spray. Surf. Coat. Technol. 2026, 525, 133290. [Google Scholar] [CrossRef] [Scilit]
  9. Khan, A.; Gayawali, G.; Shah, S.; Sohail, M.; Liu, X.; Zhang, S. Hot corrosion, wear, and oxidation performance of high-velocity oxy-fuel and plasma spray coatings in various environments: A comprehensive review. Arab. J. Chem. 2026, 19, 5182025. [Google Scholar] [CrossRef] [Scilit]
  10. Wang, Y.; Normand, B.; Mary, N.; Yu, M.; Liao, H. Microstructure and corrosion behavior of cold sprayed SiCp/Al 5056 composite coatings. Surf. Coat. Technol. 2014, 251, 264–275. [Google Scholar] [CrossRef] [Scilit]
  11. Ambhore, N.; Manikanta, J.E.; Gurajala, N.K.; Nikhare, C. Laser applications in surface treatment: A comprehensive review. Laser Phys. 2025, 35, 106101. [Google Scholar] [CrossRef] [Scilit]
  12. Cepauskaite, L.; Bendikiene, R. The role of laser surface texturing for environmentally friendly surface engineering applications: A review. Prog. Surf. Sci. 2026, 101, 100807. [Google Scholar] [CrossRef] [Scilit]
  13. Domínguez-García, A.; Mercader-Trejo, F.E.; Mondragón-Rodríguez, G.C.; Gúzman-Tapia, M.; Herrera-Basurto, R. PVD magnetron sputtering for coating thickness reference materials: A comprehensive review (1974–2025). Mater. Res. Express 2026, 13, 042003. [Google Scholar] [CrossRef] [Scilit]
  14. Zhang, J.; Zhang, Y.; Fu, Y.; Chen, R.; Li, T.; Hou, X.; Li, H. Research progress in chemical vapor deposition for high-temperature anti-oxidation/ablation coatings on thermal structural composites. Compos. Part B Eng. 2025, 291, 112015. [Google Scholar] [CrossRef] [Scilit]
  15. Hautala, J.; Kääriäinen, T.; Hoppu, P.; Kemell, M.; Heinämäki, J.; Cameron, D.; George, S.; Juppo, A.M. Atomic layer deposition—A novel method for the ultrathin coating of minitablets. Int. J. Pharm. 2017, 531, 47–58. [Google Scholar] [CrossRef] [Scilit][Green Version]
  16. Snyders, R.; Hegemann, D.; Thiry, D.; Zabeida, O.; Klemberg-Sapieha, J.; Martinu, L. Foundations of plasma enhanced chemical vapor deposition of functional coatings. Plasma Sources Sci. Technol. 2023, 32, 074001. [Google Scholar] [CrossRef] [Scilit]
  17. Shen, Y.; Zheng, H.; Cao, J.; Guo, X. Bio-Based Flame Retardant Superhydrophobic Coatings by Phytic Acid/Polyethyleneimine Layer-by-Layer Assembly on Nylon/Cotton Blend Fabrics. Coatings 2025, 15, 699. [Google Scholar] [CrossRef] [Scilit]
  18. Li, X.; Rytkin, E.; Zhao, Q.; Bhat, P.; Pfenniger, A.; Yin, L.; Huang, X.; Yang, L.; Yang, B.; Burrell, A.; et al. High-resolution liquid metal–based stretchable electronics enabled by colloidal self-assembly and microtransfer printing. Sci. Adv. 2025, 11, eadw3044. [Google Scholar] [CrossRef] [Scilit]
  19. Yang, H.; Jiang, P. Large-Scale Colloidal Self-Assembly by Doctor Blade Coating. Langmuir 2010, 26, 13173–13182. [Google Scholar] [CrossRef] [Scilit]
  20. van Dommelen, R.; Fanzio, P.; Sasso, L. Surface self-assembly of colloidal crystals for micro- and nano-patterning. Adv. Colloid Interface Sci. 2018, 251, 97–114. [Google Scholar] [CrossRef] [Scilit]
  21. Kumar, A.; Jaiswal, J.; Tsuchiya, K.; Mulik, R.S. Modern Coating Processes and Technologies. In Coating Materials: Computational Aspects, Applications and Challenges; Verma, A., Sethi, S.K., Ogata, S., Eds.; Springer Nature: Singapore, 2023; pp. 33–80. [Google Scholar]
  22. Baptista, A.; Silva, F.; Porteiro, J.; Míguez, J.; Pinto, G. Sputtering Physical Vapour Deposition (PVD) Coatings: A Critical Review on Process Improvement and Market Trend Demands. Coatings 2018, 8, 402. [Google Scholar] [CrossRef] [Scilit]
  23. Fox, V.; Jones, A.; Renevier, N.; Teer, D. Hard lubricating coatings for cutting and forming tools and mechanical components. Surf. Coat. Technol. 2000, 125, 347–353. [Google Scholar] [CrossRef] [Scilit]
  24. Patro, S.S.; Sahoo, A.K.; Roy, S. Analysis of residual stresses in cutting tools coated via physical vapour deposition: A review. Mater. Today Proc. 2023. [Google Scholar] [CrossRef] [Scilit]
  25. PalDey, S.; Deevi, S. Single layer and multilayer wear resistant coatings of (Ti,Al)N: A review. Mater. Sci. Eng. A 2003, 342, 58–79. [Google Scholar] [CrossRef] [Scilit]
  26. Ariharan, N.; Sriram, C.G.; Radhika, N.; Aswin, S.; Haridas, S. A comprehensive review of vapour deposited coatings for cutting tools: Properties and recent advances. Trans. IMF 2022, 100, 262–275. [Google Scholar] [CrossRef] [Scilit]
  27. Liu, Y.; Yu, S.; Shi, Q.; Ge, X.; Wang, W. Multilayer Coatings for Tribology: A Mini Review. Nanomaterials 2022, 12, 1388. [Google Scholar] [CrossRef] [Scilit]
  28. Xin, T.; Pei, H.; Shucai, Y. Coating and micro-texture techniques for cutting tools. J. Mater. Sci. 2022, 57, 17052–17104. [Google Scholar] [CrossRef] [Scilit]
  29. Okokpujie, I.P.; Tartibu, L.K.; Musa-Basheer, H.O.; Adeoye, A.O.M. Effect of Coatings on Mechanical, Corrosion and Tribological Properties of Industrial Materials: A Comprehensive Review. J. Bio- Tribo-Corros. 2023, 10, 2. [Google Scholar] [CrossRef] [Scilit]
  30. Shakib, S.E.; Babakhani, A.; Torbati, M.K. Nanomechanical assessment of tribological behavior of TiN/TiCN multi-layer hard coatings deposited by physical vapor deposition. J. Mater. Res. Technol. 2023, 25, 1344–1354. [Google Scholar] [CrossRef] [Scilit]
  31. Muhammed, M.; Javidani, M.; Sadrabadi, T.E.; Heidari, M.; Levasseur, T.; Jahazi, M. A Comprehensive Review of Cathodic Arc Evaporation Physical Vapour Deposition (CAE-PVD) Coatings for Enhanced Tribological Performance. Coatings 2024, 14, 246. [Google Scholar] [CrossRef] [Scilit]
  32. Kaya, E. Physical Vapor Deposition of Thin Film Coatings for Cutting Tools. In Micromanufacturing Operations; Gürgen, S., Ed.; Springer Nature: Cham, Switzerland, 2026; pp. 133–154. [Google Scholar]
  33. Zhou, M.; Makino, Y.; Nose, M.; Nogi, K. Phase transition and properties of Ti–Al–N thin films prepared by r.f.-plasma assisted magnetron sputtering. Thin Solid Films 1999, 339, 203–208. [Google Scholar] [CrossRef] [Scilit]
  34. Kimura, A.; Hasegawa, H.; Yamada, K.; Suzuki, T. Metastable Ti1−xAlxN films with different Al content. J. Mater. Sci. Lett. 2000, 19, 601–602. [Google Scholar] [CrossRef] [Scilit]
  35. Musil, J.; Hrubý, H. Superhard nanocomposite Ti1−xAlxN films prepared by magnetron sputtering. Thin Solid Films 2000, 365, 104–109. [Google Scholar] [CrossRef] [Scilit]
  36. Schäffer, E.; Kleer, G. Mechanical behavior of (Ti,Al)N coatings exposed to elevated temperatures and an oxidative environment. Surf. Coat. Technol. 2000, 133–134, 215–219. [Google Scholar] [CrossRef] [Scilit]
  37. Wu, S.K.; Lin, H.C.; Liu, P.L. An investigation of unbalanced-magnetron sputtered TiAlN films on SKH51 high-speed steel. Surf. Coat. Technol. 2000, 124, 97–103. [Google Scholar] [CrossRef] [Scilit]
  38. Kimura, A.; Murakami, T.; Yamada, K.; Suzuki, T. Hot-pressed Ti-Al targets for synthesizing Ti1−xAlxN films by the arc ion plating method. Thin Solid Films 2001, 382, 101–105. [Google Scholar] [CrossRef] [Scilit]
  39. Shugurov, A.R.; Kuzminov, E.D. Mechanical and tribological properties of Ti-Al-Ta-N/TiAl and Ti-Al-Ta-N/Ta multilayer coatings deposited by DC magnetron sputtering. Surf. Coat. Technol. 2022, 441, 128582. [Google Scholar] [CrossRef] [Scilit]
  40. Panjan, P.; Drnovšek, A.; Terek, P.; Miletić, A.; Čekada, M.; Panjan, M. Comparative Study of Tribological Behavior of TiN Hard Coatings Deposited by Various PVD Deposition Techniques. Coatings 2022, 12, 294. [Google Scholar] [CrossRef] [Scilit]
  41. Meysami, A.; Najafabadi, R.A.; Yosefnejad, T.; Isfahani, T. Enhancing Wear Behavior and Hardness of D5 Cold Work Tool Steel through TiCrN Multilayer Nanocoating via Physical Vapor Deposition. Surf. Eng. Appl. Electrochem. 2024, 60, 58–68. [Google Scholar] [CrossRef] [Scilit]
  42. Guimaraes, M.C.R.; de Castilho, B.C.N.M.; Nossa, T.d.S.; Avila, P.R.T.; Cucatti, S.; Alvarez, F.; Garcia, J.L.; Pinto, H.C. On the effect of substrate oscillation on CrN coatings deposited by HiPIMS and dcMS. Surf. Coat. Technol. 2018, 340, 112–120. [Google Scholar] [CrossRef] [Scilit]
  43. Li, Q.; Yang, L.; Wang, Z.; Zhang, H.; Liu, Z.; Chen, Q. The superior properties of CrN coatings prepared by high power pulsed reactive magnetron sputtering. AIP Adv. 2020, 10, 015125. [Google Scholar] [CrossRef] [Scilit]
  44. Codau, T.-C.; Ferreira, J.; Girão, A.V.; Codau, E.; Figueiredo, D.; Fernandes, C.M.; Guimarães, B.; Oliveira, F.J. Advanced ceramic multilayer coatings for increasing the tool life of cutting inserts: A hybrid CVD-PVD approach. Mater. Chem. Phys. 2026, 349, 131768. [Google Scholar] [CrossRef] [Scilit]
  45. Kumar, S.; Kumar, M. Tribological and Mechanical Performance of Coatings on Piston to Avoid Failure—A Review. J. Fail. Anal. Prev. 2022, 22, 1346–1369. [Google Scholar] [CrossRef] [Scilit]
  46. Liu, J.; Zhang, Y.; Liao, B. A review on preparation process and tribological performance of coatings for internal combustion engine piston ring. Adv. Mech. Eng. 2023, 15, 16878132231175752. [Google Scholar] [CrossRef] [Scilit]
  47. Harvinder, S.; Rajdeep, S.; Satish, K.; Aneesh, G. A Comprehensive Review of Tribological Performance of Coatings on Automotive Piston Rings. I-Manag. J. Mech. Eng. 2024, 14, 16. [Google Scholar] [CrossRef] [Scilit]
  48. Maria, Z.; Olivia, P.K. Coating Materials for Automotive Piston Rings: A Review of Tribological Performance and Engine Impact. Front. Emerg. Eng. Technol. 2002, 2, 8–15. [Google Scholar]
  49. Friedrich, C.; Berg, G.; Broszeit, E.; Rick, F.; Holland, J. PVD CrxN coatings for tribological application on piston rings. Surf. Coat. Technol. 1997, 97, 661–668. [Google Scholar] [CrossRef] [Scilit]
  50. Bobzin, K.; Bagcivan, N.; Goebbels, N.; Yilmaz, K.; Hoehn, B.-R.; Michaelis, K.; Hochmann, M. Lubricated PVD CrAlN and WC/C coatings for automotive applications. Surf. Coat. Technol. 2009, 204, 1097–1101. [Google Scholar] [CrossRef] [Scilit]
  51. Lin, J.; Wei, R.; Bitsis, D.C.; Lee, P.M. Development and evaluation of low friction TiSiCN nanocomposite coatings for piston ring applications. Surf. Coat. Technol. 2016, 298, 121–131. [Google Scholar] [CrossRef] [Scilit]
  52. Liu, J.; Liao, R.; Xie, G.; Xiang, J.; Luo, J.; Liao, B.; Liu, Q. Tribological properties of CrN coating deposited on 20CrMo against tin bronze. Sci. China Technol. Sci. 2018, 61, 1713–1722. [Google Scholar] [CrossRef] [Scilit]
  53. Singh, S.K.; Chattopadhyaya, S.; Pramanik, A.; Kumar, S. Wear behavior of chromium nitride coating in dry condition at lower sliding velocity and load. Int. J. Adv. Manuf. Technol. 2018, 96, 1665–1675. [Google Scholar] [CrossRef] [Scilit]
  54. Alisir, S.H.; Evrensel, D. Investigation into Coating Structure and Wear Environment Effects on Tribological Properties of Piston Ring Coated with Monolayer TiAlN and Multilayer TiN/TiAlN. J. Mater. Eng. Perform. 2022, 31, 1654–1666. [Google Scholar] [CrossRef] [Scilit]
  55. Singh, H.; Singh, V. Tribological Performance of Coatings on Automotive Piston Rings: A Review. IUP J. Mech. Eng. 2025, 18, 47–70. [Google Scholar] [CrossRef] [Scilit]
  56. Shen, Z.; Liu, G.; Dai, J.; He, L.; Mu, R. LaNdZrO thermal barrier coatings by electron beam physical vapor deposition: Morphology, thermal property and failure mechanism. Chem. Eng. J. Adv. 2022, 11, 100328. [Google Scholar] [CrossRef] [Scilit]
  57. Chen, D.; Maeder, X.; Widrig, B.; Ramm, J.; De Wet, D. Hybrid chemical-physical vapor deposition of highly durable environmental barrier coatings. Vacuum 2023, 213, 112098. [Google Scholar] [CrossRef] [Scilit]
  58. Alhazaa, A.; Shar, M.A. Aerospace and Thin Films. In Thin Films and Coatings: Engineering Applications; Chandio, A.D., Channa, I.A., Eds.; Springer Nature: Singapore, 2025; pp. 217–238. [Google Scholar]
  59. Ahanger, Z.A.; Saleem, S.S.; Dey, A. Physical vapour deposition technologies of functionally graded coatings. Proc. Inst. Mech. Eng. Part L J. Mater. Des. Appl. 2026, 240, 472–528. [Google Scholar] [CrossRef] [Scilit]
  60. Ozgurluk, Y.; Karaoglanli, A.C.; Ahlatci, H. Comparison of calcium–magnesium-alumina-silicate (CMAS) resistance behavior of produced with electron beam physical vapor deposition (EB-PVD) method YSZ and Gd2Zr2O7/YSZ thermal barrier coatings systems. Vacuum 2021, 194, 110576. [Google Scholar] [CrossRef] [Scilit]
  61. Odabas, O.; Ozgurluk, Y.; Ozkan, D.; Binal, G.; Calis, I.; Karaoglanli, A.C. Investigation of vermiculite infiltration effect on microstructural properties of thermal barrier coatings (TBCs) produced by electron beam physical vapor deposition method (EB-PVD). Surf. Coat. Technol. 2022, 443, 128645. [Google Scholar] [CrossRef] [Scilit]
  62. Kucharska, B.; Bochra, K.; Wierzchoń, T.; Sobiecki, J.R. Protective Magnetron Sputtering Physical Vapor Deposition Coatings for Space Application. Coatings 2024, 14, 1195. [Google Scholar] [CrossRef] [Scilit]
  63. Mühlbacher, M.; Mendez-Martin, F.; Sartory, B.; Schalk, N.; Keckes, J.; Lu, J.; Hultman, L.; Mitterer, C. Copper diffusion into single-crystalline TiN studied by transmission electron microscopy and atom probe tomography. Thin Solid Films 2015, 574, 103–109. [Google Scholar] [CrossRef] [Scilit]
  64. Mehta, N. Overview of Coating Deposition Techniques. In Tribology and Characterization of Surface Coatings; Scrivener Publishing LLC: Hoboken, NJ, USA; John Wiley and Sons: Hoboken, NJ, USA, 2022; pp. 1–32. [Google Scholar]
  65. Hossain, M.I.; Mansour, S. A critical overview of thin films coating technologies for energy applications. Cogent Eng. 2023, 10, 2179467. [Google Scholar] [CrossRef] [Scilit]
  66. Adeoye, A.E.; Adeaga, O.A.; Ukoba, K. Chemical vapour deposition (CVD) and physical vapour deposition (PVD) techniques: Advances in thin film solar cells. Niger. J. Technol. 2024, 43, 479–489. [Google Scholar] [CrossRef] [Scilit]
  67. Sharma, G.; Jugran, S.; Bansal, S.; Gera, R.; Rao, P.K.; Shruthi, C.M. Deposition techniques for thin film development in microelectronic devices. AIP Conf. Proc. 2025, 3157, 120025. [Google Scholar] [CrossRef] [Scilit]
  68. Zega, B. Hard decorative coatings by reactive physical vapor deposition: 12 Years of development. Surf. Coat. Technol. 1989, 39–40, 507–520. [Google Scholar] [CrossRef] [Scilit]
  69. Reiners, G.; Beck, U.; Jehn, H.A. Decorative optical coatings. Thin Solid Films 1994, 253, 33–40. [Google Scholar] [CrossRef] [Scilit]
  70. Constantin, R.; Steinmann, P.-A.; Manasterski, C. Decorative PVD Coatings. In Nanomaterials and Surface Engineering; John Wiley and Sons, Inc.: Hoboken, NJ, USA, 2013; pp. 109–162. [Google Scholar]
  71. Sathish, M.; Radhika, N.; Saleh, B. Current Status, Challenges, and Future Prospects of Thin Film Coating Techniques and Coating Structures. J. Bio- Tribo-Corros. 2023, 9, 35. [Google Scholar] [CrossRef] [Scilit]
  72. van Hove, R.P.; Sierevelt, I.N.; van Royen, B.J.; Nolte, P.A. Titanium-Nitride Coating of Orthopaedic Implants: A Review of the Literature. BioMed Res. Int. 2015, 2015, 485975. [Google Scholar] [CrossRef] [Scilit]
  73. Damiati, L.; Eales, M.G.; Nobbs, A.H.; Su, B.; Tsimbouri, P.M.; Salmeron-Sanchez, M.; Dalby, M.J. Impact of surface topography and coating on osteogenesis and bacterial attachment on titanium implants. J. Tissue Eng. 2018, 9, 2041731418790694. [Google Scholar] [CrossRef] [Scilit]
  74. Palani, S.; Desta, M.; Atnaw, S.M.; Banoth, R.; Kolanji, S. Physical Vapor Deposition Coating Process in Biomedical Applications. In Sustainable Advanced Manufacturing and Materials Processing: Methods and Technologies, 1st ed.; Kaushal, S., Singh, I., Singh, S., Gupta, A., Eds.; CRC Press: Boca Raton, FL, USA, 2022; p. 244. [Google Scholar]
  75. Schaldach, M.; Hubmann, M.; Hardt, R.; Weikl, A. Pacemaker electrodes made of titanium nitride. Biomed. Tech. 1989, 34, 185–190. [Google Scholar] [CrossRef] [Scilit]
  76. Sin, D.-C.; Kei, H.-L.; Miao, X. Surface coatings for ventricular assist devices. Expert Rev. Med. Devices 2009, 6, 51–60. [Google Scholar] [CrossRef] [Scilit]
  77. Han, W.; Xu, D.; Min, J.; Guo, Y.; Dai, G.; Sun, Z.; Chang, H.; Jia, Z. Influence of WC particle size on microstructural evolution and wear behavior of laser cladding WC/Ti6Al4V composite coatings. Ceram. Int. 2025, 51, 47119–47131. [Google Scholar] [CrossRef] [Scilit]
  78. He, R.; Cui, C.; Miao, X.; Wu, M.; Kim, H.S. Improvement in corrosion and wear resistance of Ni3Al-based superalloy coatings through laser energy density regulation. J. Mater. Res. Technol. 2026, 36, 4585–4601. [Google Scholar] [CrossRef] [Scilit]
  79. Lei, D.; Wang, L.; Li, Y.; Gao, Z.; Shi, H.; Li, X. Microstructure evolution mechanism and microhardness enhancement of (nano-CeO2 + micron TiC)/Ti6Al4V composite coating by laser cladding. Prog. Addit. Manuf. 2025, 10, 6643–6655. [Google Scholar] [CrossRef] [Scilit]
  80. Zhao, C.; Yu, Z.; Du, W.; Zhang, Z.; Ma, L.; Zhang, T.; Bai, Y.; Chen, S. Laser Cladding of High-Temperature Alloy: Research Status and Development. Adv. Eng. Mater. 2025, 27, 2402956. [Google Scholar] [CrossRef] [Scilit]
  81. Sow, M.; De Terris, T.; Castelnau, O.; Hamouche, Z.; Coste, F.; Fabbro, R.; Peyre, P. Influence of beam diameter on Laser Powder Bed Fusion (L-PBF) process. Addit. Manuf. 2020, 36, 101532. [Google Scholar] [CrossRef] [Scilit]
  82. Ren, J.; Zhang, Y.; Zhao, D.; Chen, Y.; Guan, S.; Liu, Y.; Liu, L.; Peng, S.; Kong, F.; Poplawsky, J.D.; et al. Strong yet ductile nanolamellar high-entropy alloys by additive manufacturing. Nature 2022, 608, 62–68. [Google Scholar] [CrossRef] [Scilit]
  83. Zhang, F.; He, Z.; Lu, K.; Zhan, Z.; Li, Z.; Wang, X. Interfacial microstructure and mechanical properties of 2124 aluminum alloy reinforced by AlCoCrFeNi high entropy alloy. J. Mater. Res. Technol. 2023, 26, 8846–8856. [Google Scholar] [CrossRef] [Scilit]
  84. Zhao, Q.; Huang, X.; Zhan, Z.; Zhou, S.; Liu, J.; Zhu, P.; Wei, L.; Li, X.; Li, C.; Xie, Y. Effect of alloying elements (Mn, Ti, and Mo) on the corrosion behavior of FeCoNiCr-based high entropy alloy in supercritical water. Corros. Sci. 2023, 220, 111291. [Google Scholar] [CrossRef] [Scilit]
  85. Cui, T.; Wang, K.; Sheng, Y.; Gao, P.; Guo, B.; Li, F.; Wang, Z.; Fu, Y.; Sun, B.; Chen, S.; et al. Effect of laser energy density on microstructures and properties of laser cladding CoMoCrSiFe coating. Opt. Laser Technol. 2025, 192, 113529. [Google Scholar] [CrossRef] [Scilit]
  86. Lei, X.; Du, Y.; Chen, H.; Peng, Y.; Ma, W.; Tu, J. A hybrid optimization method for determining laser cladding process parameters to control geometric morphology in CoCrFeNiMn high-entropy alloy. J. Mater. Res. Technol. 2026, 39, 1038–1052. [Google Scholar] [CrossRef] [Scilit]
  87. Liu, H.; Li, D.; Wu, D.; Wang, W.; Pan, S.; Chen, P.; He, X.; Yu, G.; Zhang, T. Improve wear resistance CoCrFeMnNiTix/WC high entropy alloy-ceramic composite coatings with hybrid ex/in-situ multi-scale reinforcement phase fabricating by laser cladding. Ceram. Int. 2025, 51, 40335–40348. [Google Scholar] [CrossRef] [Scilit]
  88. Wu, Y.; Sun, W.; Huang, Y.; Yu, S.; Liu, Y.; Wu, X. Tribological behaviour of laser cladding CoCrFeNiMo0.5Tix-hBN high-entropy alloy composite coatings under dry and tribocorrosion conditions. Ceram. Int. 2025, 51, 50396–50418. [Google Scholar] [CrossRef] [Scilit]
  89. Sexton, L.; Lavin, S.; Byrne, G.; Kennedy, A. Laser cladding of aerospace materials. J. Mater. Process. Technol. 2002, 122, 63–68. [Google Scholar] [CrossRef] [Scilit]
  90. Liu, Q.; Janardhana, M.; Hinton, B.; Brandt, M.; Sharp, K. Laser cladding as a potential repair technology for damaged aircraft components. Int. J. Struct. Integr. 2011, 2, 314–331. [Google Scholar] [CrossRef] [Scilit]
  91. Chen, M.; Yang, X.; Zhang, Z.; Gu, Y.; Li, K.; Liu, Y.; Ma, J. Research status of laser cladding technology on aluminum alloy surface. Int. J. Adv. Manuf. Technol. 2025, 137, 1–21. [Google Scholar] [CrossRef] [Scilit]
  92. Lei, J.; Wei, B.; Liu, T.; Chen, L.; Zhao, C.; Wang, L.; Sun, H.; Wang, P. Temperature and rate-dependent behavior of laser cladding IN625 alloy under dynamic loading: Experiments and constitutive model. Mater. Today Commun. 2026, 49, 114162. [Google Scholar] [CrossRef] [Scilit]
  93. Morais, E.; Silva, S.; Siqueira, R.; Carvalho, S.; Lima, M. Laser-induced diffusion of an aluminum clad in an aerospace aluminum alloy for enhanced bonding. Results Surf. Interfaces 2025, 19, 100521. [Google Scholar] [CrossRef] [Scilit]
  94. Wan, N.; Wang, Z.; Li, M.; Liu, Q.; Zhao, B.; Ding, W.; Xu, J. Design and optimization of grinding tool structures for high-performance machining of aerospace difficult-to-cut materials. J. Manuf. Process. 2025, 154, 640–658. [Google Scholar] [CrossRef] [Scilit]
  95. Xie, F.; Zhai, C.; Zhang, X.; Jiang, S.; Yang, M.; Zheng, H. Enhanced high-temperature oxidation resistance of TC11 titanium alloys via laser cladding FeCoNiCrMoBSi high-entropy alloy coatings. Mater. Chem. Phys. 2025, 340, 130861. [Google Scholar] [CrossRef] [Scilit]
  96. Wang, J.; Shao, Z.; Liu, J.; Miao, Y.; Yao, Z.; Jiang, T.; Wu, B. TiNiCuZrNbTa refractory high entropy alloy coatings fabricated using laser cladding: Microstructure and tribological behavior. Tribol. Int. 2026, 214, 111319. [Google Scholar] [CrossRef] [Scilit]
  97. Zhang, H.; Sun, X.; He, Y.; Zhao, Y.; Chen, Z.; Guo, X.; Li, Q.; Ji, S.; Li, D. Periodic multilayer functionally graded structure of Ni-NbMoTa high-entropy alloy composition materials via laser cladding deposition. Addit. Manuf. Front. 2026, 5, 200255. [Google Scholar] [CrossRef] [Scilit]
  98. Zhao, C.; Bai, Y.; Zhang, T.; Ma, L.; Zhang, N.; Wang, J.; Wang, J.; Ma, C. Review of the research status and development of laser cladding high-entropy alloys. J. Vac. Sci. Technol. A 2026, 44, 020802. [Google Scholar] [CrossRef] [Scilit]
  99. Liu, C.; Qiu, X.; Wang, Z.; Peng, J.; Liu, Z.; Qiu, C.; Meng, C.; Ren, X. Structure and properties of AlCoFeCuMox high entropy alloy coatings prepared by laser cladding and applications on drones for aerospace innovation competitions. J. Alloys Metall. Syst. 2026, 100237. [Google Scholar] [CrossRef] [Scilit]
  100. Guan, S.; Wang, L.; Gao, Q.; Fang, Y.; Zhan, X. Microstructure Evolution and Mechanical Property Enhancement of 30CrMnSiNi2A Steel Repaired by Laser Cladding with AerMet100 Steel. Met. Mater. Int. 2026, 32, 476–489. [Google Scholar] [CrossRef] [Scilit]
  101. Zhao, C.; Song, H.; Shao, H.; Bi, J.; Yang, Z.; Liu, D.; Jia, X.; Zheng, Q.; Dong, G.; Tan, C. Microstructure evolution and synergistic strengthening mechanisms of wear and corrosion resistance in laser cladding fabricated TC11-xMo coatings. Tribol. Int. 2026, 214, 111276. [Google Scholar] [CrossRef] [Scilit]
  102. Natarajan, J.; Karuppasamy, S.S.; Yang, C.-H. Repair of Engineering Components through Laser Cladding. In Tailoring of Engineering Material Properties Through Laser Cladding: Metallurgical, Mechanical and Tribological Properties; CRC Press: Boca Raton, FL, USA, 2026; p. 306. [Google Scholar]
  103. Wang, Q.-Y.; Liu, L.-Y.; Zhang, X.-S.; Xi, Y.-C.; Dong, L.-J.; Bai, S.-L. Tribo-corrosion behavior and mechanism of Ni-WC laser-clad coating in mineralizing solution. J. Mater. Sci. 2025, 60, 3408–3429. [Google Scholar] [CrossRef] [Scilit]
  104. Cui, C.; Zha, E.; Han, J.; Li, P.; Zhang, A. Design of FeCoNiCrMoX laser cladded coatings for drilling equipment in deep complex environment: Insight into microstructure of reticulated brick-mortar imitated nacre pearl layer. Surf. Coat. Technol. 2026, 521, 133065. [Google Scholar] [CrossRef] [Scilit]
  105. Karamimoghadam, M.; Rezayat, M.; Moradi, M.; Mateo, A.; Casalino, G. Laser Surface Transformation Hardening for Automotive Metals: Recent Progress. Metals 2024, 14, 339. [Google Scholar] [CrossRef] [Scilit]
  106. Wang, K.; Yin, X.; Lu, H.; Ai, Y. Enhancing the Wear Resistance of AlSi9Mg Alloys Using Rotatable Inner-Surface Laser Cladding Method. J. Therm. Spray. Technol. 2025, 34, 1747–1762. [Google Scholar] [CrossRef] [Scilit]
  107. Ying, M.; Shao, Y.; Zhang, Q. Application analysis of laser cladding technology in the automotive field. In Proceedings of the International Conference on Mechanical Manufacturing Technology and Material Engineering, MMTME 2024; Springer Proceedings in Materials; Springer: Singapore, 2025; Volume 75. [Google Scholar] [CrossRef] [Scilit]
  108. Li, D.; Zhang, J. Progress in material systems, process control, and performance enhancement of laser cladding technology. J. Adv. Mech. Des. Syst. Manuf. 2026, 20, JAMDSM0006. [Google Scholar] [CrossRef] [Scilit]
  109. Dindar, C.; Altuncu, E.; Aydın, H.; Cavusoglu, O.; Akyuz, R. Tribological and braking performance comparison of martensitic stainless steel coatings deposited by laser cladding and HVOF. Mater. Test. 2026, 68, 981–992. [Google Scholar] [CrossRef] [Scilit]
  110. Altuncu, E.; Yilmaz, H.; Ebrahimi, A.; Dak, M. Enhanced wear and corrosion resistance of high-speed laser-clad automotive brake discs for Euro-7 compliance. Eng. Res. Express 2025, 7, 035526. [Google Scholar] [CrossRef] [Scilit]
  111. Zhang, B.; Hua, X.; Yang, F. Study on Wear and Corrosion Resistance of Co-Cr-Ti Composite Coatings on Ti6Al4V by Laser Cladding. JOM 2025, 77, 4862–4876. [Google Scholar] [CrossRef] [Scilit]
  112. Sathish, M.; Radhika, N.; Saleh, B. A critical review on functionally graded coatings: Methods, properties, and challenges. Compos. Part B Eng. 2021, 225, 109278. [Google Scholar] [CrossRef] [Scilit]
  113. Marquardt, R.; Biegler, M.; Rethmeier, M. Functionally graded material for improved wear resistance manufactured by directed energy deposition. Prog. Addit. Manuf. 2025, 10, 4973–4978. [Google Scholar] [CrossRef] [Scilit]
  114. Singh, S.; Kumar, C.; Sah, S.K. Review on laser powder-based directed energy deposition for fabricating functionally graded materials: Microstructure, mechanical behavior, and defect analysis. J. Laser Appl. 2025, 37, 041202. [Google Scholar] [CrossRef] [Scilit]
  115. Kopec, M. Functionally Graded Nickel-Based Coatings: A Comprehensive Review. Coatings 2026, 16, 397. [Google Scholar] [CrossRef] [Scilit]
  116. Chen, L.; Chen, Y.; Chen, X.; Yu, T.; Wang, Z. Microstructure and properties of in situ TiC/Ni functionally gradient coatings by powder-fed laser cladding. Ceram. Int. 2022, 48, 36789–36801. [Google Scholar] [CrossRef] [Scilit]
  117. Chen, L.; Chen, Y.; Chen, X.; Yu, T.; Wang, Z. A novel laser-cladded AlCuTiVCr/Cu-Al functionally graded coating with excellent corrosion resistance on Mg-Li alloy. Mater. Lett. 2023, 350, 134944. [Google Scholar] [CrossRef] [Scilit]
  118. Wang, G.; Wang, S.; Yin, Z.; Yang, X.; Wen, D.; Sun, Y. Synthesis of Ni-WC/Al-Ni functionally graded coating with advanced corrosion and wear resistance on AZ91D Mg alloy by laser cladding. Mater. Lett. 2023, 333, 133645. [Google Scholar] [CrossRef] [Scilit]
  119. Liu, L.; Huang, X.; Wang, G.; Zhang, X.; Zhou, K.; Wang, B. Microstructure and Mechanical Properties of Functionally Graded Materials on a Ti-6Al-4V Titanium Alloy by Laser Cladding. Materials 2025, 18, 3032. [Google Scholar] [CrossRef] [Scilit]
  120. Qiu, Y.; Wang, Y.; Shu, L.; Huang, T.; Shi, J.; Li, P. Microstructure and properties of Ni-ZrB2 gradient composite coating on the 27SiMn steel surface by laser cladding. Mater. Today Commun. 2026, 43, 111657. [Google Scholar] [CrossRef] [Scilit]
  121. Sun, Q.; Bi, W.; Yao, S.; Zhu, W.; Ma, W.; Hu, B.; Bao, C.; Zhang, Y.; Niu, F. Effect of Gradient Transition Layer on the Cracking Behavior of Ni60B (NiCrBSi) Coatings by Laser Cladding. Materials 2025, 18, 419. [Google Scholar] [CrossRef] [Scilit]
  122. Wang, Z.; Fu, B.; Chen, T.; Chen, L.; Yu, T.; Zhao, J. The microstructure and mechanical properties analysis of H13/Ni60 functionally gradient coating fabricated by laser cladding method. Opt. Laser Technol. 2025, 190, 113204. [Google Scholar] [CrossRef] [Scilit]
  123. Zhang, Q.; Lou, X. Functionally graded molybdenum cladding on 316L stainless steel via laser-powder directed energy deposition. Int. J. Refract. Met. Hard Mater. 2025, 133, 107393. [Google Scholar] [CrossRef] [Scilit]
  124. Müller, S.; Pries, H.; Dilger, K.; Ocylok, S.; Weisheit, A.; Kelbassa, I. Applying Functionally Graded Materials by Laser Cladding: A cost-effective way to improve the Lifetime of Die-Casting Dies. In Glocalized Solutions for Sustainability in Manufacturing; Springer: Berlin/Heidelberg, Germany, 2011. [Google Scholar]
  125. Laser Line. Available online: https://www.laserline.com/en-int/laser-cladding/ (accessed on 23 May 2026).
  126. Marvin, R. Laser-Based Additive Manufacturing of Metal Parts from Powder in Microgravity. 2021. Available online: https://www.hitec.uni-hannover.de/en/large-scale-equipment/einstein-elevator/projects/current-projects-detail-view/projects/laser-based-additive-manufacturing-of-metal-parts-from-powder-in-microgravity (accessed on 25 May 2026).
  127. Choy, K.L. Chemical vapour deposition of coatings. Prog. Mater. Sci. 2003, 48, 57–170. [Google Scholar] [CrossRef] [Scilit]
  128. Igumenov, I.K.; Lukashov, V.V. Modern Solutions for Functional Coatings in CVD Processes. Coatings 2022, 12, 1265. [Google Scholar] [CrossRef] [Scilit]
  129. Mostafavi, A.H.; Mishra, A.K.; Gallucci, F.; Kim, J.H.; Ulbricht, M.; Coclite, A.M.; Hosseini, S.S. Advances in surface modification and functionalization for tailoring the characteristics of thin films and membranes via chemical vapor deposition techniques. J. Appl. Polym. Sci. 2023, 140, e53720. [Google Scholar] [CrossRef] [Scilit]
  130. Sabzi, M.; Anijdan, S.H.M.; Shamsodin, M.; Farzam, M.; Hojjati-Najafabadi, A.; Feng, P.; Park, N.; Lee, U. A Review on Sustainable Manufacturing of Ceramic-Based Thin Films by Chemical Vapor Deposition (CVD): Reactions Kinetics and the Deposition Mechanisms. Coatings 2023, 13, 188. [Google Scholar] [CrossRef] [Scilit]
  131. Dobrzanski, L.; Pakula, D.; Staszuk, M. Chemical Vapor Deposition in Manufacturing. In Handbook of Manufacturing Engineering and Technology; Nee, A., Ed.; Springer: London, UK, 2013; pp. 1–41. [Google Scholar]
  132. Pagliuca, J.; Macha, P.; Naeem, M.; Vasudev, M.C. Plasma enhanced vapor deposition of dipeptide nanostructures: Nanotubes to nanoflowers. Mater. Adv. 2026, 7, 4061–4073. [Google Scholar] [CrossRef] [Scilit]
  133. Zhang, C.; Wu, M.; Wang, P.; Jian, M.; Zhang, J.; Yang, L. Stability of SiNx Prepared by Plasma-Enhanced Chemical Vapor Deposition at Low Temperature. Nanomaterials 2021, 11, 3363. [Google Scholar] [CrossRef] [Scilit]
  134. Jones, A.C.; Hitchman, M.L. Overview of Chemical Vapour Deposition. In Chemical Vapour Deposition: Precursors, Processes and Applications; The Royal Society of Chemistry: London, UK, 2008. [Google Scholar]
  135. Tenhaeff, W.E.; Gleason, K.K. Initiated and Oxidative Chemical Vapor Deposition of Polymeric Thin Films: ICVD and oCVD. Adv. Funct. Mater. 2008, 18, 979–992. [Google Scholar] [CrossRef] [Scilit]
  136. Kaviani, S.; Ghaleni, M.M.; Tavakoli, E.; Nejati, S. Electroactive and Conformal Coatings of Oxidative Chemical Vapor Deposition Polymers for Oxygen Electroreduction. ACS Appl. Polym. Mater. 2019, 1, 552–560. [Google Scholar] [CrossRef] [Scilit]
  137. Gleason, K.K. Designing Organic and Hybrid Surfaces and Devices with Initiated Chemical Vapor Deposition (iCVD). Adv. Mater. 2024, 36, 2306665. [Google Scholar] [CrossRef] [Scilit]
  138. Heydari Gharahcheshmeh, M. Fabrication of Conjugated Conducting Polymers by Chemical Vapor Deposition (CVD) Method. Nanomaterials 2025, 15, 452. [Google Scholar] [CrossRef] [Scilit]
  139. Li, W.; Bradley, L.C.; Watkins, J.J. Copolymer Solid-State Electrolytes for 3D Microbatteries via Initiated Chemical Vapor Deposition. ACS Appl. Mater. Interfaces 2019, 11, 5668–5674. [Google Scholar] [CrossRef] [Scilit]
  140. Baek, J.; Shan, Y.; Mylvaganan, M.; Zhang, Y.; Yang, X.; Qin, F.; Zhao, K.; Song, H.W.; Mao, H.; Lee, S. Mold-Free Manufacturing of Highly Sensitive and Fast-Response Pressure Sensors Through High-Resolution 3D Printing and Conformal Oxidative Chemical Vapor Deposition Polymers. Adv. Mater. 2023, 35, 2304070. [Google Scholar] [CrossRef] [Scilit]
  141. Sumanth Kumar, D.; Kumar, B.J.; Mahesh, H.M. Chapter 3—Quantum Nanostructures (QDs): An Overview. In Synthesis of Inorganic Nanomaterials; Mohan Bhagyaraj, S., Ed.; Woodhead Publishing: Sawston, UK, 2018; pp. 59–88. [Google Scholar]
  142. Pochet, L.F.; Howard, P.; Safaie, S. CVD coatings: From cutting tools to aerospace applications and its future potential. Surf. Coat. Technol. 1997, 94–95, 70–75. [Google Scholar] [CrossRef] [Scilit]
  143. Grzesik, W. The role of coatings in controlling the cutting process when turning with coated indexable inserts. J. Mater. Process. Technol. 1998, 79, 133–143. [Google Scholar] [CrossRef] [Scilit]
  144. Ganeshkumar, S.; Venkatesh, S.; Paranthaman, P.; Arulmurugan, R.; Arunprakash, J.; Manickam, M.; Rajendiran, G. Performance of Multilayered Nanocoated Cutting Tools in High-Speed Machining: A Review. Int. J. Photoenergy 2022, 2022, 5996061. [Google Scholar] [CrossRef] [Scilit]
  145. Wang, Y.; Feng, C.; Lin, T.; Zhu, R.; Zhang, J.; Yang, H.; Yi, S.; He, J.; Tu, M.; Wei, G. A Review of Wear-Resistant Coatings for Steel Substrates: Applications and Challenges. Metals 2025, 15, 1231. [Google Scholar] [CrossRef] [Scilit]
  146. Ahmed, Y.S.; Fox-Rabinovich, G.; Paiva, J.M.; Wagg, T.; Veldhuis, S.C. Effect of Built-Up Edge Formation during Stable State of Wear in AISI 304 Stainless Steel on Machining Performance and Surface Integrity of the Machined Part. Materials 2017, 10, 1230. [Google Scholar] [CrossRef] [Scilit]
  147. Zhu, M.; Achache, S.; Motta, M.P.; Delblouwe, A.; Pelaingre, C.; García-Wong, A.C.; Pierson, J.-F.; Sanchette, F. Characteristics and Cutting Performance of CVD Al2O3 Multilayer Coatings Deposited on Tungsten Carbide Cutting Inserts in Turning of 24CrMoV5-1 Steel. Coatings 2023, 13, 883. [Google Scholar] [CrossRef] [Scilit]
  148. Chen, H.; Wang, Y.; Jiao, J.; Tan, Z.; Huang, L.; Zhong, Z. Combined post-treatment approach for improving the surface integrity of CVD α-Al2O3 coating and the tool wear resistance. Ceram. Int. 2023, 49, 39488–39498. [Google Scholar] [CrossRef] [Scilit]
  149. Almeida, F.; Sacramento, J.; Oliveira, F.; Silva, R. Micro- and nano-crystalline CVD diamond coated tools in the turning of EDM graphite. Surf. Coat. Technol. 2008, 203, 271–276. [Google Scholar] [CrossRef] [Scilit]
  150. Zhang, J.; Wang, X.; Shen, B.; Sun, F. Effect of boron and silicon doping on improving the cutting performance of CVD diamond coated cutting tools in machining CFRP. Int. J. Refract. Met. Hard Mater. 2013, 41, 285–292. [Google Scholar] [CrossRef] [Scilit]
  151. Saijo, K.; Yagi, M.; Shibuki, K.; Takatsu, S. Deposition of diamond for cutting tool applications. Mater. Manuf. Process. 1993, 8, 59–73. [Google Scholar] [CrossRef] [Scilit]
  152. Zhang, Z.; Xiang, D.; Zhang, Z.; Zhang, Y.; Zhao, B. Study on tribology and cutting performance of boron doped diamond composite coated tool. Int. J. Refract. Met. Hard Mater. 2023, 117, 106385. [Google Scholar] [CrossRef] [Scilit]
  153. Zhao, G.; Li, Z.; Hu, M.; Li, L.; He, N.; Jamil, M. Fabrication and performance of CVD diamond cutting tool in micro milling of oxygen-free copper. Diam. Relat. Mater. 2019, 100, 107589. [Google Scholar] [CrossRef] [Scilit]
  154. Parray, M.A.; Din, S.H.; Wani, M.F. Enhancing machining performance of EN24 steel with CVD diamond coated tool and minimal quantity lubrication. Eng. Res. Express 2024, 6, 015063. [Google Scholar] [CrossRef] [Scilit]
  155. Faßbender, F.; Schmitt, G.; Schöning, M.; Lüth, H.; Buß, G.; Schultze, J.-W. Optimization of passivation layers for corrosion protection of silicon-based microelectrode arrays. Sens. Actuators B Chem. 2000, 68, 128–133. [Google Scholar] [CrossRef] [Scilit]
  156. Martinu, L.; Zabeida, O.; Klemberg-Sapieha, J.E. Chapter 9—Plasma-Enhanced Chemical Vapor Deposition of Functional Coatings. In Handbook of Deposition Technologies for Films and Coatings, 3rd ed.; Martin, P.M., Ed.; William Andrew Publishing: Boston, MA, USA, 2010; pp. 392–465. [Google Scholar]
  157. Bonilla, R.S.; Hoex, B.; Hamer, P.; Wilshaw, P.R. Dielectric surface passivation for silicon solar cells: A review. Phys. Status Solidi A 2017, 214, 1700293. [Google Scholar] [CrossRef] [Scilit]
  158. Richter, A.; Benick, J.; Feldmann, F.; Fell, A.; Hermle, M.; Glunz, S.W. N-Type Si solar cells with passivating electron contact: Identifying sources for efficiency limitations by wafer thickness and resistivity variation. Sol. Energy Mater. Sol. Cells 2017, 173, 96–105. [Google Scholar] [CrossRef] [Scilit]
  159. Nandakumar, N.; Rodriguez, J.; Kluge, T.; Groβe, T.; Fondop, L.; Padhamnath, P.; Balaji, N.; König, M.; Duttagupta, S. Approaching 23% with large-area monoPoly cells using screen-printed and fired rear passivating contacts fabricated by inline PECVD. Prog. Photovolt. Res. Appl. 2019, 27, 107–112. [Google Scholar] [CrossRef] [Scilit]
  160. Mousumi, J.F.; Gregory, G.; Ganesan, J.P.; Nunez, C.; Provancha, K.; Seren, S.; Zunft, H.; Jurca, T.; Banerjee, P.; Kar, A.; et al. Process–Structure–Properties Relationships of Passivating, Electron-Selective Contacts Formed by Atmospheric Pressure Chemical Vapor Deposition of Phosphorus-Doped Polysilicon. Phys. Status Solidi (RRL)—Rapid Res. Lett. 2022, 16, 2100639. [Google Scholar] [CrossRef] [Scilit]
  161. Schmitt, G.; Schultze, J.-W.; Faßbender, F.; Buß, G.; Lüth, H.; Schöning, M. Passivation and corrosion of microelectrode arrays. Electrochim. Acta 1999, 44, 3865–3883. [Google Scholar] [CrossRef] [Scilit]
  162. Volksen, W.; Miller, R.D.; Dubois, G. Low Dielectric Constant Materials. Chem. Rev. 2010, 110, 56–110. [Google Scholar] [CrossRef] [Scilit]
  163. Fang, Q.; Yi, K.; Zhai, T.; Luo, S.; Lin, C.-Y.; Ai, Q.; Zhu, Y.; Zhang, B.; Alvarez, G.A.; Shao, Y.; et al. High-performance 2D electronic devices enabled by strong and tough two-dimensional polymer with ultra-low dielectric constant. Nat. Commun. 2024, 15, 10780. [Google Scholar] [CrossRef] [Scilit]
  164. Seo, C.; Baek, N.; Kang, S.; Park, G.; Cha, J.; Jang, T.; Jang, S.; Jung, D. Study on plasma-polymerized 1-(trimethylsilyl)pyrrolidine films deposited by plasma-enhanced chemical vapor deposition for use as a Cu diffusion barrier in multilevel metallization process. Microelectron. Eng. 2024, 291, 112192. [Google Scholar] [CrossRef] [Scilit]
  165. Gaitan, G.; Koufalis, P.; Liepe, M.; McNeal, S.R.; Arrieta, V. CVD Nb3Sn-on-copper SRF accelerator cavities. In Proceedings of the IPAC, Bangkok, Thailand, 12–17 June 2022; JACoW Publishing: Geneva, Switzerland, 2022; p. 1291. [Google Scholar]
  166. Gaitan, G.; Holic, A.; Howes, W.I.; Kulina, G.; Liepe, M.; Quigley, P.; Sears, J.; Sun, Z.; Wendland, B. Development of a Plasma-Enhanced Chemical Vapor Deposition System for High-Performance SRF Cavities. In Proceedings of the 21th International Conference on RF Superconductivity (SRF′23), Grand Rapids, MI, USA, 25–30 June 2023; JACOW Publishing: Geneva, Switzerland, 2023. [Google Scholar]
  167. Kosky, P.; Peters, H.; Spiro, C.; McAtee, D.; Rumaner, L.; Marsh, D. Superconducting Nb3Sn joints by chemical vapour deposition. Cryogenics 1994, 34, 753–759. [Google Scholar] [CrossRef] [Scilit]
  168. Sibanda, D.; Oyinbo, S.T.; Jen, T.-C.; Ibitoye, A.I. A Mini Review on Thin Film Superconductors. Processes 2022, 10, 1184. [Google Scholar] [CrossRef] [Scilit]
  169. Porrati, F.; Barth, S.; Gazzadi, G.C.; Frabboni, S.; Volkov, O.M.; Makarov, D.; Huth, M. Site-Selective Chemical Vapor Deposition on Direct-Write 3D Nanoarchitectures. ACS Nano 2023, 17, 4704–4715. [Google Scholar] [CrossRef] [Scilit]
  170. Zheng, J.; Yang, J.; Cao, W.; Huang, Y.; Zhou, Z.; Huang, Y.-X. Fabrication of transparent wear-resistant superhydrophobic SiO2 film via phase separation and chemical vapor deposition methods. Ceram. Int. 2022, 48, 32143–32151. [Google Scholar] [CrossRef] [Scilit]
  171. Huang, X.; Sun, M.; Shi, X.; Shao, J.; Jin, M.; Liu, W.; Zhang, R.; Huang, S.; Ye, Y. Chemical vapor deposition of transparent superhydrophobic anti-Icing coatings with tailored polymer nanoarray architecture. Chem. Eng. J. 2023, 454, 139981. [Google Scholar] [CrossRef] [Scilit]
  172. Cao, Y.; Lu, Y.; Liu, N.; Li, Y.; Wang, P.; Dai, C.; Wei, Y. Multi-applicable, durable superhydrophobic anti-icing coating through template-method and chemical vapor deposition. Surf. Interfaces 2022, 32, 102100. [Google Scholar] [CrossRef] [Scilit]
  173. Fu, J.; Sun, Y.; Ji, Y.; Zhang, J. Fabrication of robust ceramic based superhydrophobic coating on aluminum substrate via plasma electrolytic oxidation and chemical vapor deposition methods. J. Mater. Process. Technol. 2022, 306, 117641. [Google Scholar] [CrossRef] [Scilit]
  174. Lotti, F.; Ranieri, F.; Vadalà, G.; Zollo, L.; Di Pino, G. Invasive Intraneural Interfaces: Foreign Body Reaction Issues. Front. Neurosci. 2017, 11, 497. [Google Scholar] [CrossRef] [Scilit]
  175. Hayles, A.; Hasan, J.; Bright, R.; Palms, D.; Brown, T.; Barker, D.; Vasilev, K. Hydrothermally etched titanium: A review on a promising mechano-bactericidal surface for implant applications. Mater. Today Chem. 2021, 22, 100622. [Google Scholar] [CrossRef] [Scilit]
  176. Roh, S.; Jang, Y.; Yoo, J.; Seong, H. Surface Modification Strategies for Biomedical Applications: Enhancing Cell–Biomaterial Interfaces and Biochip Performances. BioChip J. 2023, 17, 174–191. [Google Scholar] [CrossRef] [Scilit]
  177. Romo-Rico, J.; Bright, R.; Krishna, S.M.; Vasilev, K.; Golledge, J.; Jacob, M.V. Antimicrobial graphene-based coatings for biomedical implant applications. Carbon Trends 2023, 12, 100282. [Google Scholar] [CrossRef] [Scilit]
  178. Saba, T.; Saad, K.S.K.; Rashid, A.B. Precise surface engineering: Leveraging chemical vapor deposition for enhanced biocompatibility and durability in biomedical implants. Heliyon 2024, 10, e37976. [Google Scholar] [CrossRef] [Scilit]
  179. Shu, H.; Chen, P.; Yang, R. Advances in Antibacterial Polymer Coatings Synthesized via Chemical Vapor Deposition. Chem. Bio Eng. 2024, 1, 516–534. [Google Scholar] [CrossRef] [Scilit]
  180. Su, C.; Ye, Y.; Qiu, H.; Zhu, Y. Solvent-Free Fabrication of Self-Regenerating Antibacterial Surfaces Resisting Biofilm Formation. ACS Appl. Mater. Interfaces 2021, 13, 10553–10563. [Google Scholar] [CrossRef] [Scilit]
  181. Greenhorn, S.; Bano, E.; Stambouli, V.; Zekentes, K. Amorphous SiC Thin Films Deposited by Plasma-Enhanced Chemical Vapor Deposition for Passivation in Biomedical Devices. Materials 2024, 17, 1135. [Google Scholar] [CrossRef] [Scilit]
  182. Li, X.; Wang, L.; Yu, X.; Feng, Y.; Wang, C.; Yang, K.; Su, D. Tantalum coating on porous Ti6Al4V scaffold using chemical vapor deposition and preliminary biological evaluation. Mater. Sci. Eng. C 2013, 33, 2987–2994. [Google Scholar] [CrossRef] [Scilit]
  183. Ghorbani, H.; Abdollah-Zadeh, A.; Bagheri, F.; Poladi, A. Improving the bio-corrosion behavior of AISI316L stainless steel through deposition of Ta-based thin films using PACVD. Appl. Surf. Sci. 2018, 456, 398–402. [Google Scholar] [CrossRef] [Scilit]
  184. Gao, H.; Yang, J.; Jin, X.; Qu, X.; Zhang, F.; Zhang, D.; Chen, H.; Wei, H.; Zhang, S.; Jia, W.; et al. Porous tantalum scaffolds: Fabrication, structure, properties, and orthopedic applications. Mater. Des. 2021, 210, 110095. [Google Scholar] [CrossRef] [Scilit]
  185. Ma, Z. Influencing factors and biological property of novel biomedical materials: Porous silicon carbide coated with bioactive tantalum. Chin. J. Tissue Eng. Res. 2021, 25, 558. [Google Scholar]
  186. Liu, B.; Ma, Z.; Li, J.; Xie, H.; Wei, X.; Wang, B.; Tian, S.; Yang, J.; Yang, L.; Cheng, L.; et al. Experimental study of a 3D printed permanent implantable porous Ta-coated bone plate for fracture fixation. Bioact. Mater. 2022, 10, 269–280. [Google Scholar] [CrossRef] [Scilit]
  187. Liu, F.; Wang, H.; Zhao, B.; Zhang, W.; Wang, Q.; Niu, Y.; Wang, Y.; Yu, H.; Wang, Q.; Yang, K. Study on deposition of biomedical Ta coating on Ti6Al4V alloy substrate by CVD and its properties. Surf. Coat. Technol. 2025, 495, 131593. [Google Scholar] [CrossRef] [Scilit]
  188. Ng, P.R.; Zhang, Y.; Min, T.J.J.; Liu, X.; Lin, M.; Ivanov, A.S.; Nikolaev, K.G.; Mahfouz, R.; Tayeb, T.M.; Qari, N.; et al. Graphene and amorphous carbon coatings for nitinol cardiovascular stents by direct chemical vapor deposition: A comparative insight. Mater. Des. 2026, 265, 115864. [Google Scholar] [CrossRef] [Scilit]
  189. Liu, Y.; Zou, T.; Xu, C.; Zhen, L.; Li, Y.; Noh, Y. Atomic Layer Deposition in Transistors and Monolithic 3D Integration. Adv. Funct. Mater. 2026, 36, e74729. [Google Scholar] [CrossRef] [Scilit]
  190. Ji, Y.J.; Kim, H.I.; Choi, S.Y.; Kang, J.E.; Ellingboe, A.R.; Chandra, H.; Lee, C.-W.; Yeom, G.Y. Plasma Enhanced Atomic Layer Deposition of Silicon Nitride for Two Different Aminosilane Precursors Using Very High Frequency (162 MHz) Plasma Source. ACS Appl. Mater. Interfaces 2023, 15, 28763–28771. [Google Scholar] [CrossRef] [Scilit]
  191. Kim, M.-S.; Lim, C.-M.; Kim, S.H.; Kim, D.; Jeon, H.; Chung, C.W. Plasma-Enhanced Atomic Layer Deposition of TiN Thin Films Using Ultralow Electron Temperature Plasma. ACS Appl. Mater. Interfaces 2025, 17, 11227–11235, Erratum in ACS Appl. Mater. Interfaces 2026, 18, 42236. [Google Scholar] [CrossRef] [Scilit]
  192. Riazimehr, S.; Esteki, A.; Otto, M.; Powell, M.; Rinke, G.; Robertz, B.; Wang, Z.; Lemme, M.C.; Hore, K.; Knoops, H. Plasma-enhanced atomic layer deposition of Al2O3 on graphene via an in situ-deposited interlayer. Mater. Sci. Semicond. Process. 2025, 199, 109829. [Google Scholar] [CrossRef] [Scilit]
  193. Hoye, R.L.; Muñoz-Rojas, D.; Sun, Z.; Okcu, H.; Asgarimoghaddam, H.; MacManus-Driscoll, J.L.; Musselman, K.P. Spatial Atomic Layer Deposition for Energy and Electronic Devices. PRX Energy 2025, 4, 017002. [Google Scholar] [CrossRef] [Scilit]
  194. Lee, J.; Oh, J.; Lee, J.; Lee, J.-M.; Kim, H.G.; Cho, B.; Kim, M.S.; Kim, W.-H. Area-selective atomic layer deposition of Al2O3 thin films for metal versus dielectric selectivity using vapor-dosed alkanethiols. Surf. Interfaces 2025, 67, 106588. [Google Scholar] [CrossRef] [Scilit]
  195. Park, J.; Kwak, S.J.; Kang, S.; Oh, S.; Shin, B.; Noh, G.; Kim, T.S.; Kim, C.; Park, H.; Oh, S.H.; et al. Area-selective atomic layer deposition on 2D monolayer lateral superlattices. Nat. Commun. 2024, 15, 2138. [Google Scholar] [CrossRef] [Scilit]
  196. Heikkinen, M.; Ghiyasi, R.; Karppinen, M. Layer-Engineered Functional Multilayer Thin-Film Structures and Interfaces through Atomic and Molecular Layer Deposition. Adv. Mater. Interfaces 2025, 12, 2400262. [Google Scholar] [CrossRef] [Scilit]
  197. Sun, H.; Dai, H.; Zhang, G.; Sun, S. Interface engineering of inorganic solid-state lithium batteries via atomic and molecular layer deposition. InfoMat 2025, 7, e12650. [Google Scholar] [CrossRef] [Scilit]
  198. Niinistö, J.; Kukli, K.; Heikkilä, M.; Ritala, M.; Leskelä, M. Atomic Layer Deposition of High-k Oxides of the Group 4 Metals for Memory Applications. Adv. Eng. Mater. 2009, 11, 223–234. [Google Scholar] [CrossRef] [Scilit]
  199. Ovanesyan, R.A.; Filatova, E.A.; Elliott, S.D.; Hausmann, D.M.; Smith, D.C.; Agarwal, S. Atomic layer deposition of silicon-based dielectrics for semiconductor manufacturing: Current status and future outlook. J. Vac. Sci. Technol. A 2019, 37, 060904. [Google Scholar] [CrossRef] [Scilit]
  200. Zhao, C.; Xiang, J. Atomic Layer Deposition (ALD) of Metal Gates for CMOS. Appl. Sci. 2019, 9, 2388. [Google Scholar] [CrossRef] [Scilit]
  201. Jeon, W. Recent advances in the understanding of high-k dielectric materials deposited by atomic layer deposition for dynamic random-access memory capacitor applications. J. Mater. Res. 2020, 35, 775–794. [Google Scholar] [CrossRef] [Scilit]
  202. Ovanesyan, R.A.; Hausmann, D.M.; Agarwal, S. A Three-Step Atomic Layer Deposition Process for SiNx Using Si2Cl6, CH3NH2, and N2 Plasma. ACS Appl. Mater. Interfaces 2018, 10, 19153–19161. [Google Scholar] [CrossRef] [Scilit]
  203. Liu, F.; Sneck, A.; Eskelinen, P.; Halonen, O.; Gillan, L.; Leppäniemi, J. ALD-Grown ZnO TFTs Patterned by High-Resolution Reverse-Offset Printing. ACS Appl. Mater. Interfaces 2025, 17, 34150–34160. [Google Scholar] [CrossRef] [Scilit]
  204. Park, C.; Kweon, M.; Mohapatra, D.; Cheon, T.; Bae, J.-S.; Jeong, D.; Jang, H.; Shim, S.; Park, Y.-B.; Kang, Y.; et al. Highly Conductive Ultrathin Niobium Carbide Thin Films as Next-Generation Diffusion Barriers for Cu and Ru Interconnects Prepared by Plasma-Enhanced Atomic Layer Deposition. Chem. Mater. 2025, 37, 4743–4757. [Google Scholar] [CrossRef] [Scilit]
  205. Hwang, Y.; Park, B.; Hwang, S.; Choi, S.; Kim, H.S.; Kim, A.R.; Choi, J.W.; Yoon, J.; Kwon, J.; Kim, Y. A Bioinspired Ultra Flexible Artificial van der Waals 2D-MoS2 Channel/LiSiOx Solid Electrolyte Synapse Arrays via Laser-Lift Off Process for Wearable Adaptive Neuromorphic Computing. Small Methods 2023, 7, 2201719. [Google Scholar] [CrossRef] [Scilit]
  206. Li, Q.; Wang, S.; Li, Z.; Hu, X.; Liu, Y.; Yu, J.; Yang, Y.; Wang, T.; Meng, J.; Sun, Q.; et al. High-performance ferroelectric field-effect transistors with ultra-thin indium tin oxide channels for flexible and transparent electronics. Nat. Commun. 2024, 15, 2686. [Google Scholar] [CrossRef] [Scilit]
  207. Zhou, X.; Sun, H.; Li, J.; Du, X.; Wang, H.; Luo, Z.; Wang, Z.; Lin, Y.; Shen, S.; Yin, Y.; et al. A flexible Hf0.5Zr0.5O2 thin film with highly robust ferroelectricity. J. Mater. 2024, 10, 210–217. [Google Scholar] [CrossRef] [Scilit]
  208. Benick, J.; Hoex, B.; van de Sanden, M.C.M.; Kessels, W.M.M.; Schultz, O.; Glunz, S.W. High efficiency n-type Si solar cells on Al2O3-passivated boron emitters. Appl. Phys. Lett. 2008, 92, 253504. [Google Scholar] [CrossRef] [Scilit]
  209. Riha, S.C.; Koegel, A.A.; Emery, J.D.; Pellin, M.J.; Martinson, A.B.F. Low-Temperature Atomic Layer Deposition of CuSbS2 for Thin-Film Photovoltaics. ACS Appl. Mater. Interfaces 2017, 9, 4667–4673. [Google Scholar] [CrossRef] [Scilit]
  210. Ukoba, O.K.; Jen, T.C. Review of Atomic Layer Deposition of Nanostructured Solar Cells 4. J. Phys. Conf. Ser. 2019, 1378, 042060. [Google Scholar] [CrossRef] [Scilit]
  211. Hossain, A.; Khoo, K.T.; Cui, X.; Poduval, G.K.; Zhang, T.; Li, X.; Li, W.M.; Hoex, B. Atomic layer deposition enabling higher efficiency solar cells: A review. Nano Mater. Sci. 2020, 2, 204–226. [Google Scholar] [CrossRef] [Scilit]
  212. Zhou, B.; Liu, M.; Wen, Y.; Li, Y.; Chen, R. Atomic layer deposition for quantum dots based devices. Opto-Electron. Adv. 2020, 3, 190043–190051. [Google Scholar] [CrossRef] [Scilit]
  213. Jia, J.; Jiang, Z.; Ma, S.; Guo, S.; Wu, J.; Zhang, Y.; Cao, B.; Dong, J. Novel Strategy for High Efficient and Stable Perovskite Solar Cells through Atomic Layer Deposition. ACS Appl. Mater. Interfaces 2024, 16, 3576–3585. [Google Scholar] [CrossRef] [Scilit]
  214. Zheng, Z.; Xue, Z.; Zhao, K.; Yang, Y.; Zhu, X.; Li, H.; Cheng, S.; Li, S.; Yan, N.; Wang, Z. Unveiling and Overcoming Instabilities in Perovskite Solar Cells Induced by Atomic-Layer-Deposition Tin Oxide. Sol. RRL 2024, 8, 2301076. [Google Scholar] [CrossRef] [Scilit]
  215. Rajbhandari, P.P.; Rijal, B.; Chen, Z.; Choudhary, A.; Efstathiadis, H.; Dhakal, T.P. Performance enhancement of inverted perovskite solar cells through lithium-ion diffusion from the nickel oxide hole transport layer to the perovskite absorber. Energy Adv. 2025, 4, 1455–1463. [Google Scholar] [CrossRef] [Scilit]
  216. Xie, Z.; Liu, X.; Wang, W.; Wang, X.; Liu, C.; Xie, Q.; Li, Z.; Zhang, Z. Enhanced photoelectrochemical and photocatalytic performance of TiO2 nanorod arrays/CdS quantum dots by coating TiO2 through atomic layer deposition. Nano Energy 2015, 11, 400–408. [Google Scholar] [CrossRef] [Scilit]
  217. Cheng, C.-Y.; Mao, M.-H. Photo-stability and time-resolved photoluminescence study of colloidal CdSe/ZnS quantum dots passivated in Al2O3 using atomic layer deposition. J. Appl. Phys. 2016, 120, 083103. [Google Scholar] [CrossRef] [Scilit]
  218. Devloo-Casier, K.; Geiregat, P.; Ludwig, K.F.; van Stiphout, K.; Vantomme, A.; Hens, Z.; Detavernier, C.; Dendooven, J. A Case Study of ALD Encapsulation of Quantum Dots: Embedding Supported CdSe/CdS/ZnS Quantum Dots in a ZnO Matrix. J. Phys. Chem. C 2016, 120, 18039–18045. [Google Scholar] [CrossRef] [Scilit]
  219. Xiang, Q.; Zhou, B.; Cao, K.; Wen, Y.; Li, Y.; Wang, Z.; Jiang, C.; Shan, B.; Chen, R. Bottom up Stabilization of CsPbBr3 Quantum Dots-Silica Sphere with Selective Surface Passivation via Atomic Layer Deposition. Chem. Mater. 2018, 30, 8486–8494. [Google Scholar] [CrossRef] [Scilit]
  220. Chen, X.; Pomerantseva, E.; Banerjee, P.; Gregorczyk, K.; Ghodssi, R.; Rubloff, G. Ozone-Based Atomic Layer Deposition of Crystalline V2O5 Films for High Performance Electrochemical Energy Storage. Chem. Mater. 2012, 24, 1255–1261. [Google Scholar] [CrossRef] [Scilit]
  221. Guan, C.; Wang, J. Recent Development of Advanced Electrode Materials by Atomic Layer Deposition for Electrochemical Energy Storage. Adv. Sci. 2016, 3, 1500405. [Google Scholar] [CrossRef] [Scilit]
  222. Liu, J.; Wang, B.; Sun, Q.; Li, R.; Sham, T.; Sun, X. Atomic Layer Deposition of Hierarchical CNTs@FePO4 Architecture as a 3D Electrode for Lithium-Ion and Sodium-Ion Batteries. Adv. Mater. Interfaces 2016, 3, 1600468. [Google Scholar] [CrossRef] [Scilit]
  223. Ma, L.; Nuwayhid, R.B.; Wu, T.; Lei, Y.; Amine, K.; Lu, J. Atomic Layer Deposition for Lithium-Based Batteries. Adv. Mater. Interfaces 2016, 3, 1600564. [Google Scholar] [CrossRef] [Scilit]
  224. Li, Z.; Su, J.; Wang, X. Atomic layer deposition in the development of supercapacitor and lithium-ion battery devices. Carbon 2021, 179, 299–326. [Google Scholar] [CrossRef] [Scilit]
  225. Gupta, B.; Hossain, A.; Riaz, A.; Sharma, A.; Zhang, D.; Tan, H.H.; Jagadish, C.; Catchpole, K.; Hoex, B.; Karuturi, S. Recent Advances in Materials Design Using Atomic Layer Deposition for Energy Applications. Adv. Funct. Mater. 2022, 32, 2109105. [Google Scholar] [CrossRef] [Scilit]
  226. Ansari, M.Z.; Hussain, I.; Mohapatra, D.; Ansari, S.A.; Rahighi, R.; Nandi, D.K.; Song, W.; Kim, S. Atomic Layer Deposition—A Versatile Toolbox for Designing/Engineering Electrodes for Advanced Supercapacitors. Adv. Sci. 2024, 11, 2303055. [Google Scholar] [CrossRef] [Scilit]
  227. Deshmukh, S.; Gao, W.; Michalička, J.; Pumera, M. Nanoscopic decoration of multivalent vanadium oxide on Laser-Induced graphene fibers via atomic layer deposition for flexible gel supercapacitors. Chem. Eng. J. 2024, 480, 147895. [Google Scholar] [CrossRef] [Scilit]
  228. Lopa, N.S.; Akbari, M.K.; Lu, H.L.; Zhuiykov, S. ALD-enabled WO3-MoO3 nanohybrid heterostructure for high-performance electrochemical supercapacitors. J. Energy Storage 2024, 84, 110777. [Google Scholar] [CrossRef] [Scilit]
  229. Juholin, P.; Kääriäinen, M.-L.; Riihimäki, M.; Sliz, R.; Aguirre, J.L.; Pirilä, M.; Fabritius, T.; Cameron, D.; Keiski, R.L. Comparison of ALD coated nanofiltration membranes to unmodified commercial membranes in mine wastewater treatment. Sep. Purif. Technol. 2018, 192, 69–77. [Google Scholar] [CrossRef] [Scilit]
  230. Weber, M.; Julbe, A.; Ayral, A.; Miele, P.; Bechelany, M. Atomic Layer Deposition for Membranes: Basics, Challenges, and Opportunities. Chem. Mater. 2018, 30, 7368–7390. [Google Scholar] [CrossRef] [Scilit]
  231. Xiong, S.; Qian, X.; Zhong, Z.; Wang, Y. Atomic layer deposition for membrane modification, functionalization and preparation: A review. J. Membr. Sci. 2022, 658, 120740. [Google Scholar] [CrossRef] [Scilit]
  232. Chen, P.; Huang, J.; Dong, Y.; Zhu, Y.; Dong, L.; Zhang, C.; Bai, Y. Dialdehyde polyethylene glycol cross-linked poly(vinyl alcohol) membranes with enhanced CO2/N2 separation performance. J. Appl. Polym. Sci. 2024, 141, e55266. [Google Scholar] [CrossRef] [Scilit]
  233. Hu, L.; Bui, V.T.; Esmaeili, N.; Lin, H. Nanoengineering membrane surfaces: A new paradigm for efficient CO2 capture. Carbon Capture Sci. Technol. 2024, 10, 100150. [Google Scholar] [CrossRef] [Scilit]
  234. Yang, X.; Sun, P.; Wen, Y.; Mane, A.U.; Elam, J.W.; Ma, J.; Liu, S.; Darling, S.B.; Shao, L. Protein-activated atomic layer deposition for robust crude-oil-repellent hierarchical nano-armored membranes. Sci. Bull. 2024, 69, 218–226. [Google Scholar] [CrossRef] [Scilit]
  235. O’nEill, B.J.; Jackson, D.H.K.; Lee, J.; Canlas, C.; Stair, P.C.; Marshall, C.L.; Elam, J.W.; Kuech, T.F.; Dumesic, J.A.; Huber, G.W. Catalyst Design with Atomic Layer Deposition. ACS Catal. 2015, 5, 1804–1825. [Google Scholar] [CrossRef] [Scilit]
  236. Yang, J.; Li, W.; Wang, D.; Li, Y. Electronic Metal–Support Interaction of Single-Atom Catalysts and Applications in Electrocatalysis. Adv. Mater. 2020, 32, 2003300. [Google Scholar] [CrossRef] [Scilit]
  237. Chen, Y.; Chen, J.; Zhang, J.; Luo, Y.; Zhang, C.; Xue, Y.; Wang, G.; Wang, R. Assist more Pt-O bonds of Pt/MoO3-CNT as a highly efficient and stable electrocatalyst for methanol oxidation and oxygen reduction reaction. J. Alloys Compd. 2021, 873, 159827. [Google Scholar] [CrossRef] [Scilit]
  238. Zhang, J.; Yuan, Y.; Gao, L.; Zeng, G.; Li, M.; Huang, H. Stabilizing Pt-Based Electrocatalysts for Oxygen Reduction Reaction: Fundamental Understanding and Design Strategies. Adv. Mater. 2021, 33, 2006494. [Google Scholar] [CrossRef] [Scilit]
  239. Yan, L.; Li, P.; Zhu, Q.; Kumar, A.; Sun, K.; Tian, S.; Sun, X. Atomically precise electrocatalysts for oxygen reduction reaction. Chem 2023, 9, 280–342. [Google Scholar] [CrossRef] [Scilit]
  240. Jung, M.; Razazzadeh, A.; Khan, H.; Kwon, S. Catalysts Design and Atomistic Reaction Modulation by Atomic Layer Deposition for Energy Conversion and Storage Applications. Exploration 2025, 5, e20240010. [Google Scholar] [CrossRef] [Scilit]
  241. Song, Z.; Zhou, X.; Sun, L.; Zhang, Q.; Li, Y.; Ren, X.; Zhang, H.; Zhang, L. Enhancing electron interaction between Pt and support for superior electrochemical performance through atomic layer deposition of tungsten oxide. J. Colloid Interface Sci. 2024, 654, 1272–1280. [Google Scholar] [CrossRef] [Scilit]
  242. Sheng, X.; Lin, G.; Zhang, K.; Han, S.; Wang, S.; Hu, T.; Li, S.; Liu, J.; Zhang, L. Advances in ultrasound-assisted electrodeposition of metals: Mechanism and processing. J. Alloys Compd. 2025, 1037, 182420. [Google Scholar] [CrossRef] [Scilit]
  243. Nazha, H.M.; Darwich, A.; Szabolcs, S.; Bognar, G. Chapter 34—Coating Materials for Artificial Knee Joint Components. In Cartilage Tissue and Knee Joint Biomechanics; Nochehdehi, A.R., Ed.; Academic Press: Cambridge, MA, USA, 2023; pp. 579–591. [Google Scholar]
  244. Fortas, G.; Ouir, S.; Manseri, A.; Djerir, W.; Smaili, F.; Gabouze, N.; Haine, N. Influence of deposition parameters on the electrodeposited ternary CoFeCu coatings. J. Mater. Sci. Mater. Electron. 2024, 35, 1462. [Google Scholar] [CrossRef] [Scilit]
  245. Ibañez, A.; Fatás, E. Mechanical and structural properties of electrodeposited copper and their relation with the electrodeposition parameters. Surf. Coat. Technol. 2005, 191, 7–16. [Google Scholar] [CrossRef] [Scilit]
  246. Kim, H.C.; Kim, M.J.; Choe, S.; Lim, T.; Park, K.J.; Kim, K.H.; Ahn, S.H.; Kim, S.-K.; Kim, J.J. Electrodeposition of Cu Films with Low Resistivity and Improved Hardness Using Additive Derivatization. J. Electrochem. Soc. 2014, 161, D749. [Google Scholar] [CrossRef] [Scilit]
  247. Khezri, R.; Motlagh, S.R.; Etesami, M.; Mohamad, A.A.; Pornprasertsuk, R.; Olaru, S.; Kheawhom, S. High current density charging of zinc-air flow batteries: Investigating the impact of flow rate and current density on zinc electrodeposition. Appl. Energy 2023, 348, 121564. [Google Scholar] [CrossRef] [Scilit]
  248. Wang, S.; Wang, J.W.; Tian, J.Y.; Yang, P.; He, Y.; Yang, C.Y.; Wang, H.F. Effect of Current Density on Growth Law of Manganese Electrodeposition. Russ. J. Electrochem. 2023, 59, 616–627. [Google Scholar] [CrossRef] [Scilit]
  249. Cho, Y.; Jiang, M.; Ahn, D.; Choi, W. Effect of Deposition Temperature on the Electrical Properties of Solid-Phase Crystallized Ge Thin Films. Electron. Mater. Lett. 2024, 20, 694–701. [Google Scholar] [CrossRef] [Scilit]
  250. Yeh, Y.-H.; Tan, Y.-F.; Huang, Y.-C.; Lin, C.C.; Wu, C.-W.; Zhang, Y.-C.; Lee, Y.-H.; Chang, T.-C.; Sze, S.M. Impact of deposition temperature on electrical properties of HZO-based FeRAM. J. Appl. Phys. 2024, 135, 064102. [Google Scholar] [CrossRef] [Scilit]
  251. Zhong, Z.; Lin, G.; Sheng, X.; Hu, T.; Wang, S.; Li, S.; Xia, H.; Cao, H.; Zhang, L. Roles and influencing mechanisms of Fe2+ and Lix984 in copper electrodeposition. Ionics 2024, 30, 7639–7651. [Google Scholar] [CrossRef] [Scilit]
  252. Sheng, X.; Lin, G.; Huang, Y.; Zhong, Z.; Wang, S.; Hu, T.; Li, S.; Liu, J.; Xia, H.; Cao, H.; et al. Enhanced Zinc Electrodeposition by Multi-Component Low-Concentration Organic Additives and Synergistic Mechanism. J. Sustain. Metall. 2025, 11, 1333–1347. [Google Scholar] [CrossRef] [Scilit]
  253. Zhang, Y.L.; Wang, Q.; Wang, D.T.; Zhang, L.; Kang, S.M.; Zhang, J.W. Effect of Current Density, Reaction Temperature and Deposition Time on the Electrodeposition of ZrB2 Coating. J. Mater. Eng. Perform. 2025, 34, 1016–1025. [Google Scholar] [CrossRef] [Scilit]
  254. Jia, H.; Lu, S.; Shin, S.H.R.; Sushko, M.L.; Tao, X.; Hummel, M.; Thallapally, P.K.; Liu, J.; Gu, Z. In situ anodic electrodeposition of two-dimensional conductive metal-organic framework@nickel foam for high-performance flexible supercapacitor. J. Power Sources 2022, 526, 231163. [Google Scholar] [CrossRef] [Scilit]
  255. Sen, S.; Chatterjee, A.; Ramakanth, D.; Singh, S.; Maji, P.K. Recent advances in cathodic electrodeposition coatings with special reference to resin materials: A comprehensive review. Prog. Org. Coat. 2024, 190, 108387. [Google Scholar] [CrossRef] [Scilit]
  256. Besra, L.; Liu, M. A review on fundamentals and applications of electrophoretic deposition (EPD). Prog. Mater. Sci. 2007, 52, 1–61. [Google Scholar] [CrossRef] [Scilit]
  257. Wei, M.; Ruys, A.; Milthorpe, B.; Sorrell, C.; Evans, J. Electrophoretic Deposition of Hydroxyapatite Coatings on Metal Substrates: A Nanoparticulate Dual-Coating Approach. J. Sol.-Gel Sci. Technol. 2001, 21, 39–48. [Google Scholar] [CrossRef] [Scilit]
  258. Du, C.; Heldbrant, D.; Pan, N. Preparation and preliminary property study of carbon nanotubes films by electrophoretic deposition. Mater. Lett. 2002, 57, 434–438. [Google Scholar] [CrossRef] [Scilit]
  259. Sridhar, T.M.; Mudali, U.K. Development of bioactive hydroxyapatite coatings on Type 316L stainless steel by electrophoretic deposition for orthopaedic applications. Trans. Indian Inst. Met. 2003, 56, 221–230. [Google Scholar]
  260. Yum, J.-H.; Seo, S.-Y.; Lee, S.; Sung, Y.-E. Y3Al5O12: Ce0.05 Phosphor Coatings on Gallium Nitride for White Light Emitting Diodes. J. Electrochem. Soc. 2003, 150, H47. [Google Scholar] [CrossRef] [Scilit]
  261. Hayashi, K.; Furuya, N. Preparation of Gas Diffusion Electrodes by Electrophoretic Deposition. J. Electrochem. Soc. 2004, 151, A354. [Google Scholar] [CrossRef] [Scilit]
  262. Altzoumailis, A.F.; Argyropoulou, R.; Ochsenkühn-Petropoulou, M.T.; Ochsenkühn, K.-M. Superconducting coatings of MgB2 prepared by electrophoretic deposition. Anal. Bioanal. Chem. 2004, 379, 792–795. [Google Scholar] [CrossRef] [Scilit]
  263. Kim, M.J.; Cho, S.K.; Koo, H.-C.; Lim, T.; Park, K.J.; Kim, J.J. Pulse Electrodeposition for Improving Electrical Properties of Cu Thin Film. J. Electrochem. Soc. 2010, 157, D564. [Google Scholar] [CrossRef] [Scilit]
  264. Dela Pena, E.M.; Roy, S. Electrodeposited copper using direct and pulse currents from electrolytes containing low concentration of additives. Surf. Coat. Technol. 2018, 339, 101–110. [Google Scholar] [CrossRef] [Scilit]
  265. Safavi, M.S.; Walsh, F.C. The electrodeposition of particle-metal matrix composite coatings to meet tribological and corrosion challenges. Adv. Colloid Interface Sci. 2025, 343, 103584. [Google Scholar] [CrossRef] [Scilit]
  266. Hou, K.; Ger, M.; Wang, L.; Ke, S. The wear behaviour of electro-codeposited Ni–SiC composites. Wear 2002, 253, 994–1003. [Google Scholar] [CrossRef] [Scilit]
  267. Chen, L.; Wang, L.; Zeng, Z.; Zhang, J. Effect of surfactant on the electrodeposition and wear resistance of Ni–Al2O3 composite coatings. Mater. Sci. Eng. A 2006, 434, 319–325. [Google Scholar] [CrossRef] [Scilit]
  268. Guo, C.; Zuo, Y.; Zhao, X.; Zhao, J.; Xiong, J. Effects of surfactants on electrodeposition of nickel-carbon nanotubes composite coatings. Surf. Coat. Technol. 2008, 202, 3385–3390. [Google Scholar] [CrossRef] [Scilit]
  269. Sen, R.; Das, S.; Das, K. Effect of stirring rate on the microstructure and microhardness of Ni–CeO2 nanocomposite coating and investigation of the corrosion property. Surf. Coat. Technol. 2011, 205, 3847–3855. [Google Scholar] [CrossRef] [Scilit]
  270. Kılıç, F.; Gül, H.; Aslan, S.; Alp, A.; Akbulut, H. Effect of CTAB concentration in the electrolyte on the tribological properties of nanoparticle SiC reinforced Ni metal matrix composite (MMC) coatings produced by electrodeposition. Colloids Surf. A Physicochem. Eng. Asp. 2013, 419, 53–60. [Google Scholar] [CrossRef] [Scilit]
  271. Su, F.; Liu, C.; Huang, P. Ultrasound-assisted pulse electrodeposition and characterization of Co–W/MWCNTs nanocomposite coatings. Appl. Surf. Sci. 2014, 309, 200–208. [Google Scholar] [CrossRef] [Scilit]
  272. Adabi, M.; Amadeh, A. Effect of electrodeposition conditions on properties of Ni–Al composite coatings. Surf. Eng. 2015, 31, 650–658. [Google Scholar] [CrossRef] [Scilit]
  273. Kartal, M.; Uysal, M.; Gul, H.; Alp, A.; Akbulut, H. Effect of surfactant concentration in the electrolyte on the tribological properties of nickel-tungsten carbide composite coatings produced by pulse electro co-deposition. Appl. Surf. Sci. 2015, 354, 328–336. [Google Scholar] [CrossRef] [Scilit]
  274. Parhizkar, N.; Dolati, A.; Aghababazadeh, R.; Lalegani, Z. Electrochemical deposition of Ni–TiN nanocomposite coatings and the effect of sodium dodecyl sulphate surfactant on the coating properties. Bull. Mater. Sci. 2016, 39, 1021–1027. [Google Scholar] [CrossRef] [Scilit]
  275. Tozar, A.; Karahan, İ.H. Investigation of the mechanical properties of Ni-B/hBN composite coatings electrodeposited in presence of CTAB as the surfactant. Mater. Res. Express 2019, 6, 126598. [Google Scholar] [CrossRef] [Scilit]
  276. Tozar, A.; Karahan, İ.H. Effect of octylphenyl ether group nonionic surfactant on the electrodepositon of the hexagonal boron nitride reinforced Ni-B matrix composite coatings. Surf. Coat. Technol. 2020, 381, 125131. [Google Scholar] [CrossRef] [Scilit]
  277. Tozar, A. Investigating the hexadecylamine as a new nonionic surfactant candidate for electrodeposition of wear-resistant metal-matrix composites. Surf. Eng. 2020, 36, 990–999. [Google Scholar] [CrossRef] [Scilit]
  278. Yang, X.; Gao, Z.; Wang, X.; Hu, W. Effect of Surfactants on the Corrosion and Wear Performance of Zinc-Epoxy Powder Composite Coatings. Int. J. Electrochem. Sci. 2021, 16, 210753. [Google Scholar] [CrossRef] [Scilit]
  279. Doğan, F.; Duru, E.; Uysal, M.; Akbulut, H.; Aslan, S.; Gurbuz, K.; Topak, D.; Ozdemir, M.A.; Kuşçu, B.; Ekinci, Y.; et al. Structural, mechanical, and tribological studies of Ni-B-TiN composite coating: Effect of SDS concentration. J. Adhes. Sci. Technol. 2023, 37, 1010–1033. [Google Scholar] [CrossRef] [Scilit]
  280. Morrissey, R.J. Palladium and palladium-nickel alloy plating. Metal. Finish. 1999, 97, 291. [Google Scholar] [CrossRef] [Scilit]
  281. Giovanardi, R.; Orlando, G. Chromium electrodeposition from Cr(III) aqueous solutions. Surf. Coat. Technol. 2011, 205, 3947–3955. [Google Scholar] [CrossRef] [Scilit]
  282. Giurlani, W.; Zangari, G.; Gambinossi, F.; Passaponti, M.; Salvietti, E.; Di Benedetto, F.; Caporali, S.; Innocenti, M. Electroplating for Decorative Applications: Recent Trends in Research and Development. Coatings 2018, 8, 260. [Google Scholar] [CrossRef] [Scilit]
  283. Verrucchi, M.; Mazzoli, G.; Comparini, A.; Emanuele, R.; Bonechi, M.; Del Pace, I.; Giurlani, W.; Fontanesi, C.; Kowalik, R.; Innocenti, M. Electrodeposition of Sn-Ru Alloys by Using Direct, Pulsed, and Pulsed Reverse Current for Decorative Applications. Materials 2024, 17, 5326. [Google Scholar] [CrossRef] [Scilit]
  284. Bonechi, M.; Mariani, E.; Pelagatti, A.; Nunziati, P.; Giurlani, W.; Fontanesi, C.; Innocenti, M. Pulsed Current Electrodeposition for Decorative and Functional Applications. ECS Meet. Abstr. 2025, MA2025-01, 1428. [Google Scholar] [CrossRef] [Scilit]
  285. Ramya, Y.A.; Krupanidhi, Y.G. Enhancing aesthetics: Advances in electroplating for decorative applications. World J. Adv. Res. Rev. 2019, 1, 089. [Google Scholar] [CrossRef] [Scilit]
  286. Benner, H.L.; Wernlund, C.J. The High Efficiency Cyanide Copper Bath. Trans. Electrochem. Soc. 1941, 80, 355. [Google Scholar] [CrossRef] [Scilit]
  287. Stareck, J.E. Electrodeposition of Copper and Bath Therefor. U.S. Patent No. 2,250,556, 29 July 1941. [Google Scholar]
  288. Willis, W.J. Electrodeposition of Copper, Acidic Copper Electroplating Baths and Additives Therefor. U.S. Patent No. 4,347,108, 31 August 1982. [Google Scholar]
  289. Mariani, E.; Giurlani, W.; Verrucchi, M.; Dell’aQuila, V.; Nostro, P.L.; Innocenti, M. Pulse Electroplating of Gold-Nickel Alloys: Morphological and Aesthetic Improvement Compared to DC. J. Electrochem. Soc. 2024, 171, 012504. [Google Scholar] [CrossRef] [Scilit]
  290. Mariani, E.; Giurlani, W.; Bonechi, M.; Dell’aQuila, V.; Innocenti, M. A systematic study of pulse and pulse reverse plating on acid copper bath for decorative and functional applications. Sci. Rep. 2022, 12, 18175. [Google Scholar] [CrossRef] [Scilit]
  291. Coey, J.M.D.; Hinds, G. Magnetic electrodeposition. J. Alloys Compd. 2001, 326, 238–245. [Google Scholar] [CrossRef] [Scilit]
  292. Rasmussen, F.; Ravnkilde, J.; Tang, P.; Hansen, O.; Bouwstra, S. Electroplating and characterization of cobalt–nickel–iron and nickel–iron for magnetic microsystems applications. Sens. Actuators A Phys. 2001, 92, 242–248. [Google Scholar] [CrossRef] [Scilit]
  293. Msellak, K.; Chopart, J.-P.; Jbara, O.; Aaboubi, O.; Amblard, J. Magnetic field effects on Ni–Fe alloys codeposition. J. Magn. Magn. Mater. 2004, 281, 295–304. [Google Scholar] [CrossRef]
  294. Jiang, Y.; Yao, S.; Zhang, W. [Ni80Fe20/Cu/Co/Cu] spin-valve multilayers electrodeposited on NiFe buffer layers. Thin Solid Films 2008, 516, 3210–3216. [Google Scholar] [CrossRef] [Scilit]
  295. Sun, X.; Zheng, Y.; Li, Z.; Yu, M.; Yuan, Q.; Li, X.; Zhang, H. Design and fabrication of flexible parylene-based inductors with electroplated NiFe magnetic core for wireless power transmission system. In Proceedings of the 2012 7th IEEE International Conference on Nano/Micro Engineered and Molecular Systems (NEMS), Kyoto, Japan, 5–8 March 2012. [Google Scholar]
  296. Torabinejad, V.; Aliofkhazraei, M.; Assareh, S.; Allahyarzadeh, M.; Rouhaghdam, A.S. Electrodeposition of Ni-Fe alloys, composites, and nano coatings—A review. J. Alloys Compd. 2017, 691, 841–859. [Google Scholar] [CrossRef] [Scilit]
  297. Deligianni, H. Electrodeposition and Microelectronics. Electrochem. Soc. Interface 2006, 15, 33. [Google Scholar] [CrossRef] [Scilit]
  298. Zangari, G. Electrodeposition of Alloys and Compounds in the Era of Microelectronics and Energy Conversion Technology. Coatings 2015, 5, 195–218. [Google Scholar] [CrossRef] [Scilit]
  299. Park, S.W.; Eom, H.W.; Kim, M.J.; Kim, J.J. Electrodeposition of Nano-Twinned Cu and their Applications in Electronics. J. Electrochem. Soc. 2022, 169, 112503. [Google Scholar] [CrossRef] [Scilit]
  300. Suzdaltsev, A. Silicon Electrodeposition for Microelectronics and Distributed Energy: A Mini-Review. Electrochem 2022, 3, 760–768. [Google Scholar] [CrossRef] [Scilit]
  301. Kotelnikova, A.; Kadyrzhanov, K.; Fedkin, V.; Shlimas, D.; Zubar, T.; Borgekov, D.; Zdorovets, M.; Trukhanov, A. Electrodeposited NiFe films for electronic applications: Structure and magnetic properties. J. Mater. Sci. Mater. Electron. 2024, 35, 2160. [Google Scholar] [CrossRef] [Scilit]
  302. Chan, T.-C.; Lin, Y.-M.; Tsai, H.-W.; Wang, Z.M.; Liao, C.-N.; Chueh, Y.-L. Growth of large-scale nanotwinned Cu nanowire arrays from anodic aluminum oxide membrane by electrochemical deposition process: Controllable nanotwin density and growth orientation with enhanced electrical endurance performance. Nanoscale 2014, 6, 7332–7338. [Google Scholar] [CrossRef] [Scilit]
  303. Park, S.; Seo, S.; Jin, S.; Yoo, B. The Effects of Bath Temperature on the Formation of Nanotwin in Electrodeposited Cu. J. Nanosci. Nanotechnol. 2016, 16, 11303–11307. [Google Scholar] [CrossRef] [Scilit]
  304. Behroozfar, A.; Daryadel, S.; Morsali, S.R.; Moreno, S.; Baniasadi, M.; Bernal, R.A.; Minary-Jolandan, M. Microscale 3D Printing of Nanotwinned Copper. Adv. Mater. 2018, 30, 1705107. [Google Scholar] [CrossRef] [Scilit]
  305. Cheng, Z.; Zhou, H.; Lu, Q.; Gao, H.; Lu, L. Extra strengthening and work hardening in gradient nanotwinned metals. Science 2018, 362, eaau1925. [Google Scholar] [CrossRef] [Scilit]
  306. Sun, F.-L.; Gao, L.-Y.; Liu, Z.-Q.; Zhang, H.; Sugahara, T.; Nagao, S.; Suganuma, K. Electrodeposition and growth mechanism of preferentially orientated nanotwinned Cu on silicon wafer substrate. J. Mater. Sci. Technol. 2018, 34, 1885–1890. [Google Scholar] [CrossRef] [Scilit]
  307. Li, S.; Zhu, Q.; Zheng, B.; Yuan, J.; Wang, X. Nano-scale twinned Cu with ultrahigh strength prepared by direct current electrodeposition. Mater. Sci. Eng. A 2019, 758, 1–6. [Google Scholar] [CrossRef] [Scilit]
  308. Tseng, C.-H.; Chen, C. Growth of Highly (111)-Oriented Nanotwinned Cu with the Addition of Sulfuric Acid in CuSO4 Based Electrolyte. Cryst. Growth Des. 2019, 19, 81–89. [Google Scholar] [CrossRef] [Scilit]
  309. Bai, Y.; Hu, H.; Ling, H.; Hang, T.; Hu, A.; Wu, Y.; Li, M. Communication—Fabrication of Vertical Nanotwinned Copper with (220) Texture by Direct Current Electrodeposition. J. Electrochem. Soc. 2021, 168, 082506. [Google Scholar] [CrossRef] [Scilit]
  310. Chen, H.-Y.; Huang, Y.-S.; Liao, C.-N. Electrodeposition and Growth Mechanism of Nanotwinned Copper in High Aspect-Ratio via Structures. J. Electrochem. Soc. 2021, 168, 102503. [Google Scholar] [CrossRef] [Scilit]
  311. Dong, M.; Chen, P.; Hang, T.; Li, M. Nanotwinned copper micro-cone array fabricated by pulse electrodeposition for low-temperature bonding. Mater. Lett. 2021, 290, 129470. [Google Scholar] [CrossRef] [Scilit]
  312. Zhan, X.; Lian, J.; Li, H.; Wang, X.; Zhou, J.; Trieu, K.; Zhang, X. Preparation of highly (111) textured nanotwinned copper by medium-frequency pulsed electrodeposition in an additive-free electrolyte. Electrochim. Acta 2021, 365, 137391. [Google Scholar] [CrossRef] [Scilit]
  313. Yan, K.; Huang, P.; Xia, M.; Xie, X.; Sun, L.; Lei, W.; Wang, F. An efficient Two-Chamber Electrodeposition-Electrodialysis combination craft for nickel recovery and phosphorus removal from spent electroless nickel plating bath. Sep. Purif. Technol. 2022, 295, 121283. [Google Scholar] [CrossRef] [Scilit]
  314. Li, S.; Dai, M.; Ali, I.; Bian, H.; Peng, C. Recovery of nickel from actual electroplating wastewater by integrated electrodeposition with adsorption pretreatment technique. Process Saf. Environ. Prot. 2023, 172, 417–424. [Google Scholar] [CrossRef] [Scilit]
  315. Li, X.; Ma, B.; Wang, C.; Hu, D.; Lü, Y.; Chen, Y. Recycling and recovery of spent copper—Indium—Gallium—Diselenide (CIGS) solar cells: A review. Int. J. Miner. Metall. Mater. 2023, 30, 989–1002. [Google Scholar] [CrossRef] [Scilit]
  316. Li, Y.; Wei, X.; Liu, H.; Sun, Y. Flotation-assisted electrodeposition process to recover copper from waste printed circuit boards. Chem. Eng. J. 2024, 497, 154747. [Google Scholar] [CrossRef] [Scilit]
  317. Wang, D.; Liang, Y.; Zeng, Y.; Liu, C.; Zhan, C.; Chen, P.; Song, S.; Jia, F. Highly selective recovery of gold and silver from E-waste via stepwise electrodeposition directly from the pregnant leaching solution enabled by the MoS2 cathode. J. Hazard. Mater. 2024, 465, 133430. [Google Scholar] [CrossRef] [Scilit]
  318. Karali, B.K.; Das, S.; Behera, G.; Mallik, M. Synthesis of hydroxyapatite nanocomposite coating by electrodeposition route: A state of the art review. Can. Metall. Q. 2025, 64, 1839–1853. [Google Scholar] [CrossRef] [Scilit]
  319. Kiey, S.A.A.; Mohamed, K.R.; Meguid, E.A.A. Smart Surfaces: A Survey of Electrodeposited Hydroxyapatite for Enhanced Biomedical Performance. ChemistrySelect 2026, 11, e07158. [Google Scholar] [CrossRef] [Scilit]
  320. Bartmański, M.; Wekwejt, M.; Urbanowicz, K.; Mielewczyk-Gryń, A.; Gajowiec, G.; Pałubicka, A.; Michno, A.; Serafin, P.K.; Koszałka, P. Chitosan-Nanogold and Chitosan-Nanozinc Electrodeposited Coatings for Biomedical Applications. J. Biomed. Mater. Res. Part B Appl. Biomater. 2025, 113, e35571. [Google Scholar] [CrossRef] [Scilit]
  321. Payampur, M.H.; Azimi, D.; Milligan, W.W.; Razzaghi, M.; Bakhsheshi-Rad, H.R.; Drelich, J.W. Electrophoretic deposition of chitosan-based coatings on magnesium alloys for implant applications: A review. Emergent Mater. 2026, 9, 100. [Google Scholar] [CrossRef] [Scilit]
  322. Zeng, Y.; Pei, X.; Yang, S.; Qin, H.; Cai, H.; Hu, S.; Sui, L.; Wan, Q.; Wang, J. Graphene oxide/hydroxyapatite composite coatings fabricated by electrochemical deposition. Surf. Coat. Technol. 2016, 286, 72–79. [Google Scholar] [CrossRef] [Scilit]
  323. Fathyunes, L.; Khalil-Allafi, J. Characterization and corrosion behavior of graphene oxide-hydroxyapatite composite coating applied by ultrasound-assisted pulse electrodeposition. Ceram. Int. 2017, 43, 13885–13894. [Google Scholar] [CrossRef] [Scilit]
  324. Fathyunes, L.; Khalil-Allafi, J. The effect of graphene oxide on surface features, biological performance and bio-stability of calcium phosphate coating applied by pulse electrochemical deposition. Appl. Surf. Sci. 2018, 437, 122–135. [Google Scholar] [CrossRef] [Scilit]
  325. Bartmański, M. An Assessment of Fabrication, Properties, and Medical Applications of Chitosan–Nanometal Coatings. Materials 2025, 18, 5322. [Google Scholar] [CrossRef] [Scilit]
  326. Chen, S.; Liang, C.; Li, P.; Liu, C.; Zeng, X.; Xiong, X.; Ni, X. Polydopamine/polyvinyl alcohol/graphene oxide transition layer for enhancing adhesive performance of HA coating on Cf/C composites prepared by hydrothermal electrodeposition/hydrothermal treatment. J. Mater. Sci. Mater. Med. 2025, 36, 67. [Google Scholar] [CrossRef] [Scilit]
  327. Phogat, D.; Awasthi, S. Material and technique fundamentals of nano-hydroxyapatite coatings towards biofunctionalization: A review. Biomed. Mater. 2025, 20, 022004. [Google Scholar] [CrossRef] [Scilit]
  328. Safavi, M.S.; Khalil-Allafi, J.; Walsh, F.C.; Visai, L. The effects of current density on the properties of HAp-Nb2O5 films electrodeposited by pulsed current. Trans. IMF 2025, 103, 21–25. [Google Scholar] [CrossRef] [Scilit]
  329. Redepenning, J.; Venkataraman, G.; Chen, J.; Stafford, N. Electrochemical preparation of chitosan/hydroxyapatite composite coatings on titanium substrates. J. Biomed. Mater. Res. Part A 2003, 66A, 411–416. [Google Scholar] [CrossRef] [Scilit]
  330. Qiu, D.; Yang, L.; Yin, Y.; Wang, A. Preparation and characterization of hydroxyapatite/titania composite coating on NiTi alloy by electrochemical deposition. Surf. Coat. Technol. 2011, 205, 3280–3284. [Google Scholar] [CrossRef] [Scilit]
  331. Isa, N.N.C.; Mohd, Y.; Yury, N. Electrochemical Deposition and Characterization of Hydroxyapatite (HAp) on Titanium Substrate. APCBEE Procedia 2012, 3, 46–52. [Google Scholar] [CrossRef] [Scilit]
  332. Ahmadi, S.; Mohammadi, I.; Sadrnezhaad, S.K. Hydroxyapatite based and anodic Titania nanotube biocomposite coatings: Fabrication, characterization and electrochemical behavior. Surf. Coat. Technol. 2016, 287, 67–75. [Google Scholar] [CrossRef] [Scilit]
  333. Park, K.H.; Kim, S.-J.; Hwang, M.-J.; Song, H.-J.; Park, Y.-J. Pulse electrodeposition of hydroxyapatite/chitosan coatings on titanium substrate for dental implant. Colloid Polym. Sci. 2017, 295, 1843–1849. [Google Scholar] [CrossRef] [Scilit]
  334. Aboudzadeh, N.; Dehghanian, C.; Shokrgozar, M.A. Effect of electrodeposition parameters and substrate on morphology of Si-HA coating. Surf. Coat. Technol. 2019, 375, 341–351. [Google Scholar] [CrossRef] [Scilit]
  335. Li, T.-T.; Ling, L.; Lin, M.-C.; Peng, H.-K.; Ren, H.-T.; Lou, C.-W.; Lin, J.-H. Recent advances in multifunctional hydroxyapatite coating by electrochemical deposition. J. Mater. Sci. 2020, 55, 6352–6374. [Google Scholar] [CrossRef] [Scilit]
  336. Lu, M.; Chen, H.; Yuan, B.; Zhou, Y.; Min, L.; Xiao, Z.; Zhu, X.; Tu, C.; Zhang, X. Electrochemical Deposition of Nanostructured Hydroxyapatite Coating on Titanium with Enhanced Early Stage Osteogenic Activity and Osseointegration. Int. J. Nanomed. 2020, 15, 6605–6618. [Google Scholar] [CrossRef] [Scilit]
  337. Mišković-Stanković, V.; Stevanović, M.; Atanackovic, T.M. Bioceramic coatings electrodeposited on titanium surface aimed for medical applications. J. Solid State Electrochem. 2025, 30, 2265–2276. [Google Scholar] [CrossRef] [Scilit]
  338. Mohammadi Kahnamouei, S.; Safavi, M.S.; Khalil-Allaf, J. Pulsed electrodeposition and characterization of HAp-Ta2O5 composite coating on NiTi for orthopedic applications. J. Mater. Res. Technol. 2026, 37, 1–11. [Google Scholar] [CrossRef] [Scilit]
  339. Sierra-Herrera, D.; Montañez, N.; Sandoval-Amador, A.; Peña-Ballesteros, D.; Blanco, S. Tuning phase composition and morphology of calcium phosphate coatings on Ti6Al4V by pulse electrodeposition. Appl. Phys. A 2026, 132, 247. [Google Scholar] [CrossRef] [Scilit]
  340. Stango, A.X.; Vijayalakshmi, U. Electrochemically grown functionalized -Multi-walled carbon nanotubes/hydroxyapatite hybrids on surgical grade 316L SS with enhanced corrosion resistance and bioactivity. Colloids Surf. B Biointerfaces 2018, 171, 186–196. [Google Scholar] [CrossRef] [Scilit]
  341. Poorraeisi, M.; Afshar, A. The study of electrodeposition of hydroxyapatite-ZrO2-TiO2 nanocomposite coatings on 316 stainless steel. Surf. Coat. Technol. 2018, 339, 199–207. [Google Scholar] [CrossRef] [Scilit]
  342. Khazeni, D.; Saremi, M.; Soltani, R. Development of HA-CNTs composite coating on AZ31 magnesium alloy by cathodic electrodeposition. Part 1: Microstructural and mechanical characterization. Ceram. Int. 2019, 45, 11174–11185. [Google Scholar] [CrossRef] [Scilit]
  343. Poorraeisi, M.; Afshar, A. Synthesizing and comparing HA–TiO2 and HA–ZrO2 nanocomposite coatings on 316 stainless steel. SN Appl. Sci. 2019, 1, 155. [Google Scholar] [CrossRef] [Scilit]
  344. Saberi, A.; Bakhsheshi-Rad, H.R.; Abazari, S.; Ismail, A.F.; Sharif, S.; Ramakrishna, S.; Daroonparvar, M.; Berto, F. A Comprehensive Review on Surface Modifications of Biodegradable Magnesium-Based Implant Alloy: Polymer Coatings Opportunities and Challenges. Coatings 2021, 11, 747. [Google Scholar] [CrossRef] [Scilit]
  345. Mohammadsadegh, A.; Allahkaram, S.R.; Gharagozlou, M. Electrophoretic deposition of chitosan/gelatin/hydroxyapatite nanocomposite coatings on 316 L stainless steel for biomedical applications. Biomed. Mater. 2025, 20, 015020. [Google Scholar] [CrossRef] [Scilit]
  346. Prasad, P.S.; Byram, P.K.; Hadem, H.; Hazra, C.; Sen, R.; Das, S.; Das, K. A comparative evaluation of green surfactant-assisted calcium phosphate (CaP) coatings developed through electrodeposition and biomimetic routes. Colloids Surf. A Physicochem. Eng. Asp. 2025, 707, 135889. [Google Scholar] [CrossRef] [Scilit]
  347. Priyadarshini, S.; Bhat, R.S.; Bindu, A.G.; Nagaraj, P.; Rekha, P.D. Electrodeposition of Anticorrosive and Antimicrobial Cu-Mn Coating on Mild Steel Using Single Bath Technique. J. Mater. Eng. Perform. 2026, 35, 8511–8524. [Google Scholar] [CrossRef] [Scilit]
  348. Souri, A.; Shanaghi, A.; Shahsavand, F.; Naseri, M. Engineering hydroxyapatite-silver nanocomposite coating on Ti–6Al–4V alloy with bio-corrosion and antibacterial performances for orthopedic implant applications. J. Mater. Res. Technol. 2026, 40, 2624–2632. [Google Scholar] [CrossRef] [Scilit]
  349. Chiorcea-Paquim, A.-M.; Brett, C.M.A. Electrodeposition in deep eutectic solvents: Perspectives towards advanced corrosion protection. Appl. Mater. Today 2025, 44, 102746. [Google Scholar] [CrossRef] [Scilit]
  350. An, W.; Xue, R.; Yuan, P.; Gao, L.; Xu, Q.; Hu, D.; Ma, J. Design strategies of MXene-based coatings towards multifunctional application. Surf. Interfaces 2024, 46, 104083. [Google Scholar] [CrossRef] [Scilit]
  351. Zhang, Y.; Yin, Y.; Li, J.; Yang, F.; Meng, L.; Cai, Y.; Wu, J.; Guo, F.; Wang, W. MXene-based anti-corrosive coatings: From physical barrier to active corrosion protection. Prog. Org. Coat. 2025, 204, 109225. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.